Roll core and battery

By using a combined design of the first tape and the second tape in the battery roll core, the structural rupture problem caused by the expansion of the electrode assembly during circulation is solved, and the battery energy density and safety performance are improved.

CN222106799UActive Publication Date: 2024-12-03ZHUHAI COSMX BATTERY CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202420422081.3
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2024-03-05
Publication Date
2024-12-03
Estimated Expiration
2034-03-05

AI Technical Summary

Technical Problem

During the cyclic charging and discharging of existing batteries, the expansion of the electrode material causes the battery cell structure to rupture, and increasing the thickness of the protective rubber layer is not conducive to improving the energy density. How to prevent the core from rupturing and deformation after multiple cycles is an urgent problem to be solved.

Method used

Using a core design including an electrode assembly, a first adhesive paper and a second adhesive paper, the first adhesive paper is provided in the arc-bending section of the electrode assembly and the second adhesive paper is provided on the electrode ear to extend to the first The arc-bending section forms a flexible buffer body to prevent corrosion and loosening of the electrolyte and reduce the risk of active materials cutting through the membrane.

Benefits of technology

Effectively prevent electrolyte corrosion and electrode assembly loosening, reduce the risk of lithium extraction, reduce the damage to the aluminium plastic membrane, and improve the energy density and safety performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN222106799U_ABST
    Figure CN222106799U_ABST
Patent Text Reader

Abstract

The utility model provides a roll core and a battery. The roll core comprises an electrode assembly, first gummed paper and second gummed paper, the electrode assembly comprises a straight section, a first arc bending section and a second arc bending section, wherein the first arc bending section and the second arc bending section are located at the two ends of the straight section respectively. A tab is arranged in the straight section, and the first arc bending section is far away from the winding ending end of the electrode assembly in the winding direction; the first gummed paper is arranged on the outermost side of the first arc bending section, the orthographic projection of the second gummed paper in the thickness direction of the roll core covers the tab, and the second gummed paper extends to the first arc bending section; wherein the first gummed paper and the second gummed paper both exceed the edge of the electrode assembly in the first direction, and the first direction is the width direction of the pole piece. And through cooperation of the first gummed paper and the second gummed paper, the problem that the roll core is prone to breakage and deformation after multiple times of circulation can be solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model belongs to the technical field of batteries, and in particular relates to a winding core and a battery. Background Art

[0002] With the rapid development of new energy vehicles and large-scale energy storage industries, higher requirements are placed on the safety performance and energy density of batteries. At present, the improvement of energy density is mostly achieved by reducing the gap between the aluminum-plastic film and the battery cell. However, during the battery's cyclic charge and discharge process, as the number of charging times increases, heat accumulates in the battery, the electrode material expands, the thickness of the battery cell expands, and especially the expansion and extension of the negative electrode sheet will cause the battery cell structure to rupture. If the battery cell is loosely packaged with aluminum-plastic film, friction and vibration will occur between the battery cell and the aluminum-plastic film during transportation, causing deformation of the battery cell structure.

[0003] At present, most of the winding core structures are fixed by coating the outer periphery of the electrode assembly with a protective rubber layer. However, the protective rubber layer can only protect the outer periphery of the electrode assembly, and the internal structure of the electrode assembly cannot be taken into account. In addition, the provision of the protective rubber layer increases the thickness of the battery cell, which is not conducive to improving the energy density of the battery. Therefore, how to prevent the winding core from being easily broken and deformed after multiple cycles is a technical problem that needs to be solved in this field. Utility Model Content

[0004] The utility model provides a winding core, which is mainly used to solve the problem that the winding core in the prior art is easy to break and deform after multiple cycles.

[0005] The utility model provides a battery, which comprises the winding core, so that a flexible buffer body is formed between the electrode assembly and the aluminum-plastic film, thereby improving both the energy density and the safety performance of the battery.

[0006] According to a first aspect of the utility model, a winding core is provided, which comprises an electrode assembly, a first adhesive tape and a second adhesive tape; the electrode assembly comprises a straight section and a first arc bending section and a second arc bending section respectively located at two ends of the straight section; a pole ear is arranged in the straight section, and the winding tail end of the electrode assembly is located in the second arc bending section; the first adhesive tape is arranged at the outermost side of the first arc bending section, the second adhesive tape covers the pole ear in the orthographic projection along the thickness direction of the winding core, and the second adhesive tape extends to the first arc bending section; wherein, the first adhesive tape and the second adhesive tape both exceed the edge of the electrode assembly in the first direction, and the first direction is the width direction of the pole piece.

[0007] The winding core as described above, wherein, along the winding center of the winding core pointing to the outer side of the winding core, the winding core includes a plurality of folded pole pieces, and the pole ear is arranged on the pole piece between the first quarter folded pole piece and the second quarter folded pole piece.

[0008] The winding core as described above, wherein the dimension of the first adhesive tape extending beyond the edge of the electrode assembly in the first direction is A, and the dimension of the second adhesive tape extending beyond the edge of the electrode assembly in the first direction is B; A and B satisfy the following relationship: 0≤BA≤2mm, 0<A≤3mm, 0<B≤3mm.

[0009] In the battery cell as described above, the spacing distance between the orthographic projection of the first adhesive tape on the first plane and the orthographic projection of the electrode tab on the first plane is J, J satisfies 0<J<60mm, and the first plane is a plane parallel to the straight section in the electrode assembly.

[0010] The battery cell as described above, wherein the extended dimension of the first adhesive tape is E, the thickness of the battery cell is H, and the maximum dimension in the second direction between the end of the pole ear closest to the first arc bending section and the side of the first adhesive tape away from the first arc bending section is F; wherein the second direction is perpendicular to the first direction; E, H and F satisfy the following relationship: 2F+(π-1)×H>E>π×H.

[0011] The battery cell as described above, wherein the electrode assembly is formed by stacking and winding a negative electrode sheet, a separator and a positive electrode sheet; the negative electrode sheet at least includes a negative electrode collector and a negative electrode active material layer arranged on at least one functional surface of the negative electrode collector; wherein the tensile strength s of the negative electrode collector in the length direction satisfies 50MPa≤s≤500MPa.

[0012] In the battery cell as described above, a first groove is provided on the negative electrode active material layer at least in the first arc bending section, and the depth of the first groove is not greater than the thickness of the negative electrode active material layer.

[0013] In the battery cell as described above, a first groove is provided on the negative electrode active material layer of the straight section, and the first groove is a strip-shaped groove or a dot-shaped groove.

[0014] The battery cell as described above, wherein the first groove is in the shape of a strip on the side of the negative electrode active material layer away from the negative electrode current collector, and there are multiple first grooves; the multiple first grooves are arranged at intervals along the length direction of the negative electrode current collector, and each first groove extends along the width direction of the negative electrode current collector; the depression size of the first groove in the thickness direction of the negative electrode current collector is h, and the size of the first groove in the length direction of the negative electrode current collector is L, both in units of μm; wherein h, L and s satisfy the following relationship: 0.03MPa / μm 2 ≤s / (h×L)≤0.75MPa / μm 2 .

[0015] The battery cell as described above, wherein, at the innermost side of the electrode assembly, the negative electrode sheet comprises a first negative electrode straight portion located in the straight section, a second negative electrode straight portion and a first negative electrode bent portion located in the second arc bent section; the first negative electrode straight portion, the first negative electrode bent portion and the second negative electrode straight portion are connected in sequence; the positive electrode sheet comprises a first positive electrode straight portion located in the straight section; the first positive electrode straight portion is located on the outside of the second negative electrode straight portion; the maximum dimension in the second direction between the head of the negative electrode active material layer on the first negative electrode straight portion and the first negative electrode bent portion is m1, and the maximum dimension in the second direction between the head of the positive electrode active material layer on the first positive electrode straight portion and the first negative electrode bent portion is m2, wherein 0<m1≤m2.

[0016] The battery cell as described above, wherein, at the outermost side of the electrode assembly, the positive electrode sheet includes a positive electrode single-sided empty foil area and a positive electrode double-sided empty foil area partially located in the second arc bending section, and the positive electrode double-sided empty foil area is located on the outside of the positive electrode single-sided empty foil area; the surface of the positive electrode single-sided empty foil area is provided with a first termination glue; the first termination glue exceeds the edge of the electrode assembly in the first direction, and the first termination glue extends out of the edge of the winding tail end in the second direction.

[0017] As described above, the size of the orthographic projection of the first termination glue on the first plane in the second direction is P, the size of the battery cell in the second direction is W, and P and W satisfy the following relationship: P = (0.5 ~ 1) W, wherein 10mm < P < 40mm.

[0018] In the battery cell as described above, a second termination glue is provided on a surface of the positive electrode double-sided empty foil area close to the positive electrode single-sided empty foil area; and the second termination glue exceeds the edge of the electrode assembly in the first direction.

[0019] The battery cell as described above, wherein a hot melt adhesive is provided on the outermost side of the tail end of the electrode assembly, a portion of the hot melt adhesive is located on the surface of the positive electrode double-sided empty foil area away from the positive electrode single-sided empty foil area, and the other portion is located on the positive electrode single-sided empty foil area; the orthographic projection of the first termination adhesive on the first plane covers the orthographic projection of the hot melt adhesive on the first plane; the ratio of the orthographic projection area of ​​the hot melt adhesive on the first plane to the orthographic projection area of ​​the battery cell on the first plane is G, 30%<G<70%.

[0020] The battery cell as described above, wherein a second groove is provided on the active material layer arranged opposite to the electrode ear; the depth of the second groove is not greater than the thickness of the active material layer, a third adhesive tape is provided on the second groove, and the orthographic projection of the third adhesive tape on the first plane is flush with the orthographic projection of the second groove on the first plane; the following relationship is satisfied: the thickness of the single-layer active material layer > the depth of the second groove ≥ the sum of the thicknesses of the second adhesive tape, the third adhesive tape and the hot melt adhesive.

[0021] The battery cell as described above, wherein the negative electrode active material layer includes graphite-doped silicon-carbon material, wherein the doping amount of the silicon-carbon material is K, 1%≤K≤30%; the particle size of the silicon-carbon material is D1; ​​h, L, and D1 satisfy the following relationship: L≥2D1, 100μm≥L≥50μm, h≥D1, 20μm≥L≥10μm.

[0022] A second aspect of the present invention provides a battery, comprising the battery cell and an aluminum-plastic film as described in the first aspect, wherein the aluminum-plastic film encloses a receiving cavity, and the battery cell is located in the receiving cavity.

[0023] The implementation of the utility model has at least the following beneficial effects:

[0024] The utility model can effectively prevent the electrolyte from corroding the outermost aluminum layer by arranging the first adhesive tape on the outermost side of the first arc bending section, thereby causing the aluminum layer of the arc section to break first under the action of stress, and even if the aluminum layer of the arc section breaks, the first adhesive tape can also effectively connect the two sides of the aluminum layer at the broken part of the arc section of the outermost aluminum layer, effectively avoiding the loosening of the winding core; in addition, since the second adhesive tape is arranged on the pole ear and extends to the first arc bending section, when the outermost side of the first arc bending section of the winding core breaks and causes the inside of the winding core to loosen, the second adhesive tape can, on the one hand, effectively offset the gap formed by the loosening under the action of its own elastic deformation, reduce the loose displacement of the arc section near the pole ear groove, thereby reducing the displacement causing the active material particles in the area to scratch the diaphragm, and on the other hand, the second adhesive tape covers the active material in the arc section, which further reduces the probability of the active material particles in the area scratching the diaphragm and reduces the risk of lithium precipitation. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a schematic diagram of the cross-sectional structure of a winding core in one embodiment of the utility model;

[0026] Figure 2 yes Figure 1 A partial enlarged view of the second adhesive tape in the reel core;

[0027] Figure 3 is a schematic diagram of the cross-sectional structure of a winding core in another embodiment of the present invention;

[0028] Figure 4 yes Figure 3 A partial enlarged view of the second adhesive tape in the reel core;

[0029] Figure 5 It is a schematic diagram of the partial cross-sectional structure of the innermost side of the electrode assembly in one embodiment of the utility model;

[0030] Figure 6 is a top view of the winding end of the winding core in one embodiment of the utility model;

[0031] Figure 7 It is a schematic diagram of a partial cross-sectional structure of a pole ear in an electrode assembly in one embodiment of the utility model;

[0032] Figure 8 is a schematic diagram of the cross-sectional structure of a winding core in another embodiment of the present invention;

[0033] Fig. 9 It is a schematic diagram of the top view of the structure of the negative electrode sheet in the electrode assembly before winding in one embodiment of the utility model;

[0034] Fig.10 It is a schematic diagram of the side view structure of the negative electrode sheet in the electrode assembly before winding in one embodiment of the utility model.

[0035] Description of reference numerals:

[0036] 1-electrode assembly; 2-first adhesive tape; 3-second adhesive tape; 4-first termination adhesive; 5-second termination adhesive; 41-hot melt adhesive; 6-third adhesive tape;

[0037] 11-straight section; 12-first arc bending section; 13-second arc bending section;

[0038] 101-ear; 102-positive electrode sheet; 103-negative electrode sheet; 104-diaphragm;

[0039] 1031 - negative electrode current collector; 1032 - negative electrode active material layer; 1033 - first groove; 1034 - second groove;

[0040] 1001 - first negative electrode straight portion; 1002 - first negative electrode bent portion; 1003 - second negative electrode straight portion; 1004 - first positive electrode straight portion; 1005 - single-sided empty foil area of ​​the positive electrode; 1006 - double-sided empty foil area of ​​the positive electrode; 1007 - winding end. DETAILED DESCRIPTION

[0041] In order to make the purpose, technical solution and advantages of the utility model clearer, the technical solution in the embodiment of the utility model will be clearly and completely described below in combination with the embodiment of the utility model. Obviously, the described embodiment is a part of the embodiment of the utility model, not all the embodiments. Based on the embodiment of the utility model, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the utility model.

[0042] Figures 1 to 10 It should be noted that X is the first direction, which is also the width direction of the electrode assembly and the width direction of the negative electrode sheet before winding; Y is the second direction, which is also the length direction of the electrode assembly and the length direction of the negative electrode sheet before winding; Z is the third direction, which is also the thickness direction of the electrode assembly and the thickness direction of the negative electrode sheet before winding.

[0043] It should be noted that the battery cell structure provided in the embodiment of the present application is preferably applicable to lithium-ion batteries; of course, it is also applicable to wound battery cells such as sodium-ion batteries, and no excessive limitations are made here.

[0044] It should be noted that during the winding process of the core, in order to ensure the tightness of each film layer inside it, it is necessary to tighten the positive electrode sheet, the diaphragm and the negative electrode sheet during the winding process, and as the winding radius increases, the stress of the arc segment of the film layer closer to the outside is more concentrated. The core in the embodiment of the present application is preferably an aluminum foil outer package of the positive electrode sheet, that is, the outermost layer of the core is aluminum, and as the number of cycles of the core increases, the electrolyte will gradually corrode the exposed outermost aluminum layer, and because the stress of the outermost arc segment of the core is the largest, the outermost aluminum layer of the core is prone to be corroded and broken first under the action of stress.

[0045] In addition, since the winding core in the embodiment of the present application preferably adopts a lug center structure, that is, part of the active material is removed at the edge of the active layer located in the middle of the positive and negative electrodes to form a lug groove, and then the lug is welded in the lug groove; in the process of forming the lug groove, a scraper or laser ablation is usually used, which will cause the active material in the vicinity of the lug groove to become fluffy due to stress and splash part of the active material particles in the vicinity of the lug groove. Therefore, after the outermost layer of the winding core breaks, the film layers inside the winding core will loosen to form a gap, and the active material particles in the vicinity of the lug groove will be displaced under the action of the active material fluffy recovery, and especially the arc segment near the lug groove has the largest loose displacement, which may puncture the diaphragm of this arc segment and cause risks such as lithium precipitation or short circuit fire.

[0046] like Figures 1 to 10As shown, in the first aspect of the utility model, a winding core is provided, which includes an electrode assembly 1, a first adhesive tape 2 and a second adhesive tape 3; the electrode assembly 1 includes a straight section 11 and a first arc bending section 12 and a second arc bending section 13 respectively located at both ends of the straight section 11; a pole ear 101 is arranged in the straight section 11, and the winding tail end 1007 of the electrode assembly is located in the second arc bending section 13; the first adhesive tape 2 is arranged on the outermost surface of the first arc bending section 12, and the second adhesive tape 3 covers the pole ear 101 along the orthographic projection of the thickness direction of the winding core, and the second adhesive tape 3 extends to the first arc bending section 12; wherein, the first adhesive tape 2 and the second adhesive tape 3 both exceed the edge of the electrode assembly 1 in the first direction, and the first direction is the width direction of the electrode sheet.

[0047] It should be noted that the winding end 1007 of the electrode assembly is located at the second arc bending section 13. Figure 1 As shown, the pole piece and / or the diaphragm at the outermost tail end of the winding core extends out from the second arc bending section 13 or is located on the second arc bending section 13 .

[0048] In the utility model, the electrode assembly 1 is a winding structure formed by stacking and winding electrode sheets and diaphragms 104 with opposite polarities. The electrode sheets and diaphragms 104 form bending portions and straight portions during the winding process. For example, each time the electrode sheets and diaphragms 104 are wound one circle, two arc bending portions and two straight portions are formed. The two arc bending portions are respectively located at the two ends of the two straight portions, and the two straight portions are connected by the two arc bending portions. Specifically, one end of the arc bending portion is connected to one straight portion, and the other end is connected to the other straight portion, thereby forming the first circle of the winding core. As the number of winding turns of the electrode sheet and the diaphragm 104 increases, multiple straight portions and multiple arc bent portions will be formed. At this time, the multiple straight portions are stacked in sequence to form a straight section of the electrode assembly; the multiple arc bent portions are stacked in sequence to form a first arc bent section 12 and a second arc bent section 13 relatively arranged at both ends of the straight section 11. At this time, the first arc bent section 12 is connected to one end of the straight section 11, and the second arc bent section 13 is connected to the other end of the straight section 11.

[0049] It should be noted that the direction from the first arc bent section 12 at one end of the electrode assembly 1 to the second arc bent section 13 at the other end thereof is the second direction of the electrode assembly (i.e., the length direction of the electrode assembly); on the first plane parallel to the straight section 11, the direction perpendicular to the second direction is the first direction of the electrode assembly (i.e., the width direction of the electrode assembly); and the direction from one straight portion of the electrode assembly 1 to another straight portion thereof is the third direction of the electrode assembly (i.e., the thickness direction of the electrode assembly, the winding core).

[0050] The winding tail end 1007 of the electrode assembly is located at the second arc bending section 13 , that is, the winding tail end 1007 of the electrode assembly is partially or entirely located at the second arc bending section 13 .

[0051] Specifically, in the winding structure, the winding starts with the winding start end of the electrode assembly 1 as the starting point, and ends with the winding end 1007 of the electrode assembly 1 as the end point. Along the winding direction, according to the distance from the winding end 1007, the arc bending section can be divided into a first arc bending section 12 away from the winding end 1007 and a second arc bending section 13 close to the winding end 1007, wherein the first arc bending section 12 is away from the winding end of the electrode assembly relative to the second arc bending section 13, and the second arc bending section 13 is close to the winding end 1007 of the electrode assembly relative to the first arc bending section 12.

[0052] The outermost side of the first arc bending section 12 refers to the outermost side of the first arc bending section 12 away from the winding center of the electrode assembly 1, and can be the inner and outer surfaces of the outermost electrode sheet or the inner and outer surfaces of the outermost diaphragm, for example, it can be the surface of the positive electrode collector (aluminum foil) of the positive electrode sheet or the surface of the diaphragm, which can be the outer surface and / or inner surface of the aluminum foil, or the outer surface and / or inner surface of the diaphragm; for example, refer to Figure 1 , the first adhesive tape 2 is only coated on the outer surface of the aluminum foil.

[0053] The winding core also includes a tab 101, through which the circuit in the winding core is led out to achieve communication with the peripheral circuit. In the utility model, the tab 101 is arranged on the straight section 11, and can be specifically arranged on a current collector of a straight portion of the straight section 11.

[0054] The number of pole ears 101 is usually two, and both are arranged in the pole ear groove of the straight section 11. The two pole ears are arranged at an orthographic projection interval on the first plane. The first plane is a plane parallel to the collector surface of the straight section 11 in the electrode assembly 1, that is, line segments are emitted from each point on the pole ear in a direction perpendicular to the first plane, and these line segments are intersected with the first plane. The projection obtained is the orthographic projection of the pole ear. It can also be understood that the two pole ears are arranged at an orthographic projection interval along the thickness direction of the core, and the thickness direction of the core is perpendicular to the first plane.

[0055] The second adhesive tape 3 covers the pole ear 101 along the orthographic projection in the thickness direction of the winding core, and the second adhesive tape 3 extends to the first arc bending section 12. At this time, the second adhesive tape 3 can be covered on the pole ear, or the second adhesive tape 3 is arranged on the diaphragm or another pole piece on the opposite side of the pole ear. At this time, when the outermost side of the first arc bending section breaks and causes the inside of the winding core to loosen, the second adhesive tape can, on the one hand, effectively offset the gap formed by the loosening under the action of its own elastic deformation, reduce the loose displacement of the first arc bending section, thereby reducing the displacement causing the active material particles in the area to scratch the diaphragm. On the other hand, the second adhesive tape covers the active material on the first arc bending section, which further reduces the probability of the active material particles in the area scratching the diaphragm and reduces the risk of lithium precipitation. When the second adhesive tape covers the pole ear, the second adhesive tape 3 also plays the role of surface protection, insulation and fixing, preventing the pole ear 101 from having burrs when cutting. If the second adhesive tape 3 is not pasted to cover, the burrs are easy to pierce the diaphragm and cause a short circuit. At the same time, the position of the pole ear 101 is fixed to prevent the pole ear 101 from falling off and causing an increase in the internal resistance of the battery.

[0056] The number of the second adhesive tape 3 is one or two. When the number of the second adhesive tape is one, the second adhesive tape 3 can be set on any side of the tab 101; when the number of the second adhesive tape is two, the two adhesive tapes are respectively set on both sides of the tab 101, and the two adhesive tapes are arranged opposite to each other.

[0057] In the electrode assembly of the utility model, at least one electrode ear is provided on each of the positive electrode sheet and the negative electrode sheet. Specifically, a positive electrode ear is provided on the positive electrode sheet, and positive electrode ear protection glue is provided on both sides of the positive electrode ear, and positive electrode ear insulation glue is provided on the negative electrode sheets on both sides of the positive electrode ear, and the positive electrode ear protection glue extends to the arc bending section along the winding direction, and the positive projection of the positive electrode ear protection glue on the first plane exceeds the edge of the positive projection of the positive electrode ear insulation glue on the first plane; a negative electrode ear is provided on the negative electrode sheet, and negative electrode ear protection glue is provided on both sides of the negative electrode ear, and negative electrode ear insulation glue is provided on the positive electrode sheets on both sides of the negative electrode ear, and the negative electrode ear insulation glue extends to the arc bending section along the winding direction, and the positive projection of the negative electrode ear insulation glue on the first plane exceeds the edge of the positive projection of the negative electrode ear protection glue on the first plane. Among them, the positive electrode ear protection glue and the negative electrode ear insulation glue are both on the positive electrode sheet.

[0058] The second adhesive tape 3 extends along the winding direction to the first arc bending section 12. In one embodiment, Figure 1 and Figure 2 As shown, the electrode ear closest to the first arc bending section 12 is the positive electrode ear, and the second adhesive tape 3 can be a positive electrode ear protective adhesive, that is, covering the electrode ear 101. At this time, the positive electrode ear protective adhesive extends to the first arc bending section 12; or, in another embodiment, as Figure 3 , Figure 4 and Figure 6As shown, the electrode ear closest to the first arc bending section is the negative electrode ear, and the second adhesive tape 3 can also be the negative electrode ear insulating adhesive, that is, it is relatively arranged on the positive electrode sheet opposite to the negative electrode ear. At this time, the negative electrode ear insulating adhesive extends to the first arc bending section 12.

[0059] Among them, in the first direction, the first adhesive tape 2 and the second adhesive tape 3 both exceed the upper edge of the electrode assembly 1. Specifically, the first adhesive tape 2, the second adhesive tape 3 and the electrode assembly 1 respectively have two oppositely arranged edges along the second direction, and both edges of the first adhesive tape 2 protrude from the edge of the electrode assembly 1, and the edge of the second adhesive tape 3 close to the tab 101 protrudes from the electrode assembly 1, so that the first adhesive tape 2 and the second adhesive tape 3 both exceed the edge of the electrode assembly in the first direction.

[0060] The embodiment of the present application sets a first adhesive tape on the outermost side of the first arc bending section, which can effectively prevent the electrolyte from corroding the outermost aluminum layer, thereby causing the aluminum layer of the arc section to break first under the action of stress, and even if the aluminum layer of the arc section breaks, the first adhesive tape can also effectively connect the two sides of the aluminum layer of the outermost aluminum layer at the broken arc section, effectively preventing the winding of the core from loosening; in addition, since the second adhesive tape is set on the pole ear and extends to the first arc bending section, when the outermost side of the first arc bending section of the winding core breaks and causes the inside of the winding core to loosen, the second adhesive tape can, on the one hand, effectively offset the gap formed by the loosening under the action of its own elastic deformation, reduce the loose displacement of the arc section near the pole ear groove, thereby reducing the displacement causing the active material particles in the area to scratch the diaphragm, and on the other hand, the second adhesive tape covers the active material in the arc section, which further reduces the probability of the active material particles in the area scratching the diaphragm and reduces the risk of lithium precipitation.

[0061] In particular, the winding core of the utility model can reduce the corner damage of the aluminum-plastic film without increasing the thickness. This is because, by making the first adhesive tape 2 and the second adhesive tape 3 protrude from the edge of the electrode assembly 1, when the aluminum-plastic film is used for packaging, the first adhesive tape 2 and the second adhesive tape 3 that exceed the edge of the electrode assembly 1 can directly contact the aluminum-plastic film, forming a flexible buffer between the electrode assembly 1 and the aluminum-plastic film, especially forming a flexible buffer outside the first arc bending section 12 and the pole ear 101, the buffer plays a role in fixing the electrode assembly to prevent the shaking of the electrode assembly 1, and can also provide sufficient space for the expansion and extension of the electrode assembly 1, preventing the electrode assembly 1 from expanding and extending during the cyclic charge and discharge process and directly puncturing the aluminum-plastic film, avoiding corner damage; in addition, since the first adhesive tape 2 is only provided at the first arc bending section 12 far away from the winding end, it helps to avoid increasing the overall thickness of the winding core. Therefore, the winding core of the utility model can reduce the corner damage of the aluminum-plastic film without increasing the thickness, which is conducive to improving the energy density and safety performance of the battery.

[0062] In some embodiments, along the winding center of the winding core pointing to the outer side of the winding core, the winding core includes a plurality of folded pole pieces, and the pole ear is arranged on the pole piece between the front quarter folded pole piece and the rear quarter folded pole piece.

[0063] That is to say, the pole ear of the pole piece in the winding core is arranged in the middle of the pole piece. At this time, the second adhesive tape 3 is located in the middle of the winding core, and can alternately cooperate with the first adhesive tape 2 to reduce the further loosening of the winding core caused by the winding stress, thereby reducing the loosening and deformation of the winding core inside the second adhesive tape 3, avoiding the further increase of the gap of the inner arc section of the winding core, thereby reducing the lithium plating phenomenon of the arc section of the winding core.

[0064] The utility model does not limit the size of the first adhesive tape 2 and the second adhesive tape 3 protruding from the edge of the electrode assembly 1, which can be adjusted according to actual needs. For example, in some embodiments, the size of the first adhesive tape 2 protruding from the edge of the electrode assembly 1 in the first direction is A, and the size of the second adhesive tape 3 protruding from the edge of the electrode assembly 1 in the first direction is B; A and B satisfy the following relationship: A and B satisfy the following relationship: 0≤BA≤2mm, 0<A≤3mm, 0<B≤3mm. In this way, the second adhesive tape 3 is equal to or longer than the size of the first adhesive tape 2 protruding from the edge of the electrode assembly in the first direction, reducing the problem of appearance bulge or wrinkle caused by the folding of the second adhesive tape 3.

[0065] Among them, A refers to the size of any edge of the first adhesive tape 2 in the second direction protruding from the electrode assembly, and B refers to the size of the edge of the second adhesive tape 3 close to the pole ear 101 side protruding from the electrode assembly. In the utility model, the second adhesive tape 3 is located in the straight section 11, the first adhesive tape 2 is located on the first arc bending section 12, and the projection of the first adhesive tape 2 on the first plane is spaced from the pole ear 101, and the first plane is a plane parallel to the straight section 11 in the electrode assembly. In this way, it is ensured that the thickness of the first adhesive tape 2 and the pole ear 101 does not overlap in the thickness direction of the winding core, which can further ensure that the thickness of the winding core is not increased. In some embodiments, the spacing distance between the orthographic projection of the first adhesive tape on the first plane and the orthographic projection of the pole ear on the first plane is J, and J satisfies 0<J<60mm.

[0066] In some embodiments, the extended dimension of the first adhesive tape 2 is E, the thickness of the winding core is H, and the maximum dimension in the second direction between the end of the pole ear 101 closest to the first arc bending section 12 and the side of the first adhesive tape 2 away from the first arc bending section 12 is F; wherein the second direction is perpendicular to the first direction; E, H and F satisfy the following relationship: 2F+(π-1)×H>E>π×H.

[0067] The extended dimension E of the first adhesive tape 2 refers to the actual dimension of the first adhesive tape 2 extending from one end to the other end of the first arc bending section 12. Figure 1 and Figure 3As shown, the extension dimension E of the first adhesive tape 2 is the sum of the distances of E1, E2 and E3. According to the distance between the pole ear 101 and the first arc bending section 12 in the second direction, the pole ear 101 can be divided into the pole ear close to the first arc bending section 12 and the pole ear far from the first arc bending section 12. The pole ear close to the first arc bending section 12 is the research object. The pole ear has two opposite ends in the second direction. The end of the pole ear closest to the first arc bending section 12 is the starting point of F. The side of the first adhesive tape 2 far from the first arc bending section 12 has an arc shape. At this time, the vertex of the arc is recorded as the end point of F, and the distance from the starting point to the end point in the second direction is recorded as F.

[0068] By limiting E, H and F to satisfy the above relationship, it is possible to avoid the first adhesive tape 2 located on the outermost layer from being wrinkled and thus aggravating the corner damage phenomenon.

[0069] In the present invention, the electrode assembly 1 is formed by stacking and winding the negative electrode sheet 103, the separator 104 and the positive electrode sheet 102; the negative electrode sheet 103 at least includes a negative electrode current collector 1031 and a negative electrode active material layer 1032 arranged on at least one functional surface of the negative electrode current collector 1031; wherein the tensile strength s of the negative electrode current collector 1031 in the length direction satisfies 50MPa≤s≤500MPa. The higher the tensile strength of the negative electrode current collector 1031, the smaller its elongation (elongation). By limiting the tensile strength of the negative electrode current collector 1031 within the above range, the ductility of the negative electrode sheet itself can be improved to prevent corner cracking. If the first adhesive tape 2 and the second adhesive tape 3 are not provided, and only the tensile strength of the negative electrode current collector 1031 is limited, there is still a problem of corner damage. The present invention can further improve the corner damage problem by limiting the tensile strength of the negative electrode current collector 1031 and combining the provision of the first adhesive tape 2 and the second adhesive tape 3.

[0070] Among them, the negative electrode sheet 103 at least includes a negative electrode current collector 1031 and a negative electrode active material layer 1032 arranged on at least one functional surface of the negative electrode current collector 1031; the positive electrode sheet 102 at least includes a positive electrode current collector and a positive electrode active material layer arranged on at least one functional surface of the positive electrode current collector. The materials of the current collector and the active material layer are determined according to the specific selection of the electrode sheet. For example, when the electrode sheet is a negative electrode sheet, the current collector is copper foil, and the material of the active material layer can contain graphite or silicon-based negative electrode active materials; when the electrode sheet is a positive electrode sheet 102, the current collector is aluminum foil, and the active material layer contains graphite, and also contains positive electrode active materials such as ternary materials or lithium iron phosphate.

[0071] like Fig. 9 and Fig.10 As shown, in some embodiments, a first groove 1033 is provided on the negative electrode active material layer 1032 at least in the first arc bending segment 12 , and the depth of the first groove 1033 is not greater than the thickness of the negative electrode active material layer 1032 .

[0072] In this way, the first groove 1033 at least provides a buffer space for the expansion of the first arc bending section 12, solves the problem of excessive extension of the pole piece along the first direction, avoids the winding core from loosening, and also prevents the corner of the aluminum-plastic film from being damaged.

[0073] The first groove 1033 may be disposed on the active material layer on one side of the negative electrode current collector 1031, or may be disposed on the active material layers on both sides of the negative electrode current collector 1031. In some embodiments, at the first arc bending section 12, the ratio of the orthogonal projection area of ​​the first groove 1033 on the negative electrode current collector 1031 to the orthogonal projection area of ​​the negative electrode active material layer 1032 on the negative electrode current collector 1031 is (0.04-0.13):1.

[0074] In some embodiments, a first groove 1033 is provided on the negative electrode active material layer 1032 of the straight section 11, and the first groove 1033 is a strip groove or a dot groove. By providing the first groove 1033 on the negative electrode active material layer 1032 of the straight section 11, the first groove increases the exposed site of the negative electrode active material layer 1032, thereby increasing the contact area between the electrolyte and the electrode sheet, which is beneficial to improving the electrolyte infiltration rate of the negative electrode sheet, improving the transmission rate of ions and electrons, and improving the kinetic performance of the negative electrode sheet, thereby improving the electrochemical performance of the battery. The depth of the first groove 1033 refers to the size of the first groove 1033 in the thickness direction of the negative electrode current collector.

[0075] The shape of the first groove 1033 on the side of the negative active material layer 1032 away from the negative current collector 1031 can be at least one of a circle and a rectangle. The first groove 1033 can extend along the length direction or the width direction of the negative current collector. In some embodiments, the shape of the first groove 1033 on the side of the negative active material layer 1032 away from the negative current collector 1031 is a strip, and there are multiple first grooves 1033; multiple first grooves 1033 are arranged at intervals along the length direction of the negative current collector 1031, and each first groove 1033 extends along the width direction of the negative current collector 1031; the concave size of the first groove 1033 in the thickness direction of the negative current collector 1031 is h, and the size of the first groove 1033 in the length direction of the negative current collector 1031 is L, and the unit is μm; wherein h, L and s satisfy the following relationship: 0.03MPa / μm 2 ≤s / (h×L)≤0.75MPa / μm 2The first groove 1033 can provide a release space for the expansion of the negative active material, thereby reducing the extension of the negative electrode sheet. At the same time, the higher the tensile strength of the negative current collector 1031, the smaller its elongation rate, and the negative active material drives the elongation rate of the negative electrode sheet to gradually decrease during the expansion process. By limiting h, L and s to satisfy the above relationship, the relationship between the elongation rate of the negative electrode sheet and the release space provided by the first groove 1033 can be balanced, thereby further avoiding the loosening of the winding core and reducing the corner damage phenomenon.

[0076] In the utility model, Figure 5 As shown, at the innermost side of the electrode assembly 1, the negative electrode sheet 103 includes a first negative electrode straight portion 1001 located in the straight section 11, a second negative electrode straight portion 1003 and a first negative electrode bent portion 1002 located in the second arc bent section 13; the first negative electrode straight portion 1001, the first negative electrode bent portion 1002 and the second negative electrode straight portion 1003 are connected in sequence; the positive electrode sheet 102 includes a first positive electrode straight portion 1004 located in the straight section 11; the first positive electrode straight portion 1004 is located on the outside of the second negative electrode straight portion 1003; the maximum size of the head of the negative electrode active material layer 1032 on the first negative electrode straight portion 1001 and the first negative electrode bent portion 1002 in the second direction is m1, and the maximum size of the head of the positive electrode active material layer on the first positive electrode straight portion 1004 and the first negative electrode bent portion 1002 in the second direction is m2, where 0<m1≤m2.

[0077] At the innermost side of the winding structure of the electrode assembly 1, along the winding direction, the negative electrode sheet 103 has a first negative electrode straight portion 1001, a first negative electrode bent portion 1002 and a second negative electrode straight portion 1003 which are connected in sequence; the positive electrode sheet 102 has a first positive electrode straight portion 1004. At this time, the first positive electrode straight portion 1004 is located on the outside of the second negative electrode straight portion 1003. It can also be understood that the head of the first positive electrode straight portion 1004 is the starting end of the winding of the positive electrode sheet 102, and the head of the first negative electrode straight portion 1001 is the starting end of the winding of the negative electrode sheet 103 (also the starting end of the winding of the electrode assembly 1).

[0078] The maximum size of the head of the negative electrode active material layer 1032 on the first negative electrode straight portion 1001 and the first negative electrode bent portion 1002 in the second direction refers to the plane where the head of the negative electrode active material layer 1032 on the first negative electrode straight portion 1001 is located is the a plane, the plane where the arc-shaped top surface of the first negative electrode bent portion 1002 is located is the b plane, and the distance from the a plane to the b plane in the second direction is m1; similarly, the maximum size of the head of the positive electrode active material layer on the first positive electrode straight portion 1004 and the first negative electrode bent portion 1002 in the second direction is m2. When 0<m1≤m2 is satisfied, that is, the negative electrode on the first negative electrode straight portion 1001 The active material layer 1032 and the positive electrode active material layer on the first positive electrode straight portion 1004 are spaced apart on the first plane, which avoids the thickness step generated in the innermost area and ensures the uniformity of the core thickness. In addition, if there are longer thickness steps at different positions of the core, in order to make the step area bond more tightly, it is necessary to apply greater pressure during hot pressing and formation of the core. Excessive pressure can easily cause the extension of the electrode in all directions, resulting in loosening and deformation of the core and cracking of the aluminum-plastic film. Therefore, the utility model can ensure the uniformity of the core thickness and balance the thickness by limiting 0<m1≤m2, further avoiding problems such as loosening and deformation of the core and damage to the corners of the aluminum-plastic film.

[0079] At the outermost side of the electrode assembly 1, the positive electrode sheet 102 includes a positive electrode single-sided empty foil area 1005 and a positive electrode double-sided empty foil area 1006, which are partially located in the second arc bending section 13, and the positive electrode double-sided empty foil area 1006 is located on the outer side of the positive electrode single-sided empty foil area 1005; the surface of the positive electrode single-sided empty foil area 1005 is provided with a first termination glue 4; the first termination glue 4 exceeds the edge of the electrode assembly 1 in the first direction, and the first termination glue 4 extends out of the edge of the winding tail end 1007 in the second direction.

[0080] Empty foil area refers to the current collector where the active material layer is removed to expose the current collector surface. Single-sided empty foil area refers to the current collector where the active material layer is removed on one functional surface, and double-sided empty foil area refers to the current collector where the active material layer is removed on both functional surfaces.

[0081] At the outermost side of the winding structure of the electrode assembly 1, the positive electrode sheet 102 includes a positive electrode single-sided empty foil area 1005 and a positive electrode double-sided empty foil area 1006, which are partially located in the second arc bending section 13. It can also be understood that the positive electrode single-sided empty foil area 1005 and the positive electrode double-sided empty foil area 1006 are partially located in the second arc bending section 13, and the remaining part extends to the straight section 11. At this time, the positive electrode double-sided empty foil area 1006 is located on the outer side of the positive electrode single-sided empty foil area 1005, and the side of the positive electrode double-sided empty foil area 1006 away from the positive electrode single-sided empty foil area 1005 is the outermost surface of the electrode assembly 1. It can also be understood that the part of the positive electrode double-sided empty foil area 1006 extending to the straight section 11 is the winding end of the positive electrode sheet 102 (also the winding end 1007 of the electrode assembly 1).

[0082] The surface of the positive electrode single-sided empty foil area 1005 is far away from the winding center of the winding structure, and a first stop glue 4 is arranged on the surface for insulation and fixing the winding core. The first stop glue 4 and the electrode assembly 1 have two edges arranged opposite to each other along the second direction, and both edges of the first stop glue 4 exceed the edge of the electrode assembly 1, so that the first stop glue 4 is ensured to exceed the edge of the electrode assembly 1 in the first direction, so that the part of the first stop glue 4 exceeding the electrode assembly 1 can cooperate with the first adhesive tape 2 and the second adhesive tape 3 to form a flexible buffer between the electrode assembly 1 and the aluminum-plastic film, further improving the safety performance of the battery.

[0083] The first termination glue 4 and the winding tail end 1007 both have an edge along the first direction, and the edge of the first termination glue 4 exceeds the edge of the winding tail end 1007, so that the first termination glue 4 extends in the second direction from the edge of the winding tail end 1007. In this way, the portion of the first termination glue 4 that exceeds the winding tail end 1007 plays a role in fixing the winding core and the aluminum-plastic film, preventing the winding core from shifting inside the aluminum-plastic film, and avoiding the problems of the winding core being broken and deformed and the aluminum-plastic film being damaged.

[0084] The utility model does not limit the size of the first stop glue 4. In some embodiments, the size of the orthographic projection of the first stop glue 4 on the first plane in the second direction is P, and the size of the winding core in the second direction is W. P and W satisfy the following relationship: P = (0.5-1) W, where 10 mm < P < 40 mm. By limiting the size of the first stop glue 4, it can be ensured that the first stop glue 4 exceeds the edge of the winding end after crossing the second arc bending section 13.

[0085] In some embodiments, a second termination glue 5 is disposed on one side of the positive electrode double-sided empty foil area 1006 close to the positive electrode single-sided empty foil area 1005 ; the edges of the second termination glue 5 in the first direction all exceed the edges of the electrode assembly 1 .

[0086] The positive electrode double-sided empty foil area 1006 has two surfaces arranged opposite to each other, wherein a second stop glue 5 is arranged on the surface close to the winding center for insulation and fixing the winding core. The second stop glue 5 and the electrode assembly 1 have two edges arranged opposite to each other along the second direction, and both edges of the second stop glue 5 exceed the edge of the electrode assembly 1, so that the second stop glue 5 is ensured to exceed the edge of the electrode assembly 1 in the first direction, so that the part of the second stop glue 5 exceeding the electrode assembly 1 can cooperate with the first adhesive tape 2, the second adhesive tape 3 and the first stop glue 4 to form a flexible buffer between the electrode assembly 1 and the aluminum-plastic film, further improving the safety performance of the battery.

[0087] like Figure 8 As shown, in some embodiments, a hot melt adhesive 41 is provided on the outermost side of the winding tail end 1007 of the electrode assembly, a part of the hot melt adhesive 41 is located on the side surface of the double-sided empty foil area of ​​the positive electrode away from the single-sided empty foil area of ​​the positive electrode, and the other part is located on the single-sided empty foil area of ​​the positive electrode; the orthographic projection of the first termination adhesive 4 on the first plane covers the orthographic projection of the hot melt adhesive 41 on the first plane; the ratio of the orthographic projection area of ​​the hot melt adhesive 41 on the first plane to the orthographic projection area of ​​the winding core on the first plane is G, 30%<G<70%.

[0088] like Figure 6 As shown, the orthographic projection of the first termination glue 4 on the first plane covers the orthographic projection of the hot melt glue 41 on the first plane. The main function of the hot melt glue 41 is to fix the tail end of the electrode assembly and fix the position of the winding core and the aluminum-plastic film to prevent displacement. In addition, when the above-mentioned projection relationship is met, the orthographic projection of the hot melt glue 41 on the first plane can be made not to exceed the orthographic projection of the first termination glue 4 on the first plane, thereby preventing the hot melt glue from directly contacting the positive electrode current collector provided with the positive electrode active material layer and causing the positive electrode sheet 102 to tear.

[0089] The orthographic projection area of ​​the hot melt adhesive 41 on the first plane is 30% to 70% of the orthographic projection area of ​​the core on the first plane. By limiting the coverage area of ​​the hot melt adhesive, the thickness of the core is prevented from being overlapped due to the large hot melt adhesive area.

[0090] like Figure 7 and Figure 8 As shown, in order to avoid the overlap of the orthographic projection of the hot melt adhesive 41 on the first plane with the area where the tab 101 is located, the thickness of the winding core is superimposed. Figure 7As shown, in some embodiments, a second groove 1034 is provided on the active material layer arranged opposite to the tab 101, and the depth of the second groove 1034 does not exceed the active material layer; a third adhesive tape 6 is provided on the second groove 1034, and the orthographic projection of the third adhesive tape 6 on the first plane is flush with the orthographic projection of the second groove 1034 on the first plane; the following relationship is satisfied: the thickness of the single-layer active material layer > the depth of the second groove 1034 ≥ the sum of the thickness of the second adhesive tape 3, the third adhesive tape 6 and the hot melt adhesive. By providing the second groove 1034 in the tab area, it is possible to avoid the overlap of the orthographic projection of the hot melt adhesive 41 on the first plane with the tab area, resulting in the superposition of the core thickness.

[0091] There are usually two tabs 101, which are arranged in the tab region of the straight section 11, and the second groove 1034 is located on the active material layer of another pole piece arranged opposite to the tab region, and the size of the second groove 1034 is substantially the same as that of the tab region. Figure 7 and Figure 8 As shown, a positive electrode ear is provided on the positive electrode sheet, positive electrode ear protective glue is provided on both sides of the positive electrode ear, positive electrode ear insulating glue is provided on the negative electrode sheets on both sides of the positive electrode ear, and the second adhesive tape 3 is the positive electrode ear protective glue; a negative electrode ear is provided on the negative electrode sheet, negative electrode ear protective glue is provided on both sides of the negative electrode ear, and negative electrode ear insulating glue is provided on the positive electrode sheets on both sides of the negative electrode ear, wherein the second groove 1034 is provided on the negative electrode active material layer on both sides of the positive electrode ear, and the third adhesive tape 6 is the positive electrode ear insulating glue.

[0092] Among them, the thickness of a single-layer active material layer refers to the coating thickness of the active material layer on one side of the current collector; the depth of the second groove 1034 refers to the recessed size of the second groove 1034 in the thickness direction of the current collector, the thickness of the second adhesive tape 3 refers to the size of the second adhesive tape 3 in the thickness direction of the current collector, the thickness of the third adhesive tape 6 refers to the size of the third adhesive tape 6 in the thickness direction of the current collector, and the thickness of the hot melt adhesive 41 refers to the size of the hot melt adhesive 41 in the thickness direction of the current collector.

[0093] The utility model does not limit the specific type of the negative electrode active material layer 1032. For example, in some embodiments, the negative electrode active material layer 1032 includes graphite doped with silicon-carbon material, wherein the doping amount of the silicon-carbon material is K, 1%≤K≤30%. By limiting the above materials, the energy density of the battery can be effectively improved. Combined with the arrangement of the first adhesive tape 2 and the second adhesive tape 3, the energy density and safety performance of the battery can be improved.

[0094] In the above embodiment, the silicon-carbon material will undergo a large expansion change during the charge and discharge process, causing the pole piece to have a large extension in the horizontal and vertical directions. In some embodiments, the particle size of the silicon-carbon material is D1; ​​h, L, and D1 satisfy the following relationship: L≥2D1, h≥D1. By limiting the above relationship, sufficient release space is provided for the negative electrode material to prevent the pole piece from extending too much and causing the aluminum-plastic film to crack at the corners.

[0095] In some embodiments, 100 μm ≥ L ≥ 50 μm, to ensure that there is enough space to accommodate the expansion of the silicon-carbon material during the cyclic charge and discharge process, reduce the elongation rate of the negative electrode sheet in the first direction, and prevent the electrode sheet from stretching too much and breaking the aluminum-plastic film to cause corner cracks. Furthermore, 20 μm ≥ L ≥ 10 μm, to prevent the silicon-carbon material from becoming too hard after expansion and exposing and then puncturing the diaphragm to avoid short circuit.

[0096] A second aspect of the present invention provides a battery, comprising the winding core and an aluminum-plastic film according to the first aspect, wherein the aluminum-plastic film encloses a receiving cavity, and the winding core is located in the receiving cavity.

[0097] By installing the winding core and the protection circuit inside the aluminum-plastic film, a battery for charging / discharging can be formed. The quality of the winding core directly determines the quality of the battery. Due to the use of the above-mentioned electrode sheet, the battery of the utility model has excellent performance in terms of corner damage and the like.

[0098] The utility model is further described below through specific embodiments and comparative examples.

[0099] Example 1

[0100] 1. Preparation of negative electrode sheet

[0101] (1) dissolving graphite doped with 10% by weight of silicon-carbon material in deionized water to obtain a negative electrode slurry; coating the negative electrode slurry on both surfaces of a negative electrode current collector (copper foil) with a thickness of 5 μm, and rolling to obtain a negative electrode sheet with a thickness of 100 μm; wherein the particle size D1 of the silicon-carbon material is 10 μm, and the tensile strength s of the negative electrode current collector in the length direction is 300 MPa;

[0102] (2) The active material layer on the negative electrode sheet on both sides of the negative electrode current collector is punched by laser to form a first strip-shaped groove 1033, wherein on one side of the negative electrode current collector, the ratio of the orthographic projection area of ​​the first groove 1033 on the negative electrode current collector to the orthographic projection area of ​​the active material layer on the negative electrode current collector is 0.07:1. Specifically, the active material layer is punched every 1.2 mm along the length direction of the negative electrode current collector. The dimension h of the first groove 1033 in the thickness direction of the current collector is 20 μm, and the dimension L of the first groove 1033 in the length direction of the current collector is 80 μm.

[0103] (3) A slot of fixed size is set at a certain position of the negative electrode sheet, and the copper-plated nickel electrode ear (negative electrode ear) is welded in this slot by laser or ultrasonic welding, and a second adhesive tape 3 is pasted on the electrode ear; in addition, a second groove 1034 is cleaned in the welding area of ​​the positive electrode ear at the position of the positive projection of the adjacent negative electrode sheet, and the size of the second groove 1034 in the third direction is 30 μm, and a third adhesive tape 6 is pasted on the second groove 1034.

[0104] 2. Preparation of positive electrode

[0105] (1) dissolving 97.6% lithium cobalt oxide in N-methylpyrrolidone to obtain a positive electrode slurry; coating the positive electrode slurry on both surfaces of an aluminum foil having a thickness of 8 μm, rolling to obtain a positive electrode sheet having a thickness of 70 μm, setting a slot of a fixed size at a certain position of the positive electrode sheet as a positive electrode ear welding area, laser or ultrasonically welding the positive electrode ear in the slot, and pasting a second adhesive tape 3 on the ear;

[0106] A first termination glue 4 and a second termination glue 5 are respectively attached to the empty foil area of ​​the positive electrode sheet; the size P of the orthographic projection of the first termination glue 4 on the first plane in the second direction is 35 mm, and the thickness of the first termination glue 4 is 12 μm; the size of the orthographic projection of the second termination glue 5 on the first plane in the second direction is 15 mm, and the thickness of the second termination glue 5 is 12 μm;

[0107] 3. Preparation of batteries

[0108] (1) Using a polyethylene (PE) porous polymer film as a separator, the positive electrode sheet, the separator, and the negative electrode sheet are stacked in sequence and wound to form a Figure 3 , Figure 4 , Figure 8 The electrode assembly 1 shown in the figure; the first adhesive tape 2 is pasted on the first arc bending section 12, wherein the extension dimension E of the first adhesive tape is 10 mm, the two edges of the first adhesive tape 2 respectively exceed the edge of the electrode assembly by a dimension A of 0.5 mm in the first direction, the second adhesive tape 3 exceeds the edge of the electrode assembly by a dimension B of 0.5 mm in the first direction, the orthographic projection of the first adhesive tape 2 on the first plane and the orthographic projection of the electrode ear 101 on the first plane are arranged at intervals, and a winding core with a certain size is obtained after pasting the hot melt adhesive 41; and during the winding process, the negative The first negative straight portion 1001, the first negative bent portion 1002, and the second negative straight portion of the first fold of the electrode sheet have negative active material layers, and the first negative straight portion 1001 satisfies m1=2mm, the first positive straight portion 1004 of the first fold of the positive electrode sheet has a positive active material layer, and m2=4mm is satisfied, and the orthographic projection area of ​​the hot melt adhesive 41 on the first plane is 50% of the orthographic projection area of ​​the winding core on the first plane; the size of the hot melt adhesive 41 in the second direction is 20mm, and the size in the first direction is 60mm;

[0109] (2) Preparation of electrolyte: In a dry argon environment, lithium hexafluorophosphate (LiPF6) was added to a solvent solution of propylene carbonate (PC), ethylene carbonate (EC), and diethyl carbonate (DEC) in a weight ratio of 1:1:1, and the mixture was mixed evenly, wherein the concentration of LiPF6 was 1.12 mol / L, and then 10 wt % of fluoroethylene carbonate (FEC) was added and mixed evenly to obtain an electrolyte;

[0110] (3) The core is packaged into the punched hole of the aluminum-plastic film (the aluminum-plastic film includes an outer layer of nylon, a middle layer of Al, and an inner layer of PP). After the core is dried, the electrolyte is injected and packaged. After formation, secondary sealing, sorting and OCV, a battery is obtained, and the electrical performance of the battery is tested.

[0111] Example 2

[0112] The preparation process is basically the same as that of Example 1, except that the extended dimension E of the first adhesive tape 2 is 18 mm, the first adhesive tape 2 partially overlaps with the orthographic projection of the tab 101 on the first plane, and other conditions remain unchanged to obtain the battery of this embodiment.

[0113] Example 3

[0114] The preparation process is basically the same as that of Example 1, except that in this embodiment, no active material layer is set on the first negative electrode straight portion 1001 and the first negative electrode bent portion 1002 (ie, m1=0), and they are empty copper foils. Other conditions remain unchanged to obtain the battery of this embodiment.

[0115] Example 4

[0116] The preparation process is basically the same as that of Example 1, except that the tensile strength s of the negative electrode current collector in the length direction of this embodiment is 50 MPa, the dimension h of the first groove 1033 in the thickness direction is 5 μm, and other conditions remain unchanged to obtain the battery of this embodiment.

[0117] Example 5

[0118] The preparation process is basically the same as that of Example 1, except that the negative electrode sheet is not provided with the second groove 1034, and other conditions remain unchanged to obtain the battery of this embodiment.

[0119] Example 6

[0120] The preparation process is basically the same as that of Example 1, with the difference that, in the preparation process of the battery, the first fold of the negative electrode sheet in this comparative example, the first negative electrode straight portion 1001 and the first negative electrode bent portion 1002 are not provided with an active material layer, but are empty copper foils, and the maximum dimension of the head of the negative electrode active material layer on the second negative electrode straight portion 1003 and the side of the first negative electrode bent portion 1002 away from the winding center is 2 mm, that is, m1 = -2 mm, and other conditions remain unchanged to obtain the battery of this embodiment.

[0121] Example 7

[0122] The preparation process is basically the same as that of Example 1, except that, during the preparation process of the battery, the size P of the orthographic projection of the first termination glue 4 of this comparative example on the first plane in the second direction is 15 mm, and other conditions remain unchanged to obtain the battery of this embodiment.

[0123] Example 8

[0124] The preparation process is basically the same as that of Example 1, except that, during the preparation process of the battery, the orthographic projection area of ​​the hot melt adhesive 41 of this comparative example on the first plane is 10% of the orthographic projection area of ​​the winding core on the first plane, and other conditions remain unchanged to obtain the battery of this embodiment.

[0125] Example 9

[0126] The preparation process is basically the same as that of Example 1, except that, during the preparation of the negative electrode sheet, the tensile strength s of the negative electrode collector of this comparative example in the length direction is 50 MPa, the depth h of the first groove 1033 on the negative electrode sheet is 5 μm, and the dimension L of the first groove 1033 in the first direction is 15 μm; other conditions remain unchanged, and the battery of this embodiment is obtained.

[0127] Example 10

[0128] The preparation process is basically the same as that of Example 1, except that in the preparation process of the negative electrode sheet, graphite is directly dissolved in deionized water to obtain the negative electrode slurry of this comparative example, and other conditions remain unchanged to obtain the battery of this comparative example.

[0129] Embodiment 11

[0130] The preparation process is basically the same as that of Example 1, except that, during the preparation process of the battery, the dimension A of the first adhesive tape 2 protruding from the electrode assembly of the first arc bending section 12 of this embodiment is 4 mm, and other conditions remain unchanged to obtain the battery of this embodiment.

[0131] Comparative Example 1

[0132] The preparation process is basically the same as that of Example 1, except that the tensile strength s of the negative electrode current collector in the length direction of this comparative example is 50 MPa, and the first groove 1033 is not set on the surface of the negative electrode sheet of this comparative example; in the preparation process of the battery, the first arc bending section 12 of this comparative example is not set with the first adhesive tape 2, and other conditions remain unchanged to obtain the battery of this comparative example.

[0133] The main parameters in the above embodiments and comparative examples can be seen in Table 1.

[0134] Table 1

[0135]

[0136] Test example

[0137] Tensile strength test: Use a fixed size cutter to cut the negative electrode current collector into samples with a width of 15 mm and a length of more than 50 mm. Use a WD-D3 electronic universal testing machine (with a precision of 0.5 level and an accuracy of ±1% of the indicated value) with a gauge length of 50 mm and a speed of 50 mm / min to perform a tensile strength test.

[0138] Appearance test during the cycle: In a 45℃ constant temperature room, use 0.5C constant current and constant voltage to the upper limit voltage, 0.05C cut-off, stand for 5 minutes, 0.5C discharge to 3.0V, cycle 500 times, and observe whether the four corners of the deep pit surface of the aluminum-plastic film opposite to the four corners of the core are damaged (corner cracks).

[0139] Elongation test: disassemble the coil after 500 cycles, use a fixed size tool to cut the negative electrode sheet after the cycle into samples with a width of 15mm and a length of more than 50mm, and use a WD-D3 electronic universal testing machine (precision of 0.5 level, accuracy of ±1% of the indicated value) with a gauge length of 50mm and a speed of 50mm / min to conduct an elongation test.

[0140] After the battery was dropped freely from a height of 1m 10 times, the core was disassembled to observe whether the structure of the core was intact. The above test results can be seen in Table 2.

[0141] Table 2

[0142]

[0143] According to Table 1 and Table 2, the battery of the embodiment has a lower pole piece elongation after cycling, and can ensure the integrity of the winding core structure, and the probability of cracking of the aluminum-plastic film corner is lower. This is because the utility model sets the first adhesive tape on the first arc bending section in the electrode assembly, sets the second adhesive tape on the pole ear, and makes the first adhesive tape and the second adhesive tape protrude from the edge of the electrode assembly. In this way, the setting of the first adhesive tape can effectively prevent the corrosion of the electrolyte to the outermost aluminum layer and cause the aluminum layer of the arc section to break first under the action of stress, and even if the aluminum layer of the arc section breaks, the first adhesive tape can effectively connect the two sides of the aluminum layer at the break, effectively avoiding the loosening of the winding core; secondly, when the outermost side of the first arc bending section of the winding core breaks and causes the inside of the winding core to loosen, the second adhesive tape can, on the one hand, Under the action of its own elastic deformation, it effectively offsets the gap formed by loosening and reduces the loose displacement of the arc section near the pole ear groove, thereby reducing the displacement that causes the active material particles in this area to scratch the diaphragm. On the other hand, the second tape covers the active material in the arc section, which further reduces the probability of the active material particles in this area scratching the diaphragm, thereby ensuring the integrity of the core structure. In addition, when aluminum-plastic film packaging is used, the parts of the first tape and the second tape that extend beyond the edge of the electrode assembly can directly contact the aluminum-plastic film, forming a flexible buffer between the electrode assembly and the aluminum-plastic film to avoid corner damage.

[0144] Comparing the examples and comparative examples, it can be seen that when the tensile strength of the negative electrode current collector is consistent, by setting the first adhesive tape and the second adhesive tape, the probability of corner cracks can be significantly reduced, and the core structure can be guaranteed to be intact. Comparing Example 4 and Comparative Example 1, it can be seen that because the tensile strength of the negative electrode current collector is too low and the size of the first groove in the thickness direction is only 5μm, the final pole piece elongation is 2.2%. Without setting the first adhesive tape as the side glue, Comparative Example 1 has a 100% probability of corner cracks, while Example 4 is provided with the first adhesive tape as the side glue, so its probability of corner cracks is reduced to 50%. Due to the presence of the first groove, the pole piece elongation of Comparative Example 3 itself is 1.2%, which is already a relatively low level, and the probability of corner cracks is lower than that of Comparative Example 1.

[0145] The above describes in detail the preferred specific embodiments and experimental verification of the utility model. It should be understood that ordinary technology in the field can make many modifications and changes according to the concept of the utility model without creative work. Therefore, all technical solutions that can be obtained by technicians in this technical field based on the concept of the utility model through logical analysis, reasoning or limited experiments on the basis of the existing technology should be within the scope of protection of the utility model.

Claims

1. A winding core, characterized in that: It includes an electrode assembly, a first adhesive tape and a second adhesive tape; The electrode assembly comprises a straight section and a first arc bending section and a second arc bending section respectively located at two ends of the straight section; a pole ear is arranged in the straight section, and the winding end of the electrode assembly is located at the second arc bending section; The first adhesive tape is arranged at the outermost side of the first arc bending section, the orthographic projection of the second adhesive tape along the thickness direction of the winding core covers the pole ear, and the second adhesive tape extends to the first arc bending section; Wherein, the first adhesive tape and the second adhesive tape both extend beyond the edge of the electrode assembly in a first direction, and the first direction is the width direction of the electrode sheet.

2. The winding core according to claim 1, characterized in that: Along the winding center of the winding core pointing to the outer side of the winding core, the winding core includes a plurality of folded pole pieces, and the pole ear is arranged on the pole piece between the first quarter folded pole piece and the second quarter folded pole piece.

3. The winding core according to claim 1, characterized in that: The dimension of the first adhesive tape extending beyond the edge of the electrode assembly in the first direction is A, and the dimension of the second adhesive tape extending beyond the edge of the electrode assembly in the first direction is B; A and B satisfy the following relationship: 0≤BA≤2mm, 0<A≤3mm, 0<B≤3mm.

4. The winding core according to claim 1, characterized in that: The spacing distance between the orthographic projection of the first adhesive tape on the first plane and the orthographic projection of the electrode ear on the first plane is J, J satisfies 0<J<60mm, and the first plane is a plane parallel to the straight section in the electrode assembly.

5. The winding core according to claim 1, characterized in that: The extended dimension of the first adhesive tape is E, the thickness of the winding core is H, and the maximum dimension of the end of the pole ear closest to the first arc bending section and the side of the first adhesive tape away from the first arc bending section in the second direction is F; wherein the second direction is perpendicular to the first direction; E, H and F satisfy the following relationship: 2F+(π-1)×H>E>π×H.

6. The winding core according to any one of claims 1 to 5, characterized in that: The electrode assembly is formed by stacking and winding a negative electrode sheet, a separator and a positive electrode sheet; The negative electrode sheet at least comprises a negative electrode current collector and a negative electrode active material layer disposed on at least one functional surface of the negative electrode current collector; Wherein, the tensile strength s of the negative electrode current collector in the length direction satisfies 50MPa≤s≤500MPa.

7. The winding core according to claim 6, characterized in that: A first groove is provided on the negative electrode active material layer at least in the first arc bending section, and the depth of the first groove is not greater than the thickness of the negative electrode active material layer.

8. The winding core according to claim 7, characterized in that: A first groove is arranged on the negative electrode active material layer of the straight section, and the first groove is a strip-shaped groove or a dot-shaped groove.

9. The winding core according to claim 8, characterized in that: The first groove is in a strip shape on the side of the negative electrode active material layer away from the negative electrode current collector, and there are a plurality of the first grooves; A plurality of the first grooves are arranged at intervals along the length direction of the negative electrode current collector, and each first groove extends along the width direction of the negative electrode current collector; The concave dimension of the first groove in the thickness direction of the negative electrode current collector is h, and the dimension of the first groove in the length direction of the negative electrode current collector is L, both in μm; Among them, h, L and s satisfy the following relationship: 0.03MPa / μm 2 ≤s / (h×L)≤0.75MPa / μm 2 .

10. The winding core according to claim 6, characterized in that: At the innermost side of the electrode assembly, the negative electrode sheet includes a first negative straight portion located in the straight section, a second negative straight portion, and a first negative bent portion located in the second arc bent section; the first negative straight portion, the first negative bent portion, and the second negative straight portion are connected in sequence; The positive electrode sheet comprises a first positive straight portion located in the straight section; the first positive straight portion is located outside the second negative straight portion; The maximum size of the head of the negative electrode active material layer on the first negative electrode straight portion and the first negative electrode bent portion in the second direction is m1, and the maximum size of the head of the positive electrode active material layer on the first positive electrode straight portion and the first negative electrode bent portion in the second direction is m2; Where 0<m1≤m2.

11. The winding core according to claim 10, characterized in that: At the outermost side of the electrode assembly, the positive electrode sheet includes a positive electrode single-sided empty foil area and a positive electrode double-sided empty foil area partially located at the second arc bending section, and the positive electrode double-sided empty foil area is located outside the positive electrode single-sided empty foil area; The surface of the single-sided empty foil area of ​​the positive electrode is provided with a first termination glue; The first termination glue exceeds the edge of the electrode assembly in the first direction, and the first termination glue extends out of the edge of the winding tail end in the second direction.

12. The winding core according to claim 11, characterized in that: The size of the orthographic projection of the first termination glue on the first plane in the second direction is P, the size of the winding core in the second direction is W, and P and W satisfy the following relationship: P=(0.5-1)W, wherein 10mm<P<40mm.

13. The winding core according to claim 12, characterized in that: A second stop glue is provided on the surface of one side of the positive electrode double-sided empty foil area close to the positive electrode single-sided empty foil area; The second termination glue exceeds the edge of the electrode assembly in the first direction.

14. The winding core according to claim 13, characterized in that: A hot melt adhesive is disposed on the outermost side of the winding tail end of the electrode assembly, a portion of the hot melt adhesive is located on the surface of the positive electrode double-sided empty foil area away from the positive electrode single-sided empty foil area, and the other portion is located on the positive electrode single-sided empty foil area; the orthographic projection of the first termination adhesive on the first plane covers the orthographic projection of the hot melt adhesive on the first plane; The ratio of the orthographic projection area of ​​the hot melt adhesive on the first plane to the orthographic projection area of ​​the winding core on the first plane is G, and 30%<G<70%.

15. The winding core according to claim 14, characterized in that: A second groove is provided on the active material layer arranged opposite to the electrode tab; the depth of the second groove is not greater than the thickness of the active material layer, a third adhesive tape is provided on the second groove, and the orthographic projection of the third adhesive tape on the first plane is flush with the orthographic projection of the second groove on the first plane; The following relationship is satisfied: the thickness of the single active material layer>the depth of the second groove≥the sum of the thicknesses of the second adhesive tape, the third adhesive tape and the hot melt adhesive.

16. A battery, characterized in that: It comprises the winding core and the aluminum-plastic film according to any one of claims 1 to 15, wherein the aluminum-plastic film encloses a receiving cavity, and the winding core is located in the receiving cavity.

Citation Information