Method for producing a metal-ceramic substrate, soldering system and metal-ceramic substrate produced by such a method

A multilayer soldering system with a separate active metal layer and a phosphorus-free soldering layer addresses the challenge of thick solder layers in metal-ceramic substrates, achieving cost-effective and efficient connections with improved processability and performance.

DE102019126954B4Active Publication Date: 2024-12-05ROGERS GERMANY
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
DE102019126954
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-10-08
Publication Date
2024-12-05
Estimated Expiration
2039-10-08

AI Technical Summary

Technical Problem

Existing methods for connecting metal layers to ceramic layers in metal-ceramic substrates, such as those used in printed circuit boards, are limited by the need for thick solder layers due to brittle intermetallic phases, which increase costs and complicate structuring processes.

Method used

A multilayer soldering system is used, comprising a soldering layer free of melting point-lowering elements and a separate active metal layer, allowing for thinner solder layers and improved connection processes.

Benefits of technology

This approach enables thinner solder layers, reduces material costs, simplifies structuring, and accelerates the connection process while maintaining strong and reliable bonds, without compromising thermal conductivity or mechanical strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Method for producing a metal-ceramic substrate (1), comprising: - Providing at least one ceramic layer (10), at least one metal layer (20) and at least one solder layer (30), in particular in the form of at least one solder foil, - Coating the at least one ceramic layer (10) and / or the at least one metal layer (20) and / or the at least one solder layer (30) with at least one active metal layer (40), - Arranging the at least one solder layer (30) between the at least one ceramic layer (10) and the at least one metal layer (20) along a stacking direction (S) forming a solder system (35) comprising the at least one solder layer and the at least one active metal layer (40), and - Bonding the at least one metal layer (20) to the at least one ceramic layer (10) via the soldering system (35) using an active soldering process, wherein the soldering layer material is AgCu28, AgCuln, AgCuSn, AgCuGa, CuSn, Culn, CuGa, CuInSn, CuInMb, CuGaSn or NiCrMn, wherein the at least one active metal layer is applied using a vapor deposition process.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a method for producing a metal-ceramic substrate, a soldering system for such a method and a metal-ceramic substrate produced by such a method.

[0002] Metal-ceramic substrates are well known in the art, for example, as printed circuit boards or circuit boards, for example from DE 10 2013 104 739 A1, DE 199 27 046 B4, and DE 10 2009 033 029 A1. Typically, connection pads for electrical components and conductor tracks are arranged on one component side of the metal-ceramic substrate, wherein the electrical components and the conductor tracks can be interconnected to form electrical circuits. Key components of metal-ceramic substrates are an insulating layer, preferably made of a ceramic, and at least one metal layer bonded to the insulating layer. Due to their comparatively high insulation strength, insulating layers made of ceramic have proven particularly advantageous in power electronics. By structuring the metal layer, conductor tracks and / or connection pads for the electrical components can then be realized.

[0003] A prerequisite for creating such a metal-ceramic substrate is a permanent bond between the metal layer and the ceramic layer. In addition to a so-called direct bonding process, i.e., DCB or DAB processes, it is known from the prior art to bond the metal layer to the ceramic layer using a solder material.

[0004] An active soldering process, e.g., for joining metal layers or metal foils, in particular copper layers or copper foils, to ceramic material, is a process specifically used to manufacture metal-ceramic substrates. This process involves creating a bond between a metal foil, e.g., a copper foil, and a ceramic substrate, e.g., an aluminum nitride ceramic, at a temperature between approximately 650 and 1000°C using a brazing alloy that, in addition to a main component such as copper, silver, and / or gold, also contains an active metal. This active metal, which, for example, is at least one element from the group consisting of Hf, Ti, Zr, Nb, and Ce, creates a bond between the solder and the ceramic through a chemical reaction, while the bond between the solder and the metal is a metallic brazing joint.

[0005] EP 3 041 042 A1 and WO 2017 / 126 653 A1, for example, disclose methods for producing a power module substrate using an active solder material. In particular, it is provided that a copper foil is bonded to a ceramic layer via a multilayer soldering system. This multilayer system consists of a layer of titanium foil and a layer of a phosphorus-containing solder filler material.

[0006] Furthermore, it is known from EP 0 153 618 A2 to create a connection between a metal layer and a ceramic layer using a soldering system in which a solder layer made of pure silver and a separate active metal layer are used. DE 10 2015 108 668 A1 relates to a method for producing a composite material, in particular a printed circuit board, wherein the composite material comprises a flat base material, in particular a ceramic, to which an additional layer, in particular a metallization, is applied on one or both sides by means of a solder layer. US 5 354 415 A relates to a method for producing a ceramic printed circuit board by forming a metal circuit pattern on a ceramic plate using a brazing material with an active metal content and removing an unnecessary part of the brazing material by chemical alkali treatment.

[0007] Based on this prior art, the present invention has for its object to realize a bonding of the metal layer to the ceramic layer using a soldering system that is improved over the prior art, in particular with regard to the solder layer connecting the metal layer and the ceramic layer and the bonding process during active soldering.

[0008] This object is achieved by a method for producing a metal-ceramic substrate according to claim 1, a soldering system for such a method according to claim 9, and a metal-ceramic substrate produced by such a method according to claim 10. Further advantages and properties emerge from the subclaims as well as the description and the accompanying figures.

[0009] According to a first aspect of the present invention, there is provided a method for producing a metal-ceramic substrate, comprising: - Providing at least one ceramic layer, at least one metal layer and at least one soldering layer, in particular in the form of at least one soldering foil or brazing foil, - coating the at least one ceramic layer and / or the at least one metal layer and / or the at least one solder layer with at least one active metal layer, - Arranging the at least one solder layer between the at least one ceramic layer and the at least one metal layer along a stacking direction to form a solder system comprising the at least one solder layer and the at least one active metal layer, wherein a solder material of the at least one solder layer is preferably free of a melting point-lowering material and / or phosphorus-free, and - Bonding the at least one metal layer to the at least one ceramic layer via the soldering system by means of an active soldering process.

[0010] Compared to the prior art methods for producing metal-ceramic substrates, the invention provides a multi-layer soldering system comprising at least one solder layer, preferably free of melting point-lowering elements, and at least one active metal layer. The separation of the at least one active metal layer and the at least one solder layer proves particularly advantageous because it allows for the realization of comparatively thin solder layers, especially when the solder layer is a foil. Otherwise, comparatively large solder layer thicknesses must be realized for solder materials containing active metals due to the brittle intermetallic phases that hinder the deformation of the solder paste or solder layer, whereby the minimum layer thickness is limited by the manufacturing properties of the active metal-containing solder material.Accordingly, for solder layers containing active metals, the minimum solder layer thickness is not determined by the minimum thickness required for the joining process, but rather by the minimum technically feasible solder layer thickness. As a result, this thicker, active metal-containing solder layer is more expensive than thinner layers.

[0011] By separating the active metal from the at least one solder layer, the thickness of the at least one solder layer can be advantageously reduced. As a result, material for the soldering system or for the at least one solder layer can be saved. It has proven particularly advantageous that such active metal-free solder layers can also be rolled down to thicknesses of less than 10 µm, preferably less than 7 µm. A further advantage is that the etching of the structuring on the manufactured metal-ceramic substrate is simplified, in particular because a second thickness of the soldering system or of the at least one solder layer is reduced. In addition, the bonding of the metal layer to the ceramic layer can be accelerated during the manufacturing process.

[0012] In particular, it has been found that the use of a separate active metal layer is possible even if the solder layer is free of melting point-lowering elements and / or phosphorus-free. This allows for greater flexibility in the choice of the material to be used for the at least one solder layer, and it is possible to use the established process parameters for the active soldering process. Furthermore, the addition of corresponding melting point-lowering elements can advantageously be dispensed with prior to the formation of the at least one solder layer. In particular, the person skilled in the art understands at least one solder layer that is free of low-melting point elements to be a layer that contains less than 3% by weight, preferably less than 2% by weight, and particularly preferably less than 1% by weight of these melting point-lowering elements. Examples of these melting point-lowering elements are phosphorus and zinc.The use of phosphorus-free solder materials, for example, allows for the advantageous separation of the active metal layer and solder layers, even for solder layers that are free of phosphorus but contain a melting-point-lowering material, the integration of which into the solder layer, in turn, does not lead to as significant a reduction in the melting point as is known for phosphorus. For example, this is a melting-point-lowering material that lowers the melting point of the solder layer by less than 100°C, preferably less than 80°C, and particularly preferably less than 50°C.

[0013] Furthermore, it is preferably provided that the at least one solder layer is free of an active metal. In particular, a person skilled in the art understands that free of active metal means that the solder layer has less than 5% by weight, preferably less than 3% by weight, and particularly preferably less than 1.5% by weight of active metal. Examples of an active metal are titanium (Ti), zirconium (Zr), hafnium (Hf), chromium (Cr), niobium (Nb), cerium (Ce), and vanadium (V). It is particularly preferably provided that the at least one solder layer is provided as a foil. This allows the foil to be handled as easily as possible when arranging it between the at least one ceramic layer and the at least one metal layer, particularly in the series production of metal-ceramic substrates.

[0014] For example, it is also conceivable that the at least one solder layer is already provided with a metal layer or the at least one metal layer. For example, the at least one solder layer is applied to one side of the at least one metal layer that is used to produce the metal-ceramic substrate. In this case, the at least one metal layer serves as a carrier for the at least one solder layer. However, it is also conceivable that the at least one solder layer is provided on a film, for example on a plastic film, which forms the carrier. Furthermore, it is conceivable that the at least one solder layer is provided on the at least one metal layer and that at least one further metal layer, preferably with a different grain size distribution ora different average grain size, is applied to the side of the at least one metal layer facing away from the solder layer, which side preferably carries the at least one solder layer. In particular, it is provided that the grain sizes, in particular their average grain sizes, of the at least one metal layer and the at least one further metal layer differ from one another, so that a two-layer metallization layer forms on the upper side of the ceramic during the bonding process. In this case, it is particularly preferably provided that the metal layer with the smaller average grain size is on the outside and the metal layer with the comparatively larger average grain size faces the soldering system or the ceramic layer.

[0015] In particular, it has proven advantageous that the at least one active metal layer can be applied selectively to the at least one ceramic layer and / or the at least one metal layer and / or the at least one solder layer. Preferably, the at least one active metal layer is applied to at least two of the aforementioned layers. Preferably, the at least one active metal layer is arranged on the at least one ceramic layer or on at least one metal layer on the side which, in the arranged state or in the metal-ceramic substrate, faces the at least one solder layer. It is particularly preferred if the at least one active metal layer is applied to the at least one solder layer.In this case, a brazing system comprising the at least one brazing layer with the at least one active metal layer can be provided, which can be easily arranged between the at least one ceramic layer and the at least one metal layer for the active brazing process. The bonding process is an active brazing process that is carried out at a process temperature between 600°C and 1000°C, preferably between 700°C and 950°C.

[0016] The solder material of the at least one solder layer is preferably a silver-based or a copper-based solder material. In a silver-based solder material, silver is the main component, i.e. the component with the highest proportion in terms of weight percentage, whereas in a copper-based solder material, copper is the main component. According to the invention, AgCu28, AgCuln, AgCuSn, AgCuGa, CuSn, Culn, CuGa, CuInSn, CuInMb, CuGaSn or NiCrMn are to be used as the solder layer material. In particular, it is preferably provided if the solder layer is silver-free, i.e. the solder layer comprises less than 3% by weight of silver, preferably less than 2% by weight of silver and particularly preferably less than 1% by weight of silver. This advantageously allows silver to be saved, which could otherwise lead to silver migration in the solder system of the manufactured metal-ceramic substrate.

[0017] Conceivable materials for the at least one metal layer include copper, aluminum, molybdenum, and / or their alloys, as well as laminates and powder metallurgical compound materials such as CuW, CuMo, CuAl, AlCu, and / or CuCu, in particular a copper sandwich structure with a first copper layer and a second copper layer, wherein a grain size in the first copper layer differs from that of a second copper layer. Furthermore, it is preferably provided that the at least one metal layer is surface-modified. A possible surface modification could be, for example, sealing with a precious metal, in particular silver and / or gold, or ENIG ("electroless nickel immersion gold"), or edge encapsulation on the first or second metallization layer to suppress crack formation or crack widening.

[0018] Preferably, the at least one ceramic layer comprises Al2O3, Si3N4, AlN, an HPSX ceramic (i.e., a ceramic with an Al2O3 matrix containing an x-percent ZrO2 content, for example Al2O3 with 9% ZrO2 = HPS9 or Al2O3 with 25% ZrO2 = HPS25), SiC, BeO, MgO, high-density MgO (> 90% of the theoretical density), TSZ (tetragonally stabilized zirconium oxide), or ZTA as the ceramic material. It is also conceivable for the insulation layer to be designed as a composite or hybrid ceramic, in which, in order to combine various desired properties, several ceramic layers, each differing in terms of their material composition, are arranged one above the other and combined to form an insulation layer. Preferably, a highly thermally conductive ceramic is used to achieve the lowest possible thermal resistance.

[0019] According to the invention, the at least one active metal layer is applied by means of a vapor deposition process, in particular a physical vapor deposition process (PVD), or by means of chemical vapor deposition (CVD). This manufacturing process makes it possible to provide comparatively thin active metal layers, which are applied as homogeneously as possible. In particular, the most controlled application possible is such that the applied at least one active metal layer has a thickness as constant as possible across the application area. For example, vapor deposition processes that can be used include evaporation processes such as thermal evaporation, electron beam evaporation, laser beam evaporation, arc evaporation, or molecular beam epitaxy; sputtering, such as ion beam-assisted deposition; ion plating, and / or an ICB technique.

[0020] Advantageously, a first thickness of the at least one active metal layer has a value between 100 nm and 1000 nm, preferably between 150 nm and 750 nm, and particularly preferably between 200 nm and 500 nm. Such thin active metal layers advantageously prevent a reduction in the thermal conductivity and a reduction in the mechanical strength of the metal-ceramic substrate, in particular at the interface between the at least one ceramic layer and the at least one metal layer. The layer thickness is particularly preferably coordinated with the expected storage time. For example, for long storage times, for example of more than 10 days, in particular for titanium as the active metal layer, it has proven advantageous to use a layer thickness between 750 and 1000 nm. For shorter storage times, it is possible to use a first thickness of 150 nm to 350 nm.

[0021] Preferably, the active soldering process is carried out at a pressure of less than 10 -2 mbar, preferably less than 10 -3 and particularly preferably less than 10 -4 and / or using process gas. For example, the active soldering process is carried out in a high vacuum or a fine vacuum with very low oxygen and argon partial pressures of less than 1 mbar. Alternatively, it is also conceivable to work at atmospheric pressure under argon or a generally noble gas. Since no organic binders are used here, it is possible to reduce the process time by up to half.

[0022] Furthermore, it is preferably provided that a second thickness of the at least one solder layer has a value between 1 and 100 µm, preferably between 1.5 and 50 µm and particularly preferably between 2 and 20 µm or even less than 10 µm. In particular, this is the second thickness before the bonding process, i.e. the active soldering process. It is particularly preferably provided that the at least one solder layer is further reduced before the bonding process, for example by rolling to a thickness of less than 10 µm, preferably to a thickness of less than 7 µm and particularly preferably to a thickness of less than 5 µm. This advantageously makes it possible to further reduce a layer thickness of the solder material or of the at least one solder layer.Furthermore, it is preferably provided that the at least one solder layer is reduced in thickness by roll bonding prior to being arranged between the at least one ceramic layer and the at least one metal layer. This allows a thinner at least one solder layer to be realized in advance, before it is reduced in a further solder layer step to the final layer thickness intended for the bonding process—for example, by rolling.

[0023] Furthermore, it is preferably provided that the at least one active metal layer is covered by at least one protective layer. By means of this at least one protective layer, it is advantageously possible to prevent oxidation of the at least one active metal layer. For example, copper (Cu), nickel (Ni), indium (In), silver (Ag), chromium (Cr) or titanium nitride (TiN) can be used as a protective layer for the at least one active metal layer. The thickness of the at least one protective layer has a value of at least 100 nm. It is particularly preferably provided that the thickness of the at least one protective layer, i.e. the third thickness, is adapted to the storage time, i.e. the time that elapses between the application of the at least one active metal layer and the actual bonding process as part of the active soldering process.This advantageously ensures the long-term storage of components covered with at least one active metal layer (be it the at least one metal layer and / or the at least one active metal layer and / or the at least one solder layer) without the at least one active metal layer oxidizing prior to the bonding process. For example, the layer thickness of the at least one protective layer, i.e., a third thickness, is between 100 nm and 1000 nm, preferably between 150 nm and 750 nm, and particularly preferably between 250 nm and 500 nm.

[0024] Furthermore, it is preferably provided that a ratio of the third thickness of the at least one protective layer to the first thickness of the at least one active metal layer, measured in the stacking direction, assumes a value between 0.5 and 1, preferably between 0.7 and 0.9 and particularly preferably between 0.75 and 0.85.

[0025] Furthermore, it is preferably provided that the at least one active metal layer changes its composition in the stacking direction. This also advantageously prevents premature oxidation of the active metal layer, in particular by increasing the proportion of deposit elements, such as nitrogen, oxygen, or carbon, with increasing distance from the surface to which the active metal has been applied (be it the at least one metal layer, the at least one ceramic layer, or the at least one solder layer).

[0026] Furthermore, it is conceivable that in order to extend the storage times of the component provided with the at least one active metal layer or of the part provided with the at least one active metal layer, be it the at least one metal layer, the at least one ceramic layer and / or the at least one solder layer, the at least one active metal layer is covered with at least one further solder layer. The thickness of the at least one further solder layer is at least a factor of 0.1, preferably 0.05 and particularly preferably 0.01 thinner than the second thickness of the at least one solder layer. The soldering system advantageously forms a sandwich structure in which the at least one active metal layer is encased or surrounded by the at least one solder layer and the at least one further solder layer.

[0027] It is preferably provided that the at least one solder layer and / or the at least one active metal layer is rolled, preferably in such a way that a first thickness of the active metal layer after rolling and / or pressing has a value of less than 1000 nm, preferably less than 750 nm and particularly preferably less than 500 nm. This advantageously makes it possible, as an alternative to application by means of a galvanic process or a gas phase deposition process, to realize a first thickness of the active metal layer which is in particular less than 1000 nm if the solder layer and the active metal layer are rolled together. The layer thicknesses of the solder layer and the active metal layer, ie the first thickness and the second thickness, are rolled and / or pressed down together.For this purpose, a solder layer, for example in the form of a thick solder foil, and an active metal layer are first joined together, for example by means of upstream rolling or a first rolling to reduce the layer thickness. It is preferably provided that a starting layer thickness of the active metal layer and a starting layer thickness of the solder foil have the same ratio to one another as the first thickness and the second thickness in the manufactured solder system, which comprises the active metal layer with the first thickness and the solder layer with the second thickness. Through the subsequent rolling, in particular multiple rolling, the active metal layer and the solder layer are rolled down to their respective thicknesses with each rolling step in order to obtain a comparatively thin solder layer on which an even thinner active metal layer is arranged.This soldering system can then be used to bond the metal layer to the ceramic layer using an active soldering process.

[0028] The present invention further provides a soldering system for a method according to the invention, wherein the soldering system comprises at least one solder layer, in particular in the form of a solder foil, and at least one active metal layer. All advantages and features described for the method for producing the metal-ceramic substrate apply analogously to the soldering system.

[0029] Another object is a metal-ceramic substrate produced by a method comprising: - Providing at least one ceramic layer, at least one metal layer and at least one solder layer, in particular in the form of at least one solder foil, - coating the at least one ceramic layer and / or the at least one metal layer and / or the at least one solder layer with at least one active metal layer, - Arranging the at least one solder layer between the at least one ceramic layer and the at least one metal layer along a stacking direction to form a solder system comprising the at least one solder layer and the at least one active metal layer, wherein a solder material of the at least one solder layer is preferably free of a melting point-lowering material, and - Bonding the at least one metal layer to the at least one ceramic layer via the soldering system using an active soldering process. All advantages and features described for the process for producing the metal-ceramic substrate apply analogously to the metal-ceramic substrate.

[0030] Further advantages and features will become apparent from the following description of preferred embodiments of the subject matter according to the invention with reference to the accompanying figures. Individual features of the individual embodiments can be combined with one another within the scope of the invention.

[0031] It shows: Fig. 1: schematically shows a method for producing a metal-ceramic substrate according to a first preferred embodiment of the present invention, Fig. 2: schematically shows a method for producing a metal-ceramic substrate according to a second preferred embodiment of the present invention, Fig. 3: schematically shows a method for producing a metal-ceramic substrate according to a third preferred embodiment of the present invention, Fig. 4: schematically shows a method for producing a metal-ceramic substrate according to a fourth preferred embodiment of the present invention and Fig. 5: schematically shows a method for producing a metal-ceramic substrate according to a fifth preferred embodiment of the present invention.

[0032] In the Fig. Figure 1 schematically illustrates a method for producing a metal-ceramic substrate 1 according to a first preferred embodiment of the present invention. Such a metal-ceramic substrate 1 preferably serves as a carrier for electronic or electrical components that can be bonded to the metal-ceramic substrate 1. An example of a manufactured metal-ceramic substrate 1 is schematically illustrated in the upper left corner. Essential components of such a metal-ceramic substrate 1 are at least one ceramic layer 10 extending along a main extension plane HSE and at least one metal layer 20 bonded to the at least one ceramic layer 10. The at least one ceramic layer 10 is made of at least one material comprising a ceramic.The at least one metal layer 20 and the at least one ceramic layer 10 are arranged one above the other along a stacking direction S running perpendicular to the main extension plane HSE and, in a manufactured state, are bonded to one another at least in regions via a soldering system 35. Preferably, the at least one metal layer 20 is then structured in the manufactured metal-ceramic substrate 1 to form conductor tracks or connection points for the electrical components. For example, this structuring is etched into the at least one metal layer 20. However, a permanent bond, in particular a bonded connection, must be formed beforehand between the at least one metal layer 20 and the at least one ceramic layer 10.

[0033] This permanent, particularly material-locking connection is used in the embodiment of the Fig. 1 is realized by means of an active soldering process. For this purpose, a soldering system 35 is arranged between the at least one ceramic layer 10 and the at least one metal layer 20, via which soldering system 35 the material-to-material connection between the ceramic layer 10 and the metal layer 20 is ensured in the finished metal-ceramic substrate 1. In particular, it is provided that the soldering system 35 is designed in multiple layers. In addition to at least one solder layer 30, the solder system 35 comprises at least one active metal layer 40. In particular, it is provided that the at least one solder layer 30 is free of an active metal, i.e. does not have any active metal. Instead, the active metal is provided with a separate layer in the soldering system 35 as an active metal layer 40.It has been advantageously found that this separation in the soldering system 35, in which an active metal-free solder material is provided in the solder layer 30 on one side and an active metal-comprising active metal layer 40 is provided on the other side, advantageously makes it possible to achieve the thinnest possible solder layer 30. Otherwise, a greater minimum layer thickness would have to be accepted for the at least one solder layer 30, in particular in the form of a solder foil, which is limited by the manufacturing process of the at least one solder layer 30 and not by the minimum thickness required for the joining process.

[0034] By separating the at least one active metal layer 40 and the at least one solder layer 30, correspondingly thinner solder foils can be produced because no brittle intermetallic phases hinder the forming process. In particular, this advantageously makes it possible to provide solder layers 30 that ensure that the at least one solder layer 30, in particular in the form of the solder foil, can be rolled to a thickness of less than 10 µm, preferably less than 8 µm, and particularly preferably less than 6 µm. In the illustrated embodiment, the at least one active metal layer 40 is applied to the at least one ceramic layer 10, for example by sputtering or CVD, and has a first thickness D1 that has a value between 100 nm and 1000 nm, preferably between 150 nm and 750 nm, and particularly preferably between 200 nm and 500 nm.

[0035] Such thin active metal layers 40 prevent a reduction in thermal conductivity and mechanical strength that would otherwise be expected with thicker active metal layers 40. This applies particularly to a layer thickness or first thickness D1 between 200 nm and 500 nm. It is provided that the at least one solder layer 30, in particular as at least one solder foil, is arranged as a separate layer between the at least one active metal layer 40 and the at least one metal layer 20 before the active soldering process is carried out. For example, it is conceivable that the at least one solder foil is applied to the at least one active metal layer 40 and plated by a rolling step to a second thickness of less than 10 µm, preferably less than 7 µm, in order to ensure the thinnest possible at least one solder layer 30.The use of a comparatively thin at least one solder layer 30 accelerates the bonding process and also advantageously reduces the material requirements when producing the connection between the at least one ceramic layer 10 and the at least one metal layer 20. The at least one ceramic layer 10 and the at least one metal layer 20 are arranged one above the other in the stacking direction S, wherein the soldering system 35 with the at least one solder layer 30 and the at least one active metal layer 40 is arranged in the stacking direction S between the at least one metal layer 20 and the at least one ceramic layer 10. In particular, it is provided that the at least one solder layer 30 is not only free of active metal, but also free of melting point-lowering elements, such as phosphorus or zinc.By essentially "free of melting point-lowering elements," a person skilled in the art understands in particular that their proportion in the solder layer is less than 3% by weight, preferably less than 2% by weight, and particularly preferably less than 1% by weight. For example, the at least one solder layer 30 dispenses with the use of a solder material containing phosphorus or zinc in order to prevent the melting temperature from being lowered. It has surprisingly been found that bonding via the separate at least one active metal layer 40 is also possible for solder materials that do not contain any melting point-lowering elements. This allows the use of comparatively thin at least one solder layer 30 for solder materials that are used at the usual process temperatures of an active soldering process.Accordingly, the usual process parameters that are typically used in the active soldering process can be used, and a comparatively very thin at least one solder layer 30 can be realized.

[0036] In Fig. 2 schematically shows a method for producing a metal-ceramic substrate 1 according to a second exemplary embodiment of the present invention. In particular, the embodiment of Fig. 2 essentially only from the embodiment of the Fig. 1 in that in addition to the at least one active metal layer 40, at least one protective layer 41 is provided. The at least one protective layer 41 extending in the main extension plane HSE covers in particular the active metal layer 40. By using such at least one protective layer 41, it is advantageously possible to prevent oxidation from taking place on the at least one active metal layer 40 or on the outside of the at least one active metal layer 40 before the actual bonding process, i.e. the active soldering process, takes place. Preferably, such at least one protective layer 41 has a third thickness D3 which has a minimum thickness of at least 100 nm. Preferably, the third thickness D3 of at least one of the protective layers is 100 nm to 1000 nm, preferably 150 nm to 750 nm and particularly preferably between 200 nm and 500 nm.Furthermore, it is preferably provided that the at least one protective layer 41 partially or preferably completely covers the at least one active element layer 40 and is arranged between the at least one active metal layer 40 and the at least one solder layer 30, as seen in the stacking direction S. The third thickness D3 is preferably adapted to the expected duration from the deposition of the active metal layer (40) and the protective layer (41) until the bonding takes place by means of the active soldering process. As a result, the intended storage time can be advantageously adjusted, in particular by means of the third thickness D3 of the protective layer 41, in order to ensure that the at least one active metal layer 40 does not undergo oxidation before bonding. It is preferably provided that the third thickness D3 of the at least one protective layer 41 substantially corresponds to the first thickness D1 of the active metal layer 40.

[0037] Furthermore, it is provided that the at least one solder layer 30 has a second thickness D2, which has a value between 0.1 and 100 µm, preferably between 0.5 and 50 µm and particularly preferably 0.2 and 20 µm. This is in particular the second thickness D2 before the at least one solder layer 30 is applied or arranged on the at least one metal layer 20 or on the at least one active metal layer 40. In this case, it is provided in particular that after the at least one metal layer 20 has been applied or laid down, the second thickness D2 of the at least one solder layer 30 is further reduced by further rolling. After the at least one metal layer 20, the at least one ceramic layer 10 and the soldering system 35 arranged between the at least one metal layer 20 and the at least one ceramic layer 10 have been arranged, a bonding takes place using a temperature between 700 °C and 900 °C.Preferably, the soldering process is carried out at a pressure of less than 10 mbar. It is also conceivable for the bonding process, i.e., the active soldering process, to be carried out using a process gas, or in a working atmosphere that includes, for example, argon or generally one or more noble gases.

[0038] In Fig. Figure 3 schematically illustrates a method for producing a metal-ceramic substrate 1 according to a third exemplary embodiment of the present invention. This embodiment differs substantially from that of Fig. 2 in that the at least one active metal layer 40 is applied to the at least one solder layer 30 before being arranged between the at least one metal layer 20 and the at least one ceramic layer 10. In other words: Here, the bonding of the at least one active metal layer 40 to the at least one solder layer 30 takes place by means of sputtering before the arrangement between the at least one ceramic layer 10 and the at least one metal layer 20. In particular, it is provided that here too at least one protective layer 41 covers the at least one active metal layer 40 partially or preferably completely, in particular on one side, in order to prevent premature oxidation of the at least one active metal layer 40.

[0039] In Fig. 4 schematically shows a method for producing a metal-ceramic substrate 1 according to a fourth embodiment of the present invention. In contrast to the embodiments from the Fig. 2 and Fig. 3 it is in the embodiment of the Fig. 4, it is provided that the at least one active metal layer 40 is bonded to the at least one metal layer 20 prior to the active soldering process. In this case, the at least one active metal layer 40 is arranged in particular on the side of the at least one metal layer 20 facing the solder layer 30 during the bonding process. For example, the at least one active metal layer 40 can be applied over the entire surface of the at least one metal layer 20 by means of a CVD process or by sputtering, i.e. generally by means of a gas phase deposition process. After the arrangement of the at least one metal layer 20, to which the at least one active metal layer 40 adheres, and the at least one ceramic layer 10, as well as the at least one solder layer 30, the bonding process is carried out by means of the active soldering process.

[0040] In Fig. Figure 5 schematically shows a method for producing a metal-ceramic substrate 1 according to a fifth preferred embodiment of the present invention. The embodiment of the Fig. 5 from the one from the Fig. 2 only in that both the front side and the back side of the at least one ceramic layer 10 are each connected to at least one metal layer 20 via respective soldering systems 35, wherein the soldering system 35 preferably comprises the at least one solder layer 30, the at least one active metal layer 40 and the at least one protective layer 41. List of reference symbols: 1 metal-ceramic substrate 10 ceramic layer 20 metal layer 30 solder layer 35 soldering system 40 active metal layer 41 Protective layer S Stacking direction HSE main extension level D1 first thickness D2 second thickness D3 third thickness

Claims

[1] A method for producing a metal-ceramic substrate (1), comprising: - Providing at least one ceramic layer (10), at least one metal layer (20) and at least one solder layer (30), in particular in the form of at least one solder foil, - coating the at least one ceramic layer (10) and / or the at least one metal layer (20) and / or the at least one solder layer (30) with at least one active metal layer (40), - arranging the at least one solder layer (30) between the at least one ceramic layer (10) and the at least one metal layer (20) along a stacking direction (S) to form a solder system (35) comprising the at least one solder layer and the at least one active metal layer (40), and - Bonding the at least one metal layer (20) to the at least one ceramic layer (10) via the soldering system (35) by means of an active soldering process, wherein AgCu28, AgCuln, AgCuSn, AgCuGa, CuSn, Culn, CuGa, CuInSn, CuInMb, CuGaSn or NiCrMn is used as the soldering layer material, wherein the at least one active metal layer is applied by means of a gas phase deposition process. [2] Method according to claim 1, wherein a solder material of the at least one solder layer (30) is free of a melting point lowering material and / or phosphorus-free. [3] Method according to one of the preceding claims, wherein a first thickness (D1) of the at least one active metal layer (40) has a value between 100 nm and 1000 nm, preferably between 150 nm and 750 nm and particularly preferably between 200 nm and 500 nm. [4] Method according to one of the preceding claims, wherein - the active soldering process at a pressure of less than 10-2 mbar, preferably less than 10 -3 and particularly preferably less than 10 -4 and / or - using a process gas is carried out. [5] Method according to one of the preceding claims, wherein a second thickness (D2) of the at least one solder layer (30) has a value between 1 µm and 100 µm, preferably between 1.5 µm and 50 µm and particularly preferably between 2 µm and 20 µm. [6] Method according to one of the preceding claims, wherein the at least one active metal layer (40) is covered by at least one protective layer (41). [7] Method according to one of the preceding claims, wherein the at least one active metal layer (40) changes its composition in the stacking direction (S). [8] Method according to one of the preceding claims, wherein the at least one solder layer (30) and / or the at least one active metal layer (40), in particular as a solder system (35), is rolled, preferably such that a first thickness (D1) of the active metal layer (40) after rolling has a value of less than 1000 nm, preferably less than 750 nm and particularly preferably less than 500 nm. [9] Soldering system (35) for a method according to one of the preceding claims, wherein the soldering system (35) comprises at least one soldering layer (30), in particular in the form of at least one soldering foil, and at least one active metal layer (40). [10] Metal-ceramic substrate (1) produced by a method comprising - Providing at least one ceramic layer (10), at least one metal layer (20) and at least one solder layer (30), in particular in the form of at least one solder foil, - coating the at least one ceramic layer (10), the at least one metal layer (20) and / or the at least one solder layer (30) with at least one active metal layer (40), - arranging the at least one solder layer (30) between the at least one ceramic layer (10) and the at least one metal layer (20) along a stacking direction (S) to form a solder system (35) comprising the at least one solder layer and the at least one active metal layer (40), and - bonding the at least one metal layer (20) to the at least one ceramic layer (10) via the soldering system (35) by means of an active soldering process, wherein AgCu28, AgCuln, AgCuSn, AgCuGa, CuSn, Culn, CuGa, CuInSn, CuInMb, CuGaSn or NiCrMn is used as the soldering layer material, wherein the at least one active metal layer is applied by means of a vapor deposition process.

Citation Information

Patent Citations

  • Electronic device

    DE102009033029A1

  • Metal-ceramic substrates and methods for producing a metal-ceramic substrate

    DE102013104739A1

  • Method for producing a composite material

    DE102015108668A1

  • Ceramic-metal substrate as multiple substrate

    DE19927046B4

  • Method for preparing highly heat-conductive substrate and copper wiring sheet usable in the same

    EP0153618A2