An airflow cavity and an annealing device
By designing a dual heating module and a gas circulation system, the problems of uneven thermal field and inert gas disturbance in the annealing device were solved, achieving uniform heating of the substrate and high-quality annealing effect of the film.
Patent Information
- Application Number
- CN202521906063.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2025-09-05
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2035-09-05
AI Technical Summary
Existing annealing equipment suffers from uneven thermal field and inert gas disturbance during large-area annealing, leading to localized rapid cooling of the substrate and film defects.
The design employs a dual heating module, which uses a suspended substrate and thermal inert gas, combined with a porous ceramic plate and a gas circulation system, to maintain an isothermal thermal field within the annealing chamber. Temperature sensors and flow control devices ensure uniform gas distribution.
Uniform heating of the substrate was achieved, avoiding thermal deformation and localized rapid cooling, and improving the annealing effect and the crystallinity and uniformity of the film.
Smart Images

Figure CN224987939U_ABST
Abstract
Description
Technical Field
[0001] This utility model relates to the technical field of annealing, and in particular to an airflow cavity and an annealing device. Background Technology
[0002] The annealing and crystallization process of the film structure is a crucial step in determining the photoelectric properties of thin films. Especially when preparing square-scale active layers, traditional annealing techniques face the following technical bottlenecks:
[0003] 1. Uncontrolled uniformity of large-area annealing
[0004] Existing annealing equipment mostly adopts contact hot plate annealing scheme: when the lower heating module is used, it relies on hot plate contact conduction, and uneven heating of glass substrate causes local temperature difference, resulting in the formation of mottled surface on perovskite, that is, a mixture of crystalline and amorphous regions; when the upper heating module is used, the radiant heat flow is interfered with by solvent vapor, the temperature gradient of the film surface changes sharply, and a hazy surface is produced, that is, large surface roughness.
[0005] 2. The introduction of inert gases disrupts the stability of the thermal field.
[0006] The annealing process requires the introduction of an inert gas to remove solvent vapors. However, existing technologies use cold gas, such as an inert gas at room temperature (23°C), which can easily cause localized rapid cooling of the substrate and induce film cracking. In addition, uneven distribution of the inert gas flow creates turbulent regions, leading to solvent vapor retention and hindering the directional growth of crystals.
[0007] To solve at least one of the above-mentioned technical problems, this utility model proposes an airflow cavity and an annealing device. Utility Model Content
[0008] The purpose of this invention is to provide an airflow cavity and an annealing device that can maintain an isothermal thermal field, prevent the heat source from directly contacting the substrate and causing substrate deformation, and prevent low-temperature inert gas from disrupting the uniformity of the thermal field, thereby improving the annealing effect.
[0009] The objective of this utility model is achieved through the following technical solution:
[0010] On the one hand, the present invention provides an airflow cavity, including a first heating module, a second heating module and a substrate, wherein the substrate is suspended between the first heating module and the second heating module, and the second heating module and the first heating module together form an annealing chamber;
[0011] The first heating module includes an air inlet, the outlet of which is connected to the annealing chamber, and the air inlet of which is connected to a gas input channel containing a thermo-inert gas.
[0012] The second heating module includes an exhaust port, the air inlet of which is connected to the annealing chamber, and the exhaust outlet of which is connected to a gas output channel.
[0013] The beneficial effects of the above solution are that the present invention maintains an isothermal thermal field in the annealing chamber through dual heating modules, and the second heating module draws in and promptly discharges solvent vapor to avoid hazy surface defects; the suspended substrate cuts off the contact heat conduction path, retaining only radiative heat transfer and hot gas convection, thus preventing temperature fluctuations caused by substrate thermal deformation from the source; and the introduction of thermal inert gas can prevent the low-temperature inert gas from disrupting the uniformity of the thermal field and causing localized rapid cooling of the substrate.
[0014] Furthermore, the first heating module includes:
[0015] A porous ceramic plate, wherein the pores of the porous ceramic plate are the air-filling pores, and the average pore diameter of the pores is greater than or equal to 20 μm.
[0016] The beneficial effect of the above solution is that the present invention ensures that the inert gas is blown evenly on the lower surface of the substrate through the porous ceramic plate, eliminating the local high temperature area caused by the heat transfer between the traditional hot plate and the substrate through contact, and avoiding surface defects.
[0017] Furthermore, the temperature of the thermal inert gas is between 120°C and 150°C.
[0018] The beneficial effect of the above solution is that, by limiting the temperature of the thermal inert gas to 120°C to 150°C, this invention can quickly remove the solvent while suppressing side reactions.
[0019] Furthermore, the gas input channel is provided with at least one of the following: a first pressure reducing valve, a first flow regulating valve, a first flow meter, a gas heater, and a first temperature sensor.
[0020] The beneficial effects of the above solution are that the present invention can respond to gas source pressure fluctuations and maintain a constant flow rate by using a first pressure reducing valve / first flow regulating valve to achieve dynamic pressure and flow stabilization; and can compensate for heat loss from gas flow by using a first temperature sensor and a gas heater to ensure temperature uniformity at the outlet of the gas input channel.
[0021] Furthermore, a second differential pressure sensor is provided on the gas output channel, which is used to monitor the pressure difference between the exhaust port and the chamber.
[0022] The beneficial effect of the above solution is that the present invention can assist in realizing closed-loop control of chamber pressure through the second differential pressure sensor.
[0023] Furthermore, the gas output channel is provided with at least one of a second pressure reducing valve, a second flow regulating valve, a second flow meter, and a second temperature sensor.
[0024] The beneficial effects of the above solution are that the present invention achieves air intake / exhaust balance with the assistance of a second flow regulating valve; and monitors the condensation point of solvent vapor with a second temperature sensor to prevent blockage of the exhaust port.
[0025] Furthermore, the outlet end of the gas input channel is connected to the porous ceramic plate, and the inlet end of the gas input channel is connected to a gas source.
[0026] The inlet of the gas output channel is connected to the exhaust port, and the outlet of the gas output channel is connected to the gas recovery system.
[0027] The beneficial effect of the above solution is that the present invention can assist in the formation of a gas circulation system through a gas source, a gas input channel, a gas output channel, an annealing chamber, and a gas recovery system, thereby reducing costs.
[0028] Furthermore, the second heating module includes a guide plate, on which a plurality of exhaust holes are formed, and the plurality of exhaust holes are evenly distributed;
[0029] The beneficial effect of the above solution is that, when using a small-sized substrate, the present invention uses uniformly distributed exhaust holes to obtain a uniform thermal field.
[0030] Furthermore, the second heating module includes a guide plate with multiple exhaust holes, the exhaust hole distribution density in the central region of the guide plate being different from the exhaust hole distribution density in the edge region of the guide plate.
[0031] The beneficial effect of the above solution is that, in the case of large-size substrates, this utility model solves the problem of rapid heat dissipation at the edges of large-size substrates by using exhaust holes with varying distribution densities. Specifically, by setting exhaust holes with a high density, the airflow at the edges can be forcibly increased, compensating for the non-uniformity of the thermal field.
[0032] Furthermore, the airflow cavity also includes:
[0033] Multiple temperature sensors are used to detect the temperature of different areas of the substrate.
[0034] On the other hand, this utility model provides an annealing apparatus, comprising:
[0035] Such as the airflow cavity described above;
[0036] A housing that encloses the airflow cavity.
[0037] The beneficial effect of the above solution is that the present invention reduces heat loss by insulating the shell.
[0038] Furthermore, the annealing apparatus also includes:
[0039] A first bracket and a second bracket are respectively disposed on opposite sides of the housing. The first side of the substrate is connected to the first bracket, and the second side of the substrate opposite to the first side is connected to the second bracket, so that the substrate is suspended between the first heating module and the second heating module.
[0040] The beneficial effect of the above solution is that the present invention avoids direct contact between the porous ceramic plate or other carrier and the substrate by suspending the substrate with a bracket, thus preventing thermal expansion of the substrate.
[0041] Compared with the prior art, the beneficial effects of this utility model include at least the following:
[0042] The airflow cavity and annealing device of this invention can maintain an isothermal thermal field, avoiding direct contact between the heat source and the substrate, thus preventing substrate deformation. It also prevents low-temperature inert gases from disrupting the uniformity of the thermal field, thereby improving the annealing effect. Specifically: a dual heating module maintains an isothermal thermal field within the annealing chamber; the second heating module draws in and promptly discharges solvent vapor, avoiding hazy surface defects; the suspended substrate cuts off the contact-type heat conduction path, retaining only radiative heat transfer and hot gas convection, preventing temperature fluctuations caused by substrate thermal deformation at the source; and the introduction of hot inert gas prevents low-temperature inert gases from disrupting the uniformity of the thermal field, thus avoiding localized rapid cooling of the substrate. Attached Figure Description
[0043] Figure 1 This is a schematic diagram of the annealing apparatus according to an embodiment of the present invention.
[0044] Figure 2 This is a schematic diagram of the airflow cavity according to an embodiment of the present invention.
[0045] Figure 3 This is a schematic diagram of the structure of a substrate according to an embodiment of the present invention.
[0046] Figure 4 This is a schematic diagram of a porous ceramic plate according to an embodiment of the present invention.
[0047] Figure 5 This is a schematic diagram of a gas input channel according to an embodiment of the present invention.
[0048] Figure 6 This is another structural schematic diagram of the airflow cavity according to an embodiment of the present invention.
[0049] Figure 7 This is a schematic diagram of the structure of a guide plate according to an embodiment of the present utility model.
[0050] Figure 8This is a schematic diagram of a gas output channel according to an embodiment of the present invention.
[0051] Figure 9 These are the ultraviolet-visible absorption spectra of Embodiment 1 and Comparative Example 1 of this utility model.
[0052] Figure 10 This is a comparison diagram of the nine-point absorption spectrum of Embodiment 1 of this utility model.
[0053] In the diagram: 1. Housing; 11. First side surface; 12. Second side surface; 13. Third side surface; 14. Fourth side surface; 15. Top surface; 16. Bottom surface; 21. First heating module; 211. Inflation port; 212. Gas input channel; 213. Porous ceramic plate; 214. First pressure reducing valve; 215. First flow regulating valve; 216. First flow meter; 217. Gas heater; 218. First temperature sensor; 2101. First through hole; 2102. First heating plate; 2103. First rectifier plate; 22. Second heating module; 221. Exhaust... 222. Gas outlet channel; 223. Guide plate; 2231. Central region; 2232. Transition region; 2233. Edge region; 224. Second pressure reducing valve; 225. Second flow regulating valve; 226. Second flow meter; 228. Second temperature sensor; 2201. Second through hole; 2202. Second heating plate; 2203. Second rectifier plate; 23. Substrate; 231. Ineffective region; 232. Effective region; 233. Sub-region; 24. Annealing chamber; 241. First chamber; 242. Second chamber; 25. Temperature sensor. Detailed Implementation
[0054] Exemplary embodiments will now be described more fully with reference to the accompanying drawings. However, these exemplary embodiments can be implemented in many forms and should not be construed as limited to the embodiments set forth herein; rather, these embodiments are provided to make the present invention more comprehensive and complete, and to fully convey the concept of the exemplary embodiments to those skilled in the art. The same reference numerals in the drawings denote the same or similar structures, and therefore repeated descriptions of them will be omitted.
[0055] The terms used to describe position and direction in this utility model are illustrated with the accompanying drawings, but changes can be made as needed, and all such changes are included within the scope of protection of this utility model.
[0056] In the description of this utility model, it should be understood that the terms "center," "longitudinal," "lateral," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," and "outer," etc., indicating orientation or positional relationships based on the orientation or positional relationships shown in the accompanying drawings, are only for the convenience of describing this utility model and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this utility model. Furthermore, the terms "first," "second," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Thus, features defined with "first," "second," etc., may explicitly or implicitly include one or more of that feature. In the description of this utility model, unless otherwise stated, "a plurality of" means two or more.
[0057] In the description of this utility model, it should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "joining" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art can understand the specific meaning of the above terms in this utility model based on the specific circumstances.
[0058] The annealing device of this utility model includes: an airflow cavity and a shell 1 covering the airflow cavity.
[0059] The shell 1 of this utility model is an insulated shell 1 made of double-layer stainless steel.
[0060] In application, the shell 1 of this utility model can be a hexahedral structure, an irregular hexahedral structure, or other shapes. Further, refer to... Figure 1 The housing 1 includes a top surface 15 and a bottom surface 16 disposed opposite to each other, a first side surface 11 and a second side surface 12 disposed opposite to each other, and a third side surface 13 and a fourth side surface 14 disposed opposite to each other. The top surface 15 and the bottom surface 16 are both perpendicular to the first side surface 11, the second side surface 12, the third side surface 13, and the fourth side surface 14. The first side surface 11, the third side surface 13, the second side surface 12, and the fourth side surface 14 are connected end-to-end in sequence, forming the sidewalls of the housing 1.
[0061] The opposite sides of the sidewall of the housing 1 (such as the first side 11 and the second side 12 arranged opposite each other, or the third side 13 and the fourth side 14 arranged opposite each other) are respectively provided with a first support and a second support. Specifically, the first side 11 of the housing 1 extends toward the center of the housing 1 to form the first support, and the second side 12 of the housing 1 extends toward the center of the housing 1 to form the second support. Furthermore, the first support and the second support can be used to connect components inside the airflow cavity, such as the substrate 23.
[0062] In practical applications, the lengths of both the first and second supports are less than the lengths of the first side 11 and the second side 12, and the widths of both the first and second supports are less than the width of the ineffective region 231 of the substrate 23. Preferably, the first and second supports are provided with a hollow structure, which can reduce the weight of the supports and further enable the airflow on the side of the supports facing the bottom surface 16 to communicate with the airflow on the side of the supports facing the top surface 15.
[0063] In actual implementation, when the first side of the substrate 23 is connected to the first support and the second side of the substrate 23 opposite to the first side is connected to the second support, the substrate 23 is suspended in the airflow cavity.
[0064] refer to Figure 2 The airflow cavity of this invention includes a first heating module 21 and a second heating module 22 arranged opposite to each other, multiple temperature sensors 25 (e.g., thermocouples), and a substrate 23. Specifically, the multiple temperature sensors 25 are used to detect the temperature of different areas of the substrate 23. The substrate 23 is suspended between the first heating module 21 and the second heating module 22, and the first heating module 21 and the second heating module 22 together form an annealing chamber 24. The first heating module 21 is parallel to and close to the bottom surface 16 of the housing 1; the second heating module 22 is parallel to and close to the top surface 15 of the housing 1.
[0065] The substrate 23 of this invention is embedded in the annealing chamber 24. The substrate 23 divides the annealing chamber 24 into a first chamber 241 and a second chamber 242. The first chamber 241 is close to the first heating module 21, and the second chamber 242 is close to the second heating module 22.
[0066] In application, the effective area 232 of substrate 23 is coated with a layer and requires annealing. The coating can be a layer structure or a perovskite precursor solution. The perovskite precursor solution includes a solvent and a solute, wherein the solute is PbI2 and CH3NH3I; the solvent is selected from at least one of N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), gamma-butyrolactone (GBL), and isopropyl alcohol (IPA). DMF has the molecular formula HCON(CH3)2 and a saturated vapor pressure of 0.47 kPa at room temperature; DMSO has the molecular formula (CH3)2SO and a saturated vapor pressure of 0.08 kPa at room temperature; GBL has the molecular formula C4H6O2 (a five-membered cyclic ester) and a saturated vapor pressure of 0.2 kPa at room temperature; IPA has the molecular formula (CH3)2CHOH and a saturated vapor pressure of 5.87 kPa at room temperature. Room temperature is generally 23°C.
[0067] In practical applications, refer to Figure 3 The invalid region 231 of substrate 23 is the outer edge of substrate 23, and the width of the invalid region 231 is 5mm to 20mm. The effective region 232 of substrate 23 is the central part of substrate 23, and the area of the effective region 232 accounts for more than 90% of the total area of substrate 23. Furthermore, the effective region 232 of substrate 23 can be equally divided into multiple sub-regions 2323, and the multiple sub-regions 2323 are arranged in an array. Each sub-region 2323 is equipped with at least one temperature sensor 25 to detect the temperature of the corresponding sub-region 2323 in real time.
[0068] The first heating module 21 of this utility model includes an air inlet 211, a porous ceramic plate 213, and a gas input channel 212.
[0069] When applying, refer to Figure 4The porous ceramic plate 213 of this invention has pores that are the air filling holes 211. The average pore diameter of the porous ceramic plate 213 is greater than or equal to 20 μm. Preferably, the air permeability of the porous ceramic plate 213 is 35%. Further, the porous ceramic plate 213 includes a first surface and a second surface arranged opposite to each other. The first surface of the porous ceramic plate 213 is connected to the gas input channel 212, and the second surface of the porous ceramic plate 213 faces the second heating module 22. The gas input channel 212 of this invention is used to introduce thermal inert gas and is connected to the porous ceramic plate 213. Specifically, the inlet end of the gas input channel 212 is connected to a gas source, which can be an inert gas storage device, including a storage tank, and the storage tank pipeline is connected to the inlet end of the gas input channel 212; the outlet end of the gas input channel 212 is connected to the first surface of the porous ceramic plate 213, so that the hot inert gas flows from the first surface to the second surface through the pores of the porous ceramic plate 213 and flows to the annealing chamber 24, so as to form a uniform heat flow through the lower surface of the substrate 23 and from the periphery of the substrate 23 to the upper surface of the substrate 23, so as to provide hot inert gas for annealing the effective area 232 of the substrate 23. The hot inert gas is generally 120°C to 150°C.
[0070] In practical applications, refer to Figure 5The gas input channel 212 of this invention is equipped with at least one of the following: a first pressure reducing valve 214, a first flow regulating valve 215, a first flow meter 216, a gas heater 217, and a first temperature sensor 218. Preferably, along the direction of inert gas flow within the gas input channel 212, the gas input channel 212 is sequentially equipped with the first pressure reducing valve 214, the first flow regulating valve 215, the first flow meter 216, the gas heater 217, and the first temperature sensor 218. Furthermore, a first differential pressure sensor may also be provided on the gas input channel 212. The first pressure reducing valve 214 stabilizes the inert gas source pressure, buffers fluctuations in external gas supply, and prevents sudden changes in airflow velocity from causing a sudden change in the local temperature of the substrate 23. The first flow regulating valve 215 dynamically regulates the flow rate of the inert gas in the gas input channel 212, for example, from 80 L / min to 120 L / min, maintaining a constant air curtain thickness around the porous ceramic plate 213 and ensuring uniform thermal convection below the substrate 23. The first flow meter 216 monitors the inlet flow rate in real time and feeds it back to the first flow regulating valve 215. The gas heater 217 heats the inert gas to 120 L / min. The inert gas is preheated to 150°C to avoid cold shock to the annealing chamber 24. At the same time, it can also compensate for the heat loss of the gas input channel 212 and ensure that the gas temperature in the gas input channel 212 is uniform. The first temperature sensor 218 is used to monitor the gas temperature of the inert gas at the gas inlet end of the gas input channel 212 and feed it back to the gas heater 217. The first differential pressure sensor is used to detect the pressure difference near the first surface and the second surface of the porous ceramic plate 213 to determine whether the ceramic plate is blocked, so as to ensure that the inert gas penetrates the porous ceramic plate 213 uniformly.
[0071] In actual implementation, when the first differential pressure detected by the first differential pressure sensor is greater than the first differential pressure threshold, it indicates that the pores of the porous ceramic plate 213 are blocked, triggering an alarm (e.g., an alarm buzzer) and reducing the gas flow rate of the inert gas by adjusting the first flow regulating valve 215.
[0072] refer to Figure 6 The first heating module 21 of this utility model may further include a first heating plate 2102 and a first rectifier plate 2103.
[0073] In application, the first heating plate 2102 is used to heat the annealing chamber 24 to provide environmental conditions for the annealing of the substrate 23. Furthermore, the first heating plate 2102 is provided with a first through hole 2101, which is used to avoid the gas input channel 212.
[0074] In practical applications, the first rectifier plate 2103 is disposed between the porous ceramic plate 213 and the first heating plate 2102, and the first rectifier plate 2103 is connected to the outlet end of the gas input channel 212. The thermal inert gas is sequentially filled into the gas flow cavity through the gas input channel 212, the first rectifier plate 2103, and the porous ceramic plate 213.
[0075] In actual implementation, the first heating plate 2102 and the first rectifier plate 2103 can be implemented using existing heating plates and rectifier plates, so this utility model will not be described in detail.
[0076] The second heating module 22 of this utility model includes an exhaust port 221, a guide plate 223, and a gas output channel 222. The guide plate 223 may be an aluminum plate.
[0077] When applying, refer to Figure 7 The guide plate 223 has multiple exhaust holes 221. The air inlet of the exhaust hole 221 is connected to the annealing chamber 24. The exhaust outlet of the exhaust hole 221 is connected to the inlet of the gas output channel 222 for discharging gas. The outlet of the gas output channel 222 is connected to the gas recovery system to avoid environmental pollution.
[0078] The distribution of vent holes 221 on the guide plate 223 includes two types: one is that multiple vent holes 221 are evenly distributed, which is suitable for small-sized substrates 23; the other is that the distribution density of vent holes 221 in the central region 2231 of the guide plate 223 is different from the distribution density of vent holes 221 in the edge region 2233 of the guide plate 223, which is suitable for large-sized substrates 23. Preferably, the substrate 23 and the guide plate 223 are coaxially arranged, and from the center point of the guide plate 223 to the edge, it is divided into a central region 2231, a transition region 2232, and an edge region 2233. The edge region 2233 corresponds to the ineffective region 231 and part of the effective region 232 of the substrate 23, and the central region 2231 and the transition region 2232 correspond to the effective region 232 of the substrate 23.
[0079] Furthermore, the distribution density of vent holes 221 in the central region 2231 is less than that in the transition region 2232, which is less than that in the edge region 2233. The lower distribution density of vent holes 221 in the central region 2231 reduces the extraction speed, preventing overheating of the substrate 23 region corresponding to the central region 2231 of the guide plate 223. The higher distribution density of vent holes 221 in the edge region 2233 increases the exhaust flow rate, enhancing airflow convection heat transfer efficiency and preventing excessively low temperatures in the substrate 23 region corresponding to the edge region 2233 of the guide plate 223. This invention, by matching the heat dissipation gradient and setting unevenly distributed vent holes 221, can both form a uniform, constant-temperature thermal field with the first heating module 21 and prevent solvent vapor from accumulating and stagnating at angles.
[0080] In practical applications, each area of the guide plate 223 has an exhaust port 221 that is independently matched with a gas output channel 222.
[0081] Furthermore, a second differential pressure sensor is provided on the gas output channel 222. Additionally, refer to... Figure 8 The gas output channel 222 is equipped with at least one of the following: a second pressure reducing valve 224, a second flow regulating valve 225, a second flow meter 226, and a second temperature sensor 228. Preferably, along the direction of inert gas flow within the gas output channel 222, the gas output channel 222 is sequentially equipped with the second pressure reducing valve 224, the second flow regulating valve 225, the second flow meter 226, and the second temperature sensor 228. Specifically, the second pressure reducing valve 224 is used to stabilize the exhaust back pressure, preventing pressure fluctuations downstream (e.g., in a gas recovery system) from affecting the pressure stability of the annealing chamber 24; the second flow regulating valve 225 is used to dynamically adjust the exhaust flow rate to match the intake flow rate, maintaining a slight positive pressure of 5 Pa to 10 Pa in the chamber to prevent backflow of external air; the second flow meter 226 is used to monitor the exhaust flow rate in real time, and the exhaust flow rate can be compared with the intake flow meter data to calculate the gas retention; the second temperature sensor 228 is used to monitor the exhaust temperature to warn of solvent condensation risk and prevent blockage of the exhaust port 221; and the second differential pressure sensor is used to monitor the pressure difference between the exhaust port and the annealing chamber.
[0082] In actual implementation, when the second differential pressure detected by the second differential pressure sensor is greater than the second differential pressure threshold, it indicates that the airflow in the annealing chamber 24 is turbulent and the thermal field is distorted, triggering an alarm (e.g., an alarm buzzer). The flow rate of the inert gas in the gas output channel 222 is reduced by adjusting the second flow regulating valve 225. When the second differential pressure detected by the second differential pressure sensor is less than the second differential pressure threshold, it indicates poor exhaust and solvent vapor retention. The flow rate of the inert gas in the gas output channel 222 is increased by adjusting the second flow regulating valve 225 to accelerate solvent vapor extraction.
[0083] When the temperature difference between a sub-region 2323 of a substrate 23 and the average temperature of the substrate 23 is detected to be greater than the first temperature threshold, the second flow regulating valve 225 on the gas output channel 222 corresponding to the guide plate 223 region of the current sub-region 2323 is adjusted so that the first temperature difference between the temperature of each sub-region 2323 of the substrate 23 and the average temperature of the substrate 23 is less than or equal to the first temperature threshold.
[0084] The second heating module 22 of this utility model may further include a second heating plate 2202 and a second rectifier plate 2203.
[0085] In application, the second heating plate 2202 is used to heat the annealing chamber 24 to provide environmental conditions for the annealing of the substrate 23. Furthermore, the second heating plate 2202 is provided with a second through hole 2201, which is used to avoid the gas output channel 222.
[0086] In practical applications, the second rectifier plate 2203 is positioned between the guide plate 223 and the second heating plate 2202, and the second rectifier plate 2203 is connected to the inlet of the gas output channel 222. The gas in the annealing chamber 24 is discharged from the gas flow chamber sequentially through the exhaust port 221, the second rectifier plate 2203, and the gas output channel 222.
[0087] In actual implementation, the second heating plate 2202 and the second rectifier plate 2203 can be implemented using existing heating plates and rectifier plates, so this utility model will not be described in detail.
[0088] To make the objectives, technical solutions, and advantages of this utility model clearer, specific embodiments and comparative examples are provided to further illustrate this utility model in detail. It should be understood that the specific embodiments and comparative examples described herein are merely illustrative of this utility model and are not intended to limit its scope.
[0089] Example 1 / Case 1
[0090] Components of the perovskite precursor solution:
[0091] Solute mass ratio: Formamidine iodide (FAI): Lead iodide (PbI2): Cesium bromide (CsBr) = 5.93:18.07:1.
[0092] Solvent volume ratio: N,N-dimethylformamide (DMF):acetonitrile (ACN) = 9:1.
[0093] The mass fraction of the solute is 43.3%.
[0094] Perovskite precursor coating:
[0095] Substrate 23: Glass, with dimensions of 1m × 0.6m × 2.2mm.
[0096] Process: Slot coating. Dispensing speed: 40 μL / s; Dispensing speed: 50 mm / s.
[0097] Thin film solvent removal: The substrate 23 coated with perovskite precursor solution is subjected to vacuum crystallization (VCD) at a pressure of 5 Pa.
[0098] Thin film annealing: achieved using the annealing apparatus of this invention. Inert gas temperature: 130℃; inert gas flow rate: 80L / min; annealing time: 20min.
[0099] Comparative Example 1
[0100] The difference between Comparative Example 1 and Example 1 lies in the film annealing step. The film annealing step of Comparative Example 1 is as follows:
[0101] The annealing process was achieved using an existing annealing apparatus, with the substrate 23 in direct contact with the stage. The inert gas temperature was 130°C; the inert gas flow rate was 80 L / min; and the annealing time was 20 min.
[0102] The perovskite films obtained in Example 1 and Comparative Example 1 were characterized by UV-Vis absorption. (Reference) Figure 9 It can be seen that, within the wavelength range of 338 nm to 813 nm, the perovskite film obtained in Example 1 exhibits stronger UV-Vis absorption than that in Comparative Example 1. This indicates that the perovskite film obtained in Example 1 possesses stronger absorption and better crystallinity.
[0103] Furthermore, the perovskite films obtained in Example 1 and Comparative Example 1 were subjected to UV-Vis absorption characterization at 9 points, with reference to... Figure 10 .Will Figure 10 The values obtained were used to calculate the uniformity of UV-Vis absorption. The UV-Vis absorption uniformity of Example 1 was 1.83%, while that of Comparative Example 1 was 10.88%, indicating that the perovskite film obtained in Example 1 had better uniformity.
[0104] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and alterations to the above embodiments within the scope of the present invention without departing from the principles and spirit of the present invention, and all such changes should fall within the protection scope of the claims of the present invention.
Claims
1. An airflow cavity, characterized in that, include: A first heating module (21), a second heating module (22), and a substrate (23) are provided. The substrate (23) is suspended between the first heating module (21) and the second heating module (22). The second heating module (22) and the first heating module (21) together form an annealing chamber (24). The first heating module (21) includes an air filling hole (211), the air outlet of the air filling hole (211) is connected to the annealing chamber (24), the air filling port of the air filling hole (211) is connected to the gas input channel (212), and the gas input channel (212) contains a thermo-inert gas. The second heating module (22) includes an exhaust port (221), the air inlet of which is connected to the annealing chamber (24), and the exhaust port of which is connected to the gas output channel (222).
2. The airflow cavity according to claim 1, characterized in that, The first heating module (21) includes: A porous ceramic plate (213), wherein the pores of the porous ceramic plate (213) are the air filling holes (211), and the average pore diameter of the pores is greater than or equal to 20 μm.
3. The airflow cavity according to claim 1, characterized in that, The temperature of the thermal inert gas is between 120°C and 150°C.
4. The airflow cavity according to claim 1, characterized in that, The gas input channel (212) is provided with at least one of the following: a first pressure reducing valve (214), a first flow regulating valve (215), a first flow meter (216), a gas heater (217), and a first temperature sensor (218).
5. The airflow cavity according to claim 1, characterized in that, The gas output channel (222) is equipped with a second differential pressure sensor, which is used to monitor the pressure difference between the exhaust port and the chamber.
6. The airflow cavity according to claim 2, characterized in that, The outlet end of the gas input channel (212) is connected to the porous ceramic plate (213), and the inlet end of the gas input channel (212) is connected to a gas source. The inlet of the gas output channel (222) is connected to the exhaust port (221), and the outlet of the gas output channel (222) is connected to the gas recovery system.
7. The airflow cavity according to claim 1, characterized in that, The second heating module (22) includes a guide plate (223), on which a plurality of exhaust holes (221) are provided, and the plurality of exhaust holes (221) are evenly distributed; Alternatively, the second heating module (22) includes a guide plate (223), on which a plurality of exhaust holes (221) are provided. The distribution density of the exhaust holes (221) in the central region (2231) of the guide plate (223) is different from the distribution density of the exhaust holes (221) in the edge region (2233) of the guide plate (223).
8. The airflow cavity according to claim 1, characterized in that, The airflow cavity further includes: Multiple temperature sensors (25) are used to detect the temperature of different areas of the substrate (23).
9. An annealing apparatus, characterized in that, include: The airflow cavity as described in any one of claims 1 to 8; The housing (1) covers the airflow cavity.
10. The annealing apparatus according to claim 9, characterized in that, The annealing apparatus further includes: The first bracket and the second bracket are respectively disposed on opposite sides of the housing (1). The first side of the substrate (23) is connected to the first bracket, and the second side of the substrate (23) opposite to the first side is connected to the second bracket, so that the substrate (23) is suspended between the first heating module (21) and the second heating module (22).