Resin composition and semiconductor device
A polyamideimide resin with specific structural units addresses the challenge of insulating and flexible film formation in power semiconductor devices, enhancing reliability by achieving high dielectric breakdown voltage and elastic modulus.
Patent Information
- Application Number
- DE102019219591
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-12-17
- Filing Date
- 2019-12-13
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2039-12-13
AI Technical Summary
Conventional resins used in power semiconductor devices face challenges in achieving satisfactory insulating properties and flexibility, particularly in forming insulating films with sufficient thickness, leading to potential leakage currents and operational defects.
A resin composition comprising a polyamideimide resin with specific structural units, having a weight average molecular weight of at least 100,000, which includes structural units (1A) and/or (1B) and (2A) and/or (2B), providing excellent insulating properties, flexibility, and thick film forming ability.
The resin composition achieves a dielectric breakdown voltage of at least 150 kV/mm, an elastic modulus of 0.5 to 3.0 GPa, and a glass transition temperature of 200°C, ensuring reliable insulation and flexibility in semiconductor devices.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
TECHNICAL FIELD
[0001] This invention relates to a resin composition exhibiting excellent insulation properties, flexibility, and the ability to form a thick film. Another aspect of this invention relates to a semiconductor device with excellent reliability using the resin composition. BACKGROUND
[0002] Polyimide resin, polyamide resin, and polyamideimide resin are known as typical heat-resistant resins and are used in a wide variety of applications. In addition to heat resistance, polyimide resin, polyamide resin, and polyamideimide resin also exhibit excellent chemical resistance and mechanical properties. Consequently, these resins are widely used in the field of electronic devices, for example, as materials for surface protective films or interlayer insulating films, or the like in semiconductor devices.
[0003] In recent years, along with the advancement of miniaturization of power semiconductor devices, the electric current has also increased. As the current increases, leakage current may sometimes occur from circuits or elements, and it is known that this type of leakage current can cause defects in power semiconductor devices. Therefore, improvements in the insulation properties of power semiconductor devices are highly desirable in terms of semiconductor device reliability.
[0004] In order to improve the insulation properties of power semiconductor devices, studies are being conducted on methods in which a partial insulation film is formed using a polyimide resin, a polyamide resin, or a polyamideimide resin or the like to ensure satisfactory insulation properties in certain required areas, thereby preventing the occurrence of leakage current between various parts during operation of the semiconductor device.
[0005] In the above methods, the formation of the insulation film is typically performed by applying a solvent solution (varnish) of the above resin to the power module prior to encapsulation and then drying the resulting coating film. Examples of the method used to apply the resin solvent solution include typical methods such as dispensing, dipping, potting, spray coating, and spin coating.
[0006] Patent Document 2 describes a resin composition comprising a heat-resistant resin soluble in a solvent at room temperature, a heat-resistant resin insoluble in a solvent at room temperature but soluble upon heating, and a solvent. In Example 2 of Patent Document 2, the heat-resistant resin soluble in a solvent at room temperature is a polyetheramideimide prepared from bis[4-(4-aminophenoxy)phenyl]sulfone (BAPS), 1,3-bis(aminopropyl)tetramethyldisiloxane, and trimellitic anhydride chloride, and the thermosetting resin insoluble in a solvent at room temperature but soluble upon heating is a polyetheramideimide prepared from 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), isophthalic acid dichloride, and 3,4,3',4'-benzophenonetetracarboxylic dianhydride.In addition, Patent Document 2 describes a film of the resin composition on a semiconductor substrate described in.
[0007] Patent Document 3 relates to a polyamideimide, a thermosetting resin composition, and a method for producing a polyamideimide. The polyamideimide is obtained by reacting a diimide dicarboxylic acid obtained by reacting a diamine mixture containing p-phenylenediamine and m-phenylenediamine with trimellitic anhydride with an aromatic diisocyanate.
[0008] Patent Document 4 describes a polyimide precursor containing a crosslinking group, a polyimide containing a crosslinking group, and a heat-resistant adhesive. The polyimide precursor has crosslinking groups at 5 to 99 mol% of the molecular ends of repeating units represented by the following formula.
[0009] In the formula, K is a direct bond or a divalent linking group selected from CO, SO2, S, O, CH2, C(CH3)2, and C(CF3)2. Ar1 is a tetravalent group of the following formula (V), and X is a divalent group of the following formula (VI).
[0010] Patent Document 5 describes a polyimide resin and a resin-based adhesive suitable for bonding and fixing a semiconductor device to a lead frame or package. The polyimide resin has repeating units of the following formulas.
[0011] In the formulas, Ar1 and Ar3 are each a tetravalent organic group, Ar2 is a divalent organic group and 0.5 ≤ a / (a+b) ≤ 1.
[0012] Patent Document 6 describes a resin composition comprising a siloxane-modified polyamide, a (methyl)allyl group-containing compound, a compound having maleimide groups, and a diamine compound or a polysiloxane compound having amino groups at both molecular terminals.
[0013] Patent Document 7 describes a polyimide resin comprising a structural unit represented by the following general formula:
[0014] In the above formula, A represents one of the following formulas and X represents a direct bond, -O-, -SO2- or -C(CF3)2-.
[0015] In the above formulas, A1 represents a direct bond, -O-, -S-, -SO2-, -CO-, -C(CH3)2- or -C(CF3)2-, R1 and R2 represent H, Cl, Br, CH3 or CF3, R3, R4 and R5 independently represent H, Cl, Br, CN, CH3 or CF3, A2 represents a direct bond, -O-, -S-, -SO2-, -CO-, -C(CH3)2- or -C(CF3)2 and R6 and R7 represent H or CF3.
[0016] Patent Document 8 describes a thermosetting resin composition comprising a polycarbodiimide soluble in organic solvents and a polyimide soluble in organic solvents. The polycarbodiimide is represented by the following formula:
[0017] In the above formula, X is a hydrogen atom or a fluorine atom and 1 is an integer from 2 to 400. The polyimide may have a repeating unit represented by the following formulas:
[0018] In the above formulas, R Si a silicondiamine residue, R 10 is a diamine residue, R 20 is an acid dianhydride residue and (m+n) is an integer from 6 to 200.
[0019] Patent Document 9 describes a curable polyimide having a structure according to one of the following formulas:
[0020] In the formulas, R is independently a substituted or unsubstituted aliphatic radical, cycloaliphatic radical, alkenyl radical, polyether radical, polyester radical, polyamide radical, aromatic radical, heteroaromatic radical or siloxane radical, R' is independently a diamine containing an alcohol radical, each Q is independently a substituted or unsubstituted aliphatic, cycloaliphatic, alkenyl radical, polyether radical, polyester radical, polyamide radical, aromatic radical, heteroaromatic radical or siloxane radical, R'' is H or methyl, z is independently a substituted or unsubstituted alkyl group or aromatic group and n and m are integers having a value of 10 to about 100, with the proviso that the average molecular weight of the curable polyimide is greater than 20,000 Daltons.
[0021] Patent Document 10 describes a halogen-free flame retardant composition comprising a combination of a linear high-molecular-weight polyester and a halogen-free flame retardant. The flame retardant can be either a polyetherimide-organopolysiloxane copolymer or a mixture of the latter with a polyphenylene sulfite and / or a polyetherimide.
[0022] Patent Document 11 describes a polyimide resin containing at least one repeating unit selected from the group consisting of a repeating unit represented by the following formula (1) and a repeating unit represented by the following formula (2), and a polyimide resin containing at least one repeating unit selected from the group consisting of a repeating unit represented by the following formula (1) and a repeating unit represented by the following formula (2), and at least one repeating unit represented by the following formula (3):
[0023] In formula (3), X represents a divalent aliphatic group having 2 to 39 carbon atoms, a divalent alicyclic group having 3 to 39 carbon atoms, a divalent aromatic group having 6 to 39 carbon atoms, or a divalent group composed of a combination thereof. At least one kind of a bonding group selected from the group consisting of -O-, -SO2-, -CH2-, -C(CH3)2-, -OSi(CH3)2-, -C2H2O-, and -S- may be inserted into a main chain of X, and X may have at least one kind of a functional group selected from the group consisting of a carboxyl group, a hydroxyl group, and a carbonyl group. PRIOR ART PATENTS DOCUMENTS Patent Document 1: JP H02-173073 Patent document 2: US 2006 / 0 180 908 A1 Patent Document 3: JP 4 277 513 B2 Patent document 4: JP 2001- 323 065 A Patent document 5: JP H10-36 507 A Patent document 6: JP 2000-204 251 A Patent document 7: US 2003 / 0 064 235 A1 Patent document 8: US 6,068,932 A Patent document 9: WO 2018 / 237 377 A1 Patent document 10: EP 0 636 655 A2 Patent Document 11: CN 1 01 454 378 A SUMMARY OF THE INVENTION PROBLEMS TO BE SOLVED BY THE INVENTION
[0024] Due to the increasing electric current flowing through power semiconductor devices and the shift from Si to other substrate materials such as SiC, the current required for power semiconductor devices has increased in recent years. As a result, achieving satisfactory insulation properties and flexibility with conventional resins has become difficult, and improvements in these resins are desirable. In particular, to ensure satisfactory insulation properties, a resin capable of forming an insulation film of sufficient thickness in a desired location is desired.
[0025] If the thickness of a resin coating film forming an insulating film is insufficient, ensuring satisfactory insulation properties between various parts becomes difficult. As a result, for example, a leakage current may develop in a power semiconductor device, leading to operational defects. A well-known method used to ensure sufficient film thickness involves dispersing an inorganic filler in the resin paste (Patent Document 1). However, when this method is used, the insulation properties of the insulating film tend to deteriorate due to the current passing through the interface of the inorganic filler.Therefore, to achieve excellent insulation properties, it is necessary to maintain a balance between the insulation properties of the resin itself and the ability to form a thick film, which allows the desired film thickness to be easily achieved during coating film formation. In order to achieve excellent reliability for the semiconductor device, it is also necessary for the coating film obtained from the resin to have excellent flexibility.
[0026] In view of the above circumstances, this invention provides a resin composition exhibiting excellent insulation properties, flexibility, and thick film formability. Furthermore, this invention also provides a semiconductor device with excellent reliability produced using the resin composition. MEANS TO SOLVE THE PROBLEMS
[0027] The inventors of this invention conducted various studies on resin compositions containing a polyimide resin, polyamide resin, and polyamideimide resin as a resin, and found that a resin having specific structural units had excellent insulating properties and excellent flexibility and was capable of easily forming a coating film having a desired thickness, thereby completing this invention.
[0028] Embodiments of this invention relate to the following aspects. However, this invention is not limited to the preferred embodiments described below.
[0029] One embodiment of the present invention relates to a resin composition comprising a resin component (A) and an organic solvent (B), wherein the resin component (A) contains a polyamideimide resin containing a structural unit represented by the following formula (1A) and / or (1B) and a structural unit represented by the following formula (2A) and / or (2B) and having a weight-average molecular weight of at least 100,000:
[0030] In the formulas, each of R1 to R4 is independently a hydrogen atom or one or more substituents selected from the group consisting of alkyl groups having 1 to 9 carbon atoms, alkoxy groups having 1 to 9 carbon atoms and halogen atoms, and X is a divalent organic group shown below:
[0031] In the formula, each of R5 and R6 independently represents an alkyl group having 1 to 9 carbon atoms.
[0032] In the formulas, R7 to R 10each independently represents an alkyl group having 1 to 9 carbon atoms and n is an integer from 1 to 6.
[0033] In the above-described embodiment of the present invention, the polyamideimide resin is preferably a resin containing 3 to 7 mol% of the structural unit represented by the above formula (2A) and / or (2B) based on the total number of moles of the structural unit represented by the above formula (1A) and / or (1B) and the structural unit represented by the above formula (2A) and / or (2B).
[0034] In the above-described embodiment of the present invention, the dielectric breakdown voltage of a film obtained by drying the resin composition is preferably at least 150 kV / mm.
[0035] In the above-described embodiment of the invention, the glass transition temperature of the polyamideimide resin is preferably at least 200°C.
[0036] In the above-described embodiment of the present invention, the elastic modulus at 35°C of a film obtained by drying the resin composition is preferably 0.5 to 3.0 GPa.
[0037] Another aspect of the invention relates to a semiconductor device having a film formed using the resin composition of the above-described embodiment of the invention on a surface of a structural component. EFFECTS OF THE INVENTION
[0038] This invention is capable of providing a resin composition exhibiting excellent insulation properties, flexibility, and thick film formability. Furthermore, this invention can also provide a semiconductor device with excellent reliability produced using the resin composition. BRIEF DESCRIPTION OF THE DRAWINGS Fig.1 is a schematic cross-sectional view showing an example of a semiconductor device according to an embodiment. Fig. 2 is a schematic cross-sectional view showing an example of a semiconductor device according to an embodiment. EMBODIMENTS FOR CARRYING OUT THE INVENTION
[0039] Embodiments of this invention are described below in more detail, but this invention is not limited to the following preferred embodiments. 1. Resin composition
[0040] One aspect of the invention relates to a resin composition as defined in claim 1, comprising a resin component (A) and an organic solvent (B), wherein the resin component (A) contains a polyamideimide resin containing two specific types of structural units. Each of these components is described in more detail below. (A) Resin component
[0041] The resin component constituting the above resin composition contains a polyamideimide resin containing a structural unit represented by the formula (1A) and / or (1B) shown below and a structural unit represented by the formula (2A) and / or (2B) shown below and having a weight-average molecular weight of at least 100,000.
[0042] In the formula, R1 to R4 are each independently a hydrogen atom or one or more substituents selected from the group consisting of alkyl groups having 1 to 9 carbon atoms, alkoxy groups having 1 to 9 carbon atoms and halogen atoms.
[0043] In one embodiment, each of R1 to R4 is preferably a hydrogen atom. In another embodiment, each of R1 to R4 is preferably an alkyl group having 1 to 9 carbon atoms, an alkoxy group having 1 to 9 carbon atoms, or a halogen atom. The alkyl groups and alkoxy groups mentioned above may have a linear, branched, or cyclic structure. The alkyl groups and alkoxy groups more preferably have 1 to 6 carbon atoms, and even more preferably 1 to 3 carbon atoms.
[0044] The halogen atom can be one of a fluorine atom, chlorine atom and bromine atom.
[0045] X is an organic group shown below.
[0046] In the formulas, each of R5 and R6 is independently an alkyl group having 1 to 9 carbon atoms. In one embodiment, each of R5 and R6 in the above formula is preferably an alkyl group having 1 to 6 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms, and even more preferably an alkyl group having 1 or 2 carbon atoms.
[0047] In the formula, R7 to R 10 each independently represents an alkyl group having 1 to 9 carbon atoms. Furthermore, n is an integer from 1 to 6.
[0048] The alkyl groups may have a linear, branched, or cyclic structure. In one embodiment, each of R7 to R 10 preferably an alkyl group having 1 to 6 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms.
[0049] In the above resin composition, by using the resin component having a structural unit represented by the above formula (1A) and / or (1B) (hereinafter referred to as "structural unit (1A) and / or (1B)") and a structural unit represented by the above formula (2A) and / or (2B) (hereinafter referred to as "structural unit (2A) and / or (2B)"), excellent insulation properties and excellent flexibility can be obtained. When a polyamideimide resin is used, even more excellent heat resistance can be easily obtained. In the following description, the polyamideimide resin is sometimes simply referred to as "the resin."
[0050] The resin described above can be obtained, for example, via a reaction between trimellitic anhydride or an acid halide represented by the formula (III) shown below and two compounds having the formula (I-1) shown below and the formula (II-1) shown below. In each formula, R1 to R 10and n are each the same as described above with respect to formulas (1A), (1B), (2A) and (2B), and Y is an amino group or isocyanate group.
[0051] Further, n is preferably an integer from 2 to 4, and more preferably 3 or 4.
[0052] The polyamideimide resin is a resin having amide bonds and imide bonds within the molecular skeleton and can be obtained, for example, by forming a precursor (a polyamic acid) by reacting a diamine component with an acid component containing a tricarboxylic acid anhydride or acid halide thereof, and then subjecting the precursor to dehydration cyclization. Except for using at least the compounds represented by the above formulas (I-1) and (II-1) as the diamine component or diisocyanate component and trimellitic acid anhydride or an acid halide represented by the formula (III) shown below, the polyamideimide resin can be produced without any limitations.
[0053] Trimellitic anhydride is used in view of cost, reactivity and solubility and the like.
[0054] In the above formula, R is a hydroxyl group or a halogen atom. The halogen atom is preferably a chlorine atom or bromine atom, and is more preferably a chlorine atom.
[0055] In one embodiment, when a diamine is used, the use of an acid halide of trimellitic anhydride as the acid component is preferred, and the use of trimellitic anhydride chloride having the formula (III-1) shown below is particularly desirable.
[0056] In one embodiment, the polyamideimide resin may be a resin obtained by using a compound represented by the above formula (I-1) or formula (II-1) as the diamine component or diisocyanate component and using a compound represented by the above formula (III) as the acid component. In another embodiment, the polyamideimide resin may be a resin obtained by using not only the compounds represented by the above formulas (I-1), (II-1), and (III), but also one or more other diamine components or diisocyanate components and / or other acid components.
[0057] The polyamideimide resin may, for example, be a resin obtained by using compounds represented by the above formulas (I-1) and (II-2) as well as another aromatic diamine or aromatic diisocyanate, aliphatic diamine or aliphatic diisocyanate, or alicyclic diamine or alicyclic diisocyanate as needed.
[0058] Furthermore, a resin obtained by using another acid component in addition to the compound represented by formula (III) can also be used. Examples of the other acid components that can be used include tricarboxylic acid anhydrides or halides thereof other than the compounds represented by formula (III), and tricarboxylic acids such as trimellitic acid. Furthermore, the acid component can also include tetracarboxylic acid dianhydrides such as pyromellitic anhydride and biphenyltetracarboxylic acid dianhydride, aromatic dicarboxylic acids such as terephthalic acid and isophthalic acid, alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid, and aliphatic dicarboxylic acids such as adipic acid and sebacic acid, and the like.
[0059] In the polyamideimide resin, the proportion of the structural units (1A) and / or (1B) derived from the compounds represented by the formula (I-1) and compounds represented by the formula (III) and the structural units (2A) and / or (2B) derived from the compounds represented by the formula (II-1) and compounds represented by the formula (III) relative to the total of all the structural units derived from the diamine components and / or diisocyanate components is preferably within a range of 93 to 97 mol%, and more preferably 94 to 96 mol%. In one embodiment, in the resin, the proportion of structural units (1A) and / or (2A) derived from compounds of formula (I) and compounds of formula (III), and structural units (2A) and / or (2B) derived from compounds of formula (II-1) and compounds of formula (III), relative to the total of all structural units derived from diamine components and / or diisocyanate components, may be 100 mol%.The proportion (mol%) of a structural unit is calculated from the number of added monomers of the monomer compounds corresponding to each of the structural units.
[0060] In one embodiment, as typified by the polyamideimide resin, the proportion of the structural unit (2A) and / or (2B) relative to the total moles of the structural unit (1A) and / or (1B) and the structural unit (2A) and / or (2B) in the resin is preferably within a range of 3 to 7 mol%, and more preferably 4 to 6 mol%. By ensuring that the proportion of the structural unit (2A) and / or (2B) falls within the above range, the insulation properties and flexibility can be improved with a good balance.
[0061] The polyamideimide resin of the above-described embodiment preferably contains a structure (1A-1) and / or (1B-1) and a structure (2A-1) and / or (2B-1) as shown below.
[0062] The polyamideimide resin can be produced by conventional methods, and there are no particular restrictions. For example, the polyamideimide resin can be produced via a reaction between a diamine component and / or a diisocyanate component and an acid component. The diamine component, diisocyanate component, and acid component are as described above. The reaction can be carried out in a solvent-free state or in the presence of an organic solvent. The reaction temperature is preferably within a range of 25 to 250°C. The reaction time can be appropriately adjusted according to factors such as batch size and the reaction conditions used.
[0063] There are no specific restrictions on the organic solvent (reaction solvent) used during the production of the polyamideimide resin. Examples of the organic solvent that can be used include ether-based solvents such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, triethylene glycol dimethyl ether, triethylene glycol diethyl ether and ethylene glycol monoethyl ether acetate (ethylene glycol monoethyl ether acetate), sulfur-containing solvents such as dimethyl sulfoxide, diethyl sulfoxide, dimethyl sulfone and sulfolane, cyclic ester-based solvents (lactone-based) such as γ-butyrolactone, ketone-based solvents such as cyclohexanone and methyl ethyl ketone, nitrogen-containing solvents such as N-methyl-2-pyrrolidone, dimethylacetamide and 1,3-dimethyl-3,4,5,6-tetrahydro-2(1H)-pyrimidinone and aromatic hydrocarbon-based solvents such as toluene and xylene.One of these organic solvents can be used alone, or a combination of two or more solvents can be used. In one embodiment, an organic solvent capable of dissolving the produced resin is preferred, and the use of a polar solvent is preferred. Details regarding polar solvents are described below, but nitrogen-containing solvents are preferred.
[0064] In a solvent, the polyamideimide resin can be produced by a method in which a precursor for the polyamideimide resin is first produced by a reaction between an acid component and a diamine component, and then this precursor is subjected to a dehydration-cyclization reaction to obtain the polyamideimide resin. However, there are no particular restrictions on the precursor cyclization method, and methods known in the art can be used. For example, a thermal cyclization method in which dehydration-cyclization is achieved by conducting heating either under normal or reduced pressure, or a chemical cyclization method using a dehydrating agent such as acetic anhydride, either in the presence of a catalyst or without a catalyst, can be used.
[0065] In a thermal cycling process, the cycling is preferably carried out while removing water generated by the dehydration reaction from the system. During the dehydration reaction, the reaction liquid can be heated to a temperature within a range of 80 to 400°C, and preferably 100 to 250°C. Furthermore, the water can also be removed by azeotropic distillation using an organic solvent capable of forming an azeotrope with water, such as benzene, toluene, and xylene.
[0066] In a chemical cyclization process, the reaction is carried out in the presence of a chemical dehydrating agent at a temperature of 0 to 120°C, preferably 10 to 80°C. Examples of chemical dehydrating agents that can be advantageously used include acid anhydrides such as acetic anhydride, propionic anhydride, butyric anhydride, and benzoic anhydride, and carbodiimide compounds such as dicyclohexylcarbodiimide. During the reaction, a material that accelerates the cyclization reaction, such as pyridine, isoquinoline, trimethylamine, triethylamine, aminopyridine, or imidazole, is preferably used in combination with the chemical dehydrating agent.The chemical dehydrating agent is used in a ratio of 90 to 600 mol% relative to the total amount of the diamine component, and the cyclization reaction accelerator is used in a ratio of 40 to 300 mol% relative to the total amount of the diamine component. A dehydration catalyst, including phosphorus compounds such as triphenyl phosphite, tricyclohexyl phosphite, triphenyl phosphate, phosphoric acid, and phosphorus pentoxide, and boron compounds such as boric acid and boric anhydride, can also be used.
[0067] In the production of the polyamideimide resin, the usage ratio (molar ratio) between the acid component and the diamine component (diisocyanate component) is not particularly limited and can be adjusted to ensure that the reaction proceeds without excess or deficiency. In one embodiment, in view of the molecular weight and crosslinking degree of the produced polyamideimide resin, the total amount of the diamine component per 1.00 mol of the total acid component is preferably within a range of 0.80 to 1.10 mol, more preferably 0.95 to 1.08 mol, and even more preferably 0.95 to 1.03 mol.
[0068] As indicated by the polyamideimide resin described above, the weight-average molecular weight (Mw) of the resin constituting the above-mentioned resin composition is preferably at least 100,000. Although this is not particularly limited, on the other hand, in view of solubility, Mw is preferably not more than 160,000. In one embodiment, the Mw of the above resin is preferably within a range of 110,000 to 160,000. When the Mw of the resin falls within this range, a coating film of the most appropriate thickness can be easily formed during the coating process. The Mw of the resin is more preferably within a range of 120,000 to 160,000, and even more preferably within a range of 130,000 to 150,000. In this description, “Mw” values mean values measured relative to standard polystyrene using gel permeation chromatography.
[0069] In one embodiment, a film can be obtained by drying the resin composition described above. The film formation may also include a step of applying the above resin composition before drying the resin composition. The term "drying" herein means volatilizing the organic solvent contained in the resin composition, for example, by natural drying or drying with heat. The formation of a film by drying can be carried out, for example, according to the method described in the examples below. With a view to achieving more satisfactory drying, the drying step may be performed multiple times (two or more times).
[0070] In one embodiment, the thick film formability of the coating film obtained using the above resin composition can be evaluated based on the aspect ratio (= coating film thickness / coating film width) of the dried coating film obtained after dispensing. From the viewpoint of achieving a film thickness capable of easily providing satisfactory insulation properties, the above aspect ratio is preferably at least 0.05, more preferably at least 0.06, and even more preferably 0.07 or more. The measurement of the aspect ratio can be performed using a Dektak 6M Surface Profiler manufactured by ULVAC, Inc.
[0071] In one embodiment, as exemplified by the polyamideimide resin described above, the resin used to form the resin composition preferably has a glass transition temperature (Tg) of 180°C or more. In this specification, the "glass transition temperature (Tg)" is a value obtained by conducting a dynamic viscoelasticity test using a film obtained by coating and then drying a resin dissolved in a solvent. The above resin more preferably has a Tg of 200°C or more. By ensuring that the resin has a Tg of 200°C or more, excellent reliability can be achieved even in heat cycle tests, which are typically conducted at high temperatures of 200°C or more.When a power semiconductor device is produced using the resin, any softening of the resin and deterioration of adhesion due to heat generation during operation of the device can be suppressed.
[0072] In the resin composition described above, from the viewpoint of processability and the like during film formation, the above resin is preferably soluble in the organic solvent at room temperature. In this specification, the term "soluble in the organic solvent at room temperature" means that when a solution obtained by adding the organic solvent to the resin at room temperature and stirring is visually inspected, there is no sediment and no turbidity, so that the entire solution exists in a transparent state. "Room temperature" can be a temperature within a range of about 10 to 40°C, and is preferably a temperature within 20 to 30°C. In one embodiment, the above "solution" means a solution obtained by adding 1 to 30 mg of a powder of the above resin to 100 ml of the organic solvent. The organic solvent is described below. (B) Organic solvent
[0073] The resin composition described above contains the resin component described above and an organic solvent. In this description, the resin composition is sometimes referred to as a varnish.
[0074] The organic solvent is not particularly limited, provided it is a solvent capable of dissolving the resin component, such as the polyamideimide resin. In one embodiment, the organic solvent may be a solvent composed of polar molecules (sometimes referred to as a "polar solvent"). In one embodiment, the organic solvent constituting the resin composition may be the same solvent as the reaction solvent used in the resin formation.
[0075] Examples of organic solvent include: Nitrogen-containing solvents such as N-methylpyrrolidone, dimethylacetamide, dimethylformamide and 1,3-dimethyltetrahydro-2(1H)-pyrimidone, Sulphur-containing solvents such as sulfolane and dimethyl sulfoxide, Lactones such as γ-butyrolactone, γ-valerolactone, γ-caprolactone, γ-heptalactone, α-acetyl-γ-butyrolactone and ε-cyprolactone, Ketones such as methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone and acetophenone, polyhydric alcohols such as ethylene glycol and glycerin, Ethers containing: Diethylene glycol dialkyl ethers such as diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether and diethylene glycol dibutyl ether, Triethylene glycol dialkyl ethers such as triethylene glycol dimethyl ether, triethylene glycol diethyl ether, triethylene glycol dipropyl ether and triethylene glycol dibutyl ether, Tetraethylene glycol dialkyl ethers such as tetraethylene glycol dimethyl ether, tetraethylene glycol diethyl ether, tetraethylene glycol dipropyl ether and tetraethylene glycol dibutyl ether, Diethylene glycol monoalkyl ethers such as diethylene glycol monomethyl ether and diethylene glycol monoethyl ether, Triethylene glycol monoalkyl ethers such as triethylene glycol monomethyl ether and triethylene glycol monoethyl ether, Tetraethylene glycol monoalkyl ethers such as tetraethylene glycol monomethyl ether and tetraethylene glycol monoethyl ether and Ethylene glycol monoalkyl ether acetates such as ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate and ethylene glycol monobutyl ether acetate (butyl cellosolve acetate).
[0076] One of these organic solvents may be used alone, or a combination of two or more organic solvents may be used. In one embodiment, the organic solvent preferably contains a nitrogen-containing solvent, and among such solvents, N-methylpyrrolidone is particularly preferred. In another embodiment, the organic solvent preferably contains an ether, and among such solvents, diethylene glycol dialkyl ether and ethylene glycol monoalkyl ether acetates are particularly preferred. In yet another embodiment, the organic solvent may be a mixed solvent comprising a nitrogen-containing solvent and an ether. For example, the organic solvent is preferably a mixed solvent of N-methylpyrrolidone and butyl cellosolve acetate, and there are no particular restrictions on the mixing ratio.
[0077] The blending amount of the organic solvent in the above resin composition can be appropriately adjusted in consideration of the storage elastic modulus or viscosity. In one embodiment, the blending amount of the organic solvent is preferably within a range of 350 to 500 parts by weight per 100 parts by weight of the total weight of the resin component in the resin composition. The organic solvent is more preferably added in an amount within a range of 400 to 500 parts by weight per 100 parts by weight of the total weight of the polyamideimide resin. By adjusting the blending amount of the organic solvent relative to the resin to fall within the above range, the resin can be easily dissolved, and a viscosity suitable for forming a thick film can be more easily obtained. (Other components)
[0078] If necessary, additives such as colorants and coupling agents, and additional components such as resin modifiers can be added to the above resin composition (varnish). When the resin composition contains additional components, the blending amount of these additional components is preferably no more than 50 parts by weight per 100 parts by weight of the total weight of the resin (solid fraction) in the resin composition. By ensuring that the blending amount of these additional components is no more than 50 parts by weight, any deterioration in the physical properties of the resulting coating film can be more easily suppressed.
[0079] In one embodiment, the resin composition preferably also contains a coupling agent. When a coupling agent is used, the adhesion of the composition to various parts can be more easily improved. There are no particular restrictions on the types of coupling agents that can be used, and examples include silane-based, titanium-based, and aluminum-based coupling agents, but silane-based coupling agents are most preferred.
[0080] There are no particular restrictions on the silane-based coupling agents, and examples include vinyltrichlorosilane, vinyltris(β-methoxyethoxy)silane, vinyltriethoxysilane, vinyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropylmethyldimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, γ-aminopropyltriethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-Mercaptopropyltriethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-ureidopropyltriethoxysilane, 3-ureidopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltris[2-(2-methoxyethoxy)ethoxy]silane, N-methyl-3-aminopropyltrimethoxysilane, triaminopropyltrimethoxysilane, 3-4,5-Dihydroimidazol-1-yl-propyltrimethoxysilane,3-Methacryloxypropyltrimethoxysilan, 3-Mercaptopropylmethyldimethoxysilan, 3-Chlorpropylmethyldimethoxysilan, 3-Chlorpropyldimethoxysilan, 3-Cyanopropyltriethoxysilan, Hexamethyldisilazan, N,O-Bis(trimethylsilyl)acetamid, Methyltrimethoxysilan, Methyltriethoxysilan, Ethyltrichlorsilan, n-Propyltrimethoxysilan, Isobutyltrimethoxysilan, Amyltrichlorsilan, Octyltriethoxysilan, Phenyltrimethoxysilan, Phenyltriethoxysilan, Methyltri (methacryloyloxyethoxy)silan, Methyltri(glycidyloxy)silan, N-β-(N-Vinylbenzylaminoethyl)-y-aminopropyltrimethoxysilan, Octadecyldimethyl-[3-(trimethoxysilyl)propyl]ammoniumchlorid, γ-Chlorpropylmethyldichlorsilan, γ-Chlorpropylmethyldimethoxysilan, γ-Chlorpropylmethyldiethoxysilan, Trimethylsilylisocyanat, Dimethylsilylisocyanat, Methylsilyltriisocyanat, Vinylsilyltriisocyanat, Phenylsilyltriisocyanat,Tetraisocyanatosilane and ethoxysilane isocyanate. One of these silane coupling agents can be used alone, or a combination of two or more silane coupling agents can be used.
[0081] There are no particular restrictions on the titanium-based coupling agents, and examples include isopropyl trioctanoyl titanate, isopropyl dimethacrylisostearoyl titanate, isopropyl tridodecylbenzenesulfonyl titanate, isopropyl isostearyl diacryl titanate, isopropyl tri(dioctyl phosphate) titanate, isopropyl tricumyl phenyl titanate, isopropyl tris(dioctyl pyrophosphate) titanate, isopropyl tris(n-aminoethyl) titanate, tetraisopropyl bis(dioctyl phosphite) titanate, tetraoctyl bis(ditridecyl phosphite) titanate, tetra(2,2-diallyloxymethyl-1-butyl) bis(ditridecyl) phosphite titanate, dicumyl phenyl oxyacetate titanate, bis(dioctyl pyrophosphate) oxyacetate titanate, tetraisopropyl titanate, tetra-n-butyl titanate, butyl titanate dimer, Tetra(2-ethylhexyl)titanate, titanium acetylacetonate, polytitanium acetylacetonate, titanium octylene glycolate, ammonium titanium lactate, titanium lactate, titanium lactate ethyl ester, titanium triethanolamine, polyhydroxytitanium stearate, tetramethyl orthotitanate, tetraethyl orthotitanate, tetrapropyl orthotitanate, tetraisobutyl orthotitanate,Stearyl titanate, cresyl titanate monomer, cresyl titanate polymer, diisopropoxybis(2,4-pentadione)titanium(IV), diisopropylbistriethanolaminotitanate, octylene glycol titanate, tetra-n-butoxytitanium polymer, tri-n-butoxytitanium monostearate polymer, and tri-n-butoxytitanium monostearate. One of these titanium coupling agents can be used alone, or a combination of two or more titanium coupling agents can be used.
[0082] There are no particular restrictions on the aluminum-based coupling agents, and examples include aluminum chelate compounds such as ethyl acetoacetate aluminum diisopropylate, aluminum tris(ethyl acetoacetate), alkyl acetoacetate aluminum diisopropylate, aluminum monoacetylacetoacetate bis(ethyl acetoacetate), aluminum tris(acetylacetonate), aluminum monoisopropoxymonooleoxyethyl acetoacetate, aluminum di-n-butoxide monoethyl acetoacetate and aluminum diisopropoxide monoethyl acetoacetate and aluminum alcoholates such as aluminum isopropylate, mono-secbutoxyaluminum diisopropylate, aluminum sec-butylate and aluminum ethylate.
[0083] In one embodiment, the dried coating film of the resin composition preferably has a dielectric breakdown voltage at room temperature of at least 150 kV / mm. This dielectric breakdown voltage is more preferably at least 180 kV / mm, and even more preferably 200 kV / mm or more. When the dielectric breakdown voltage is at least 150 kV / mm, even a leakage current from a power semiconductor device can be satisfactorily prevented, and excellent reliability for the semiconductor device can be more easily achieved.
[0084] In one embodiment, a dielectric breakdown voltage of at least 200 kV / mm can be achieved with only the resin component, such as the polyamideimide resin, used in the resin composition. Accordingly, the resin composition can be formed without using an inorganic filler or the like. In this regard, in one embodiment, the resin composition can be composed of only the resin component and the organic solvent.
[0085] The "dielectric breakdown voltage (kV / mm)" disclosed in this specification is a value obtained by conducting a dielectric breakdown test using a film formed from the resin composition or the resin dissolved in a solvent. More specifically, a measurement is performed using a sample prepared by forming a film by applying the resin composition (varnish) to an Al substrate and then drying the composition. Representative measurement conditions may include a voltage increase rate of 0.5 kV / s (AC 50 Hz), electrode dimensions using a high-voltage side of φ20 mm (spherical) and a low-voltage side formed from a metal plate, and a test atmosphere of oil.
[0086] In one embodiment, the viscosity of the above resin composition is preferably within a range of 7,000 to 15,000 mPa·s, and more preferably within a range of 8,000 to 13,000 mPa·s. The "viscosity" is a value obtained by measuring a varnish obtained by dissolving the resin in the solvent to obtain a non-volatile fraction (solid fraction component) of 15 to 20% using an E-type viscometer at 25°C and 10 rpm. If the viscosity, measured at 10 rpm, is less than 7,000 mPa·s, ensuring an adequate film thickness upon application becomes difficult. If the viscosity exceeds 15,000 mPa·s, forming a uniform film during application becomes difficult. In the above resin composition, by using a resin having the specific structural units and having a weight average molecular weight of at least 100,000, the desired viscosity can be easily obtained.
[0087] The measurement of the above viscosity can be performed, for example, by using a viscometer (RE type) manufactured by Toki Sangyo Co., Ltd. During the measurement, the measurement temperature is set to 25°C±0.5°C, 1 to 1.5 ml of the resin composition is added to the viscometer, and the viscosity is recorded 10 minutes after the start of the measurement.
[0088] In one embodiment, the elastic modulus at 35°C of the film obtained by applying and drying the resin composition (varnish) is preferably within a range of 0.5 to 3.0 GPa, and more preferably within a range of 1.0 to 3.0 GPa. This elastic modulus is a value measured using a dynamic viscoelasticity measuring device. If the elastic modulus is less than 0.5 GPa, the film becomes too soft, and there is a possibility that the reliability of the energy semiconductor devices may deteriorate. On the other hand, if the elastic modulus exceeds 3.0 GPa, the stress relaxation properties of the film may deteriorate, which may cause deterioration of the reliability of the energy semiconductor devices.In view of obtaining favorable flexibility to further enhance the reliability of energy semiconductor devices, the elastic modulus is more preferably within a range of 2.2 to 3.0 GPa, and most preferably within a range of 2.2 to 2.8 GPa.
[0089] The measurement of the above elastic modulus can be performed, for example, using a dynamic viscoelasticity measuring device "Rheogel-E4000" manufactured by UBM Co., Ltd. A sample is prepared by cutting a film prepared by applying and drying the resin composition (varnish) to a width of 4 mm, and the measurement of the elastic modulus is performed using this sample under measurement conditions including a clamping separation of 20 mm, a measurement frequency of 10 MHz, and a measurement temperature of 35°C. 2. Semiconductor device
[0090] The resin composition of the above-described embodiments exhibits excellent heat resistance and also has excellent insulation properties, flexibility, and thin-film formability, and can therefore be advantageously used as a structural material for semiconductor devices. Another aspect of the invention relates to a semiconductor device having a film formed using the resin composition of any of the above-described embodiments on a surface of a structural member. For example, the above film may constitute an insulating film in the semiconductor device. Alternatively, the film may constitute an adhesive layer or a protective layer, or the like. A semiconductor device having the above film exhibits excellent adhesion between various parts and has excellent reliability.In one embodiment, the resin composition described above can be advantageously used as a structural material of a power semiconductor device using a silicon carbide (SiC) substrate or a gallium nitride (GaN) substrate.
[0091] The Fig. 1 and Fig. 2 are schematic cross-sectional views showing embodiments of semiconductor devices. The semiconductor devices shown in the Fig. 1 and Fig. 2 each have a nozzle pad 1a, a semiconductor element 2, insulating films 3a and 3b or 3, leads 1b, wires 4 and a resin encapsulation layer 5, wherein each insulating film is formed of the resin composition of an embodiment described above.
[0092] In a semiconductor device, the location where leakage current is most likely to occur is at the ground end portions of the wires bonded to the semiconductor element. As shown in Fig.1, in one embodiment, the insulating films 3a are preferably provided at least at the bottom end portions of the wires connected to the semiconductor element. In another embodiment, in addition to the insulating films 3a, the insulating films 3b may also be provided at the bottom end portions of the wires connected to the leads 1b. In yet another embodiment, as shown in Fig. 2, the insulating films 3 formed from the resin composition as described above may be provided on the upper surface and side surfaces of the semiconductor element and on the upper surface of the nozzle pad.
[0093] In this way, by providing an insulating film formed of the resin composition of an embodiment described above, a leakage current occurring inside the semiconductor device can be prevented more effectively, which means that the reliability of the semiconductor device can be enhanced.
[0094] In one embodiment, the method used to produce the semiconductor device includes at least applying the resin composition of an embodiment described above to the surface of a substrate on which a semiconductor element is mounted, and then drying the resin composition to form an insulating film, and forming a resin encapsulation layer on the upper side of the insulating film.
[0095] In the above production method, in view of processability, the above resin composition preferably contains a polyamideimide resin as a resin component. The formation of the above insulating film can be achieved by applying the resin composition to specific locations and then drying the applied coating film. The application of the resin composition can be carried out using any of various coating methods. There are no particular restrictions on the method used for the application, and examples include spray coating methods, potting methods, dipping methods, and metering methods, and the like. Considering processability or the like, a potting method or metering method is preferred.
[0096] There are no particular restrictions on the substrate material, and materials known in the art can be used. Regarding the production of energy semiconductor devices, the nozzle pad material preferably contains at least one material selected from the group consisting of Ni, Cu, and these materials with Ag plating formed thereon. The lead frame material is preferably selected from the group consisting of Ni and Cu.
[0097] The material of the semiconductor element is not particularly limited and may be, for example, a silicon wafer or a silicon carbide wafer or the like.
[0098] The resin encapsulation layer can be formed from the cured product of a resin known in the art as an encapsulating material. For example, liquid or solid epoxy-based resin compositions can be used as the encapsulating material. The resin encapsulation layer can be formed, for example, by performing transfer molding using the encapsulating material.
[0099] In another embodiment, the method for producing the semiconductor device includes, for example, applying the polyamideimide resin composition of an embodiment described above to a semiconductor substrate on which a plurality of wires of the same structure are formed, then drying the composition to form a resin layer and, if necessary, forming a new wire formation on the upper side of the resin layer for electrical connection to the electrodes on the semiconductor substrate. In addition to these steps, if necessary, the production method may also include forming a protective layer (resin layer) on the upper side of the redistribution or the resin layer using the above resin composition.In addition to the above steps, if necessary, the production may also include forming external electrode terminals on the above resin layer and then performing cutting if necessary.
[0100] In the semiconductor device described above, there are no particular restrictions on the semiconductor element, and examples include a silicon wafer and a silicon carbide wafer. There are no particular restrictions on the coating method used to form the above resin layer, but spin coating, spray coating, or metering coating is preferred. The method used to dry the resin layer can be any method known in the art.The resin composition of the above-described embodiments also exhibits other excellent properties such as sputtering resistance, plating resistance, and alkali resistance, which may be necessary in the step of forming a wiring, and therefore, the resin composition is not limited to the types of semiconductor device structures described above and can be advantageously used as a structural material in all types of semiconductor devices. EXAMPLES
[0101] This invention will be described in detail below using a series of examples, but this invention is not limited to these examples. 1. Synthesis of polyamideimide resins (Synthesis Example 1)
[0102] A 1-liter four-necked flask equipped with a thermometer, stirrer, nitrogen inlet tube, and condenser equipped with an oil-water separator was charged with 108.08 g of 2,2-bis[4-(4-aminophenoxy)phenyl]propane and 3.45 g of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane under nitrogen flow, and these components were then dissolved by adding 700 g of N-methyl-2-pyrrolidone (NMP).
[0103] Subsequently, 59.00 g of trimellitic anhydride chloride (TAC) was added while cooling the flask to ensure that the reaction solution temperature did not exceed 20°C. After stirring at room temperature for 1 hour, 33.96 g of triethylamine (TEA) was added while cooling the flask to ensure that the reaction solution temperature did not exceed 20°C, and the reaction was then allowed to proceed for 3 hours at room temperature to produce a polyamic acid solution.
[0104] The resulting polyamic acid solution was then subjected to a dehydration reaction at 190°C for 6 hours to produce a polyamideimide resin solution. This polyamideimide resin solution was poured into water, and the resulting precipitate was separated, crushed, and dried to obtain a powdered polyamideimide resin (PAI-1). Measurement of the polystyrene equivalent weight-average molecular weight (Mw) of the thus-obtained polyamideimide resin (PAI-1) using gel permeation chromatography (GPC) revealed an Mw value of 140,000.
[0105] The detailed conditions for measuring the Mw value were as follows. Feed pump: LC-20AD, manufactured by Shimadzu Corporation UV-Vis detector: SPD-20A, manufactured by Shimadzu Corporation Columns: Shodex KD-806M, manufactured by Showa Denko KK Eluent: NMP, manufactured by Mitsubishi Chemical Corporation Flow rate: 1 ml / min Column temperature: 40°C Molecular weight standard: standard polystyrene (Synthesis example 2)
[0106] A 1-liter four-necked flask equipped with a thermometer, stirrer, nitrogen inlet tube, and condenser equipped with an oil-water separator was charged with 110.35 g of 2,2-bis[4-(4-aminophenoxy)phenyl]propane and 2.07 g of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane under nitrogen flow, and these components were then dissolved by adding 700 g of N-methyl-2-pyrrolidone (NMP).
[0107] Subsequently, 59.00 g of trimellitic anhydride chloride (TAC) was added while cooling the flask to ensure that the reaction solution temperature did not exceed 20°C. After stirring at room temperature for 1 hour, 33.96 g of triethylamine (TEA) was added while cooling the flask to ensure that the reaction solution temperature did not exceed 20°C, and the reaction was then allowed to proceed for 3 hours at room temperature to produce a polyamic acid solution.
[0108] The resulting polyamic acid solution was then subjected to a dehydration reaction at 190°C for 6 hours to produce a polyamideimide resin solution. This polyamideimide resin solution was poured into water, and the resulting precipitate was separated, crushed, and dried to obtain a powdered polyamideimide resin (PAI-2). Measurement of the polystyrene equivalent weight-average molecular weight (Mw) of the thus-obtained polyamideimide resin (PAI-2) using gel permeation chromatography (GPC) revealed an Mw value of 150,000. (Synthesis Example 3)
[0109] A 1-liter four-necked flask equipped with a thermometer, stirrer, nitrogen inlet tube, and condenser equipped with an oil-water separator was charged with 105.80 g of 2,2-bis[4-(4-aminophenoxy)phenyl]propane and 4.82 g of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane under nitrogen flow, and these components were then dissolved by adding 700 g of N-methyl-2-pyrrolidone (NMP).
[0110] Subsequently, 59.00 g of trimellitic anhydride chloride (TAC) was added while cooling the flask to ensure that the reaction solution temperature did not exceed 20°C. After stirring at room temperature for 1 hour, 33.96 g of triethylamine (TEA) was added while cooling the flask to ensure that the reaction solution temperature did not exceed 20°C, and the reaction was then allowed to proceed for 3 hours at room temperature to produce a polyamic acid solution.
[0111] The resulting polyamic acid solution was then subjected to a dehydration reaction at 190°C for 6 hours to produce a polyamideimide resin solution. This polyamideimide resin solution was poured into water, and the resulting precipitate was separated, crushed, and dried to obtain a powdered polyamideimide resin (PAI-3). Measurement of the polystyrene equivalent weight-average molecular weight (Mw) of the thus-obtained polyamideimide resin (PAI-3) using gel permeation chromatography (GPC) revealed an Mw value of 130,000. (Synthesis Example 4)
[0112] A 1-liter four-necked flask equipped with a thermometer, stirrer, nitrogen inlet tube, and condenser equipped with an oil-water separator was charged with 102.389 g of 2,2-bis[4-(4-aminophenoxy)phenyl]propane and 6.89 g of 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane under nitrogen flow, and these components were then dissolved by adding 700 g of N-methyl-2-pyrrolidone (NMP).
[0113] Subsequently, 59.00 g of trimellitic anhydride chloride (TAC) was added while cooling the flask to ensure that the reaction solution temperature did not exceed 20°C. After stirring at room temperature for 1 hour, 33.96 g of triethylamine (TEA) was added while cooling the flask to ensure that the reaction solution temperature did not exceed 20°C, and the reaction was then allowed to proceed for 3 hours at room temperature to produce a polyamic acid solution.
[0114] The resulting polyamic acid solution was then subjected to a dehydration reaction at 190°C for 6 hours to produce a polyamideimide resin solution. This polyamideimide resin solution was poured into water, and the resulting precipitate was separated, crushed, and dried to obtain a powdered polyamideimide resin (PAI-4). Measurement of the polystyrene equivalent weight-average molecular weight (Mw) of the thus-obtained polyamideimide resin (PAI-4) using gel permeation chromatography (GPC) revealed an Mw value of 85,000. (Synthesis Example 5)
[0115] A 1-liter four-necked flask equipped with a thermometer, stirrer, nitrogen inlet tube, and condenser equipped with an oil-water separator was charged with 113.77 g of 2,2-bis[4-(4-aminophenoxy)phenyl]propane under nitrogen flow, and this component was then dissolved by adding 700 g of N-methyl-2-pyrrolidone (NMP).
[0116] Subsequently, 59.00 g of trimellitic anhydride chloride (TAC) was added while cooling the flask to ensure that the reaction solution temperature did not exceed 20°C. After stirring at room temperature for 1 hour, 33.96 g of triethylamine (TEA) was added while cooling the flask to ensure that the reaction solution temperature did not exceed 20°C, and the reaction was then allowed to proceed for 3 hours at room temperature to produce a polyamic acid solution.
[0117] The resulting polyamic acid solution was then subjected to a dehydration reaction at 190°C for 6 hours to produce a polyamideimide resin solution. This polyamideimide resin solution was poured into water, and the resulting precipitate was separated, crushed, and dried to obtain a powdered polyamideimide resin (PAI-5). Measurement of the polystyrene equivalent weight-average molecular weight (Mw) of the thus-obtained polyamideimide resin (PAI-5) using gel permeation chromatography (GPC) revealed an Mw value of 180,000. 2. Preparation of polyamideimide resin compositions (Example 1)
[0118] At room temperature (25°C), a 0.5-liter four-necked flask was charged with 18 g of the polyamideimide resin (PAI-1) obtained in Synthesis Example 1, 32.8 g of N-methyl-2-pyrrolidone, and 49.2 g of butylcellulose acetate under nitrogen flow, and the mixture was stirred for 12 hours to obtain a polyamideimide resin composition. Visual inspection of the obtained resin composition at room temperature (25°C) revealed a yellow transparent composition. The resin composition was placed in a filter device (KST-47, manufactured by Advantec Group), and pressure filtration was performed at a pressure of 0.3 MPa to obtain a polyamideimide resin composition (P-1). (Example 2)
[0119] Except for using the polyamideimide resin (PAI-2) obtained in Synthesis Example 2 as the polyamideimide resin, a polyamideimide resin composition (P-2) was prepared in the same manner as in Example 1. Visual inspection of the obtained resin composition at room temperature (25°C) revealed a yellow transparent composition. (Example 3
[0120] Except for using the polyamideimide resin (PAI-3) obtained in Synthesis Example 3 as the polyamideimide resin, a polyamideimide resin composition (P-3) was prepared in the same manner as in Example 1. Visual inspection of the obtained resin composition at room temperature (25°C) revealed a yellow transparent composition. (Comparison example 1)
[0121] Except for using the polyamideimide resin (PAI-4) obtained in Synthesis Example 4 as the polyamideimide resin, a polyamideimide resin composition (P-4) was prepared in the same manner as in Example 1. Visual inspection of the obtained resin composition at room temperature (25°C) revealed a yellow transparent composition. (Comparison example 2)
[0122] At room temperature (25°C), a 0.5-liter four-necked flask was charged with 18 g of the polyamideimide resin (PAI-4) obtained in Synthesis Example 4, 32.8 g of N-methyl-2-pyrrolidone, and 49.2 g of butylcellulose acetate under a nitrogen stream, and the mixture was stirred for 12 hours to obtain a polyamideimide resin composition. Visual inspection of the resulting resin composition at room temperature (25°C) revealed a yellow, transparent composition.
[0123] Subsequently, 10 g of a silica filler (SC2050) manufactured by Admatechs Co., Ltd. was added to the above resin composition, and stirring was performed using Disper (5,000 rpm, 10 minutes). The resulting composition was then placed in a filtration device (KST-47, manufactured by Advantec Group), and pressure filtration was performed at a pressure of 0.3 MPa to obtain a polyamideimide resin composition (P-5). (Comparison example 3)
[0124] Except for using the polyamideimide resin (PAI-5) obtained in Synthesis Example 5 as the polyamideimide resin, a polyamideimide resin composition (P-6) was prepared in the same manner as in Example 1. Visual inspection of the obtained resin composition at room temperature (25°C) revealed a yellow transparent composition. 3. Evaluation of the properties of polyamideimide resin compositions
[0125] Using each polyamideimide resin composition obtained in Examples 1 to 3 and Comparative Examples 1 to 3, various properties were evaluated using the methods described below. The results are shown in Table 1. (Viscosity)
[0126] The viscosity of each polyamideimide resin composition obtained in Examples 1 to 3 and Comparative Examples 1 to 3 was measured using a viscometer (RE type) manufactured by Toki Sangyo Co., Ltd. under the following conditions. Sample volume: 1.2 ml Measuring temperature: 25°C Cone rotation rate: 10 rpm Measurement time: 10 minutes (Elastic modulus)
[0127] Each polyamideimide resin composition obtained in Examples 1 to 3 and Comparative Examples 1 to 3 was coated onto a substrate using a bar coater and then dried to obtain a film with a thickness of 10 µm. Complete drying of the film was then carried out at 230°C for a period of 2 hours. The thus obtained coating film was cut to a width of 4 mm and used as a measurement sample.
[0128] The test sample was placed in a dynamic viscoelasticity measuring device "Rheogel-E4000" manufactured by UBM Co., Ltd., and the elastic modulus of the polyamideimide resin was measured. The measurement was performed using a 20 mm clamp separation, and the elastic modulus was obtained by reading the value at 35°C. (Dielectric breakdown voltage)
[0129] Each polyamideimide resin composition obtained in Examples 1 to 3 and Comparative Examples 1 to 3 was coated onto an Al metal substrate using a bar coater and dried to obtain a film with a thickness of 10 µm. Complete drying of the film was then carried out at 230°C for a period of 2 hours. The dielectric breakdown voltage of the thus-obtained film was measured under the following conditions. Test temperature: 25°C Rate of voltage increase: 0.5 kV / s (AC 50 Hz) Electron dimension: High voltage side: φ20 mm spherical, low-voltage logs: metal plate Test atmosphere: in oil (Measurement of the aspect ratio)
[0130] Using each polyamideimide resin composition (varnish) obtained in Examples 1 to 3 and Comparative Examples 1 to 3, coating was carried out under the following conditions. Nozzle diameter: φ29 mm Nozzle speed: 10 mm / s Drain pressure: 0.3 MPa
[0131] Subsequently, drying was performed, and then complete drying was carried out at 230°C for a period of 2 hours. The shape of the dried coating film was measured using a Dektak 6M Surface Profiler (manufactured by ULVAQC, Inc.), and the coating film aspect ratio (= coating film thickness / coating film width) was calculated. [Table 1] Resin composition (resin Mw) filler Viscosity (mPa s) Dielectric breakdown voltage (kV / mm) Thick film forming ability (aspect ratio) Elastic modulus (GPa) Tg (°C) Example 1 P-1 (140.000) nothing 9.800 211 0,07 2, 6 210 Example 2 P-2 (150.000) Nothing 10.300 210 0,07 2,7 215 Example 3 P-3 (130.000) Nothing 8.300 210 0,06 2,2 206 Comparison example 1 P-4 (85.000) Nothing 430 208 0,02 2,0 199 Comparison example 2 P-5 (85.000) Yes 11.000 18 0,10 4,2 199 Comparison example 3 P-6 (180.000) Nothing 14.500 203 0,08 3, 9 220
[0132] As is apparent from Table 1, with respect to the resin compositions of Examples 1 to 3, which were embodiments of this invention, in each case the dielectric breakdown voltage was at least 150 kV / mm and the dried coating film aspect ratio after metering was at least 0.05. Furthermore, the elastic modulus was within a range of 0.5 to 3.0 GPa. Based on these results, it was apparent that by using a resin containing the structural unit (1A) and / or (1B) and the structural unit (2A) and / or (2B) and having an Mw value of at least 100,000, a resin composition exhibiting excellent insulation properties, flexibility, and thick film formability could be obtained.
[0133] In contrast, the resin composition of Comparative Example 1 used a resin with an Mw value of less than 100,000, and the results showed low viscosity and poor thick film formability compared to Examples 1 to 3. In the resin composition of Comparative Example 2, an inorganic filler (silica) was added to improve the viscosity of the resin composition of Comparative Example 1. The results revealed that although Comparative Example 2 had similar viscosity and aspect ratio values to Examples 1 to 3, the dielectric breakdown voltage was significantly inferior. The resin composition of Comparative Example 3 used a resin containing structural unit (1A) and / or (1B) but not structural unit (2A) and / or (2B).The results revealed that although Comparative Example 3 had similar viscosity and aspect ratio values to Examples 1 to 3, the reliability of the energy semiconductor device was inferior even though the elastic modulus was high.
[0134] Based on these results, it is apparent that a resin composition of this invention can be advantageously used as a structural material in power semiconductor devices requiring excellent insulation properties at specific locations and is capable of ensuring satisfactory insulation properties. DESCRIPTION OF REFERENCE SYMBOLS 1 lead frame 1a nozzle pad 1b line 2 semiconductor element 3a, 3b, 3 Insulation film (cured film of the resin composition) 4 wire 5 Resin encapsulation layer
Claims
[1] A resin composition containing a resin component (A) and an organic solvent (B), wherein the resin component (A) contains a polyamideimide resin containing a structural unit represented by the following formula (1A) and / or (1B) and a structural unit represented by the following formula (2A) and / or (2B) and having a weight-average molecular weight of at least 100,000: wherein each of R1 to R4 is independently a hydrogen atom or one or more substituents selected from the group consisting of alkyl groups having 1 to 9 carbon atoms, alkoxy groups having 1 to 9 carbon atoms, and halogen atoms, and X is a divalent organic group shown below: wherein R5 and R6 are each independently an alkyl group having 1 to 9 carbon atoms, wherein R7 to R 10 each independently represents an alkyl group having 1 to 9 carbon atoms and n is an integer from 1 to 6. [2] The resin composition according to claim 1, wherein the polyamideimide resin contains 3 to 7 mol% of the structural unit represented by the formula (2A) and / or (2B) based on a total number of moles of the structural unit represented by the formula (1A) and / or (1B) and the structural unit represented by the formula (2A) and / or (2B). [3] The resin composition according to claim 1 or 2, wherein the polyamideimide resin contains a structure represented by the following formula (1A-1) and / or (1B-1) and a structure represented by the following formula (2A-1) and / or (2B-1): [4] The resin composition according to any one of claims 1 to 3, wherein a dielectric breakdown voltage of a film obtained by drying the resin composition is at least 150 kV / mm. [5] The resin composition according to any one of claims 1 to 4, wherein a glass transition temperature of the polyamideimide resin is at least 200°C. [6] The resin composition according to any one of claims 1 to 5, wherein an elastic modulus at 35°C of a film obtained by drying the resin composition is within a range of 0.5 to 3.0 GPa. [7] A semiconductor device having a film formed using the resin composition according to any one of claims 1 to 6 on a surface of a structural component.
Citation Information
Patent Citations
Insulating paste
JP1990173073A
Polyimide resin
CN101454378A
Halogen-free flame retardant compositions
EP0636655A2
Polyimide resin and resin varnish for adhesion
JP1998036507A
Thermosetting, lowly dielectric resin composition and circuit laminate
JP2000204251A