Nylon elastic jacquard anti-wrinkle fabric
By using the matching weaving of plain-weave surface tissue and floating-line point-grained jacquard in nylon elastic jacquard fabric, the problem of poor wrinkle resistance after multiple elastic deformation and washing is solved, and the tight and full structure of the fabric and good wrinkle resistance are achieved.
Patent Information
- Application Number
- CN202421788142.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2025-06-10
- Estimated Expiration
- 2034-07-26
AI Technical Summary
Nylon elastic jacquard fabrics are prone to wrinkles under multiple elastic deformations and external force losses, and have poor wrinkle resistance, especially after multiple washes.
The plain-wavy surface tissue is used to combine and woven with the inner tissue of floating thread lifting. Through the reasonable coordination of the arrangement of tissue voids and floating threads, the inner tissue restricts the deformation of the surface tissue, limits the shrinkage of the yarn, and forms a tight and full inner-wavy structure.
After elastic deformation and washing, the inside and inside of the fabric is more tight, the feel is crisp, the smoothness after washing is high, the wrinkle resistance is good, and it is not easy to wrinkle.
Smart Images

Figure CN222961679U_ABST
Abstract
Description
Technical Field
[0001] The utility model belongs to the technical field of woven fabrics, and particularly relates to a nylon elastic jacquard anti-wrinkle fabric. Background Art
[0002] Nylon, also known as nylon and polyamide fiber, has good strength, wear resistance, corrosion resistance and elasticity; spandex, also known as polyurethane fiber, has high elasticity and can be stretched 6-7 times, but can quickly return to the initial state with the disappearance of tension. After blending nylon with spandex, the fabric can have excellent resilience and stretchability, and has high wear resistance, is not easy to wear and pilling, can withstand long-term use and multiple washes while maintaining good quality, and the clothing comfort is relatively high. Although the elasticity and elastic recovery of nylon are better with the addition of spandex, when used as a sportswear fabric, the fabric is prone to deformation and wrinkles under multiple elastic deformations and large external force losses. Especially after multiple washes, it is easy to wrinkle and has poor anti-wrinkle performance. Summary of the Utility Model
[0003] The purpose of the utility model is to provide a nylon elastic jacquard anti-wrinkle fabric that is not easy to wrinkle after washing.
[0004] The technical solution of the utility model is as follows:
[0005] A nylon elastic jacquard anti-wrinkle fabric includes a surface weave and an inner weave at the bottom; the surface weave is a plain weave formed by the interweaving of a first warp yarn and a first weft yarn; the inner weave is a floating line dot jacquard weave, and the floating line dot jacquard weave cycle includes a single weft tissue point and a floating line: the single weft tissue point is formed by the interweaving of a second weft yarn with the first warp yarn and the first weft yarn; the floating line is formed by the second weft yarn between two adjacent single weft tissue points, and the length is 3 or 5 tissue points; the floating line dot jacquard weave cycles are continuously arranged in the weft direction of the surface weave; the floating line dot jacquard weave cycles are staggered and cyclically arranged in the warp direction of the surface weave.
[0006] The nylon elastic jacquard anti-wrinkle fabric of the utility model is woven by matching a plain surface weave with a floating line dot jacquard inner weave. The tissue gaps and the floating line arrangements are reasonably matched with each other. The second weft yarn of the inner weave and the first weft yarn of the surface weave are simultaneously restricted by the same first warp yarn, so that the inner weave has a certain restrictive effect on the deformation of the surface weave. Therefore, after the woven fabric undergoes elastic deformation and washing, the shrinkage of the yarn is restricted, and the shrunk surface and inner weaves are more tightly packed and not easy to wrinkle, with a crisp handfeel, high flatness after washing, and good anti-wrinkle performance.
[0007] Preferably, the length of the floating line is 5 tissue points, and the staggered cyclic arrangement mode of the floating line dot jacquard weave cycles in the warp direction of the surface weave is one of the following modes:
[0008] a. With a 3 - warp - end interval in the warp direction and a 3 - weft - end offset in the weft direction; b. With a 2 - warp - end interval in the warp direction and a 2 - weft - end offset in the weft direction; c. With a 3 - warp - end interval in the warp direction and a 1 - weft - end offset in the weft direction.
[0009] Preferably, the length of the float line is 3 warp - ends, and the interleaved cyclic arrangement of the float - line point - jacquard tissue cycle in the warp direction of the surface tissue is one of the following ways:
[0010] a. With a 2 - warp - end interval in the warp direction and a 2 - weft - end offset in the weft direction; b. With a 3 - warp - end interval in the warp direction and a 1 - weft - end offset in the weft direction.
[0011] Preferably, the first warp yarn is a DTY polyamide fiber (PA) wrapped 20D - 40D spandex yarn with a specification of 40D - 70D, and the wrapping method of the spandex is air - wrapped or machine - wrapped; the first weft yarn is a DTY polyamide fiber (PA) wrapped 20D - 40D spandex yarn with a specification of 40D - 70D, and the wrapping method of the spandex is air - wrapped or machine - wrapped. More preferably, the air - wrapping of the first warp yarn is air - wrapped with twist; the second weft yarn is a DTY polyamide fiber (PA) yarn or an ATY polyamide fiber (PA) yarn with a specification of 70D - 160D.
[0012] The DTY polyamide fiber (PA) wrapped spandex yarn can better exert the advantage of strong cohesion of polyamide fiber (PA), and has better recovery ability under external interference, and the woven finished product is not easy to produce fuzz. The reasonable combination of the above - mentioned first warp yarn, first weft yarn and second weft yarn enables the polyamide fiber (PA) to have good elastic recovery and good wrinkle resistance.
[0013] Preferably, the warp density of the polyamide fiber (PA) elastic jacquard anti - wrinkle fabric is 120 - 250 ends per inch, and the weft density is 100 - 200 picks per inch. Weaving with the above - mentioned density makes the surface and inner tissues more compact and plump after the yarn shrinks, and the hand feeling is more crisp.
[0014] The beneficial effects of the present utility model are as follows:
[0015] The polyamide fiber (PA) elastic jacquard anti - wrinkle fabric of the present utility model is woven with a plain - weave surface tissue and a cyclic and interleaved float - line point - jacquard inner tissue, so that the surface tissue and the inner tissue restrict each other, forming a compact and plump surface - inner tissue structure, restricting the deformation of the fabric under external force, having good morphological stability and not being easy to wrinkle. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is the organizational structure diagram of the polyamide fiber (PA) elastic jacquard anti - wrinkle fabric produced in Example 1;
[0017] Figure 2 It is the organizational structure diagram of the polyamide fiber (PA) elastic jacquard anti - wrinkle fabric produced in Example 2;
[0018] Figure 3 The organizational structure diagram of the polyamide elastic jacquard anti-wrinkle fabric produced in Example 3;
[0019] Figure 4 The organizational structure diagram of the polyamide elastic jacquard anti-wrinkle fabric produced in Example 4;
[0020] Figure 5 The organizational structure diagram of the polyamide elastic jacquard anti-wrinkle fabric produced in Example 5.
[0021] In the figure: 1. The first weft yarn; 2. The first warp yarn; 3. The second weft yarn. Detailed implementation manners
[0022] The following is a detailed description of the present utility model in conjunction with the embodiments.
[0023] The NK GUARD S-573 waterproof agent used in the following embodiments is produced by Nihon Kayaku Chemical (China) Co., Ltd., and its full name is "Environmentally Friendly Tri-proof Waterproof Agent NK GUARD S-573"; the TUBINGAL RNJ softener is produced by Ambrosia Silicon Materials (Tianjin) Co., Ltd. The desizing agent is the scouring emulsifying desizing agent Scotol TS-759A produced by Suzhou Weiming Chemical Industry Co., Ltd.; the scouring agent is PITCHRUN L-271EZ produced by Nihon Kayaku Chemical (China) Co., Ltd.; the penetrant is WDN defoamer.
[0024] Example 1
[0025] Manufacture a polyamide elastic jacquard anti-wrinkle fabric, the organizational structure of which is as Figure 1 shown, including a surface weave and an inner weave at the bottom; the surface weave is a plain weave, formed by the interweaving of the first warp yarn 2 and the first weft yarn 1; the inner weave is a floating line dot jacquard weave, and the floating line dot jacquard weave cycle includes a single weft tissue point and a floating line: the single weft tissue point is formed by the interweaving of the second weft yarn 3 with the first warp yarn 2 and the first weft yarn 1; the floating line is formed by the second weft yarn 3 between two adjacent single weft tissue points, and the length is 5 tissue points. The floating line dot jacquard weave cycles are continuously arranged in the weft direction of the surface weave; the floating line dot jacquard weave cycles are staggered and cyclically arranged in the warp direction of the surface weave, and the staggered and cyclical arrangement method is: at an interval of 3 tissue points in the warp direction and offset by 3 tissue points in the weft direction. The ratio of the first weft yarn to the second weft yarn is 3:1.
[0026] The production method is as follows:
[0027] Step 1, weaving
[0028] The first warp yarn uses 40D DTY nylon air-covered 20D spandex yarn, the first weft yarn uses 40D DTY nylon air-covered 20D spandex yarn, the second weft yarn uses 70D ATY nylon yarn, and the fabric structure uses the warp and weft double-sided organization described above Figure 1 in which the warp and weft double-sided organization combines the plain weave surface organization with the inner organization of the second weft yarn of the floating line point jacquard organization. The warp density of the woven fabric is 220 threads / inch, and the weft density is 200 threads / inch. It is woven using the Tsudakoma 8100 combined with Stäubli electronic dobby, with electronic beam, electronic take-up, and electronic weft storage.
[0029] Step 2: Desizing and pre-setting;
[0030] The desizing process is as follows: fabric feeding - desizing - soaping - hot water washing - cold water washing; the auxiliaries used for desizing include: 6 - 8 g / L desizing agent, 1.5 - 3 g / L scouring agent, 2 - 3 g / L penetrant, and the desizing temperature is 95°C; the soaping temperature is 80 - 85°C, the hot water washing temperature is 60 - 70°C, and the vehicle speed during the desizing process is controlled at 45 m / min.
[0031] Pre-setting is carried out using a hot air stenter: the pre-setting temperature is 195°C, and the setting time is 80 s. Through pre-setting, the fabric reaches an ideal and stable density.
[0032] The desized fabric can be dyed and fixed according to needs.
[0033] Step 3: Drying: After dehydration using a drum centrifugal dehydrator, it is fully dried on a non-tension guiding mesh flat dryer. The drying temperature is 130°C, and the vehicle speed is 35 m / min.
[0034] Step 4: Setting
[0035] Prepare the setting solution: Dissolve NK GUARD S-573 waterproofing agent and TUBINGAL RNJ softening agent in water so that the concentration of NK GUARD S-573 waterproofing agent is 60 g / L and the concentration of TUBINGAL RNJ softening agent is 20 g / L; use citric acid to adjust the pH value to 5.5.
[0036] After impregnating and padding the nylon stretch jacquard and wrinkle-resistant fabric obtained in Step 3 in the above setting solution, setting and baking are carried out. The setting temperature is 160°C, and the setting time is 70 s.
[0037] Example 2
[0038] Manufacture a nylon stretch jacquard and wrinkle-resistant fabric, the fabric structure of which is as Figure 2As shown in the figure, it includes the surface organization and the lining organization at the bottom; the surface organization is a plain weave, formed by the interweaving of the first warp yarn 2 and the first weft yarn 1; the lining organization is a floating line dot jacquard organization, and the floating line dot jacquard organization cycle includes a single weft organization point and a floating line: the single weft organization point is formed by the interweaving of the second weft yarn 3 with the first warp yarn 2 and the first weft yarn 1; the floating line is formed by the second weft yarn 3 between two adjacent single weft organization points, and the length is 5 organization points. The floating line dot jacquard organization cycles are continuously arranged in the weft direction of the surface organization; the floating line dot jacquard organization cycles are staggered and cyclically arranged in the warp direction of the surface organization, and the staggered cyclic arrangement method is: spaced 2 organization points in the warp direction and offset 2 organization points in the weft direction. The ratio of the first weft yarn to the second weft yarn is 2:1.
[0039] The production method is as follows:
[0040] Step 1, weaving
[0041] The first warp yarn uses 70D DTY nylon machine-wrapped 40D spandex yarn, the first weft yarn uses 70D DTY nylon machine-wrapped 40D spandex yarn, the second weft yarn uses 160D DTY nylon yarn, and the organizational structure uses the above Figure 2 warp and weft double-sided organization inside and outside, the plain weave surface organization is combined with the second weft yarn of the floating line dot jacquard organization of the lining, and the warp density of the woven organization is 120 roots / inch and the weft density is 100 roots / inch. Use Tsudakoma 8100 combined with Stäubli electronic dobby to weave, with electronic let-off, electronic take-up, and electronic weft storage.
[0042] Step 2, desizing, pre-setting;
[0043] The desizing process is: fabric feeding - desizing - soaping - hot water washing - cold water washing; the auxiliaries used in desizing include: 6 - 8g / L desizing agent, 1.5 - 3g / L refining agent, 2 - 3g / L penetrant, and the desizing temperature is 95°C; the soaping temperature is 80 - 85°C, the hot water washing temperature is 60 - 70°C, and the vehicle speed during the desizing process is controlled at 45m / min.
[0044] Use a hot air stenter for pre-setting: the pre-setting temperature is 190°C and the setting time is 80s. Through pre-setting, the fabric reaches an ideal and stable density.
[0045] The desized fabric can be dyed and fixed according to needs.
[0046] Step 3, drying: After dehydrating with a cylindrical centrifugal dehydrator, conduct sufficient drying on a non-tension guiding net type flat dryer, with a drying temperature of 135°C and a vehicle speed of 35m / min.
[0047] Step 4, setting
[0048] Prepare the setting solution: Dissolve NK GUARD S-573 water repellent and TUBINGAL RNJ softener in water to make the concentration of NK GUARD S-573 water repellent 40 g / L and the concentration of TUBINGAL RNJ softener 10 g / L; adjust the pH value to 4.0.
[0049] Dip and pad the polyamide elastic jacquard wrinkle-resistant fabric obtained in Step 3 in the above setting solution, and then perform setting and baking. The setting temperature is 150 °C and the setting time is 60 s.
[0050] Example 3
[0051] Manufacture a polyamide elastic jacquard wrinkle-resistant fabric, the organizational structure of which is as Figure 3 shown, including a surface weave and an inner weave at the bottom; the surface weave is a plain weave, formed by the interweaving of the first warp yarn 2 and the first weft yarn 1; the inner weave is a floating-point jacquard weave, and the floating-point jacquard weave cycle includes a single weft tissue point and a floating line: the single weft tissue point is formed by the interweaving of the second weft yarn 3 with the first warp yarn 2 and the first weft yarn 1; the floating line is formed by the second weft yarn 3 between two adjacent single weft tissue points, and the length is 5 tissue points. The floating-point jacquard weave cycles are continuously arranged in the weft direction of the surface weave; the floating-point jacquard weave cycles are staggered and cyclically arranged in the warp direction of the surface weave, and the staggered cyclic arrangement method is: spaced 3 tissue points in the warp direction and offset 1 tissue point in the weft direction. The ratio of the first weft yarn to the second weft yarn is 3:1.
[0052] The production method is as follows:
[0053] Step 1, weaving
[0054] The first warp yarn uses 50D DTY polyamide air-covered yarn twisted with 40D spandex yarn, the first weft yarn uses 50D DTY polyamide air-covered yarn twisted with 40D spandex yarn, the second weft yarn uses 160D ATY polyamide yarn, and the organizational structure uses the warp and weft double-sided weave described above Figure 3 in which the plain surface weave is combined with the second weft yarn of the floating-point jacquard inner weave. The warp density of the woven structure is 180 ends / inch and the weft density is 150 picks / inch. Use Tsudakoma 8100 combined with Stäubli electronic dobby for weaving, with electronic let-off, electronic take-up, and electronic weft storage.
[0055] Step 2, desizing, pre-setting;
[0056] The desizing process is as follows: fabric feeding - desizing - soaping - hot water washing - cold water washing; the auxiliaries used in desizing include: 6 - 8 g / L of desizing agent, 1.5 - 3 g / L of scouring agent, 2 - 3 g / L of penetrant, and the desizing temperature is 95°C; the soaping temperature is 80 - 85°C, the hot water washing temperature is 60 - 70°C, and the vehicle speed during the desizing process is controlled at 45 m / min.
[0057] Pre - setting is carried out using a hot - air stenter: the pre - setting temperature is 200°C and the setting time is 60 s. Through pre - setting, the fabric reaches an ideal and stable density.
[0058] The desized fabric can be dyed and fixed according to requirements.
[0059] Step three, drying: After dehydration using a cylindrical centrifugal dewatering machine, it is fully dried on a non - tension guiding net flat - width dryer. The drying temperature is 140°C and the vehicle speed is 35 m / min.
[0060] Step four, setting
[0061] Prepare the setting solution: Dissolve NK GUARD S - 573 waterproof agent and TUBINGAL RNJ softener in water so that the concentration of NK GUARD S - 573 waterproof agent is 60 g / L and the concentration of TUBINGAL RNJ softener is 10 g / L; adjust the pH value to 6.0.
[0062] After impregnating and padding the polyamide elastic jacquard and wrinkle - resistant fabric obtained in step three in the above - mentioned setting solution, setting and baking are carried out. The setting temperature is 165°C and the setting time is 90 s.
[0063] Example 4
[0064] Manufacture a polyamide elastic jacquard and wrinkle - resistant fabric, whose tissue structure is as Figure 4 shown, including a surface weave and an inner weave at the bottom; the surface weave is a plain weave, formed by the interweaving of the first warp yarn 2 and the first weft yarn 1; the inner weave is a floating - line dot - pattern jacquard weave, and the floating - line dot - pattern jacquard weave cycle contains a single weft - tissue point and a floating line: the single weft - tissue point is formed by the interweaving of the second weft yarn 3 with the first warp yarn 2 and the first weft yarn 1; the floating line is formed by the second weft yarn 3 between two adjacent single weft - tissue points, and the length is 3 tissue points. The floating - line dot - pattern jacquard weave cycles are continuously arranged in the weft direction of the surface weave; the floating - line dot - pattern jacquard weave cycles are arranged in an alternating cycle in the warp direction of the surface weave, and the alternating cycle arrangement method is: with an interval of 2 tissue points in the warp direction and an offset of 2 tissue points in the weft direction. The ratio of the first weft yarn to the second weft yarn is 2:1.
[0065] The production method is as follows:
[0066] Step one, weaving
[0067] The first warp yarn uses 40D DTY nylon air-covered yarn and 20D spandex yarn, the first weft yarn uses 40D DTY nylon air-covered yarn and 20D spandex yarn, the second weft yarn uses 140D DTY nylon yarn, and the fabric structure uses the above warp and weft double-sided organization. The plain weave surface organization is combined with the inner organization of the floating line dot jacquard organization for the second weft yarn. The warp density of the woven fabric is 220 threads / inch, and the weft density is 200 threads / inch. It is woven using the Tsudakoma 8100 combined with the Staubli electronic dobby, with electronic let-off, electronic take-up, and electronic weft storage.
[0068] Step 2: Desizing and pre-setting;
[0069] The desizing process is as follows: fabric feeding - desizing - soaping - hot water washing - cold water washing; the auxiliaries used for desizing include: 6 - 8 g / L of desizing agent, 1.5 - 3 g / L of scouring agent, 2 - 3 g / L of penetrant, and the desizing temperature is 95°C; the soaping temperature is 80 - 85°C, the hot water washing temperature is 60 - 70°C, and the vehicle speed during the desizing process is controlled at 45 m / min.
[0070] Pre-setting is carried out using a hot air stenter: the pre-setting temperature is 195°C, and the setting time is 90 s. Through pre-setting, the fabric reaches an ideal and stable density.
[0071] The desized fabric can be dyed and fixed according to needs.
[0072] Step 3: Drying: After dehydration using a cylindrical centrifugal dehydrator, it is fully dried in a non-tension guiding net flat dryer. The drying temperature is 130°C, and the vehicle speed is 35 m / min.
[0073] Step 4: Setting
[0074] Prepare the setting solution: Dissolve NK GUARD S-573 waterproofing agent and TUBINGAL RNJ softener in water so that the concentration of NK GUARD S-573 waterproofing agent is 40 g / L and the concentration of TUBINGAL RNJ softener is 20 g / L; adjust the pH value to 5.0.
[0075] After impregnating and padding the nylon elastic jacquard and wrinkle-resistant fabric obtained in Step 3 in the above setting solution, setting and baking are carried out. The setting temperature is 170°C, and the setting time is 80 s.
[0076] Example 5
[0077] Manufacture a nylon elastic jacquard and wrinkle-resistant fabric, the fabric structure is as Figure 5As shown, it includes a surface weave and a bottom lining weave; the surface weave is a plain weave, which is interwoven by the first warp yarn 2 and the first weft yarn 1; the lining is a floating point jacquard weave, and the floating point jacquard weave cycle includes a single weft weave point and a floating line: the single weft weave point is interwoven by the second weft yarn 3, the first warp yarn 2 and the first weft yarn 1; the floating line is formed by the second weft yarn 3 between two adjacent single weft weave points, and the length is 3 weave points. The floating point jacquard weave cycle is continuously arranged in the weft direction of the surface weave; the floating point jacquard weave cycle is staggered and cyclically arranged in the warp direction of the surface weave, and the staggered cyclic arrangement is: 3 weave points are spaced in the warp direction, and 1 weave point is offset in the weft direction. The ratio of the first weft yarn to the second weft yarn is 3:1.
[0078] The production method is as follows:
[0079] Step 1: Weaving
[0080] The first warp yarn is made of 50D DTY nylon empty package 20D spandex yarn, the first weft yarn is made of 50D DTY nylon empty package 20D spandex yarn, and the second weft yarn is made of 70D ATY nylon yarn. The weave structure is as follows: Figure 5 The warp and weft double-sided weave shown is a plain weave with a second weft yarn in the inner weave of a floating jacquard weave. The weaving density is 200 strands / inch and the weft density is 190 strands / inch. Weaving is done using Tsudakoma 8100 combined with Stäubli electronic faucet, electronic warp feeding, electronic winding, and electronic weft storage.
[0081] Step 2: desizing and pre-setting;
[0082] The desizing process is: cloth feeding - desizing - soap washing - hot water washing - cold water washing; the auxiliaries used for desizing include: 6-8g / L desizing agent, 1.5-3g / L refining agent, 2-3g / L penetrant, desizing temperature is 95℃; the temperature of soap washing is 80-85℃, the temperature of hot water washing is 60-70℃, and the vehicle speed during desizing is controlled at 45m / min.
[0083] The pre-setting is done by using a hot air stenter: the pre-setting temperature is 195°C and the setting time is 80s. The pre-setting allows the fabric to achieve an ideal and stable density.
[0084] The desized fabric can be dyed and fixed as needed.
[0085] Step 3, drying: After dehydration using a drum centrifugal dehydrator, fully dry on a tension-free guide-net open-width dryer at a drying temperature of 130°C and a speed of 35m / min.
[0086] Step 4: Finalize
[0087] Prepare the setting solution: Dissolve NK GUARD S-573 water repellent and TUBINGAL RNJ softener in water to make the concentration of NK GUARD S-573 water repellent 50 g / L and the concentration of TUBINGAL RNJ softener 15 g / L; adjust the pH value to 5.5.
[0088] Dip and pad the nylon elastic jacquard anti-wrinkle fabric obtained in Step 3 in the above setting solution, and then carry out setting and baking. The setting temperature is 160 °C and the setting time is 70 s.
[0089] The nylon elastic jacquard anti-wrinkle fabric of the present utility model is woven with a plain surface weave and a floating line dot jacquard inner weave arranged in a cycle and staggered, and is desized, pre-set, dried and set using the production process of the present utility model. A flexible hydrophobic film with good folding resistance is formed on the fabric surface, so that it can maintain its original crisp shape without wrinkling after washing, has high shape stability, has good anti-wrinkle performance while maintaining good elasticity, and is not easy to wrinkle after washing.
[0090] It should be noted here that the description of these embodiments is used to help understand the present utility model, but does not constitute a limitation to the present utility model. In addition, the technical features involved in the various embodiments of the present utility model described above can be combined with each other as long as they do not conflict with each other. In addition, the above are only some embodiments of the present utility model, rather than all embodiments. All other embodiments obtained by those of ordinary skill in the art based on the embodiments of the present utility model without creative work fall within the scope of protection of the present utility model.
Claims
1. A nylon elastic jacquard wrinkle-resistant fabric, characterized in that: Including the surface organization and the bottom organization; The surface structure is a plain weave structure formed by interweaving the first warp yarn and the first weft yarn; The lining structure is a floating point jacquard structure, and the floating point jacquard structure cycle includes a single weft structure point and a floating line: the single weft structure point is formed by interweaving the second weft yarn, the first warp yarn and the first weft yarn; the floating line is formed by the second weft yarn between two adjacent single weft structure points, and the length is 3 or 5 structure points; The floating thread point jacquard structure cycles are continuously arranged in the weft direction of the surface structure; and the floating thread point jacquard structure cycles are staggered and cyclically arranged in the warp direction of the surface structure.
2. The nylon elastic jacquard anti-wrinkle fabric according to claim 1, characterized in that: The length of the floating thread is 5 tissue points, and the floating thread point jacquard tissue cycle is arranged in an interlaced cycle in the warp direction of the surface tissue in one of the following ways: a. There are 3 tissue points in the longitude direction and 3 tissue points are offset in the latitude direction; b. There are 2 tissue points in the longitude direction and 2 tissue points are offset in the latitude direction; c. There are 3 tissue points in the longitude direction and 1 tissue point is offset in the latitude direction.
3. The nylon elastic jacquard anti-wrinkle fabric according to claim 1, characterized in that: The length of the floating thread is 3 tissue points, and the floating thread point jacquard tissue cycle is arranged in an interlaced cycle in the warp direction of the surface tissue in one of the following ways: a. There are 2 tissue points in the longitude direction and 2 tissue points in the latitude direction; b. There are 3 tissue points in the longitude direction and 1 tissue point in the latitude direction.
4. The nylon elastic jacquard anti-wrinkle fabric according to claim 1, characterized in that: The first warp yarn is 40D-70D DTY nylon coated with 20D-40D spandex yarn, and the spandex is coated in an empty package or a machine package; the first weft yarn is 40D-70D DTY nylon coated with 20D-40D spandex yarn, and the spandex is coated in an empty package or a machine package.
5. The nylon elastic jacquard anti-wrinkle fabric as claimed in claim 4, characterized in that: The empty packages of the first warp yarns are empty package twisted; the second weft yarns are 70D-160D DTY nylon yarns or ATY nylon yarns.
6. The nylon stretch jacquard anti-wrinkle fabric according to any one of claims 1 to 5, characterized in that: The warp density is 120-250 strands / inch, and the weft density is 100-200 strands / inch.
Citation Information
Cited By
Nylon elastic jacquard anti-wrinkle fabric and production method thereof
CN118756405A
Ice silk cool jacquard fabric
CN224362986U