Partially electroplatable multi-component plastic blank; plastic component and method for manufacturing the plastic component from the multi-component plastic blank

The multi-component plastic blank with a recessed geometric structure effectively prevents overgrowth at the border areas between different plastics, improving production efficiency and appearance while maintaining cost-effectiveness.

DE102012109659B4Active Publication Date: 2024-11-14KUNST BERNT
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
DE102012109659
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2012-10-10
Publication Date
2024-11-14
Estimated Expiration
2032-10-10

AI Technical Summary

Technical Problem

Existing methods for partially metallizing plastic components face issues such as overgrowth at the border areas between different plastics, leading to unsatisfactory appearance and increased production costs, especially in high-visibility areas.

Method used

A multi-component plastic blank with a recessed geometric structure is used, where the boundary line between two plastics with different electroplating properties is positioned within a recessed geometric feature, preventing overgrowth during electroplating.

Benefits of technology

This approach reduces overgrowth at the border areas, enhances production efficiency, and maintains the desired appearance of the component without significant cost increase, allowing for high-quality, partially metallized plastic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Partially electroplatable multi-component plastic blank (10) with a metal layer (20), comprising at least a first region (11) made of a first plastic and a second region (12) made of a second plastic, which are arranged at least partially adjacent to one another on the surface of the multi-component plastic blank (10), whereby a boundary line (15) is formed between the two regions (11; 12) made of different plastics, wherein the first plastic of the first region (11) is a plastic with which an electroplatable region can be produced by pretreatment steps, while the second plastic of the second region (12) is a plastic with which an electroplatable region cannot be produced by the same pretreatment steps. where in the surface of the multi-component plastic blank (10) at least one recessed geometric structure (30') is formed and the boundary line (15) between the two plastics runs at least partially within the recessed geometric structure (30'), wherein the recessed geometric structure is formed as a groove (30') and the boundary line (15) runs within the area of ​​a side wall (33) of the groove characterized in that the boundary line (15) divides the side wall (33).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a partially electroplated multi-component plastic blank, as well as a plastic component provided with a metal decorative layer and a method for producing such a plastic component from the multi-component plastic blank.

[0002] It is known in the art to metallize the surface of plastic components to give them an attractive appearance, particularly for decorative purposes. This is done, for example, for control elements in motor vehicles, such as handles, buttons, knobs, and gearshift knobs, but also for trim strips, speakers, etc. Such plastic components are also frequently used in the household appliance sector.

[0003] There are essentially two processes used to produce metallized plastic elements. These are based either on the metallization of a plastic component using PVD (physical vapor deposition) or on the galvanization of a plastic element using electrochemical processes. While both processes generally allow the application of durable metal coatings to plastic components, it is still difficult to metallize control elements, for example, using PVD in such a way that the metal layer deposited on the plastic part has sufficient abrasion and corrosion resistance even without an additional protective layer, e.g. a transparent protective coating. Furthermore, plastic parts metallized using PVD do not have the often desired "cold touch" due to the low layer thicknesses of the applied metal layers.The feel of the metallized plastic part does not correspond to that of a metal part. Electroplating of plastic components has therefore proven more advantageous, particularly in the area of ​​control elements in motor vehicles.

[0004] Furthermore, it may be necessary to metallize only partially a plastic component because some areas are intended to have a metallic appearance while others are not. This can be due to technical and / or optical reasons. Various processes are known for the partial or selective electroplating of plastic components. One approach involves preparing the surface of the plastic component differently in certain areas so that metallization subsequently takes place in one area while not in another.

[0005] For example, patent DE 102 08 674 B4 describes a method for producing operating, decorative, or display elements with backlit symbols. In this method, an area of ​​a plastic component is first covered to prevent electroplating of the plastic in this area. The covering can be achieved, for example, with a sticker or a so-called masking varnish, and the area covered in this way has the shape of the symbol to be created. A thin metal layer is then applied, which can, however, be easily removed again in the area of ​​the previous covering. This can be done by laser ablation. The metallic surface coating can then be completed in the remaining area of ​​the metal layer by electroplating, while retaining the symbol.

[0006] Another approach involves constructing a component from various plastics with different properties to enable selective electroplating. An example of this is published patent application DE 10 2006 037 535 A1, which discloses a method for manufacturing a composite product with selective electroplating from a hard plastic component and a soft plastic component. The material used for the soft plastic component is a thermoplastic made of a styrene-based elastomer and polyolefin, which is resistant to chromic acid.

[0007] Selective electroplating based on the different properties of the plastics used in a component can also be used for two or more rigid plastics, whereby such composite components can be manufactured, for example, in a multi-shot process. For example, one plastic can be a non-electroplating material such as polycarbonate (PC), polymethyl methacrylate (PMMA), or polyethylene terephthalate (PET), while the electroplating material is typically acrylonitrile butadiene styrene (ABS) or an ABS / PC blend. The component is then molded so that at least two different plastics are present on its surface, which determine the electroplating capability of the corresponding areas.

[0008] This selective electroplating of plastic components through the use of different plastics within the surface of the component and a specific pretreatment has proven advantageous and can be carried out reliably from a process engineering perspective. However, metal overgrowth can still occur in the boundary between the two plastic types on areas not to be electroplated. This overgrowth is often unacceptable, especially in clearly visible areas, because the boundary line between the metallized and non-metallized areas is then blurred, thus impairing the desired properties of the component. Such overgrowth therefore often has to be removed in subsequent process steps, which can be very complex, or it can result in large amounts of scrap, which is also disadvantageous.

[0009] DE 199 19 709 A1 discloses a partially electroplated polymer molded part that has sections with varying degrees of electroplating capability. These sections consist of electroplatable or non-electroplatable polymers and are separated from each other by V-shaped grooves. The sections made of electroplatable polymers have a galvanic coating.

[0010] A partially electroplated polymer molded part with comparable properties is known from US 3 640 789 A.

[0011] Based on this, it is the object of the present invention to provide a partially electroplated plastic blank made of at least two different plastics, which reduces the risk of overgrowth in the boundary area between the two plastics during electroplating and at the same time can be produced on a large-scale at low cost.

[0012] It is a further object of the invention to provide a plastic component comprising such a plastic blank and a method for producing the plastic component.

[0013] According to the invention, this object is achieved by a multi-component plastic blank according to independent claim 1. Advantageous developments of this multi-component plastic blank are set out in subclaims 2-10. Furthermore, the object is achieved by a plastic component according to independent claim 11 and a method for producing this plastic component according to claim 12. An advantageous development of the method is set out in claim 13.

[0014] The multi-component plastic blank according to the invention can be partially electroplated with a metal layer because it has at least a first region made of a first plastic and a second region made of a second plastic. These two regions are arranged adjacent to one another in the surface of the multi-component plastic blank, at least in some areas, whereby a boundary line is formed on the surface between the two regions made of different plastics. The first plastic of the first region is selected such that a electroplatable region can be produced from it through specific pretreatment steps, while the second plastic of the second region is selected such that no electroplatable region can be produced from it through the same pretreatment steps.The entire multi-component plastic blank can thus be subjected to the same process steps, but the second region survives the electroplating process essentially unchanged while the first region is electroplated. This makes the blank a partially electroplatable component, as the plastics used in it react differently to the same pretreatment steps, resulting in regions with and without a metal layer forming during subsequent electroplating of the component. Therefore, in the context of this invention, the first plastic of the region to be electroplated can also be referred to as an electroplatable plastic, while the second plastic of the region not to be electroplated is referred to as a non-electroplatable plastic.

[0015] The surface of the first plastic can be converted into a surface that is electroplatable, in particular through pretreatment steps such as pickling, roughening, and / or swelling, while the surface of the second plastic cannot be simultaneously converted into a surface that is electroplatable through the same pretreatment steps. Thus, the surface of the area not to be electroplated is not altered by these pretreatment steps, or at least not in such a way that it becomes electroplatable.

[0016] For electroplating, the surface of the first plastic can, for example, be converted by the pretreatment steps into a surface that can be activated by palladium nuclei, while the surface of the second plastic cannot be converted by the same pretreatment steps into a surface that can be activated by palladium nuclei.

[0017] The first plastic can be, for example, polyamide, acrylonitrile butadiene styrene (ABS), or an ABS / polycarbonate blend, while the second plastic can be polycarbonate (PC), polymethyl methacrylate (PMMA), or polyethylene terephthalate (PET). In the case of ABS or an ABS / PC blend as the first plastic, the butadiene components would be at least partially dissolved out by pickling, for example in a chromic acid bath, so that pores and cavities would form in the surface, which could then be nucleated, for example, from a colloidal solution with palladium nuclei. In the case of polyamide as the first plastic, the roughness of the surface could be increased by swelling, so that the surface could then also be nucleated with palladium nuclei from a colloidal solution.However, the plastics of the second group, especially PC, survive pretreatment steps such as pickling or swelling largely unchanged, so that even when placed in a colloidal solution containing palladium nuclei, their surface is not nucleated to such an extent that electroplating could subsequently occur.

[0018] In order to prevent overgrowth of the metal layer from the area of ​​galvanizable plastic to the area of ​​non-galvanizable plastic, according to the invention at least one recessed geometric structure is formed in the surface of the multi-component plastic blank, wherein the boundary line between the two plastics runs at least partially within the recessed geometric structure.

[0019] It has been shown that by forming a recessed geometric structure and arranging the boundary line within this recessed structure, overgrowth in the boundary area between the two plastics can be prevented during partial electroplating of the plastic blank. Tests have shown that components with this recess exhibit little or no overgrowth, whereas otherwise identical components and identical process conditions showed increased overgrowth. It is assumed that this is due to the drainage of the media during the pre-treatment of the plastic blank for subsequent electroplating. Although components with a defect-free coating can be manufactured without this recess, it is safer to use the recess in the boundary area of ​​the process window, resulting in less scrap and a smaller number of components that require rework.Furthermore, the multi-component plastic blank according to the invention can be produced on a large-scale without the recessed structure significantly increasing production costs compared to components without a recess. It is therefore a simple but effective means of improving the quality of partially galvanized multi-component plastic components.

[0020] It is essential that the boundary line between the two plastics runs within the recessed geometric structure so that the geometric structure can prevent overgrowth in precisely this area. However, the boundary line between the two plastics does not have to run entirely within the recess; it would also be possible for overgrowth to be prevented only in certain areas. In such a case, the recessed geometric structure would enclose the boundary line only in these areas, while in other areas the boundary line would run without additional measures, i.e., without a recessed structure, as the basic geometry of the respective component dictates for partial electroplating.

[0021] The multi-component plastic blank according to the invention can be constructed in different ways. In a first exemplary embodiment of the invention, the areas of the surface of the multi-component plastic blank that border the recessed geometric structure on opposite sides lie on the same plane. These two surface areas are thus aligned, and without the recess, the plastic blank would have a continuous surface without steps or the like. Without the recess according to the invention, overgrowths would thus protrude clearly visible from the metal layer on the electroplatable plastic beyond the boundary line onto the non-electroplatable plastic. However, the common plane of the two areas does not have to be flat; it can also be a curved plane if, for example, the surface of the plastic blank is curved or even wavy.

[0022] In another exemplary embodiment, the areas of the surface of the multi-component plastic blank that border on the recessed geometric structure on opposite sides lie in two different planes. The surface areas made of different plastic are therefore not aligned; even without the recess, there would be some type of step, edge or angle in the boundary area between the two plastics. The two planes can, for example, run essentially parallel to one another. There is therefore a step, so that the plastic blank is higher on one side of the recessed geometric structure than on the other side, but the two step planes run essentially parallel to one another. However, here too, the two planes do not necessarily have to be flat; they can also be curved planes if the surface of the plastic blank is curved.

[0023] In another embodiment, the two planes extend at an angle other than 180° to each other. Even without the recess, the two areas made of different plastics would meet at an angle, allowing overgrowths to protrude beyond the inner edge between the two plastics.

[0024] The geometric structure provided according to the invention is preferably made as small as possible so as not to change the fundamentally desired geometry of the plastic component too significantly. This applies in particular to boundary lines in the visible and / or tactile area of ​​a component. However, even with boundary lines in less sensory relevant areas, it can be useful to make the recessed geometric structure as small as possible, for example, so as not to weaken the component too much. However, the recess must be made large enough to achieve the desired effect. The recess could also be integrated into the geometry of the component in such a way that it fulfills additional technical or optical functions. Furthermore, the minimum dimensions of the recessed geometric structure are also limited by parameters during production of the plastic blank.If the component is manufactured using an injection molding process, for example, the width and depth of the geometric structure are limited by the tool used if only certain minimum dimensions can be realized.

[0025] For example, the depth of the geometric structure can range from 0.3 to 1.0 millimeters, with approximately 0.5 millimeters being preferred. A depth of 0.5 millimeters has produced good results in tests for various plastic components without significantly compromising the fundamental design of the respective plastic component. Furthermore, such depths can be easily implemented in injection molding tools. However, the recessed geometric structure can also be made shallower or much deeper if necessary.

[0026] The width of the recessed geometric structure can also be in the range between 0.3 and 1.0 millimeters, preferably 0.5 millimeters, whereby the selection of the width is essentially subject to the same criteria as for the depth.

[0027] The recessed geometric structure can have various shapes, but is preferably a groove with a square cross-section, comprising a bottom wall and two opposing side walls. However, the cross-section of this groove does not have to be rectangular; the bottom wall and the side walls can also be at angles to each other that differ from 90°. For example, the groove can also have a trapezoidal cross-section. Furthermore, individual walls of the groove can also be curved and / or have rounded inner edges.

[0028] According to the invention, the boundary line between the two plastics runs within the surface of a side wall of the groove. Part of the surface of this side wall thus consists of the electroplatable plastic, while the other part consists of the non-electroplatable plastic. The boundary line divides the side wall, for example, in a ratio of approximately 2:1, with the smaller part bordering the inner edge of the groove formed by the bottom wall and the side wall within which the boundary line runs.

[0029] Particularly good results can be achieved if the groove is formed largely from the non-galvanizable plastic material. For example, if the boundary line between the plastics coincides with an inner edge of the groove, the surface of one side wall of the groove is formed by the galvanizable plastic, while the bottom surface and the other side wall are formed by the non-galvanizable plastic.

[0030] Even in embodiments where this boundary line runs within the side wall of a groove, this can be implemented in a fundamentally similar manner. In this case, the surface of a first side wall, the bottom wall, and a portion of the second side wall are formed by the non-electroplatable plastic, while the surface of the other portion of the second side wall is formed by the electroplatable plastic. This other portion of the second side wall made of electroplatable plastic is the portion of the side wall facing the opening of the groove.

[0031] The invention further encompasses a plastic component comprising a multi-component plastic blank according to one or more of the described embodiments. A metal layer is applied to the first region of the multi-component plastic blank made of a first plastic, while no metal layer is applied to the second region made of a second plastic. The metal layer then protrudes at least partially into the recessed geometric structure.

[0032] Furthermore, the invention also encompasses a related method for producing such a plastic component, which provides for a multi-component plastic blank according to one or more of the described embodiments to be completely treated with pretreatment steps such that the surface of the first plastic of the first region becomes electroplatable, while the surface of the second plastic of the second region cannot be electroplated by the same pretreatment steps. Subsequently, electroplating of the electroplatable region can be carried out with or without further intermediate steps.

[0033] In a preferred embodiment of the invention, the multi-component plastic blank was previously produced in an injection molding process.

[0034] Further advantages, special features and expedient developments of the invention emerge from the subclaims and the following representation of preferred embodiments with reference to the figures.

[0035] From the illustrations shows: Fig. 1a shows a schematic cross-section through an embodiment of a partially electroplated multi-component plastic blank without the geometric structure according to the invention for preventing overgrowth; Fig. 1b a multi-component plastic blank according to Fig. 1a after selective electroplating; Fig. 1c a plan view of a galvanized multi-component plastic blank according to Fig. 1b; Fig. 2a shows a schematic cross section through a first embodiment of a partially electroplated multi-component plastic blank with the geometric structure not according to the invention for preventing overgrowth; Fig. 2b an enlarged view of the geometric structure for preventing overgrowth according to Fig. 2a; Fig. 2c a multi-component plastic blank according to Fig. 2a after selective electroplating; Fig. 2d a plan view of a multi-component plastic blank according to Fig. 2c; Fig. 3 a schematic cross-section through a second embodiment of a partially electroplated multi-component plastic blank with the geometric structure according to the invention for preventing overgrowth; and Fig. 4 a schematic cross section through a third embodiment of a partially electroplated multi-component plastic blank with the geometric structure not according to the invention for preventing overgrowth.

[0036] The Fig. Figure 1a shows a schematic cross-section through an embodiment of a partially electroplated multi-component plastic blank without the inventive geometric structure for preventing overgrowth, as is known from the prior art. The plastic blank is a preferably circular and hollow button that can be used in a motor vehicle, for example, as a start-stop button. At least the outer surfaces of the hollow-cylindrical button are to be provided with a metallic layer by electroplating. This metallic layer also extends into the interior of the hollow button, but no metallization is to be applied to the back of the button's pressing surface.On the front side of the button's printing surface, the metal layer can then be removed again in some areas to create a symbol that can be backlit from the inside of the button, since the plastic blank is preferably transparent or at least translucent.

[0037] For this purpose, the button is manufactured as a multi-component plastic blank from different plastics before electroplating. A first plastic is electroplatable, and from this plastic, those areas of the blank are formed that are later to be metallized, for example, with chrome. This first area 11 of the multi-component plastic blank is also marked with the letter "G" in the figures to indicate it as a electroplatable area. For example, this includes the front side of the printing surface and the surrounding side wall of the round button.

[0038] On the inside of the hollow blank, a second, flat area 12 is formed from a second plastic material, which, due to the properties of the selected plastic, cannot be electroplated. This area 12 is therefore not coated with a metallic layer during electroplating, but remains exposed. The second area 12 of the multi-component plastic blank is also marked in the figures with the letters "NG" to indicate it as a non-electroplatable area. Various locking elements 14 can also be formed from the non-electroplatable plastic material, allowing the button to be attached to another component.

[0039] After galvanization, a metal layer 20 is formed on the area 11 of the multi-component plastic blank, as shown in the Fig. 1b. On the front side of the component's printing surface, which is facing downward in the illustration, the metal layer can be partially removed to form a symbol 23. This can be done, for example, by laser treatment. If both plastics of the multi-component plastic blank are translucent, the button can be backlit from the inside, causing the symbol 23 on the metallic front side to glow and be easily visible even in the dark.

[0040] As from the Fig. 1b, the metal layer 20 covers the entire galvanizable area 11, so that it extends on the inside of the circumferential side wall of the button up to the non-galvanizable plastic of the area 12. In this transition area between the galvanizable areas 11 and the non-galvanizable area 12, however, undesirable overgrowths 21 and 22 often arise during galvanization, as shown in Fig. 1b are shown as examples at two opposite locations. These overhangs 21 and 22 are also under the supervision of the Fig. 1c on the inside of the button.

[0041] In order to prevent these overgrowths, a multi-component plastic blank according to the invention has a recessed geometric structure in the boundary area between the two plastics used in the component, the geometry and arrangement of which is selected such that it prevents an overgrowth of the metal layer forming on the electroplatable plastic onto the non-electroplatable plastic during selective electroplating of the multi-component plastic blank.

[0042] The Fig. 2a to Fig. 2d show an embodiment not according to the invention.

[0043] This is in Fig. 2a based on the already in Fig. 1a. The button is formed from a multi-component plastic blank 10, which is to be partially coated with a metal layer, such as chrome. A first region 11 is again formed from a plastic that is electroplatable (G), while a second region 12 consists of a plastic that is not electroplatable (NG). The electroplatable region 11 forms the front side 16 in the form of the pressure surface and the circumferential side wall of the button, while the non-electroplatable region 12 forms the back side 17 of the pressure surface of the button.

[0044] The multi-component plastic blank 10 is a so-called 2K component, which is manufactured from two different plastic components using a suitable injection molding process. Preferably, the two components 11, 12 of the base body are manufactured in a sequence in which the plastic component whose plastic material requires processing at a higher temperature, i.e., generally the one with the higher melting point, is injected first. In a subsequent process step, the second plastic component, which is to be processed at a lower temperature, is then injection-molded onto the preferably already completely solidified first plastic component. In the case of a multi-component plastic blank 10 for a button, for example, the non-electroplatable region 12 can be manufactured first before the electroplatable region 11 is injection-molded onto the solidified region 12.

[0045] Furthermore, the injection molding process known as in-mold decoration (IMD) has also proven suitable for producing the multi-component plastic blank according to the invention. In such an IMD process, a film made of a galvanizable plastic is inserted into an injection mold and subsequently back-injected with a non-galvanizable plastic. Depending on the shape of the base body or the material properties of the film, it is also conceivable to insert a film made of a non-galvanizable plastic into an injection mold to form the non-galvanizable back of the base body and to back-inject this with a galvanizable plastic, whereby the component consisting of the plastic forms the galvanizable surface of the base body in the finished base body.The latter variant of the process offers the advantage that the surface of an injection-molded plastic part can be metallized, for which there is significantly more experience in the state of the art than for the metallization of plastic films.

[0046] Polycarbonate (PC) has proven to be a particularly suitable plastic for forming the non-electroplatable region 12. In addition to the fact that it is virtually unaffected by the subsequent electroplating process steps, this material has the advantage of being particularly well-suited as a light guide. Furthermore, PC can be easily doped with light-scattering particles, which allows for particularly homogeneous light distribution, particularly when using the multi-component plastic blank according to the invention as an illuminated control element.

[0047] Polyamide, ABS (ABS - acrylonitrile butadiene styrene), or an ABS / polycarbonate blend have proven particularly suitable plastics for forming the electroplatable area 11. A highly resilient mechanical connection between the subcomponents 11, 12 of the multi-component plastic blank 10 is achieved when the electroplatable component 11 consists of an ABS / polycarbonate blend and the non-electroplatable component 12 of polycarbonate, since polycarbonate has good adhesion to ABS or PC / ABS, for example. If a polyamide is used for the electroplatable component 11, it has proven advantageous to create additional mechanical interlocking between the two, for example by appropriately shaping the electroplatable area 11 and the subbody 12.

[0048] On the surface of the multi-component plastic blank 10, a boundary line 15 is formed by the two subcomponents 11 and 12, which separates the two plastics from each other at the surface of the component. The recessed geometric structure provided according to the invention is arranged in the region of this boundary line 15, wherein the boundary line 15 runs at least partially within the recess. In the exemplary embodiment of the Fig. 2a, a circumferential groove 30 is provided in the boundary area between the two plastics G and NG, and the two plastic components 11, 12 abut each other at the boundary line 15 within the groove 30.

[0049] Fig. Figure 2b shows an enlarged view of the groove 30, which is essentially formed within the material of the non-electroplatable subcomponent 12. The groove 30 has a rectangular cross-section and thus a bottom wall 31 and two opposing side walls 32 and 33. The bottom wall 31 and the first side wall 32 are formed by the material of the non-electroplatable subcomponent 12, while the other side wall 33 is formed by the material of the electroplatable subcomponent 11. The boundary line 15 between the two plastics thus coincides with the inner edge of the groove 30, which is formed by the side wall 33 and the bottom wall 31.

[0050] This shift of the boundary line 15 into a correspondingly shaped and arranged groove 30 ensures that, during partial electroplating of the multi-component plastic blank 10, there is as little overgrowth as possible at the boundary line 15. This condition is in the Fig. 2c, which shows a plastic component 40 or a button comprising the multi-component plastic blank 10, which has been partially electroplated, so that a metal layer 20 has formed on the surface of the electroplatable plastic G, while this is not the case on the surface of the non-electroplatable subcomponent 12. The metal layer 20 completely surrounds the surface of the subcomponent 11 and extends on the inside of the button into the groove 30, where it meets the subcomponent 12 or the bottom wall 31 of the groove 30 at the boundary line 15.

[0051] Fig. Figure 2d shows a view of the partially galvanized button 40 from the rear side, revealing the peripheral edge of the button 40 and the rear side of the pressure surface. Furthermore, two opposing locking elements 13 and 14 can be seen in this illustration, although these are shown only schematically and merely as examples. Additional locking elements may be present, and the locking elements may also be more complex.

[0052] The groove 30 is circular and runs along the inner edge of the knob. In the illustrated embodiment, the circular shape of the groove 30 is interrupted in the area of ​​the locking elements 13, 14, resulting in two semicircular grooves. The groove 30 can also enclose the locking elements 13, 14, or the locking elements can be mounted high enough on the inner wall of the knob that the groove 30 can run underneath them. In any case, the groove is provided where overgrowth of the metal of the metal layer 20 from the electroplatable plastic 11 onto the non-electroplatable plastic 12 is to be prevented.

[0053] Again Fig. 2c, the metal layer 20 on the front surface of the button can be partially removed in order to form, for example, a symbol 23. This symbol 23 is also visible in the rear view of the Fig. 2d, if the non-electroplatable material of subcomponent 12 is transparent or at least translucent. The labeling of a start-stop button, for example, can then be backlit.

[0054] Suitable pretreatment steps and the electroplating process of a multi-component plastic blank for forming a backlit control element can be found in the applicant's patent application DE 10 2010 016 973 A1, the corresponding description of which is hereby incorporated by reference. A possible process for applying a decorative metal layer to a multi-component plastic blank according to the invention will therefore only be explained in its essential principles below.

[0055] If ABS or an ABS / polycarbonate blend is used for the electroplatable area 11, the plastic undergoes a chemical treatment prior to metallization, which increases the roughness of the surface. For example, it has proven advantageous if the butadiene components of the ABS plastic are at least partially dissolved from the surface of the electroplatable plastic. This can be achieved, for example, by chemically treating at least the electroplatable area 11, but preferably the entire plastic blank, e.g., by pickling in a chromic acid bath.

[0056] If, on the other hand, a galvanizable plastic made of polyamide is used, the surface roughness can be increased before the metallization is applied by chemically pretreating at least the galvanizable area made of polyamide, but preferably the entire plastic blank, in a suitable manner in order to cause the polyamide layer to swell.

[0057] Subsequently, a layer of palladium nuclei is deposited from an electrolyte solution onto the electroplatable area 11. This process step is often referred to as "activating the surface" of the component to be electroplated. For example, it is known to apply palladium nuclei from a colloidal solution to the electroplatable area to activate the surface, with the palladium already dispersed in metallic form in the colloidal activator. However, silver nuclei, for example, can also be used for activation.

[0058] Applied palladium nuclei can be protected by a tin protective colloid layer. It has proven advantageous to remove any tin protective colloid layer covering the palladium nuclei before the subsequent application of the first metal layer to the activated electroplatable layer. This process, also known as "stripping," can be performed, for example, by washing the activated electroplatable surface of the base body.

[0059] In addition to colloidal activators, ionic activators can also be used for activation with palladium nuclei. For example, a hydrochloric acid solution with 0.5 to 2 g / l PdCl2 is used as an ionic activator, which contains not only Pd2 + ions, but also complex ions, such as [PdCI 4] 2- , [PdCl 3] - and [PdCl] +For nucleation, the Pd ions must be reduced to the palladium atom, which can be achieved using a reducing solution.

[0060] Subsequently, a first metal layer, preferably made of nickel or copper, is deposited as the first metal layer (so-called "chemical nickel" or "chemical copper") on the colloidally or ionogenically activated surface of the base body by chemical, non-electrochemical means (i.e., without current) in a suitable metal bath. As an alternative to chemical deposition of the first metal layer, deposition by physical processes is available, which can be achieved, in particular, by PVD (physical vapor deposition).

[0061] This first metal layer can be suitably patterned to create a symbol, for example, on a start-stop button. The chemically or physically deposited first metal layer typically has a thickness of one micrometer or less, so it can be easily patterned, for example, by laser ablation or lithography—i.e., by applying a patterned protective lacquer, followed by etching the metal layer and washing off the protective lacquer.

[0062] Preferably, at least the process steps “activating the surface”, “applying the first metal layer (chemical nickel / chemical copper)” and “structuring the first metal layer to form the symbolism” are completed in less than 24 hours in order to avoid passivation of the reactive surface of the chemical nickel / chemical copper.

[0063] If the electrolessly deposited first metal layer has only a low current carrying capacity, which would be disadvantageous for the subsequent electrochemical process steps, a first metal layer, e.g. made of copper or nickel, can optionally be deposited galvanically on the first metal layer at low currents (so-called "pre-copper" or "pre-nickel"), whereby this is possible both before and after the structuring of the first metal layer.

[0064] To complete the metallized component, the thickness of the first metal layer is then increased using a galvanic, i.e. electrochemical process. As a rule, this process involves depositing a first intermediate layer of copper onto the first metal layer. Due to its high ductility, this intermediate layer forms a bridge between the plastic base body, which has a high level of elasticity, and a decorative layer made of a hard decorative metal such as nickel or chromium, which is deposited on the surface of the control element in a subsequent process step. This first intermediate layer of copper can have a layer thickness of 10 to 40 micrometers or more. As a rule, the electroplating process for depositing the first intermediate layer of copper is adjusted so that a layer thickness of this first intermediate layer of at least 20 micrometers is ensured on all control elements coated at the same time in the electroplating bath.

[0065] Often, a second metallic intermediate layer is deposited on top of the first intermediate layer of copper in order to increase the corrosion resistance of the metal coating. This second intermediate layer can also increase the adhesion of the decorative layer applied to the surface of the control element to the first intermediate layer. Finally, the appearance of the decorative layer can also be specifically influenced by choosing the appropriate material for the second intermediate layer. The application of a second intermediate layer of nickel has proven particularly successful. This second intermediate layer can consist of cracked nickel, matte nickel, semi-bright nickel or bright nickel and can in turn be further divided into intermediate layers. For control elements that are subject to particularly high mechanical stress, such asFor example, for the gearshift lever of a transmission or for control elements that are particularly exposed to corrosive media such as hand sweat, a layer structure consisting of a layer of cracked nickel applied to the first intermediate layer of copper and a layer of matte, semi-gloss, or bright nickel deposited on its surface has proven successful. The cracked nickel layer contributes to a significant increase in the corrosion resistance of the entire layer structure, with controlled corrosion attack on the cracked nickel layer being considered the cause of this. However, the adhesion of the decorative layer is also further increased by this intermediate layer. The layer thickness of the second intermediate layer is typically between 5 and 30 micrometers, preferably 10 micrometers and more, which is particularly the case with a second intermediate layer made of nickel.

[0066] Subsequently, a layer of a decorative metal, which can be chromium or nickel, for example, is electroplated onto the first intermediate layer of copper or the optional second intermediate layer of nickel. This involves the use of conventional processes for forming a semi-gloss or bright nickel layer (aluminum design), a cracked nickel layer, or a bright chrome layer. Typical layer thicknesses for this decorative layer are generally between 100 nanometers and a few micrometers; in the case of chromium, preferably at least 300 nanometers.

[0067] However, shortened processes can also be used in which the component is moved into a so-called primer after nucleation without chemical nickel, accelerator and pre-copper in order to then apply copper using electricity.

[0068] Finally, the metallized surface of the control element can be provided with a suitable protective and / or decorative lacquer, which is applied to the decorative layer made of the decorative metal, such as chrome, and further increases the corrosion resistance of the entire layer structure applied to the control element.

[0069] Tests on such selective electroplating of multi-component plastic blanks 10 for the production of metallized start-stop buttons have shown that the recessed geometric structure in the form of the groove 30 effectively prevents overgrowths at the boundary line 15 between the two plastics.

[0070] However, not only in the described geometry of a start-stop button, but also in the partial electroplating of other components, a recessed geometric structure in the boundary area between the two plastics has proven to be an effective means of reliably preventing overgrowth. While the two plastics in the described blank 10 meet at the boundary line 15 at an angle of approximately 90°, there are also multi-component plastic blanks in which two different plastics form a boundary line on a continuous surface. A metallized area would therefore transition almost flush into a non-metallized area on the surface.

[0071] Fig. 3 shows a section of such a component 40', in which a left-hand region 11 has been galvanized with a metal layer 20, while no metal layer has been deposited on a right-hand region 12. For simplicity, these two regions are again labeled G and NG. In the boundary region between the two plastics, a groove 30' is again formed, although the boundary line 15 does not coincide with an inner edge of the groove 30', but rather runs in the surface of a side wall 33 of the groove 30'. The metal layer 20 covers the galvanizable plastic G and projects at least as far as the boundary line 15. This may result in a slight overlap 24 with a radius corresponding to the thickness of the metal layer 20. However, this overlap occurs everywhere along the boundary line 15, so that it is not to be regarded as undesirable overgrowth.Local overgrowth, on the other hand, does not occur or only to a small extent, and a narrow groove 30' with a width of about 0.5 millimeters can be well integrated into the design of the component 40' without affecting the appearance too much.

[0072] The groove 30' is trapezoidal in shape with a bottom wall 31 and two side walls 32 and 33, with the bottom wall 31 and the side wall 32 being formed in the non-galvanizable area 12. The other side wall 33 is also made of non-galvanizable plastic NG in the lower part, while the part facing the opening of the groove 30' is made of the galvanizable plastic G.

[0073] Here, but also with other components, certain dimensions of the groove 30' have proven advantageous. So that the groove 30' does not change the appearance of the surface too much, its width B should be as small as possible, whereby a width of 0.5 millimeters is suitable. The same applies to the depth T of the groove 30', which can also be in the range of 0.5 millimeters. The boundary line 15 running within the surface of the side wall 33 between the two plastics G and NG preferably divides the side wall in a ratio of 2:1, so that the partial depth T1 is approximately 0.3 millimeters, while the partial depth T2 is approximately 0.2 millimeters. Furthermore, the opening edges of the groove 30' can also be rounded, as is the case with the embodiment of the Fig. 3 is the case.

[0074] Such shapes and partially metallized components are used, for example, in loudspeaker grilles, where a peripheral edge of the loudspeaker is to be chrome-plated, while this is not the case for the grille. Fig. 4 shows a section of another embodiment of a multi-component plastic component 40", in which an edge in the form of a first region 11 is to be chrome-plated, while the rest in the form of a second region 12 is not to be chrome-plated. The surface of the entire component is curved, and the plane of the edge is slightly higher than the plane of the remaining component.

[0075] In the boundary area between the two plastics G and NG, a boundary line 15 is again formed, which coincides with the inner edge of a 30" groove. This 30" groove has a polygonal cross-section, although the bottom wall 31 and the side walls 32 and 33 are not trapezoidal, but rather slightly slanted. In particular, the angle between the side wall 33 and the bottom wall 31 is less than 90°, while the angle between the bottom wall 31 and the other side wall 32 is greater than 90°. The opening edges of the 30" groove are again rounded, and the surfaces of the component 40" that border these opening edges are located at different levels, so that the surface of the component would have a step even without the 30" groove. Therefore, the 30" groove can be well integrated into the design of the component without overly compromising it. List of reference symbols: 10 multi-component plastic blank 11 Subcomponent, electroplatable area (G) 12 subcomponent, non-galvanizable area (NG) 13,14 locking element 15 Boundary line 16 Front, pressure surface of a button 17 Back of the pressure surface of a button 20 metal layer 21,22 Surveillance 23 Symbolism 24 Overlap 30,30',30" Recessed geometric structure, recess, groove 31 Bottom wall of the groove 32,33 Side wall of the groove 40,40',40" plastic component, partially metallized T Depth T1, T2 partial depth B Width

Claims

[1] A multi-component plastic blank (10) partially electroplated with a metal layer (20), comprising at least a first region (11) made of a first plastic and a second region (12) made of a second plastic, which are arranged adjacent to one another at least in some regions in the surface of the multi-component plastic blank (10), whereby a boundary line (15) is formed between the two regions (11; 12) made of different plastics, wherein the first plastic of the first region (11) is a plastic with which a electroplatable region can be produced by pretreatment steps, while the second plastic of the second region (12) is a plastic with which no electroplatable region can be produced by the same pretreatment steps, where at least one recessed geometric structure (30') is formed in the surface of the multi-component plastic blank (10) and the boundary line (15) between the two plastics runs at least partially within the recessed geometric structure (30'), wherein the recessed geometric structure is formed as a groove (30') and the boundary line (15) runs within the surface of a side wall (33) of the groove characterized by that the boundary line (15) divides the side wall (33). [2] Multi-component plastic blank according to claim 1, characterized by that the surface of the first plastic can be converted into a surface that can be electroplated by pretreatment steps in the form of pickling, roughening and / or swelling, while the surface of the second plastic cannot be simultaneously converted into a surface that can be electroplated by the same pretreatment steps. [3] Multi-component plastic blank according to one or both of claims 1 and 2, characterized by that the surface of the first plastic can be converted by the pretreatment steps into a surface that can be activated by palladium nuclei, while the surface of the second plastic cannot be converted by the same pretreatment steps into a surface that can be activated by palladium nuclei. [4] Multi-component plastic blank according to one or more of claims 1 to 3, characterized by that the first plastic is polyamide, acrylonitrile butadiene styrene (ABS) or an ABS / polycarbonate blend, and the second plastic is polycarbonate (PC), polymethyl methacrylate (PMMA) or polyethylene terephthalate (PET). [5] Multi-component plastic blank according to one or more of claims 1 to 4, characterized bythat the areas of the surface of the multi-component plastic blank (10) which border on the recessed geometric structure (30') on opposite sides lie on the same or on different levels. [6] Multi-component plastic blank according to claim 5, characterized by that the areas of the surface of the multi-component plastic blank (10) which border on the recessed geometric structure (30') on opposite sides lie on two different planes which run essentially parallel or at an angle different from 90° to one another. [7] Multi-component plastic blank according to one or more of claims 1 to 6, characterized by that the depth of the recessed geometric structure (30') is in the range between 0.3 and 1.0 millimeters, preferably 0.5 millimeters. [8] Multi-component plastic blank according to one or more of claims 1 to 7, characterized bythat the width of the recessed geometric structure (30') is in the range between 0.3 and 1.0 millimeters, preferably 0.5 millimeters. [9] Multi-component plastic blank according to one or more of claims 1 to 8, characterized by that the recessed geometric structure (30') is a groove with a substantially quadrangular cross-section, the groove having a bottom wall (31) and two opposite side walls (32;33). [10] Multi-component plastic blank according to claim 9, characterized by that the boundary line (15) divides the side wall (33) in a ratio of approximately 2:1, the smaller part being adjacent to that inner edge of the groove (30') formed by the bottom wall (31) and the side wall (33) within which the boundary line (15) runs. [11] Plastic component, characterized bythat the plastic component (40') comprises a multi-component plastic blank (10) according to one or more of claims 1 to 10, and that a metal layer (20) is applied to the first region (11) of the multi-component plastic blank (10) made of a first plastic, while no metal layer is applied to the second region (12) made of a second plastic (NG), wherein the metal layer (20) protrudes at least partially into the recessed geometric structure (30'). [12] Method for producing a plastic component (40') according to claim 11, characterized bythat a multi-component plastic blank (10) according to one or more of claims 1 to 10 is completely treated with pretreatment steps such that the surface of the first plastic of the first region (11) becomes galvanizable, while the surface of the second plastic of the second region (12) does not become galvanizable by the same pretreatment steps, and a galvanization of the galvanizable region (11) is carried out. [13] Method according to claim 12, characterized by that the multi-component plastic blank (10) is produced in an injection molding process.

Citation Information

Patent Citations

  • Process to manufacture a two-part composite plastic of soft and hard plastic with selective galvanized finish

    DE102006037535A1

  • Producing single metalized control element comprises producing plastic base body with non-electroplatable and electroplatable layers made of plastics, depositing first metal layer on electroplatable layer and depositing second metal layer

    DE102010016973A1

  • Method for producing electroplated elements with backlit symbols and elements produced according to the method

    DE10208674B4

  • Partially electroplatable polymer molded part

    DE19919709A1

  • Method of making metal-plated plastic articles

    US3640789A