Attachment of a fastening object to a base component via an intermediate heat spreader, which is sintered under pressure onto the fastening object and soldered to the base component.

A two-stage process of pressure sintering an intermediate heat spreader to semiconductor power modules and soldering it to a base component addresses the inefficiencies of conventional methods, ensuring reliable and flexible assembly with reduced waste and improved heat transfer.

DE102023110701B3Active Publication Date: 2024-10-02SEMIKRON DANFOSS GMBH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
DE102023110701
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-04-26
Publication Date
2024-10-02
Estimated Expiration
2043-04-26

AI Technical Summary

Technical Problem

Conventional methods for attaching semiconductor power modules to base components using soldering are prone to damage from high temperature peaks and uneven heat distribution, while pressure sintering requires complex tools and quality control is difficult, leading to production inefficiencies and waste.

Method used

A two-stage process involving pressure sintering an intermediate heat spreader to the fastening object and then soldering it to the base component, allowing for non-destructive quality control of the pressure sintered layer and reducing the complexity of the sintering process.

Benefits of technology

This method enhances operational reliability by shielding the solder layer from high temperatures, ensuring uniform heat transfer, and reduces production waste by enabling flexible, cost-effective assembly in secondary facilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The invention relates to a manufacturing method for attaching a mounting object (50), e.g., a semiconductor power module, to a base component (10; 210), e.g., a heat sink, a heat sink, and / or (a connection for) a cooler. To provide a mounting method that exhibits high operational reliability and production flexibility, the method comprises providing an intermediate heat spreader (30) and attaching the latter to an interface side (51) of the mounting object (50) by pressure sintering, thereby forming a pressure-sintered layer (40) between the interface side (51) and an object side (32) of the intermediate heat spreader (30).The intermediate heat spreader (30) with the pressure-sintered mounting object (50) attached to it is then fastened to the base component (10; 210) by soldering, whereby a solder layer (20) is formed between the base component (10; 210) and a base side (31) of the intermediate heat spreader (30). The invention further relates to an assembly (100; 200) comprising a base component (10; 210) and a mounting object (50) which is connected to the base component (10; 210) via a pressure-sintered layer (40), an intermediate heat spreader (30), and a solder layer (20).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a manufacturing method for fastening a fastening object, e.g. semiconductor power module, to a base component, e.g. to a heat sink, a heat sink and / or (a part for) a cooler. It further relates to an assembly comprising a base component and a Fastening object includes.

[0002] The manufacturing method is applicable to the production of power module assemblies. Such Power module assembly (hereinafter referred to as ´´assembly´´) may include several fastening objects, which are attached to the base component. Typically, the assembly is configured to be part of an electrical circuit, e.g., a powertrain circuit of an electric vehicle. The demand for electric vehicles, especially for electric cars, is increasing rapidly these days.

[0003] The power module assembly and in particular its mounting objects are designed to At least some of the attachment objects may contain semiconductor Power modules. These can be insulated gate bipolar transistors (IGBTs) and / or metal oxide semiconductor field-effect transistors (MOSFETs).

[0004] During operation of the circuit, the attachments generate heat, particularly through electrical currents. To avoid overheating and damage to the attachments, the attachments are attached to the base component. Often the base component is a heat sink, a heatsink and / or (a part for) a cooler. The base component takes absorbs a significant portion of the heat generated by the attachments and dissipates it.

[0005] The fastening objects should be attached to the base component in such a way that sufficient heat transfer from the fastening objects on the base component is possible. In addition, the mechanical connection between the Fastening objects and the base component must be reliable.

[0006] Conventionally, the fastening objects are fixed by soldering directly onto the base component. Soldering is comparatively simple and inexpensive to produce. However, the solder layers between the fastening objects and the base components to become soft and finally to be damaged by high temperature peaks that the interface sides of the fastening objects directly facing the solder layers are damaged. During operation, the components (e.g. semiconductor power modules) sometimes ´´pulse´´ with heat. Heat development of the attachments can be uneven over time. In addition, the heat generated by the internal Components of the individual attachment generate heat spatially unevenly on the interface side of this attachment.

[0007] Alternatively, the fastening objects can be attached directly to the base component by pressure sintering. A sintered layer of sintered material is applied between the fastening objects and the base component. In the subsequent solidification step, the sintered material is heated to a maximum sintering temperature. For example, the attachment objects and the base component are aligned along a normal direction that is perpendicular to the The solidification step compacts and strengthens the sintered material. A pressure sintered layer is formed from the sintered layer directly between the fastening objects and the base component. The pressure-sintered layer fixes the fastening objects directly to the base component. Pressure-sintered layers are less susceptible for damage caused by high-temperature peaks that occur at the interface sides of the attachments. The direct However, attaching the semiconductor power modules to the base component by pressure sintering is comparatively difficult and demanding. It requires more complex tools and is usually more expensive than fixing by soldering. In particular, the fastening objects and the base component must be pressed together evenly in order to To obtain a thin and even pressure sintered layer, the tools should be adapted to the individual shapes of the Fastening objects and the base components must be adapted. This results in high effort and low Production flexibility.

[0008] Often the same type of mounting objects (e.g. semiconductor power modules) is used by different Secondary manufacturers (hereinafter referred to as customers) for various purposes, e.g., for the production various customer-specific assemblies. Since pressure sintering is difficult and demanding, some customers Problems with attaching objects to their customer-specific base components by pressure sintering in sufficient To fix quality.

[0009] A high quality of the pressure sintered layers must be ensured so that sufficient heat transfer from the fastening objects to the base components is ensured and the fixation is mechanically robust. significant voids or delaminations in or on the pressure sintered layer. Currently, there are no adequate measurement technology to Quality of the pressure-sintered connection formed directly between the fastening objects and the base components non-destructive and sufficiently detailed in industrial production. Either the measurement methods too slow or too expensive for adequate quality control in industrial production, or the measurement resolution is too low to detect small cavities or delaminations of the pressure sintered layer, or the measurement is due to the complex and / or irregular internal structures of the fastening objects and the base components disabled.

[0010] Typically, several fastening objects are solidified in a common solidification step by pressure sintering simultaneously attached to the base component. Due to the high temperature and pressure required for pressure sintering However, there is a risk that some of the attachment objects will be damaged during pressure sintering. resulting pressure sintered layers are rigid and permanently fix the fastening objects to the base component, the The entire assembly must be discarded if only one of the fastening objects is damaged during pressure sintering becomes.

[0011] DE 10 2008 009 510 B3 discloses a method in which a heat sink plate is coated by means of silver low-temperature Pressure sintering technology on a substrate of an electronic assembly in the area of ​​a connection surface is connected.

[0012] In US 2019 / 0 122 955 A1, a semiconductor element is formed by means of a sintered metal, for example by means of sintered aluminum, or by a solder layer to a first surface of an insulating substrate. A cooling device is attached to an opposite second surface of the insulating substrate. The insulating The substrate comprises an insulating ceramic sandwiched between conductive plates. Components are pre-integrated with a material such as wax to form the insulating substrate Due to the insulating ceramic, there is no optimal heat transfer from the semiconductor element to the Cooling device possible.

[0013] The task is to attach a fastening object to a base component that has a high operational reliability and flexibility in production.

[0014] This object is achieved by a manufacturing method for attaching a fastening object to a Base component according to claim 1.

[0015] The manufacturing process comprises the following steps: - Providing an intermediate heat spreader in addition to the fastening object; - Attaching the intermediate heat spreader to an interface side of the attachment object by pressure sintering, whereby a pressure sintered layer is formed between the interface side and an object side of the intermediate heat spreader is formed; and - Attaching the intermediate heat spreader with the pressure-sintered fastening object to the base component by soldering, whereby a solder layer is formed between the base component and a base side of the intermediate heat spreader, which is opposite the object side.

[0016] In other words, the fastening object is attached to the base component in a two-stage process. A first stage involves the attachment of the intermediate heat spreader to the interface side of the attachment object by pressure sintering. A second stage involves the attachment of the intermediate heat spreader to the attachment object by pressure sintering on the base component. The first step and the second step can be carried out at different locations and / or with different tools. For example, the first stage can be carried out in a primary manufacturing facility and the second stage in a secondary manufacturing facility. The first stage and the second stage, the corresponding tools and the corresponding quality controls can be individually optimized become.

[0017] The intermediate heat spreader with the pressure-sintered fastening object can be used as a ´´subassembly of the first stage. An ´´assembly´´ can comprise the base component with at least one attached Include first-level subassembly (corresponding to the second level).

[0018] On the one hand, pressure sintered layers are less susceptible to damage caused by excessively high temperatures during operation than solder layers. On the other hand, the production of pressure sintered layers is more demanding than the production of Solder layers. It requires more complex tools and quality control can be more difficult. Conversely, The production of solder layers requires less complex tools and is simpler.

[0019] In the approach presented, the more demanding first stage can be carried out centrally, e.g. in the same primary manufacturing facility, while the second stage is carried out in various secondary manufacturing facilities For example, different customers can produce their final assemblies in their own secondary production facilities produce.

[0020] In final assembly (e.g. as described below), the attachment object (e.g. a semiconductor power module) During operation, heat is typically generated. The heat is transferred to the base component and then Spatial and / or temporal temperature peaks at the interface side of the mounting side appear.

[0021] The pressure sintered layer, which is next to the heat-generating fastening object, is more temperature-resistant and has a good heat transfer from the fastening object to the intermediate heat spreader. The connection adjacent to the interface side must be of very good quality.

[0022] The intermediate heat spreader serves to shield the solder layer against high temperatures.

[0023] The intermediate heat spreader distributes the heat absorbed by the fastening object. Intermediate heat spreader smooths spatial and / or temporal high temperature peaks (and corresponding spatial and / or temporal heat flow peaks) generated by the fastening object. In general, the temperature and the heat flow at the bottom of the intermediate heat spreader is more uniform than at the interface side of the The risk of high temperature peaks is much lower on the base side than on the As a result, the connection between the intermediate heat spreader and the base component can be the solder layer (instead of a pressure sintered layer) can be produced without affecting the reliability of the final assembly affect.

[0024] In general, a temperature gradient occurs between the object side and the base side during operation, ie within the intermediate heat spreader along a normal direction. The temperature at the base side is - even without Consideration of spatial and / or temporal high temperature peaks - usually lower than on the object side.

[0025] The normal direction can be perpendicular to the intermediate heat spreader, in particular to its object-side surface (at least where the pressure sintered layer forms).

[0026] There are no very strict requirements on the quality of the solder layer, e.g. regarding voids in the Solder layer. First, the solder layer is shielded from high temperature peaks by the intermediate heat spreader. Secondly, the heat flow is introduced more evenly into the solder layer than into the pressure sintered layer. Thirdly, the Solder layer is cooled directly through the base component. Therefore, inhomogeneities and / or local defects within the Solder layer less susceptible to affecting the performance and / or reliability of the assembly.

[0027] The pressure sintered layer is made from a sintered material by pressure sintering. The sintered material is between the fastening object and the intermediate heat spreader, more precisely between the interface side and the The pressure sintering process involves applying heat and pressure to the sintered material. Pressure sintering compacts and solidifies the sintered material. This creates the pressure sintered layer from the sintered material generated.

[0028] According to one aspect, the manufacturing method (the step(s)) may comprise: - non-destructive measurement of the pressure sintered layer and / or - Testing the electrical properties of the fastening object after attaching the intermediate heat spreader to the attachment object by pressure sintering, but before Attaching the intermediate heat spreader with the pressure-sintered fastening object to the base component.

[0029] If the non-destructive measurement shows that the quality of the pressure sintered layer in the first stage subassembly is unacceptable, only the affected first subassembly of the first level needs to be rejected. base component is wasted. If several first-level subassemblies are to be attached to the same base component only the first stage subassembly with the unacceptable pressure sintered layer shall be rejected; no other of the first-stage subassemblies must be discarded. The non-destructive measurement of the pressure sintered layer can be performed for each first Subassembly must be carried out individually.

[0030] During pressure sintering, the fastening object is exposed to increased pressure and elevated temperatures. can be damaged during pressure sintering. Even if it has the desired electrical properties before pressure sintering properties, this is after pressure sintering (ie when the fastening object is part of the subassembly of the first level) may no longer be guaranteed. According to this aspect, the testing of the electrical Properties of the fastening object for first-level subassemblies can be done individually and an incorrect The first-stage subassembly can be selectively sorted out before being attached to the base component (where further first-stage subassemblies attached This helps to reduce production waste.

[0031] The non-destructive measurement of the pressure sintered layer can include (the step) of acoustic microscopy (SAM) of the The SAM can be sintered after the intermediate heat spreader is attached to one interface side of the fastening object by pressure sintering, but before the fastening of the intermediate heat spreader with the pressure-sintered attachment object to the base component by soldering. The measurement can be carried out by the In particular, acoustic test waves can be emitted from the side of the intermediate heat spreader in the direction of the pressure sintered layer, e.g. at least essentially along the normal direction, and reflections that carry the information to be measured can be found on the side of the Intermediate heat spreader. SAM checks the quality of the finished pressure sintered layer in a non-destructive manner.

[0032] It would be difficult to check the pressure sintering layer if SAM is applied from the side of the attachment object The fastening object may have a complex and / or irregular structure that could measurement if the acoustic waves (e.g. incoming waves and / or reflections) affect the In addition, the base component may have a complex and / or irregular structure, e.g. with a plurality of cooling fins and / or a plurality of cooling channels or similar. The complex and / or irregular structure of the base component may affect the measurement if acoustic waves (e.g. B. incident acoustic waves and / or reflections) must pass through the base component.

[0033] This means that when the fastening object is directly attached to the base component by a conventionally applied pressure sintered layer a reliable quality control of this conventionally applied Pressure sintering layer by SAM would be difficult or even impossible. The two-stage fixation according to the present The invention enables reliable non-destructive measurement of the finished pressure sintered layer between the Attachment object and the intermediate heat spreader, before the intermediate heat spreader with the already fixed The fastening object is further attached to the base component.

[0034] According to a further aspect, the manufacturing method (step) may comprise: - Non-destructive measurement of the solder layer using X-rays.

[0035] The non-destructive measurement of the solder layer with X-rays can be carried out despite a complex and / or irregular structure of the base component and a complex and / or irregular structure of the The fastening object can be secured. It is quick and cost-effective.

[0036] As mentioned above, there are no very strict requirements regarding voids in the solder layer. The required quality can be adequately verified by measuring with X-rays.

[0037] The manufacturing method may comprise (the step of): - Arranging a sintering pad and / or a sintering paste between the intermediate heat spreader and the Fastening object.

[0038] More generally, the sintering material may comprise the sintering paste and / or the sintering pad (in particular consist of it).

[0039] The sintered material may comprise metallic particles and at least one volatile component. metallic particles may contain or be silver particles and / or copper particles. The volatile component(s) 3 3 can be organic. The density of the sintered material can be in the range of 2.5 g / cm to 3.5 g / cm. Sinter material can be applied wet in one application step, e.g., on the object side and / or on the Interface side.

[0040] The sintered material can be pre-dried. In particular, the manufacturing process can include a step of Pre-drying of the sintering material, e.g., after the application step and before placing the Attachment object to the object side with the sintering material in between. During pre-drying, at least a portion of the volatile organic component, e.g. at least 70%.

[0041] According to one aspect, the formation of the pressure sintered layer (for permanent fixation of the fastening object at the intermediate heat spreader) a sintering with a maximum sintering temperature in the range of 200 °C to 300 °C and / or with a maximum sintering pressure in the range of 10 MPa to 40 MPa. This ensures a proper sintering and thus a rigid and firm fixation of the fastening object to the intermediate heat spreader. The increased pressure reduces the risk of voids in the pressure sintered layer and contributes to the The pressure sintered layer is particularly dense and thin. This is advantageous for good thermal conductivity of the Attachment object to the intermediate heat spreader. This increases ultimately the reliability of final assembly in operation.

[0042] In one embodiment, the thickness of the pressure sintered layer (e.g. along the normal direction) is a maximum of 70 µm. Additionally or alternatively, the thickness of the pressure sintered layer can be at least 20 µm. The thickness of the Pressure sintered layer can be 50 µm ± V. V can be, for example, 10 µm or 6 µm. The thickness of the Pressure sintering layer may be less than the thickness of the previous sintering layer (i.e. a layer of the sintering material before pressure sintering). The density of the pressure sintered layer can be higher than the density of the previous sintered layer. Pressure sintered layer can consist of at least 90 wt.%, possibly at least 96 wt.%, metal, which can be e.g. from the metallic component of the sintered material. The density of the pressure sintered layer can be Essentially correspond to a density of the metallic material component of the sintered material.

[0043] In one embodiment, the base component is made of metal. Additionally or alternatively, the base component a heat sink, a heatsink and / or a cooler.

[0044] The base component may be configured to transfer heat to at least one fluid, e.g., to the Ambient air and / or a coolant.

[0045] The base component may comprise cooling fins, e.g., elongated fins and / or pin fins. Additionally or alternatively the base component may have grooves and / or walls to form coolant channels.

[0046] In particular, the base component can be made of aluminum (including aluminum alloys). This facilitates the production of a complex structure of the base component by drop forging, e.g., the cooling fins and / or the grooves for forming coolant channels. Furthermore, aluminum is cheaper than copper. Copper (including copper alloys) enables a strong and reliable fixation of the pressure sintered layer and has a higher thermal conductivity. Since the base component is heated indirectly via the solder layer, the intermediate heat spreader and the pressure sintered layer is connected to the attachment, i.e. no direct fixation of the pressure sintered layer to the base component and the intermediate heat spreader shields the base component from high temperatures, the present Invention utilizes the advantages of both materials.

[0047] According to a more general aspect, the intermediate heat spreader may be made of a different material than the Basic component.

[0048] The fastening of the intermediate heat spreader with the fastening object sintered thereon to the Base component by soldering may involve heating the base component with a hot fluid, e.g. with hot air (ie performed or supported). Since the base component can be configured to transfer heat to at least a fluid, it can be easily heated by exposing it to a hot fluid. This enables cost-effective soldering and the uncomplicated use of tools. Furthermore, it is possible to to use the same heating tools for base components with different complex cooling structures.

[0049] According to one aspect, the fastening object may comprise at least one of the following elements: - a heat-generating component; - an electronic component, e.g. a semiconductor component; and - a semiconductor power module.

[0050] In particular, the attachment object may be the semiconductor power module. The semiconductor power module may have at least one semiconductor component.

[0051] The electronic component and the semiconductor power module may generate heat during operation; therefore they can also be considered as a heat-generating component.

[0052] The semiconductor device may comprise a semiconductor switch, an insulated-gate bipolar transistor (insulated-gate bipolar transistor) (IGBT), a metal-oxide-semiconductor field-effect transistor (MOSFET) and / or similar or consisting of consist.

[0053] The attachment object as such, e.g., the semiconductor power module as such, may have various layers and / or components.

[0054] In particular, the fastening object may comprise a cast-in semiconductor power module or be made of This is a semiconductor power module with a resin cover. The resin cover can be Resin transfer molding. If several fixture objects are part of the assembly, at least one of them, a part of them or all of them have an encapsulated semiconductor power module or such a thing exists.

[0055] The manufacturing method may include a step of forming the resin cover.

[0056] The resin cover can be formed before fixing the intermediate heat spreader to the fixing object, which is pressed onto the base component by soldering.

[0057] The resin cover can be applied to the interface side of the Fastening object can be formed by pressure sintering.

[0058] Alternatively, the resin cover may be applied after the intermediate heat spreader is attached to the interface side of the fastening object by pressure sintering. In this context, it may be advantageous to non-destructive measurement of the pressure sintered layer and / or testing of the electrical properties of the fastening object after (the step of) forming the resin cover. In this way, even Damage to the fastening object can be detected, which is caused by the formation of the resin cover after Attaching the heat spreader to the attachment object.

[0059] According to one aspect, the attachment object may have an integrated heat spreader on the interface side wherein the pressure sintered layer (directly) connects the intermediate heat spreader to the integrated Heat spreader fixed.

[0060] In one embodiment, the fastening object comprises an insulating layer, a (directly) on the insulating layer attached internal electrical circuit layer and at least one on the insulating layer and / or the internal electrical Circuit layer mounted semiconductor component.

[0061] In particular, the insulation layer can be (directly) attached to the integrated heat spreader (on one side of the integrated heat spreader, which is facing away from the interface side). The insulation layer can be placed between the integrated heat spreader and the internal circuit layer. The insulating layer can be made of ceramic material.

[0062] The fastening object may further comprise one, several or all of the following elements: - an internal attachment layer (e.g. an internal pressure sintered layer) for attaching the semiconductor component to the insulation layer and / or the internal electrical circuit layer, - connecting wires, and - the resin cover (´´encapsulated semiconductor power module´´).

[0063] The internal pressure sintered layer (within the semiconductor power module) and the pressure sintered layer can be the same solidification step. In this context, it may be advantageous to cover the resin after fixing the intermediate heat spreader to the interface side of the fixing object by pressure sintering to form.

[0064] In one embodiment, the attachment object (e.g., the semiconductor power module) comprises a directly bonded direct bonded copper (DCB) structure. It can have a substrate, e.g., a ceramic substrate, which supports the In addition, the DCB structure can form the insulation layer and one or both of the internal electrical circuit layer and the integrated heat spreader.

[0065] In one embodiment, the intermediate heat spreader is made of copper, is flat in shape and / or has a thickness in the range of 2 mm to 4 mm.

[0066] In this context, the term 'copper' can include pure copper and copper alloys. particularly easy to achieve a strong mechanical connection and good thermal conductivity between the Intermediate heat spreader and the pressure sintered layer of the intermediate heat spreader made of copper (including copper alloys).

[0067] The intermediate heat spreader must not have any (additional) metallization. The intermediate heat spreader can, for example, For example, they can be manufactured from a single bulk material. This reduces costs.

[0068] The formation of the intermediate heat spreader may involve rolling. In other words: Intermediate heat spreader can be made of rolled material, especially rolled metal. This is a cost-effective and reliable method to ensure the flatness and smoothness of the intermediate heat spreader. This allows a particularly thin and uniform pressure sintered layer to be achieved.

[0069] The intermediate heat spreader can have a simple geometry. Pressure sintering requires the use of suitable pressure sintering tools. The use of the intermediate heat spreader with the simple geometry enables the use of simple and efficient sintering tools. In addition, the intermediate heat spreader can be quickly and can be manufactured cost-effectively. As already mentioned, the intermediate heat spreader can be flat (planar). It can have a rectangular shape, a polygonal shape, a disc shape or similar. In one embodiment, it has a rectangular shape.

[0070] The intermediate heat exchanger may, for example, be free of cooling fins and cooling channels.

[0071] If the intermediate heat spreader is flat (planar), this facilitates a uniform heat transfer from the Pressure sintering tool onto the sintering material through the intermediate heat spreader during pressure sintering. In addition, It is particularly easy to apply uniform pressure to the sintered material during pressure sintering. The flat Form enables the use of an efficient flat sintering tool for pressure sintering.

[0072] A planar shape of the intermediate heat spreader can be adapted to a planar shape of the fastening object on the interface side. This facilitates the handling of the first-level subassembly. In addition, the First stage subassembly can be easily fitted into a corresponding recess in the base component.

[0073] In particular, a surface area of ​​the intermediate heat spreader can be at least substantially equal to a The surface area of ​​the interface side can be the same. For example, the surface area of ​​the intermediate heat spreader deviate by a maximum of 10% from the surface area of ​​the interface side.

[0074] According to one aspect, the intermediate heat spreader may at least cover the entire integrated heat spreader This ensures good heat transfer to the intermediate heat spreader.

[0075] According to another aspect, the intermediate heat spreader may support the attachment object on the interface side cover it properly when it is attached to it by the pressure sintered layer. In other words, the Intermediate heat spreader can be designed so that the fastening object fits the intermediate heat spreader overlapped. According to a further aspect, the pressure-sintered layer can also be shaped accordingly.

[0076] In particular, side walls of the intermediate heat spreader and the fastening object, which are parallel to the normal direction, be flush with each other.

[0077] In one embodiment, the base component comprises a recess which accommodates the intermediate heat spreader, wherein a shape of the recess is at least substantially adapted to the planar shape of the intermediate heat spreader This supports the correct positioning of the first-stage subassembly on the base component. In addition, the solder layer is (at least partially) between the side walls of the intermediate heat spreader and the side walls In this way, the heat transfer from the intermediate heat spreader to the base component In addition, the recess can help to correct the position of the soldering material. ensure.

[0078] In particular, the area of ​​the recess may be 1.01 to 1.20 times the area of ​​the The tolerance is large enough to allow the intermediate heat spreader to be inserted easily. small enough to ensure sufficiently correct alignment of the first stage subassembly with the base component ensure, and small enough for the solder layer to be (at least partially) sandwiched between the side walls of the intermediate heat spreader and the side walls of the recess.

[0079] The above-mentioned problem is further solved by an assembly comprising a base component and a Base component includes fastening object attached, wherein the assembly comprises an additional intermediate heat spreader (an additional intermediate connection heat spreader) which is arranged between the base component and the fastening object, and wherein a pressure sintering layer forms an object side of the intermediate heat spreader on the fastening object and a Solder layer fixes a base side of the intermediate heat spreader opposite the object side to the base component.

[0080] The features and advantages described with regard to the manufacturing process apply accordingly to the assembly and vice versa.

[0081] According to one aspect, the fastening object and the intermediate heat spreader may be made with the method disclosed herein manufacturing process (permanently) attached to the base component.

[0082] The fastening object may be a semiconductor power module with at least one semiconductor component Additionally or alternatively, the base component may be a heat sink, a heatsink, and / or a cooler.

[0083] In one embodiment, the fastening product comprises - an integrated heat spreader, which is connected through the pressure sintered layer (directly) to the intermediate heat spreader is attached, - an insulating layer attached (directly) to the integrated heat spreader, and - an internal electrical circuit layer attached (directly) to the insulating layer.

[0084] In particular, the attachment object may be the semiconductor power module and the at least one semiconductor Component is attached to the insulation layer and / or the electrical circuit layer (e.g. by an internal Attachment layer of the semiconductor power module, e.g. an internal pressure sintered layer).

[0085] According to one aspect, the above-mentioned problem is solved by an assembly comprising a base component and comprises at least two sub-assemblies, each of the sub-assemblies comprising a fastening object, a The intermediate heat spreader (an additional intermediate connection) arranged between the fastening object and the base component Heat spreader) and a pressure sintered layer, wherein the pressure sintered layer forms an object side of the intermediate heat spreader fixed to the fastening object, where base sides of the intermediate heat spreaders, which are opposite to their object sides, are each connected to the base component by soldering are attached.

[0086] Further features, advantages and possible applications of the invention will become apparent from the following Description of exemplary embodiments and the drawings. All described and / or graphically The features shown form the subject matter of the invention, either alone or in any combination, independently how they are combined in the claims or in their references to preceding claims.

[0087] Preferred embodiments of the invention will now be described with reference to the drawings, in which those: Fig. 1 shows a schematic example of a manufacturing process with a two-stage fixation process, which a first stage, pressure sintering to form a first stage subassembly having a Intermediate heat spreader comprises a fastening object fixed by a pressure sintering layer, and a second stage which comprises fixing the first stage subassembly to a base component by soldering; Fig. 2 shows the first stage symbolically; Fig. 3 shows an embodiment of a first stage subassembly in which one interface side of the Attachment object through the pressure sintered layer on one side of the object of the intermediate heat spreader is attached; Fig. 4 shows a schematic of a non-destructive measurement to check the quality of the pressure sintered layer; Fig. 5 shows an exemplary embodiment of the base component; Fig. 6 symbolically illustrates the second stage; Fig. 7 shows a first embodiment of an assembly formed by the manufacturing process; Fig. 8 shows a schematic of a non-destructive measurement to check the quality of the solder layer; and Fig. 9 shows a second embodiment of an assembly formed by the manufacturing process.

[0088] Figure 1 shows an example of a manufacturing process according to the present disclosure.

[0089] Step S10 serves to provide an intermediate heat spreader 30. An embodiment of the Intermediate heat spreader 30 is shown in Fig. 2, for example.

[0090] The intermediate heat spreader 30 should be made of a material with high thermal conductivity. For example, the intermediate heat spreader 30 is made of metal. In the embodiment shown in Fig. 2, the intermediate heat spreader 30 made of copper (which may also include copper alloys).

[0091] The intermediate heat spreader 30 is flat (planar). A normal direction N can be perpendicular to the Intermediate heat spreader 30. In particular, the normal direction N is perpendicular to an object side 32 of the Intermediate heat spreader 30.

[0092] In a plane perpendicular to the normal direction N, the intermediate heat spreader 30 has a shape resembling a shape of a Interface side 51 of a fastening object 50 which is attached to the object side 32 of the intermediate heat spreader 30 is to be attached. For example, the intermediate heat spreader 30 has a rectangular shape.

[0093] The intermediate heat spreader 30 may be made of rolled material. Accordingly, the thickness T particularly even and can be precisely controlled. In addition, a side facing away from the object 32 Base side 31 and the object side 32 of the intermediate heat spreader 30 are smooth or planar. Step S10 can be the production of the Intermediate heat spreader 30 by rolling and / or cutting the rolled material.

[0094] Furthermore, the manufacturing method may comprise a step S20 which provides for the application of sintering material. The sintering material is placed between the object side 32 of the intermediate heat spreader 30 and the interface side 51 of the As shown in Fig. 2, a sintering paste 41 can be applied to the object side 32 to which the fastening object 50 is to be fastened. The sintering paste 41 contains metal particles, e.g. silver particles and / or copper particles. This ensures a high thermal conductivity of the subsequent sintered layer 40, which consists of the Sinter paste 41 is formed by pressure sintering. The sinter paste 41 contains at least one organic, volatile Component and is applied in a wet state. This facilitates the application of the sintering paste 41. The applied Sintered material can form a sintered layer with a thickness in the range of 80 µm to 200 µm, e.g., 150 µm ± V, where V 10 µm or 6 µm. The temporary sinter layer must not be mixed with the final pressure sinter layer 40 be confused.

[0095] In the embodiments shown, the attachment object 50 is a semiconductor power module. It comprises a direct bonded copper structure (DCB) 52. The DCB structure 52 has an insulation layer 54, which is formed by a ceramic substrate. The DCB structure 52 further comprises the integrated heat spreader 53, which directly attached to the insulation layer 54 at the interface side 51. On one side (along the normal direction N), which is opposite to the interface side 51, an internal electrical circuit layer 55 of the DCB structure 52 is directly connected to the insulating layer 54. The integrated heat spreader 53 is not to be connected to the intermediate heat spreader 30. confuse with.

[0096] In addition, the attachment object 50, e.g., the semiconductor power module according to Fig. 2, may comprise at least one Semiconductor component 57, e.g., a semiconductor switch, an insulated gate bipolar transistor (IGBT), a metal oxide Semiconductor field-effect transistor (MOSFET) and / or the like. The semiconductor component 57 may comprise a chip or consist of such a semiconductor component 57. The semiconductor component 57 can be attached to the DCB structure 52, e.g., by a internal pressure sintered layer 56. In some embodiments (not shown), the fastening object 50 may have several Semiconductor components 57. They can all be of the same type or of different types.

[0097] The fastening object 50 may further comprise connecting wires, for example a connecting wire 60 for electrical connection of the semiconductor component 57 with the internal electrical circuit layer 55, as shown in Fig. 2 and Fig. 3. Optionally, it may comprise a mechanical buffer layer 59 which is bonded to the corresponding semiconductor component 57 is attached. The bond buffer 59 can connect the semiconductor component 57 with respect to the corresponding semiconductor component 57. The bond buffer 59 can be formed, for example, by a further internal pressure sintering layer 58 on the corresponding semiconductor component 57.

[0098] The fastening object 50 may have electrical connectors 61. The electrical connectors 61 may serve to provide electrical connections with further attachments 50, e.g. further semiconductor power modules belonging to the same End assembly 200 (see Fig. 9) with several first stage subassemblies 80, each containing at least one semiconductor power module) and / or with other electrical components, e.g. a drive train circuit. In one embodiment, the electrical connector(s) 61 may be made of a Connection frame must be formed.

[0099] The fastening object 50 can be finished (delivered) as shown in Fig. 2. It can even already have a prefabricated resin cover 62' (shown in dashed lines in Fig. 2).

[0100] However, the manufacturing process may include one or more steps of shaping / manufacturing the fastening object 50.

[0101] For example, the manufacturing method may include a step S50 for forming the resin cover 62', 62 of the fastening object 50. The molding of the resin cover 62', 62 may comprise plastic transfer molding.

[0102] The resin cover 62' may be formed before the intermediate heat spreader 30 is pressure sintered to the Attachment object 50 is attached (see dashed line in Fig. 2). In this case, unlike in Fig. 1, the Step S50 must be performed before step S30.

[0103] The resin cover 62', 62 protects the internal components of the fastening object 50 from physical and / or chemical damage. In another embodiment, the fastening object 50 has no Resin cover 62', 62 on.

[0104] A step S30 relates to pressure sintering to form first stage subassembly 80 (see Fig. 3), in which the fortification object 50 is attached to the intermediate heat spreader 30 by the pressure sintered layer 40.

[0105] In Fig. 2, the arrow A1 symbolically illustrates the fixing of the intermediate heat spreader 30 to the Interface side 51 of the fastening object 50 by pressure sintering, whereby the pressure sintered layer 40 (see Fig. 3) between the interface side 51 and the object side 32 of the intermediate heat spreader 30. This occurs in Course of step S30.

[0106] The pressure sintered layer 40 in Fig. 3 is made from the sinter paste 41 shown in Fig. 2 on the object side 32 formed. Step S30 comprises a solidification step, which is carried out using a pressure sintering tool.

[0107] The solidification step may comprise applying pressure (e.g. by the pressure sintering tool) to the sintered material in a sintering pressure range of 10 MPa to 40 MPa, in one embodiment from 15 MPa to 30 MPa. It can have that the sintered material, especially during, an elevated temperature in the sintering temperature range from 200 °C to 300 °C. The temperature can be kept within the sintering temperature range and / or the applied pressure can be maintained in the sintering pressure range for a period of 2 minutes to 10 minutes.

[0108] A thickness of the resulting pressure sintered layer 40 may be in the range of 20 µm to 70 µm.

[0109] The pressure sintered layer 40 permanently and rigidly fixes the fastening object 50 to the intermediate heat spreader 30. It has a high thermal conductivity from the fastening object 50 (in particular from the integrated heat spreader 53) to the intermediate heat spreader 30.

[0110] According to a further aspect, step S30 may further comprise fixing the semiconductor component(s) 57 to the DCB- Structure 52 by pressure sintering and / or the bond buffer 59 on the corresponding semiconductor component 57 by In other words, one, several or all of the inner pressure sintered layers 56, 58 of the same Attachment object 50 can be formed together with the pressure sintered layer 40, in particular in a common solidification process and / or within the same pressure sintering tool.

[0111] Accordingly, step S20, which is directed to the application of sintering material, may comprise the provision of sintering material, e.g. sintering paste and / or sintering pad(s), for forming one, several or all of the inner pressure sintered layers 56, 58.

[0112] Of course, step S30 may involve arranging all components to be sintered in a Collocation and arranging the collocation into a pressure sintering tool.

[0113] Optionally, the manufacturing method may comprise a contacting and / or welding step S40 to Connecting wire(s) 60 and / or the electrical connector(s) 61. Of course, This must be done before the resin cover 62', 62 is formed.

[0114] It is possible to mold the resin cover 62 after step S30 (and optionally after step S40). This facilitates the formation of the inner pressure sintered layers 56, 58 within the fastening object 50 together with the Pressure sintering layer 40, in particular to solidify it entirely in a single solidification step.

[0115] During pressure sintering, heat must be applied to the sintering material. Typically, the resin cover 62, 62' only has limited thermal conductivity. Therefore, pressure sintering can be made simpler and more efficient if the resin cover 62 is formed after pressure sintering. The formation of the resin cover 62' before pressure sintering can but facilitate handling at a location where pressure sintering takes place.

[0116] Fig. 3 shows a first stage subassembly 80 which allows the attachment of the intermediate heat spreader 30 to the Interface side 51 of the fastening object 50 by pressure sintering, whereby the permanent and rigid Pressure sintering layer 40 is formed between the interface side 51 and the object side 32 of the intermediate heat spreader 30 In Fig. 3, the first stage subassembly 80 includes the optional resin cover 62.

[0117] Optionally, the manufacturing method comprises a step S60 in which the electrical properties of the Mounting object 50, e.g., the desired switching functionalities, must be checked. Since there is a certain risk that Components of the fastening object 50 are damaged during step S30 and / or step S40 (if applicable) step S50 may be performed thereafter. In other words, step S60 may be directed to electrical properties of the first stage subassembly 80.

[0118] Additionally or alternatively, the manufacturing method may include a step S70 for non-destructive measurement of the Pressure-sintered layer 40. Step S70 may include checking the quality of the pressure-sintered layer 40. The Testing may reveal voids in the pressure sintered layer 40, thickness variations of the pressure sintered layer 40 and / or Delaminations between the pressure sintered layer 40 and the interface side 51 or the object side 32.

[0119] A suitable exemplary measurement method is scanning acoustic microscopy (SAM) from the Base side 31 of the intermediate heat spreader 30. Acoustic test waves can be emitted from the base side 31 towards the Pressure sintered layer 40. Reflected acoustic wave components can be detected. The SAM can with a SAM head 90, as shown in Fig. 4. The SAM head 90 can be mounted on the base side 31 in an xy- plane perpendicular to the normal direction N. Of course, other approaches to achieving a spatial resolution in addition to or instead of it.

[0120] An evaluation unit 91 can automatically evaluate the signals acquired by the SAM head 90 in order to determine the quality of the pressure sintered layer 40. Optionally, a separation mechanism 92 can automatically separate each subassembly first stage 80, in which the quality of the pressure-sintered layer 40 is evaluated by the evaluation unit 91 is considered inadequate.

[0121] Since a configuration of the DCB structure 52 (in particular the integrated heat spreader 53 and the Insulation layer 54) is comparatively uniform in the xy plane, step S70 can even perform a non-destructive measurement the inner pressure sintered layer 56 in the same way.

[0122] Of course, step S70 must be performed after step S30 and before a step S100 explained below However, in a variation of Fig. 1, step S70 may be performed before any of steps S40, S50, S60, S80, S90 and S100 can be carried out.

[0123] The manufacturing method optionally comprises a step S80 in which the first stage subassembly 80 is connected to a other manufacturing facility. For example, at least step S30 can be carried out in a primary manufacturing facility, and step S80 is directed to producing the first subassembly of the first stage 80 to a secondary manufacturing facility. For example, steps S90 to S110 in Fig. 1 can be secondary manufacturing facility, e.g., in a customer's production facility that manufactures the subassemblies first stage to attach them to custom base components 10, 210.

[0124] Step S90 relates to the provision of the base component 10, 210. Fig. 5 shows an exemplary base component 10 in the form of a heat sink. This base component 10 is made of aluminum (including aluminum alloys). It has a side 12 to which the base side 31 of the intermediate heat spreader 30 is attached by soldering in step S100. This side can be called distribution side 12. A side 11 of the Base component 10, which can also be referred to as dissipation side 11, comprises a plurality of cooling fins 14, e.g. Pin ribs and / or elongated ribs.

[0125] In the embodiment shown in Fig. 5, a recess 13 is provided on the distributor side 12 for receiving the intermediate heat spreader 30. The size and shape of the recess 13 are designed to facilitate the fixation of the Support the first-stage subassembly 80 in a suitable position and orientation. A floor the recess 13 is flat.

[0126] In other modifications (not shown), the distributor side 12 may be at least substantially flat.

[0127] In step S100, the first stage subassembly 80 is soldered to the base component 10. This second This manufacturing step is symbolically represented by an arrow A2 in Fig. 6. Between the base side 31 of the Intermediate heat spreader 30 and the bottom of the corresponding recess 13 on the distributor side 12 of the base component 10, a solder material 21 is provided to be converted into the solder layer 20. The first stage subassemblies 80, the Soldering material 21 and the base component 10 are brought together in such a way that the base side 31 is on a first side along the normal direction N directly against the soldering material 21 and that the bottom of the recess 13 is at a second, the first side opposite side directly against the soldering material 21.

[0128] Fig. 7 shows an assembly 100 resulting from step S100. The fastening object 50 is Pressure sintering layer 40, the intermediate heat spreader 30 and the solder layer 20 are firmly connected to the base component 10. The Fastening object 50 is indirectly connected to the base component 10.

[0129] Compared to the solder layer 20, the pressure sintered layer 40 is less susceptible to damage by spatial and / or high temperature peaks that may occur during operation at the interface side 51. For example, Semiconductor component (the semiconductor components) 57, the connecting wire (the connecting wires) 60, the internal electrical Circuit layer 55 and / or the electrical connectors 61 generate heat during operation. Due to the internal structure of the fastening object 50, the heat is generated spatially unevenly. Since the operation of the attachment 50 involves the switching of electrical currents, e.g. B. of a drive circuit, the heat development can also be uneven over time.

[0130] The intermediate heat spreader 30 protects the solder layer 20 from high temperatures. Even with a constant Heat development during operation typically involves a temperature gradient along the normal direction N. The Temperatures at the base side 31 (and thus at the solder layer 20) are generally lower than at the Interface side 51 (and thus on the pressure sintered layer 40). In addition, the intermediate heat spreader 30 spatial and temporal heat peaks.

[0131] The assembly 100 can be designed for operation with high electrical currents and yet the Solder layer 20 produced by soldering without increased risk of failure during operation.

[0132] The intermediate heat spreader 30 can completely cover the interface side 51 of the fastening object 50, e.g. B. suitable as shown in Fig. 3. In particular, the intermediate heat spreader 30 can the integrated heat spreader 53 Furthermore, the pressure sintered layer 40 can completely cover at least the integrated heat spreader 53 (at the interface side 51). This enables optimal transmission of the forces from the fastening object 50 heat generated during operation to the intermediate heat spreader 30.

[0133] Typically, it is much easier for secondary manufacturing facilities to assemble components by soldering. than by pressure sintering. Less complex tools and machining are required. In addition, The described manufacturing process and assembly 80 allow lower quality requirements for the Solder layer 20.

[0134] The fixation directly on the interface side 51 is due to the high temperature peaks and the corresponding thermal stresses are the most critical. With the method described here, the more complex and difficult Process of pressure sintering a fixation layer directly adjacent to the interface side 51 (ie the pressure sintering layer 40) can be carried out centrally in a single primary production facility. Nevertheless, the first subassembly of the first stage 80 of the same type also in various secondary production facilities on simple Connect to various customer-specific base components 10, 210 by cost-effective soldering.

[0135] Apart from that, the pressure sintering step S30 is more efficient, flexible and cost-effective than the case where various customers attach objects directly to their customer-specific base components by pressure sintering It is not necessary to adapt the pressure sintering tool to the shape of the base component 10. In addition, the intermediate heat spreader 30 has a smaller thickness and / or a lower heat capacity than the base component 10. Therefore, the heating of the sintering material in step S30 can be done faster and with less energy than in cases where in which the pressure sintered layer is formed directly on the base component 10. In addition, the heat transfer from Pressure sintering tool in step S30 particularly high, since the base side 31 is flat and no cooling fins 14 with has gaps in between.

[0136] The thickness T of the intermediate heat spreader 30 may, for example, be in the range of 2 mm to 4 mm (see Fig. 3). On the one hand, the thickness T is large enough to ensure the advantageous shielding for the solder layer 20. On the other hand, it is thinner than the base component 10.

[0137] Compared to a case where fastening objects are fixed directly to a base component by pressure sintering the quality requirements for the solder layer 20 can be more easily checked non-destructively.

[0138] Step S110 relates to the non-destructive measurement of the solder layer 20. A suitable exemplary The measurement method is X-ray measurement. An X-ray source 95 can emit X-rays and the X-rays can penetrate the assembly 100 with the solder layer 20. The X-rays that penetrated the assembly 100 can be detected by an X-ray detector 96. The X-ray detector 96 can have a spatial resolution Of course, in addition to or instead of this, other methods can be used to achieve the spatial resolution be used.

[0139] An evaluation unit 97 can automatically evaluate the signals detected by the X-ray detector 96 in order to to determine the quality of the solder layer 20. Optionally, a rejection mechanism 98 can separate each assembly 100 whose Quality of the solder layer 20 is classified as insufficient by the evaluation unit 97, automatically display and / or carry out an elimination.

[0140] Fig. 9 shows another embodiment of the assembly 200 (semiconductor power module). The same Reference symbols for the same elements are used and the above explanations apply accordingly. Only the differences pointed out.

[0141] In Fig. 9, a base component 210 of the assembly 200 is a cooler. It comprises a channel structure with a fluid inlet 216, a fluid outlet 217 and inner fluid channels 215. Between adjacent fluid channels 215 are inner walls 214 trained.

[0142] The base member 210 may be configured to be cooled by a coolant, e.g., water.

[0143] However, step S100 may include heating the base component 210 for soldering by applying a hot fluid, e.g. B. Hot air, is passed through the channel structure. This is schematically represented by the arrow HF in Fig. 9.

[0144] According to a further aspect, the assembly 200 comprises three first-stage subassemblies 80. Each of them is attached to the base component 210 by soldering, which in particular comprises step S100. One, two or all of the First stage subassemblies 80 may be according to the embodiment shown in Fig. 3. Reference symbol: 10, 210 basic component 11 Dissipation side 12 Distribution page 13 Recess 14 cooling fins 20 solder layer 21 Soldering material 30 intermediate heat spreaders 31 Base page 32 Object page 40 pressure sintered layer 41 sinter paste (sinter material) 50 Mounting object (e.g. semiconductor power module) 51 Interface side 52 direct copper bonded (DCB) structure 53 integrated heat spreader 54 Insulation layer 55 internal electrical circuit layer 56, 58 internal pressure sintered layer 57 semiconductor component 59 Bond buffer / buffer layer 60 connecting wire 61 electrical connector 62', 62 resin cover 80 First stage subassembly 90 Acoustic Microscopy Head (SAM) 91, 97 Evaluation unit 92, 98 Excretion mechanism 95 X-ray source 96 X-ray detector 100, 200 assembly 214 Interior wall 215 inner fluid channel 216 Fluid inlet 217 Fluid outlet A1 Arrow (first level) A2 Arrow (second stage) HF arrow (hot fluid) N Normal direction T Thickness

Claims

1. Manufacturing method for fastening a fastening object (50) to a base component (10; 210), wherein the Procedure comprising the following steps: - providing an intermediate heat spreader (30) in addition to the fastening object (50); - Attaching the intermediate heat spreader (30) to an interface side (51) of the attachment object (50) by Pressure sintering, whereby a pressure sintered layer (40) is formed between the interface side (51) and an object side (32) of the intermediate heat spreader (30); and - Attaching the intermediate heat spreader (30) with the pressure-sintered attachment object (50) to the Base component (10; 210) by soldering, whereby a solder layer (20) is formed between the base component (10; 210) and a base side (31) of the intermediate heat spreader (30) which is opposite the object side (32).

2. Manufacturing process according to claim 1, characterized by: - a non-destructive measurement of the pressure sintered layer (40) and / or - Testing the electrical properties of the fastening object (50) after fastening the intermediate heat spreader (30) to the fastening object (50) by pressure sintering, but before fastening the intermediate heat spreader (30) with the pressure-sintered fastening object (50) to the base component (10; 210).

3. Manufacturing method according to claim 2, wherein the non-destructive measurement of the pressure sintered layer (40) is acoustic Microscopy of the pressure sintered layer (40).

4. Manufacturing process according to one of the preceding claims, characterized by: - non-destructive measurement of the solder layer (20) using X-rays.

5. Manufacturing process according to one of the preceding claims, characterized by: - Arranging a sintering pad and / or a sintering paste (41) between the intermediate heat spreader (30) and the Fastening object (50).

6. Manufacturing method according to one of the preceding claims, wherein the formation of the pressure sintered layer (40) sintering with a maximum sintering temperature in the range of 200 °C to 300 °C and with a maximum sintering pressure in the range from 10 MPa to 40 MPa.

7. Manufacturing method according to one of the preceding claims, wherein the base component consists of metal and a heat dissipator, a heat sink (10) and / or a cooler (210).

8. Manufacturing method according to one of the preceding claims, wherein the fastening object (50) comprises at least one which is or has the following elements: - a heat-generating component (55, 57, 59, 60, 61); - a semiconductor component (57); and - a semiconductor power module (50).

9. Manufacturing method according to one of the preceding claims, wherein the fastening object (50) is Interface side (51) has an integrated heat spreader (53), wherein the pressure sintered layer (40) Intermediate heat spreader (30) fixed to the integrated heat spreader (53).

10. Manufacturing method according to one of the preceding claims, wherein the fastening object (50) has a Insulation layer (54), an internal electrical circuit layer (55) attached to the insulation layer (54) and at least one attached to the insulation layer (54) and / or the internal electrical circuit layer (55) semiconductor component (57).

11. Manufacturing method according to one of the preceding claims, wherein the intermediate heat spreader (30) is made of copper is flat and has a thickness (T) in the range of 2 mm to 4 mm.

12. Manufacturing method according to one of the preceding claims, wherein a flat shape of the Intermediate heat spreader (30) adapted to a flat shape of the fastening object (50) on the interface side (51) becomes.

13. Manufacturing method according to one of the preceding claims, wherein the base component (10; 210) has a recess (13) which accommodates the intermediate heat spreader (30), wherein a shape of the recess (13) at least in the Essentially adapted to the planar shape of the intermediate heat spreader (30).

14. Assembly (100; 200) with a base component (10; 210) and a with respect to the base component (10; 210) fixed fortification object (50), characterized in that the assembly (100; 200) comprises an additional, between the base component (10; 210) and the fastening object (50) arranged heat spreader (30), wherein a pressure sintering layer (40) attaches an object side (32) of the intermediate heat spreader (30) to the fastening object (50) and a solder layer (20) connects a base side (31) of the intermediate heat spreader (30) opposite the object side (32) to the base component (10; 210).

15. The assembly (100; 200) according to claim 14, wherein the attachment object (50) is a semiconductor power module with at least one semiconductor component (50), wherein the base component is a heat sink, a heat sink (10) and / or a cooler (210).

16. The assembly (10; 210) according to claim 15, wherein the fastening object (50) further comprises - an integrated heat spreader (53) which is connected to the central heat spreader (30) by the pressure sintered layer (40) is attached - an insulating layer (54) attached to the integrated heat spreader (53), and - an internal electrical circuit layer (55) attached to the insulation layer (54), wherein the at least one Semiconductor component (57) is attached to the insulating layer (54) and / or the internal electrical circuit layer (55).

Citation Information

Patent Citations

  • process for low-temperature pressure sintering

    DE102008009510B3

  • Semiconductor device and method for manufacturing same

    US20190122955A1