CVD-coated cutting insert and method for its manufacture
The multi-layer coating scheme with alternating aluminum oxide and nitrogen-containing TiOxCyNz layers, applied via chemical vapor deposition, addresses the challenges of crack propagation and improves cutting edge stability and service life in coated cutting inserts.
Patent Information
- Application Number
- DE102016106952
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2015-04-20
- Filing Date
- 2016-04-14
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2036-04-14
AI Technical Summary
Existing coated cutting inserts face challenges in extending service life, improving performance characteristics, especially during heavily interrupted turning and milling, and controlling crack growth and propagation due to mechanical stress or temperature changes.
A coated cutting insert with a multi-layer coating scheme featuring alternating layers of aluminum oxide and nitrogen-containing TiOxCyNz, where each layer has a distinct crystal structure, ensuring clear boundaries and a transition layer for enhanced adhesion and nucleation, applied via chemical vapor deposition.
The multi-layer coating scheme enhances cutting edge stability, prevents crack propagation, and extends the service life of the cutting insert, particularly in demanding machining conditions.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
BACKGROUND OF THE INVENTION
[0001] The present invention relates to a coated cutting insert and in particular to a coated Cutting insert coated using a chemical vapor deposition (CVD) technique and suitable for Applications for material removal by machining such as machining, turning and milling, as well as a method for its production. In particular, the present invention relates to a CVD-coated Cutting insert comprising a substrate having a coating scheme thereon, wherein the coating scheme comprises a a plurality of coating layers, including a multi-layer coating scheme having a A plurality of repeating coating sets. Each coating set comprises a coating layer of Aluminium oxide and a coating layer of a nitrogen-containing material (e.g. titanium aluminium oxynitride or Titanium nitride or zirconium nitride), whereby the coating scheme applied by CVD offers higher strength, good crack resistance, acceptable adhesion properties, acceptable resistance to abrasive wear and has an acceptable cutting edge stability. Furthermore, the present invention relates to a method for producing of the coated cutting insert.
[0002] To date, coated bodies such as coated cutting inserts have been used in applications for the removal of material by machining. Such coated cutting inserts typically comprise a substrate with a Cutting insert geometry and a coating scheme on the substrate. The coating scheme comprising Coating layers typically comprise refractory hard materials that provide the wear resistance property The main purpose of using a coating on a cutting insert is to To extend the service life of the cutting insert in material removal applications. Examples of these Coating schemes using refractory hard materials are described in the following documents described: European Patent No. EP 1 245 698 B1, Mitsubishi Materials Corp.; European Patent Application No. EP 1 455 003 A2, Sandvik AB; European Patent No. EP 1 980 649 B1, Iscar Ltd.; published US patent application No. US 2012 / 0 202 032 A1, Tatsuoka et al.; published US patent application No. US 2013 / 0 045 057 A1, Kojima et al.; US- Patent Nr. US 7 132 153 B2, Zackisson et al.; US-Patent Nr. US 7 396 371 B2, Cedergren et al.; US-Patent Nr. US 7 455 918 B2, Gates, Jr. et al.; US-Patent Nr. US 7 470 296 B2, Londholm et al.; US-Patent Nr. US 7 597 951 B2, Björmander et al.; US- Patent Nr. US 7 727 592 B2, Cedergren et al.; US-Patent Nr. US 7 785 665 B2, Gates, Jr. et al.; US-Patent Nr. US 8 080 312 B2, McNerny et al.; US-Patent Nr. US 8 080 323 B2, Ban et al.; US-Patent Nr. US 8 323 783 B2, Sottke et al.; US-Patent Nr. US 8 557 406 B2, Ban et al.; Chinchanikar et al., ´´Wear behavior of single-layer and multi-layer coated carbide inserts in high speed machining of hardened AISI 4340 steel´´, Journal of Mechanical Science and Technology, 27 (5), (2013), S. 1451 - 1459 und Halvarsson et al., ´´Microstructure and performance of CVD &kgr;-Al O multilayers´´, Materials Science and 2 3 Engineering, A209 (1996) S. 337 - 344.
[0003] From DE 11 2014 001 640 T5 a cutting tool is known which comprises a substrate; and a cutting tool arranged on the substrate adhesive coating, wherein the coating comprises a multi-layer structure including a plurality of structural units, each comprising a bonding layer and an adjacent aluminum oxide layer, wherein the aluminum oxide layer has a thickness of less than 0.5 µm and the bonding layer has a thickness of less than 1 µm, wherein the bonding layer comprises TiCN and TiAlOC. US 2005 / 0 202 283 A1 shows a Cutting tool comprising a substrate and a coating applied to the substrate which has an alpha- aluminum oxide layer with plate-like morphology. Furthermore, US 2010 / 0 255 345 A1 discloses a coated cutting insert made of polycrystalline cubic boron nitride, which has a substrate made of polycrystalline cubic boron nitride with a rake face and at least one flank and a cutting edge at the junction between the Cutting edge formed by the rake face and the flank face.
[0004] As can be seen from the above documents, in the past, for a coated Many different coating schemes are used for cutting inserts. According to these documents, each individual These coating schemes offer certain advantages. Even though coating schemes exist that offer certain advantages, there is still a need to provide a coating scheme that Extends the service life of a coated cutting insert and improves the performance characteristics of a coated cutting insert in a material removal application. In addition, the Need to provide an improved coated cutting insert, wherein the coating scheme has a has high strength, which leads to better cutting edge stability, especially in heavily interrupted turning and milling. There is still a need to provide an improved coated cutting insert that coating scheme that includes a multi-layer coating scheme that inhibits crack growth and Crack propagation in the coating scheme due to mechanical stress or temperature change better In addition, there is a need to provide an improved coated cutting insert that a transition layer that allows better nucleation and adhesion of the multilayer coating scheme favored.
[0005] Therefore, it would be highly desirable to develop an improved coated cutting insert and a method its production, whereby the cutting insert is useful in material removal applications. It It would be highly desirable to develop an improved coated cutting insert and a process for its manufacture where the cutting insert is useful in material removal applications and the coated Cutting insert has a longer service life. It would be highly desirable to have an improved coated Cutting insert and a method for its production, wherein the cutting insert is used in applications for material removal and the coated cutting insert has improved performance characteristics.
[0006] It would be highly desirable to provide an improved coated cutting insert and a method for its manufacturing, the cutting insert being useful in material removal applications and the coated cutting insert has a coating scheme with a high strength, which is particularly suitable for the strongly interrupted turning and milling leads to better cutting edge stability. It would be highly desirable to have a to provide an improved coated cutting insert and a method for its manufacture, wherein the Cutting insert is useful in material removal applications, where the coated cutting insert is a coating scheme that includes a multi-layer coating scheme that inhibits crack growth and Crack propagation in the coating scheme due to mechanical stress or temperature change better It would be highly desirable to develop an improved coated cutting insert and a process to provide its manufacture, the cutting insert being useful in material removal applications and the coated cutting insert has a coating that includes a transition layer that provides better Nucleation and adhesion of the multilayer coating scheme are favored. SUMMARY OF THE INVENTION
[0007] In one embodiment thereof, the invention is a coated cutting insert for use in a Method for removing material by machining. The coated cutting insert comprises a substrate and a Coating scheme on the substrate. The coating scheme has a support coating scheme formed by chemical vapor deposition, with the support coating scheme based on the surface of the substrate. By chemical vapor deposition, a transition layer is formed on the Surface of the support coating scheme. On the surface of the transition layer, chemical A multilayer coating scheme was deposited by vapor deposition, comprising a plurality of repeating coating sets. Each of the coating sets is formed from a coating layer of Aluminium oxide, which has an alpha-aluminium oxide crystal structure, and a nitrogen-containing TiO CN - xyz Coating layer that has a crystal structure of a nitrogen-containing TiO CN coating. The aluminum oxide xyz Crystal structure differs from the crystal structure of the nitrogen-containing TiO CN coating layer, which xyz between adjacent coating layers of aluminum oxide and the nitrogen-containing TiO CN - xyz coating layers there is a clear boundary, and the TiO CN coating layer with the xyz aluminum oxide layer of an adjacent coating set. The variables x, y and z in the nitrogen-containing TiO CN coating layer has the following values: 0 <x<0,7, 0<y<0,7 und 0<z<0,7. xyz
[0008] In a further embodiment thereof, the invention is a method for producing the coated Cutting insert comprising the following steps: providing a substrate; applying a Support coating schemes on the substrate by chemical vapor deposition Applying a Transition layer on the support coating scheme by chemical vapor deposition; application of a multilayer coating schemes on the transition layer by chemical vapor deposition, whereby the multi-layer coating scheme comprises a plurality of repeating coating sets and wherein the Steps for applying each coating set include: first applying a Coating layer of aluminum oxide without variation of the parameters for deposition of the coating, whereby the Aluminum coating layer oxide has an alpha-aluminum oxide crystal structure; and interrupting the application of the coating layer of Aluminium oxide by applying a nitrogen-containing coating layer which has the crystal structure of a nitrogen-containing coating layer, wherein the crystal structure of the nitrogen-containing coating layer from the alpha-aluminium oxide crystal structure, whereby between the coating layer of aluminium oxide and the nitrogen-containing coating layer a clear boundary is formed, and wherein the TiO CN - xyz coating layer is in contact with the aluminum oxide layer of an adjacent coating set. The variables x, y and z in the nitrogen-containing TiO CN coating layer have the following values: 0 <x<0,7, 0<y<0,7 und 0<z<0,7 xyz BRIEF DESCRIPTION OF THE DRAWINGS
[0009] The following is a brief description of the drawings which form a part of this patent application: Fig. 1 shows an isometric view of a coated cutting insert forming a applied coating scheme, wherein a part of the coating scheme is used to represent the substrate was removed; Fig. 2 is a cross-sectional view of a first specific embodiment of a coated Cutting insert, which schematically shows the substrate and the coating layers that make up the Coating scheme includes, shows; Fig. 3 (not according to the invention) is a cross-sectional view of a second specific embodiment of a coated cutting insert, which schematically shows the substrate and the coating layers that make up the Coating scheme includes, shows; Fig. 4 is a micrograph (with a scale of 10 µm) of the cross-sectional view of a coated insert, which shows the different layers formed by the majority of coating sets that deposited on a support coating scheme on a hard metal substrate; Fig. 5 (not according to the invention) is a cross-sectional view of a fourth specific embodiment of a Coating schemes of a coated cutting insert, showing in schematic form the substrate and the shows coating layers comprising the coating scheme; Fig. 6A (not according to the invention) is a micrograph (with a scale of 500 µm) of a cross-sectional view of a worn coated cutting insert according to the invention, wherein an area of the micrograph is ´´6B / C´´; Fig. 6B (not according to the invention) is a photomicrograph (with a scale of 100 µm) of the area of Fig. 6A, which is designated as 6B / C; Fig. 6C (not according to the invention) is a photomicrograph (with a scale of 100 µm) of the area of Fig. 6A, which is designated as 6B / C, but rotated relative to Fig. 6B and with the coating layers marked; Fig. 7A is a photomicrograph (with a scale of 500 µm) of a cross-sectional view of a worn conventional coated cutting insert, with one area of the micrograph being labeled ´´7B / C´´; Fig. 7B is a photomicrograph (scale of 100 µm) of the area of Fig. 7A, designated 7B / C is; and Fig. 7C is a photomicrograph (scale of 100 µm) of the area of Fig. 7A, designated 7B / C but rotated relative to Fig. 7B and with the coating layers marked. DETAILED DESCRIPTION
[0010] The present invention relates to a coated cutting insert which is suitable for the removal of material by When removing material through machining, the cutting insert penetrates into a workpiece to To remove material, typically in the form of chips, from a workpiece. A process for removing material, in which material is typically removed from the workpiece in the form of chips, is known to the person skilled in the art as a method for Material removal by machining. The book Machine Shop Practice [Industrial Press Inc., New York, New York (1981)] by Moltrecht contains on pages 199 - 204, among other things, a description of chip formation and the different types of chips (ie continuous chip, discontinuous chip, segmented chip). Moltrecht says [from preferably] on pages 199-200: ´´When the cutting tool makes first contact with the metal, it compacts the metal in front of the cutting edge. As the tool advances, the metal in front of the cutting edge is cut to the point stressed, at which it shears inside, so that the metal grains deform and plastically along a Shear plane... If the type of metal being cut is ductile, such as steel, the Chip in a continuous band ....´´. Moltrecht continues with the description of a discontinuous chip and of a segmented chip.
[0011] Another example can be found on pages 302 - 315 of the ASTE Tool Engineers Handbook, McGraw Hill Book Co., New York, New York (1949), a longer description of chip formation in the metal cutting process. On page 303, The ASTE Handbook clearly shows the relationship between chip formation and machining operations such as Turning, milling and drilling. The following patents discuss the formation of chips in a process for Material removal: US Patent No. US 5,709,907 A, Battaglia et al. (issued to Kennametal Inc.), US Patent No. US 5,722,803 A, Battaglia et al. (issued to Kennametal Inc.) and US Patent No. US 6,161,990 A, Oles et al. (issued to Kennametal Inc.).
[0012] Referring to the drawings, a number of specific embodiments of a coated Referring to Fig. 1, a coated cutting insert is illustrated which generally referred to as 20, wherein the coated cutting insert 20 comprises a substrate 22 and a coating scheme 24 on the substrate 22. The coated cutting insert 20 illustrates a typical type of geometry that as a coated cutting insert. Each of these specific embodiments of the coating schemes is explained in more detail below.
[0013] Referring to the coating scheme shown in Fig. 2, a coated cutting insert can be seen which generally referred to as 30, which comprises a substrate 32 and a surface 31 of the substrate 32 Coating scheme 32A comprises. The coating scheme 32A comprises a support coating scheme 33 comprising a TiN coating layer 34 on the surface of the substrate 32 and an MT-TiCN coating layer 36 on the TiN coating layer 34 and a TiCN coating layer 37 on the MT-TiCN coating layer 36. The The term ´´MT-TiCN coating layer´´ refers to a coating layer of titanium carbonitride, which is chemical vapor deposition (CVD) at an average temperature between about 750 °C and about 920 ° C. In contrast to the MT-TiCN coating layer, the term ´´HT-TiCN´´ or ´´TiCN´´ coating layer on a coating layer of titanium carbonitride, which is deposited by CVD at a temperature of more than about 950 °C, and typically within a range of about 950 °C to about 1020 °C, becomes.
[0014] On the HT-TiCN coating layer 37 there is also a Ti+O+C+N transition layer 38 containing titanium and Contains oxygen, carbon and nitrogen. It is important to consider that the applicants, with regard to the Function of the Ti+O+C+N transition layer, although one does not want to be bound to a specific theory, assumes that the Ti+O+C+N transition layer promotes the nucleation and adhesion of the coating layers of the multilayer coating schemes favored.
[0015] The multilayer coating scheme 49 is located on the Ti+O+C+N transition layer 38, wherein the multilayer coating scheme 49 comprises a plurality of coating sets (39, 43). Although Fig. 2 shows two coating sets, it must be mentioned that for this specific embodiment and the other coating sets In the specific embodiments mentioned, a different number of coating sets can also be used. Use in this specific embodiment and the other specific embodiments mentioned herein For example, between two and sixteen coating sets are suitable, which is between about four and thirty-two Coating layers. The coating set 39 comprises a coating layer of aluminum oxide 40 and a TiO CN coating layer 42. The coating set 43 comprises a coating layer of aluminum oxide 44 xyz and a TiO CN coating layer 46. In this specific embodiment, as well as in all of the xyz Embodiments, the coating layers of aluminum oxide have the alpha-crystalline phase of aluminum oxide Referring to the TiO CN coating layers 42 and 46, the values for x, y and z are as follows: 0 <x<0,7, xyz 0 <y<0,7, 0<z<0,7.
[0016] The composition of the coating layers which make up the coating sets of the multi-layer Coating schemes, is chosen so that the deposition of the individual coating layers by the Deposition of the subsequent coating layer is abruptly interrupted.
[0017] The result is the complete interruption of the crystal growth of the previous coating layer by the Initiation of the subsequent coating layer. This abrupt interruption can be caused by a change in the coating composition or coating parameters, which leads to the nucleation of a layer with its own crystal structure. Such a change can lead to neighboring Coating layers have different crystal structures. These interruptions result in Coating layers with a clear boundary between the adjacent coating layers, so that it can be There is no mixed phase of a composite material between the individual coating layers.
[0018] Although not shown in Fig. 2, another embodiment of the invention includes an external Coating scheme applied by CVD to the surface of the outermost repeating layer set Such an outer coating layer may be a group IV b element formed by carbide, carbonitride, nitride or oxycarbonitride.
[0019] The following Table 1 shows the thickness ranges of the coating schemes and coating layers for the coated cutting insert 30 shown in Fig. 2. Table 1 - Thickness of coating schemes and Coating layers of FIG. 2 Thickness range Alternative thickness range Coating layer or coating scheme (micrometers) (micrometers) Coating scheme 32A 2 - 35 5-30 Support coating scheme 33 1 - 20 2-18 TiN coating layer 34 up to 2 up to 1 MT-TiCN coating layer 36 1 - 18 2-15 HT-TiCN coating layer 37 up to 5 up to 2 Ti + O + C + N transition layer 38 up to 3 up to 2 Multi-layer coating scheme 49 1 - 15 2-12 Coating sets 39 and 43 0.1 - 0.8 0.2 - 0.7 Coating layers of aluminum oxide 40 and 0.05 - 0.7 0.1 - 0.5 44 TiOxCyNz coating layers 42 and 46 0.01 - 0.5 0.05 - 0.25
[0020] Table 2 below shows the deposition parameters for the deposition of coating scheme 32A of the coated cutting insert 30 of Fig. 2. Table 2 - Method for producing the coating scheme of FIG. 2 Repeat sequence Support substance Support substance Support substance Transition for multi-layer Coating scheme AlO TiN MT-TiCN HT-TiCN Ti+O+C+N TiOxCyNz 2 3 Temp.- 950 - (°C) 850 - 960 750 - 900 950 - 1020 950 - 1020 920 - 1020 Area 1050 Pressure range (mb) 60 - 90 40 - 90 300 - 700 100 - 400 50 - 120 200 - 500 Duration Minutes 10 - 90 50 - 400 5-60 30 - 70 5-30 3-15 H Vol% to the rest to the rest to the rest to the rest to the rest to the rest 2 N Vol% 15-20 25 - 35 20 - 40 15 - 20 30 - 45 2 CH Vol% 1 -5 2-3 2-3 4 CO Vol% 2.0 - 2.8 2 0.8 HCl Vol% 1.0 - 1.5 2.5 - 3.5 - 1.5 HS Vol% 0.1 - 1.0 2 TiCl Vol% 0.5 - 2.5 1.0 - 2.0 1 -3 0.5 - 1.3 0.5 - 1.2 4 CH CN Vol% 0.001 - 0.03 3 AlCl Vol% 4.0 - 6.0 3 CO Vol% 1.0 - 1.5 0.8 - 1.5
[0021] Referring to the coating scheme shown in Fig. 3 (not according to the invention), a coated Cutting insert, generally designated 50, which comprises a substrate 52 and a surface 51 of the Substrate 52 comprises coating scheme 52A. The coating scheme 52A comprises a Support coating scheme 54 comprising a TiN coating layer 56 on the surface of the substrate 52 and a MT-TiCN coating layer 58 on the TiN coating layer 56 and an HT-TiCN coating layer 59 on the MT-TiCN coating layer 58.
[0022] On the TiCN coating layer 59 there is a Ti+O+C+N transition layer 60 containing titanium and oxygen and contains carbon and nitrogen. It is important to consider that the applicants have not yet fully considered the function of the Ti+O+C+N transition layer, although we do not want to be bound to a specific theory, it is assumed that the Ti+O+C+N transition layer the nucleation and adhesion of the coating layers of the multilayer coating schemes favored.
[0023] The multilayer coating scheme 69 is located on the Ti+O+C+N transition layer 60, wherein the multilayer coating scheme 69 comprises a plurality of coating sets (64, 70). The coating set 64 comprises a coating layer of aluminum oxide 66 and a TiN coating layer 68, and the coating set 70 comprises a coating layer of aluminum oxide 72 and a TiN coating layer 74. Although not shown in Fig. 3 As shown, another embodiment of the invention includes an external coating scheme deposited by CVD on the surface of the outermost layer of the repeating set. Such an external The coating layer may be a carbide, carbonitride, nitride or oxycarbonitride formed by a group IVb element include.
[0024] The following Table 3 shows the thickness ranges of the coating schemes and coating layers for the coated cutting insert 30 shown in Fig. 3. Table 3 - Thickness of coating schemes and Coating layers of FIG. 3 (not according to the invention) Coating layer or alternative thickness range Thickness range (micrometers) Coating scheme (micrometers) Coating scheme 52A 2 - 35 5 - 30 Support coating scheme 54 1 - 20 2-18 TiN coating layer 56 up to 2 up to 1 MT-TiCN coating layer 58 1 - 18 2-15 HT-TiCN coating layer 59 up to 5 up to 2 Ti + O + C + N transition layer up to 3 up to 2 Multi-layer coating scheme 69 1 - 15 2-12 Coating sets 64 and 70 0.1 - 0.8 0.2 - 0.7 Coating layers of 0.1 - Aluminum oxide 66 and 72 0.5 TiN coating layers 68 and 0.01 - 0.5 0.05 - 0.25 74
[0025] Table 4 below shows the deposition parameters for the deposition of coating scheme 52A of the coated cutting insert 50 of Fig. 3 (not according to the invention). Table 4 - Method for producing the Coating schemes of FIG. 3 (not according to the invention) Repeat sequence for Supporting substance Supporting substance Supporting substance Transition multi-layer Coating scheme AlO TiN MT-TiCN MT-TiCN Ti+O+C+N TiN 2 3 Temp.- 950 - (°C) 850 - 960 750 - 900 950 - 1020 950 - 1020 920 - 1020 Area 1050 60 - Pressure range (mb) 60 - 90 40 - 90 300 - 700 100 - 400 50 - 120 250 Duration Minutes 10 - 90 50 - 400 5-60 30 - 70 5-30 3-15 for the H Vol% to the rest to the rest to the rest to the rest to the rest 2 rest 20 - N Vol% 15-20 25 - 35 20 - 40 15-20 2 30 CH Vol% 1 -5 2-3 4 CO Vol% 2.0 - 2.8 2 0.5 - HCl Vol% 1.0 - 1.5 2.5 - 3.5 1.0 HS Vol% 0.1 - 1.0 2 0.5 - TiCl Vol% 0.5 - 2.5 1.0 - 2.0 1 -3 0.5 - 1.3 4 2.5 CH CN Vol% 0.001 - 0.03 3 AlCl Vol% 4.0 - 6.0 3 CO Vol% 1.0 - 1.5
[0026] Referring to the microstructure of the coated cutting insert shown in the micrograph of Fig. 4 As can be seen, the cross-sectional view of a coated cutting insert shows the different layers that are formed by the Variety of coating sets are formed based on the support coating scheme on a hard metal substrate are secluded.
[0027] Referring to the coating scheme shown in Fig. 5 (not according to the invention), a coated Cutting insert, generally referred to as 130, which comprises a substrate 132 and a surface 131 of the substrate 132. The coating scheme 133 comprises a Support coating scheme 134 comprising a TiN coating layer 136 on the surface of the substrate 132 and an MT-TiCN coating layer 138 on the TiN coating layer 136 and an HT-TiCN coating layer 140 on the MT-TiCN coating layer 138.
[0028] On the TiCN coating layer 140 there is a Ti+O+C+N transition layer 139, which contains titanium and Contains oxygen, carbon and nitrogen. It is important to consider that the applicants, with regard to the Function of the Ti+O+C+N transition layer, although one does not want to be bound to a specific theory, assumes that the Ti+O+C+N transition layer promotes the nucleation and adhesion of the coating layers of the multilayer coating schemes favored.
[0029] On the Ti+O+C+N transition layer 139 there is a multilayer coating scheme 141, wherein the multi-layer coating scheme 141 a variety of coating sets (146, 152, 158) The coating set 146 comprises a coating layer of aluminum oxide 148 and a TiAlOCN Coating layer 150. The coating set 152 comprises a coating layer of aluminum oxide 154 and a TiAlOCN coating layer 156. The coating set 158 includes a coating layer of aluminum oxide 160 and a TiAlOCN coating layer 162. In one embodiment of the invention, the outermost repeating layer exposed. Another embodiment of the invention has an optional external coating layer scheme applied by CVD to the surface of the outermost layer of the repeating set The specific embodiment in Fig. 5 shows an external TiOCN coating layer 164. Table 5 below shows the thickness ranges of the coating schemes and coating layers for the coated cutting insert 130 shown in Fig. 5. Table 5 - Thickness of coating schemes and Coating layers of FIG. 5 (not according to the invention) Thickness range Alternative thickness range Coating layer or coating scheme (micrometers) (micrometers) Coating scheme 133 2 - 35 5 - 30 Support coating scheme 134 1 - 20 2-18 TiN coating layer 136 up to 2 up to 1 MT-TiCN coating layer 138 1 - 18 2-15 HT-TiCN coating layer 140 up to 5 up to 2 Ti + O + C + N transition layer up to 3 up to 2 Multi-layer coating scheme 141 1 - 15 2-12 Coating sets 146, 152 and 158 0.1 - 0.8 0.2 - 0.7 Coating layers of aluminum oxide 148, 154, 0.05 - 0.7 0.1 - 0.5 160 TiAlOCN coating layers 150, 156, 162 0.01 - 0.5 0.05 - 0.25 External TiOCN coating layer 164 1.0 - 3.0 1.5 - 2.5
[0030] Table 6 below shows the deposition parameters for the deposition of the coating scheme 133 of the coated cutting insert 130 of Fig. 5. Table 6 - Method for producing the coating scheme of FIG. 5 (not according to the invention) Repeat sequence Supporting substance Supporting substance Supporting substance Transition for multi-layer external Coating scheme AlO TiN MT-TiCN HT-TiCN Ti+O+C+N TiAlOCN TiOCN 2 3 Temp.- 970 - (°C) 850 - 960 750 - 900 970 - 1000 950 - 1020 920 - 1020 970 - 1000 Area 1000 60 - Print range (mb) 60 - 90 40 - 90 120 - 380 100 - 400 50 - 120 60 - 200 400 Duration Minutes 10-90 50 - 400 30 - 70 5 - 30 for the H Vol% to the rest to the rest to the rest to the rest to the rest to the rest 2 rest 35 - N Vol% 15 - 20 25 - 35 15 - 45 15-20 5-20 2 45 2.5 - CH Vol% 1 - 4.5 2-3 0-3 4 3.5 CO Vol% 2.0 - 2.8 2 1 HCl Vol% 1.0 - 2.0 2.5 - 3.5 0-3 - 1.5 HS Vol% 0.1 -1.0 2 1.8 - TiCl Vol% 0.5 - 2.5 1.0 - 2.0 0.8 - 3 0.5 - 1.3 0.1 - 2.5 4 2.4 CH CN Vol% 0.001 - 0.03 3 AlCl Vol% 4.0 - 6.0 2-4 3 1 - CO Vol% 1 -2 1.0 - 1.5 1 - 5.5 1.5
[0031] Cutting tests were carried out to evaluate the performance of the coated cutting inserts of the invention in comparison to conventional coated standard cutting inserts. Tables 7 and 8 below show the Test results are listed, which were carried out in several machining steps taking into account the following wear criteria were measured. The tests were carried out under the following parameters: Cutting insert geometry CNMG432RN (straight cutting edge); pitch angle 0° / 90°; cutting tool diameter = 2.48 inches; maximum 3 Tool diameter = 2.48 inches; machining pass length = 12 inches; metal removal rate = 1.95 inches / min.; Cutting speed = 820 feet per minute; revolutions per minute = 1263; feed per tooth (fz) = 0.008 inch / tooth; Feed rate (Vf) = 10.104 in / min; axial depth of cut (Ap) = 0.098 in; radial depth of cut (Ae) = 1.969 in; Machine = Mazak AJV; Coolant = dry; and Workpiece material = DCI 80-55-06. Table 7 - Test results for coated cutting inserts Repeat. Repeat. % Pattern Standard Deviation Average 1 2 Improvement Control standard coated cutting inserts 12.00 15.00 2.12 13.50 - Coated cutting insert from Fig. 2 with 4 19.00 24.00 3.54 21.50 59% Coating sets made of Al2O3 / TiOCN Coated cutting insert from Fig. 2 with 8 15.00 19.00 2.83 17.00 26% Coating sets made of Al2O3 / TiOCN Table 8 - Test results for coated cutting inserts Recovered % Pattern Repeat 1 Standard Deviation Average 2 Improvement Control standard coated 9.80 14.30 3.18 12.05 - Cutting inserts Coated Cutting insert from Fig. 2 18.50 21.50 2.12 20.00 66% with 4 coating sets from Al2O3 / TiOCN Coated Cutting insert from Fig. 2 38 14.60 18.80 2.97 16.70 with 8 coating sets from % Al2O3 / TiOCN
[0032] A major failure mode of a coating structure described in this invention is the Wear mechanism that occurs during heavily interrupted machining. In applications with interrupted During cutting, any contact with the workpiece material affects the coating. Ongoing impacts can lead to lead to fatigue failure of the coating, which in conventional coatings results in chipping of one or In the coating according to the invention described herein, the failure a single coating layer unit does not adversely affect the integrity of the entire coating scheme because a crack between coating layer units (e.g. two coating layers containing an Al O -Ti 2 3 layer). In other words, the present coating scheme according to the invention limits the extent of damage to a specific single coating layer (or two Coating layers containing Al O -Ti) and thereby prevents the propagation of one or more cracks in the 2 3 entire coating scheme. Damage to a single coating layer (or two Coating layers containing Al O -Ti) does not adversely affect the integrity of the entire 2 3 coating scheme, nor on the underlying coating layer pairs containing Al O -Ti. These 2 3 Property is shown in Figures 6A to 6C.
[0033] The coating scheme in Fig. 6A to 6C (not according to the invention) comprises a TiN base layer on the Surface of a substrate, an MT-TiCN coating layer on the TiN base layer, an HT-TiCN Coating layer on the MT-TiCN coating layer and a repeating series of Coating layer pairs each consisting of a Ti-containing and an Al O -coating layer, wherein the Ti-containing 2 3 Coating layer HT-TiCN is on the HT-TiCN coating. On the outermost Al O coating layer of the 2 3 repeating series there is an outermost HT-TiCN coating layer, and on the outermost HT-TiCN coating layer is a TiN coating layer. Fig. 6A is a micrograph showing some of the Coating layers of a coating scheme according to the invention in cross-section. Fig. 6A contains a Area designated 6B / C. This area can be seen in the photomicrographs of Fig. 6B and Fig. 6C. Fig. 6B and Fig. 6C are the same photomicrograph, except that Fig. 6C is rotated relative to Fig. 6B and Fig. 6C markings to identify the coating layers. As previously described, crack propagation between Coating layer units (e.g. between two coating layers comprising an Al O -Ti-containing layer) in 2 3 Figs. 6A to 6C, and in particular in Fig. 6B and Fig. 6C .
[0034] The conventional coating scheme of a conventional tool is shown in Fig. 7A to 7C. The conventional coating scheme of Fig. 7A to 7C includes a TiN base coating layer on the surface a substrate, an MT-TiCN coating layer on the TiN base coating layer, a TiCN coating layer on the MT-TiCN coating layer, a Ti-containing coating layer on the TiCN coating layer, a single Al O coating layer on the Ti-containing coating layer. On the Al O coating layer is 2 3 2 3 There is an outermost TiCN coating layer, and on the outermost TiCN coating layer there is a TiN Coating layer. Fig. 7A is a micrograph showing some of the coating layers of a conventional Coating schemes in cross-section. Fig. 7A contains an area labeled 7B / C. This area is in the photomicrographs of Fig. 7B and Fig. 7C. Fig. 7B and Fig. 7C are the same photomicrograph, except that Fig. 7C is rotated relative to Fig. 7B and Fig. 7C contains markings to identify the coating layers. As can be seen in Figs. 7A to 7C, the conventional coating scheme has a complete defect, exposing the underlying coating structure and the cutting tool is subject to greater wear, resulting in a shorter useful service life.
[0035] The substrate for each of the specific embodiments may be selected from the same group of materials. In this regard, suitable materials for the substrate include hard metals (e.g., tungsten carbide-cobalt materials). Another preferred substrate material is based on cobalt tungsten carbide cemented carbide, which contains about 0.1 weight percent to about 20 percent by weight cobalt and the rest tungsten carbide. It is possible that such a cobalt Tungsten carbide additives such as titanium, tantalum, niobium, zirconium, hafnium, vanadium and chromium, either alone or in any combination, these additives being in the form of carbides and / or nitrides and / or carbonitrides, as well as other additives which typically added to hard metals. In yet another composition, the substrate comprises a Tungsten carbide cemented carbide comprising: between about 89.8 weight percent and about 92.3 weight percent tungsten carbide, between about 5.7 weight percent and about 11.5 weight percent cobalt, up to about 3.0 weight percent tantalum, up to about 2 weight percent titanium, up to about 2.4 weight percent niobium and up to about 0.8 weight percent chromium.
[0036] The applicants also contemplate that the substrate may have gradient compositions, especially in the concentration of the binder, the concentration of the carbonitride and the concentration of the Carbides. Substrates could include, for example, a cemented carbide substrate having a surface area with a binder enrichment, or a hard metal substrate having a binder-depleted surface area with a hard metal enrichment in solid solution.
[0037] For each of these specific embodiments, it should be noted that prior to the deposition of the Coating schemes the surface of the substrate should be treated to ensure the adhesion of the coating scheme on the substrate. Pretreatments include, for example, a process for removing or reducing the Amount of binder on the substrate surface. In the case of a cobalt tungsten carbide substrate, Such pretreatment removes the cobalt from the surface of the substrate or treats the surface to improve the adhesion of the coating. Another example of such a pretreatment would be a process that mechanically acts on the substrate surface, so that it is roughened and the adhesion of the Coating improved.
[0038] It should be noted that the surface of the coating scheme for performance improvement in some cases must be treated after deposition by smoothing the coating and applying a voltage-changing effect on the coating. An example of a treatment is the removal of unevenness on the Surface of the coating scheme to reduce the number of points with increased stress or Another example of treatment is the preferential removal of the coating (or part of the coating layer) of selected areas of the cutting insert. Surface treatment reduces typically increases the tensile stress or compressive stress in the coating layer(s). For example: PCT Patent Publication No. WO 02 / 077 312 A2, Widia GmbH, discloses the shot peening of a coating (PVD or PCVD or CVD) to increase the internal compressive stress in the outer coating layers or to increase the internal to reduce tensile stress.
[0039] It should also be taken into account that in order to improve the adhesion of the coating layers microscopically rough interfaces between the individual coating layers can be provided. These Microscopically rough cut surfaces can be achieved by setting the parameters for the CVD process (or the MT-CVD process, MT-CVD = chemical vapor deposition at medium temperature) in order to Coating layers promote high growth rates. High growth rates can be achieved with CVD processes (including MT-CVD processes) due to the application of relatively high deposition temperatures and / or relatively high pressures. Another alternative to improve adhesion between coating layers is the following: In the deposition process, the composition of adjacent layers can be changed step by step to the number of sharp interfaces affecting the composition between adjacent to reduce coating layers.
[0040] In view of the above, it can be concluded that an improved coated cutting insert and a method for its manufacture are provided, wherein the cutting insert is used in applications for the removal of material and the coated cutting insert has a coating scheme with high strength, which leads to better cutting edge stability, especially in heavily interrupted turning and milling operations. An improved coated cutting insert and a method for its manufacture are provided, wherein the Cutting insert is useful in material removal applications, where the coated cutting insert is a coating scheme that includes a multi-layer coating scheme that inhibits crack growth and Crack propagation in the coating scheme due to mechanical stress or temperature change better An improved coated cutting insert and a method for its production are provided, whereby the cutting insert is useful in material removal applications and the coated cutting insert has a coating that includes a transition layer that provides better nucleation and adhesion of the multilayer coating scheme.
[0041] Further embodiments of the invention will be apparent to those skilled in the art upon consideration of the description or a application of the invention disclosed herein. It is intended that the description and examples be are illustrative and are not intended to limit the scope of the invention. The actual scope of the invention is indicated by the following claims.
Claims
1. Coated cutting insert (30) for removing material by machining, with: a substrate (32) and a coating pattern (32A) on the substrate (32); wherein the coating scheme (32A) comprises: a chemical vapor deposition support coating scheme (33), wherein the Support coating pattern (33) is located on the surface of the substrate (32); a transition layer (38) deposited by chemical vapor deposition on the surface of the Support coating schemes (33); and a multilayer coating scheme (49) deposited by chemical vapor deposition, which A plurality of repeating coating sets (39, 43), wherein the multi-layer coating scheme (49) lies on the surface of the transition layer (38); and wherein each of the coating sets (39, 43) is formed from a coating layer of aluminum oxide (40, 44) having a alpha-aluminum oxide crystal structure, and a nitrogen-containing TiO CN coating layer (42, 46) which has a xyz Crystal structure of the nitrogen-containing TiO CN coating layer (42, 46), wherein the aluminum oxide xyz crystal structure differs from the crystal structure of the nitrogen-containing TiO CN coating layer (42, 46), whereby xyz between adjacent coating layers of aluminum oxide (40, 44) and the nitrogen-containing TiO CN - xyz Coating layer (42, 46) of the coating sets (39, 43) a clear boundary is formed, and wherein the TiO CN - xyz coating layer (42) is in contact with the aluminum oxide layer (44) of an adjacent coating set (43), and where x, y and z in the nitrogen-containing TiO CN coating layer (42,46) have the following values: 0 <x<0,7, xyz 0 <y<0,7, 0<z<0,7.
2. Coated cutting insert (30) according to claim 1, wherein in each of the coating sets (39, 43) the Coating layer of aluminum oxide (40, 44) has a thickness between 0.05 µm and 0.7 µm and the nitrogen-containing TiO CN coating layer (42, 46) has a thickness between 0.01 µm and 0.5 µm. xyz 3. Coated cutting insert (30) according to claim 1 or 2, wherein the multi-layer coating scheme (49) has a thickness between 1 µm and 15 µm.
4. Coated cutting insert (30) according to one of claims 1 to 3, wherein the support coating scheme (33) comprises a inner coating layer of titanium nitride (34) with a thickness of up to 2 µm, a middle coating layer of MT titanium carbonitride (36) with a thickness between 1 µm and 18 µm and an outer coating layer (37) comprising either a titanium nitride coating layer or an HT titanium carbonitride coating layer.
5. Coated cutting insert (30) according to claim 4, wherein the outer coating layer (37) comprises the HT- Titanium carbonitride coating layer.
6. Coated cutting insert (30) according to one of claims 1 to 5, wherein in each coating set (39, 43) the Coating layer of aluminum oxide (40, 44) is closer to the substrate (32) than the nitrogen-containing TiO CN - xyz Coating layer (42, 46).
7. Coated cutting insert (30) according to one of claims 1 to 6, wherein the substrate (32) is a tungsten carbide Hard metal comprises, with between 89.8 weight percent and 92.3 weight percent tungsten carbide, between 5.7 weight percent and 11.5 weight percent cobalt, up to 3.0 weight percent tantalum, up to 2 weight percent titanium, up to 2.4 weight percent niobium and up to 0.8 weight percent chromium.
8. Coated cutting insert (30) according to one of claims 1 to 7, wherein the coating scheme (32A) further comprises a external coating scheme on the multi-layer coating scheme (49).
9. Coated cutting insert (30) according to claim 8, wherein the external coating scheme comprises an HT- Titanium oxycarbonitride coating layer.
10. Coated cutting insert (30) according to one of claims 1 to 9, wherein the transition layer (38) comprises titanium, oxygen, carbon and nitrogen.
11. A method for producing a coated cutting insert (30) according to any one of claims 1 to 10, wherein the Procedure includes the following steps: Providing a substrate (32); Applying a support coating scheme (33) to the substrate (32) by chemical vapor deposition; Applying a transition layer (38) on the support coating scheme (33) by chemical deposition from the gas phase; Applying a multilayer coating scheme (49) to the transition layer (38) by chemical deposition from the gas phase, wherein the multi-layer coating scheme (49) comprises several repeating coating sets (39, 43) and wherein the steps for applying the individual coating sets (39, 43) each comprise the following: Applying a coating layer of aluminum oxide (40, 44) without varying the parameters for deposition of the Coating, wherein the coating layer of aluminum oxide (40, 44) has an alpha-aluminum oxide crystal structure and Interrupting the application of the coating layer of aluminum oxide (40, 44) by applying a nitrogen-containing TiO CN coating layer (42, 46) which represents the crystal structure of the nitrogen-containing xyz coating layer (42, 46), wherein the crystal structure of the nitrogen-containing TiO CN coating layer (42, xyz 46) differs from the alpha-alumina crystal structure, thus creating a clear boundary between the Coating layer of aluminum oxide (40, 44) and the nitrogen-containing TiO CN coating layer (42, 46) of the xyz coating sets (39, 43), and wherein the TiO CN coating layer (42) is coated with the aluminum oxide layer xyz (44) of an adjacent coating set (43), and wherein x, y and z in the nitrogen-containing TiO CN - xyz Coating layer (42,46) have the following values: 0 <x<0,7, 0<y<0,7, 0<z<0,7.
12. The method according to claim 11, wherein in each of the coating sets (39, 43) the coating layer consists of Aluminium oxide (40, 44) has a thickness between 0.05 µm and 0.7 µm and the nitrogen-containing TiO CN - xyz Coating layer (42, 46) has a thickness between 0.01 µm and 0.5 µm.
13. The method according to claim 11, wherein the multi-layer coating scheme (49) has a thickness between 1 µm and 15 µm has.
14. The method of claim 11, wherein the support coating scheme (33) comprises an internal Titanium nitride coating layer (34) with a thickness of up to 2 µm and a middle coating layer of MT- titanium carbonitride (36) with a thickness between 1 µm and 18 µm.
15. The method of claim 14, further comprising applying an outer support coating layer (37) to the support coating scheme (33) is applied, which may be either a titanium nitride coating layer or a coating layer made of HT titanium carbonitride.
16. The method of claim 11, further comprising applying an external coating scheme to the multilayer Coating scheme (49) is applied by chemical deposition from the gas phase, wherein the outer Coating scheme has a coating layer of titanium oxycarbonitride.
17. The method of claim 11, wherein the transition layer (38) comprises titanium, oxygen, carbon and nitrogen and the step of applying the transition layer (38) at a temperature between 950 °C and 1020 °C and a pressure between 100 millibar and 400 millibar and uses a gas mixture with TiCl , CH , CO, N and hydrogen 4 4 2 becomes.
18. The process according to claim 17, wherein N is present in a proportion between 15 volume percent and 20 volume percent of the 2 gas mixture, CH in a proportion between 2 and 3 volume percent of the gas mixture, TiCl in 4 4 a proportion between 0.5 volume percent and 1.3 volume percent of the gas mixture, CO in a proportion between 1.0 Volume percent and 1.5 volume percent of the gas mixture and hydrogen in a proportion between 74.2 volume percent and 81.5 volume percent of the gas mixture.
19. The method according to claim 11, wherein the step of first applying a coating layer of Aluminium oxide (40, 44) at a temperature between 920 °C and 1020 °C and a pressure between 50 millibar and 120 millibar and a gas mixture of CO, HCl, HS, AlCl and hydrogen is used. 2 2 3 20. A process according to claim 19, wherein CO is present in a proportion of between 2.0 volume percent and 2.8 volume percent of the 2 gas mixture, HCl in a proportion between 2.5 volume percent and 3.5 volume percent of the gas mixture, HS 2 in a proportion between 0.1 volume percent and 1.0 volume percent of the gas mixture, AlCl in a proportion between 3 4.0 volume percent and 6.0 volume percent of the gas mixture and hydrogen in a proportion between 85.2 volume percent and 89.4 volume percent of the gas mixture.
21. The method according to claim 11, wherein the step of applying the nitrogen-containing TiO CN coating layer xyz (42, 46) at a temperature between 950 °C and 1050 °C and a pressure between 200 millibar and 500 millibar takes place and a gas mixture of N , CH , HCl, TiCl , CO and hydrogen is used. 2 4 4 22. A process according to claim 21, wherein N is present in a proportion of between 30% by volume and 45% by volume of the 2 gas mixture, CH in a proportion between 2 and 3 volume percent of the gas mixture, HCl in 4 a proportion between 0.8 volume percent and 1.5 volume percent of the gas mixture, TiCl in a proportion between 0.5 4 volume percent and 1.2 volume percent of the gas mixture, CO in a proportion between 0.8 volume percent and 1.5 Volume percent of the gas mixture and hydrogen in a proportion between 47.8 volume percent and 65.9 Volume percent of the gas mixture.
Citation Information
Patent Citations
Multilayer structured coatings for cutting tools and method for producing a cutting tool
DE112014001640T5
Coated cemented carbide cutting tool
EP1245698B1
Coated cemented carbide insert
EP1455003A2
Cutting insert having ceramic coating
EP1980649B1
Alumina coating, coated product and method of making the same
US20050202283A1