Rare earth metal sintered magnet and process for its manufacture
A rare earth sintered magnet with controlled additions of nickel and other metals achieves high coercivity and remanence, overcoming the limitations of Dy scarcity and Al/Cu effects.
Patent Information
- Application Number
- DE112006000070
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2006-02-16
- Filing Date
- 2006-07-14
- Publication Date
- 2024-12-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The increasing demand for high-coercivity rare earth magnets, particularly for electric vehicle motors, is threatened by the scarcity of Dy and the adverse effects of adding Al and Cu, which enhance coercivity but reduce remanence.
A rare earth sintered magnet composition comprising specific amounts of rare earth elements, boron, and very small additions of nickel, silver, and optionally other metals like Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W, with controlled impurities, to achieve high coercivity without significantly reducing remanence.
The magnet exhibits coercivity comparable to conventional magnets with Cu or Al additions but with higher remanence, addressing the scarcity issue and maintaining performance.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Technical field
[0001] The present invention relates to a rare earth metal sintered magnet and to a method for manufacturing the magnet. Technical background
[0002] A rare earth metal sintered magnet based on rare earths, iron and boron, which is a typical high-performance permanent magnet, has a structure that includes a crystalline phase of R2Fe 14 -B-type (main phase), which is a tetragonal compound, and grain boundary phases, and it exhibits excellent magnetic properties. Its formula is R₂Fe₂ 14-B stands for R, representing at least one element selected from the rare earth elements and yttrium, and includes Nd and / or Pr as its main components. Fe stands for iron, B stands for boron, and these elements may be partially replaced by other elements. The grain boundary phases comprise an R-rich phase containing a rare earth element R in a relatively high concentration, and a B-rich phase containing boron in a relatively high concentration.
[0003] The rare-earth metal sintered magnet described here, based on rare-earth iron and boron, is referred to as an "RTB-based sintered magnet," where T stands for a transition metal element consisting primarily of iron. In the RTB-based sintered magnet, the R2T 14 The B-phase (main phase) is a ferromagnetic phase that contributes to magnetization, and the R-rich phase at the grain boundary is a low-melting non-magnetic phase.
[0004] A sintered magnet based on RTB (Real-Time Base) is produced by pressing and compacting a fine powder (with an average particle size of a few micrometers) of a (mother) alloy for the production of an RTB-based sintered magnet using a press, followed by sintering the resulting preform (green body or blank). The sintered blank is then subjected to an aging treatment, if necessary. The mother alloy for producing such an RTB-based sintered magnet is preferably produced using an ingot process involving die casting or a strip casting process in which a molten alloy is quenched using a cooling or quenching roller.
[0005] To produce an RTB-based sintered magnet with high coercivity, it is proposed to partially replace Nd or Pr, which is widely used as a rare earth element R, with a heavy rare earth element (heavy metal), such as Dy, Ho, and / or Tb (see, for example, patent document no. 1 below). Since Dy, Tb, and Ho are rare earth elements with strongly anisotropic magnetic fields, the coercivity can be effectively increased by replacing Nd with at least one of these elements in place of the rare earth element R in the main phase.
[0006] On the other hand, since the development of an RTB-based sintered magnet, a very small amount of Al or Cu has been added to improve the coercivity (see, for example, patent document no. 2 below). In particular, when an RTB-based sintered magnet was first developed, Al and Cu were considered impurities inevitably present in the base alloy (the parent alloy). Later, however, it was discovered that Al and Cu are actually almost essential elements that should be added to increase the coercivity of the RTB-based sintered magnet. It is also already known that if Al and Cu were intentionally eliminated, the coercivity of the RTB-based sintered magnet would be too low for its use in various applications.
[0007] Patent documents Nos. 5 and 6 also state that vanadin (V) is preferably added to sufficiently increase the coercive force.
[0008] Patent documents Nos. 7 to 11 also describe rare earth metal sintered magnets to which various metal elements have been added. Patent document no. 1: Published Japanese patent application no. JP S6 0 - 32 306 Patent document no. 2: Published Japanese patent application no. JP H05 - 234 733 A Patent document no. 3: Published Japanese patent application no. JP H04 - 217 302 A Patent document no. 4: published Japanese patent application no. S60 - 138 056 A Patent document no. 5: Published Japanese patent application no. JP 2004 - 277 795 A Patent document no. 6: Japanese patent no. JP 2 787 580 B2 Patent document no. 7: Published Japanese patent application no. JP S59-89401A Patent document no. 8: Published Japanese patent application no. JP S59 - 132 104 A Patent document no. 9: Published Japanese patent application no. JP H01 - 220 803 A Patent document no. 10: published Japanese patent application no. H05 - 205 927 A Patent document no. 11: Published Japanese patent application no. JP 2003 - 17 308 A Patent document JP H04 - 293 206 A relates to a rare earth Fe-B magnet containing one or more of Ag, Au, Pt, Sn or Zn. Patent document JP S63 - 241 141 A relates to a Fe-BRM ferromagnetic alloy, wherein R is Nd and / or Pr and M is one or more of Ti, Ni, Bi, V, Nb, Ta, Cr, MO, W, Mn, Al, Sb, Ge, Sn, Zr and Hf. Patent document JP H02 - 3 206 A relates to a permanent magnet made of rare earth elements and iron of the composition RFeBM, where R is a rare earth element and M is Cu, Ag, Au or Zn. Patent document WO 2005 / 043 558 A1 relates to a rare earth sintered magnet containing a rare earth element, a transition metal and boron, and one or more additional additive metals. Description of the invention: Problems to be solved according to the invention
[0009] The higher the added amount of Dy, Tb, or Ho, the higher the coercivity (coercive field strength) can be. However, Dy, Tb, and Ho are very rare elements. This means that if the demand for high-melting-point (refractory) magnets for use in electric vehicle motors continues to increase due to the growing popularity of electric vehicles in the near future, Dy resources will soon be nearly depleted. In this case, a serious problem would arise regarding a potential increase in material costs. For this reason, it is an urgent task to develop a method for reducing the amount of Dy used in high-coercivity magnets. While the addition of Al, Cu, and V also increases the coercivity, they reduce the remanence B. r , which is also a problem.
[0010] To solve or overcome the problems described above, a main objective of the present invention is to provide a rare earth metal sintered magnet that has a coercivity as high as that of a magnet to which Al or Cu has been added, and that has a higher remanence than such a magnet. Means to solve the problems
[0011] A rare-earth metal sintered magnet according to the invention comprises 12.0 to 15.0 atomic percent of one or more rare-earth elements, wherein at least one element is selected from the group consisting of Nd, Pr, Gd, Tb, Dy, and Ho, and comprises at least 50 percent Nd and / or Pr; 5.5 to 8.5 atomic percent boron (B); a predetermined percentage of an additive metal A; and iron (Fe), as well as unavoidable impurities contained therein as the remainder. The predetermined percentage of additive metal A comprises 0.005 to 0.20 atomic percent nickel, wherein the unavoidable impurities contained include aluminum, the content of which is 0.4 atomic percent or less.
[0012] In yet another preferred embodiment, the magnet also contains 0.05 to 1.0 atomic percent of element M, which is at least one element selected from the group consisting of Ti, V, Cr, Zr, Nb, Mo, Hf, Ta and W.
[0013] A method for producing a rare-earth metal sintered magnet (rare-earth sintered magnet) according to the present invention comprises the following steps: producing or providing an alloy containing 12.0 to 15.0 atomic percent of one or more rare-earth elements, wherein at least one element is selected from the group consisting of Nd, Pr, Gd, Tb, Dy, and Ho, and comprising at least 50 percent Nd and / or Pr; 5.5 to 8.5 atomic percent boron (B); a predetermined percentage of an additive metal A; and iron (Fe), as well as unavoidable impurities contained therein as a residue, and wherein the predetermined percentage of additive metal A comprises 0.005 to 0.20 atomic percent nickel (Ni); pulverizing the alloy to produce a powder and sintering the powder, wherein the unavoidable impurities contained therein comprise Al, the content of which is 0.4 atomic percent or less.
[0014] In a preferred embodiment, the alloy also contains 0.05 to 1.0 atomic % of an element M, which is at least one element selected from the group consisting of Ti, V, Cr, Zr, Nb, Mo, Hf, Ta and W.
[0015] Another method for producing a rare-earth metal sintered magnet (rare-earth sintered magnet) according to the present invention comprises the following steps: producing or providing an alloy containing 12.0 to 15.0 atomic percent of one or more rare-earth elements, wherein at least one element is selected from the group consisting of Nd, Pr, Gd, Tb, Dy and Ho, and comprising at least 50% Nd and / or Pr; 5.5 to 8.5 atomic percent boron (B); and iron (Fe), as well as unavoidable impurities contained therein as residue; pulverizing the alloy to produce a powder; Addition of 0.005 to 0.20 atomic percent nickel (Ni) to the powder to produce a powder containing a very small amount of an additive element, and sintering the powder containing the very small amount of the additive element, in which the unavoidable impurities contained include Al, the content of which is 0.4 atomic percent or less.
[0016] In a preferred embodiment, 0.05 to 1.0 atomic percent of an element M, which is at least one element selected from the group consisting of Ti, V, Cr, Zr, Nb, Mo, Hf, Ta and W, is added to the powder containing the very small amount of an additive element.
[0017] Another process for producing a rare-earth metal sintered magnet (rare-earth sintered magnet) according to the present invention comprises the following steps: (A) producing or providing an alloy powder for producing a rare-earth metal magnet, wherein the powder contains 12.0 to 15.0 atomic percent of one or more rare-earth elements, comprising at least one element selected from the group consisting of Nd, Pr, Gd, Tb, Dy, and Ho, and comprising at least 50% Nd and / or Pr; 5.5 to 8.5 atomic percent boron (B); and iron (Fe), as well as unavoidable impurities present as the remainder, wherein a lubricant is added to the powder; and (B) producing a pellet from the alloy powder and sintering the pellet. The lubricant comprises an aliphatic silver carboxylate or an aromatic silver carboxylate.
[0018] In a preferred embodiment, the amount of aliphatic silver carboxylate or aromatic silver carboxylate added is adjusted so that the rare earth metal sintered magnet contains 0.005 to 0.20 atomic % Ag.
[0019] In yet another preferred embodiment, stage (A) of the manufacture or provision of the alloy powder comprises the following stages: (a1) manufacture or provision of an alloy for the manufacture of a rare-earth metal magnet (rare-earth magnet), wherein the alloy contains 12.0 to 15.0 atomic percent of one or more rare-earth elements, wherein the rare-earth element is at least one element selected from the group consisting of Nd, Pr, Gd, Tb, Dy, and Ho, and comprising at least 50 percent Nd and / or Pr; 5.5 to 8.5 atomic percent boron (B); and iron (Fe), as well as unavoidable impurities present as a residue; (a2) manufacture of a coarsely powdered alloy; (a3) manufacture of a finely powdered alloy from the coarsely powdered alloy; and (a4) addition of a lubricant to the powder between steps (a2) and (a3) or after step (a3).
[0020] In yet another preferred embodiment, the aliphatic silver carboxylate or the aromatic silver carboxylate has 6 to 20 carbon atoms.
[0021] In yet another preferred embodiment, the unavoidable impurities contained therein include Al, the content of which is 0.4 atomic percent or less. Effect of the invention
[0022] Thanks to the effect of the very small amount of the additive ANi, a rare earth metal sintering magnet according to the invention (rare earth sintering magnet) can have as high a coercive force (coercive field strength) as a conventional sintering magnet based on R-Fe-B, Cu or Al, and can also have a higher remanence than such a magnet. Brief description of the drawings Fig. Figure 1 represents a diagram showing how the magnetic power changes with the added amount of Ag, with the coercive force H on the left side of the ordinate. cJ (kA / m), represented by O, is given, and on the ordinate on the right-hand side the remanence B r (T), represented by +, is specified. Fig. 2 represents a diagram showing how the coercive force H changes cJ with the amount of Ag added, where O indicates the results obtained with the addition of Ag metal powder, and X indicates the results obtained with the addition of Ag2O powder. Fig. Figure 3 presents a diagram showing how the remanence B r changes with the amount of Al added. Fig. Figure 4 shows a diagram illustrating how the coercive force H changes. cJ changes with the amount of Ag added. Fig. Figure 5 shows a diagram illustrating how the coercive force H changes. cJ changes with the added amount of element M. Fig. Figure 6 presents a diagram showing how the magnetic power changes with the amount of Ag added, with the coercive force H on the ordinate on the left side. cJ (kA / m), represented by +, is given, and on the ordinate on the right-hand side is the remanence B. r (T), represented by □, is specified. Fig. Figure 7 presents a diagram showing how the remanence B r changes with the added amount of Al. Fig. Figure 8 shows a diagram illustrating how the magnetic power changes with the amount of Ni added, with the coercive force H on the left side of the ordinate. cJ (kA / m), represented by O, is given, and on the ordinate on the right-hand side the remanence B r (T), represented by +, is specified. Fig. Figure 9 shows a diagram illustrating how the coercive force H changes. cJ with the added amount of Ni, where O indicates the results obtained with the addition of Ni metal powder, and X indicates the results obtained with the addition of NiO powder. Fig. Figure 10 presents a diagram showing how the remanence B r changes with the added amount of Al. Fig. Figure 11 presents a diagram showing how the magnetic power changes with the amount of Au added, with the coercive force H on the left side of the ordinate. cJ (kA / m), represented by O, is given, and on the ordinate on the right-hand side the remanence B r (T), represented by +, is specified. Fig. 12 presents a diagram showing how the remanence B r changes with the added amount of Al. Best way of implementing the invention
[0023] In the prior art, attempts were made to increase the coercivity by adding various elements. However, the RTB-based sintered magnets under comparison contained aluminum and copper as unavoidable impurities. This is because, without these elements, the resulting coercivity would be too low.
[0024] Nevertheless, the inventors of the present invention ventured to use a simple ternary composition, to which no Al or Cu had been added, for a sintered magnet based on Nd-Fe-B, and they experimented with adding various elements in very small quantities. As a result, the inventors of the present invention found that when a very small amount of Ag, Ni, or Au was added, the effect was a significant increase in coercivity without a decrease in remanence, thus giving rise to the basic idea of the present invention. It was also found that a beneficial effect was achieved in the form of a further increase in coercivity by adding not only these elements in very small quantities, but also by adding at least one element selected from the group consisting of Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W.
[0025] It is not the case that no one in the prior art had attempted to add silver to RTB-based sintered magnets. For example, patent documents 2, 3, and 4 describe the addition of silver to RTB-based sintered magnets, albeit for a different purpose. Patent documents 7, 8, and 9 also state that nickel was added to RTB-based sintered magnets. Patent documents 10 and 11 state that gold was added to RTB-based sintered magnets.
[0026] However, the RTB-based sintered magnets to which these elements were added contained Al and Cu, which were either intentionally added or present as unavoidable impurities. Therefore, the effect of increased coercivity achieved by adding a very small amount of Ni was masked by the effect of increased coercivity achieved by adding Al, Cu, or Dy, and was therefore not detectable. Furthermore, the effects produced by adding very small amounts of these elements, which were first observed by the inventors of the present invention, cannot be achieved unless the amounts added are very small and within very narrow ranges, as explained in more detail below. These effects could therefore not be adequately achieved when the elements were added in the amounts described in patent documents No.2, 3 and 4 are indicated.
[0027] It is evident from this that the present invention, which is based on these new findings, could not have been made if the RTB-based sintered magnet with the basic composition had not been used as a comparative example and if Ni had not been added in a very small quantity. For the sake of simplicity, the element Ni, which is to be added in a very small quantity according to the invention, is referred to below as "additive metal A".
[0028] According to the results of experiments carried out by the inventors of the present invention, the additive metal A is present at the grain boundary phase of a sintered magnet. It is known that the grain boundary phase of an RTB-based sintered magnet plays a key role in determining the magnitude of its coercivity. It was therefore assumed that the very small amount of additive metal A would have some effect on increasing the coercivity in the grain boundary phase. However, at that time it was not entirely clear how and why the coercivity increased with such a small amount of the additive, although the inventors of the present invention made considerable efforts to elucidate the mechanism.
[0029] In a preferred embodiment, Ag can be mixed with the alloy powder in the form of a lubricant without being added to the base alloy itself. By adding a lubricant containing either an aliphatic silver carboxylate or an aromatic silver carboxylate, the Ag contained in the silver salt of the lubricant diffuses into the particles of the alloy powder during the sintering process, thereby improving the properties of the resulting sintered magnet.
[0030] Preferred embodiments of a rare earth metal sintering magnet according to the invention (rare earth sintering magnets) are described in more detail below. Design of base alloy (mother alloy)
[0031] First, a base alloy (master alloy) is produced or provided, containing 12.0 to 15.0 atomic percent of a rare earth element R, 5.5 to 8.5 atomic percent of B, a predetermined percentage of the additive metal A, and iron, along with any unavoidable impurities present. R represents at least one element selected from the group consisting of Nd, Pr, Gd, Tb, Dy, and Ho, and at least 50% of R comprises Nd and / or Pr. The predetermined percentage of the additive metal A contains 0.005 to 0.20 atomic percent of Ni. Optionally, 0.05 to 1.0 atomic percent of the element M may also be added, which is at least one element selected from the group consisting of Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W.
[0032] If the molar amounts of R and B are outside these ranges, the RTB-based sintered magnet loses its basic structure and the desired magnetic performance cannot be achieved. According to the invention, by adding a very small amount of the additive metal A, the coercive force (coercive field strength) can be more than doubled, while the remanence hardly increases, compared to a rare-earth metal magnet based on R-Fe-B with a ternary basic composition. If the molar fraction of the additive metal A is below 0.005 atomic percent, the coercive force cannot increase significantly. Conversely, if the molar fraction of the additive metal A exceeds the upper limit of the specified range, the coercive force will tend to decrease. Based on the results of experiments carried out by the inventors of the present invention, the molar fraction of Ni is set to be within the range of 0.005 to 0.20 atomic percent.
[0033] It should be noted that when the molar fraction of element M exceeds 1.0 atomic percent, the coercive force increases, but the remanence decreases significantly. Therefore, when element M is added, its molar fraction is preferably set to be within the range of 0.05 to 1.0 atomic percent, and particularly preferably within the range of 0.1 to 0.5 atomic percent.
[0034] The additive metal A and the element M can be added at any time prior to the sintering process. That is, these elements can be added while the base alloy (parent alloy) is being melted. Alternatively, a parent alloy containing neither additive metal A nor element M can be produced or provided, and then elements A and M can either be added to the alloy, which is to be pulverized by a jet mill, or they can be added to the alloy once it has been pulverized into fine powders. As another alternative, a parent alloy containing only additive metal A can be produced or provided, which is then pulverized by a jet mill, and a fine powder of element M can then be added to the pulverized powder. In yet another alternative, the parent alloy containing only element M can be produced or provided...The material is prepared, pulverized using a jet mill, and then a fine powder of additive metal A can be added to the pulverized powder. That is, it is not necessary to add additive metal A and element M simultaneously.
[0035] The fine powder of additive metal A can be produced by pulverizing either nickel metal or a compound thereof, such as a metal oxide. The powder or compound of additive metal A can have an average particle size of, for example, 0.5 to 50 µm. This is because, if the powder or compound has a particle size within this range, a suitable sintered body can still be obtained even when the powder or compound is mixed with any other alloy powder. The same applies to the powder of element M as well as to the powder of additive metal A. The powder or compound of element M can have an average particle size of, for example, 0.5 to 50 µm.
[0036] It should be noted that the sintered magnet according to the invention may contain Al and / or Cu as unavoidable impurities. However, the higher the Al content, the lower the remanence. For this reason, the Al content is preferably adjusted to a value of 0.4 atomic percent or less.
[0037] To produce a mother alloy (base alloy) for use in the manufacture of a sintered magnet according to the invention, an ingot casting process or a quenching process (for example, a strip casting process or a centrifugal casting process) can be used. A process for producing a mother alloy (base alloy) using a strip casting process is described below by way of example.
[0038] First, a molten alloy is produced by melting an alloy with the composition specified above in an argon atmosphere using an induction melting process. This molten alloy is then held at 1350 °C and rapidly cooled (quenched) by a single-roll process, yielding alloy flakes approximately 0.3 mm thick. This rapid solidification process can be carried out at a roller peripheral speed of approximately 1 m / s, a cooling rate of 500 °C / s, and a subcooling temperature of 200 °C. The rapidly solidified alloy block obtained in this way is pulverized into flakes 1 to 10 mm in size before undergoing a subsequent hydrogen pulverization process.Such a method for producing a mother alloy (base alloy) using a strip casting process is described, for example, in US patent no. 5,383,978.
[0039] The additive metal A or element M may either already have been added to the mother alloy (base alloy) or it may be added during the pulverization process described below. Coarse pulverization process
[0040] The mother alloy block, which has been coarsely pulverized into flakes, is then placed in a hydrogen furnace and subjected to a hydrogen decrepitation process (occasionally referred to here as a "hydrogen pulverization process") within the furnace. Once the hydrogen pulverization process is complete, the coarsely pulverized alloy powder is transferred from the hydrogen furnace to an inert atmosphere to prevent exposure to air. This prevents oxidation or heat generation of the coarsely pulverized powder and improves the magnetic properties of the resulting magnet.
[0041] As a result of this hydrogen pulverization process, the rare-earth metal alloy is pulverized to particle sizes of approximately 0.1 to several mm, with an average particle size of 500 µm or less. After hydrogen pulverization, the decrepitated parent alloy is preferably further comminuted to finer particle sizes and cooled using a cooling system, such as a rotary chiller. If the parent alloy still has a relatively high temperature, it is then removed and cooled for an extended period using a rotary chiller or other suitable device. Lubricant addition process
[0042] Ag can be added by adding a lubricant containing a predetermined amount of aliphatic silver carboxylate or aromatic silver carboxylate to the coarsely powdered material produced by hydrogen pulverization, and the powder and lubricant can be mixed together. By adjusting the amount of aliphatic silver carboxylate or aromatic silver carboxylate such that the resulting sintered magnet contains 0.005 to 0.20 atomic percent Ag, the same effects can be achieved as those obtained by adding Ag by another method.
[0043] Examples of carboxylic acids used to form silver salts include straight-chain saturated fatty acids, such as caprylic acid, capric acid, lauric acid, and stearic acid, as well as aromatic carboxylic acids, such as benzoic acid and tert-butylbenzoic acid. These silver carboxylates can be used individually or in combination with two or more. Alternatively, a different, non-silver lubricant can be added. The essential requirement is that the amount of silver in the resulting sintered magnet remains within the predetermined range specified above. To achieve this, zinc stearate can be added to the coarsely powdered material, followed by a lubricant containing silver stearate to the finely powdered material.It should be noted that with aliphatic silver carboxylate or with aromatic silver carboxylate containing fewer than six carbon atoms, the effects expected from the addition of the lubricant cannot be fully achieved. Conversely, if the number of carbon atoms exceeds 20, the increase in carbon content can lead to insufficient sinter density or deteriorated magnetic performance. To minimize this deterioration in magnetic performance resulting from an excess of carbon, the amount of lubricant added or retained is preferably adjusted so that the carbon concentration of the resulting sintered magnet does not exceed 2000 ppm.
[0044] According to the invention, the sintered magnet must contain an Ag molar fraction within the range of 0.005 to 0.20 atomic percent. However, the amount of lubricant added for this purpose changes precisely when the lubricant is added. If silver stearate is added prior to the fine pulverization process as described below, approximately 0.03 to approximately 1.23 wt.% silver stearate can be added to the alloy powder. The amount of lubricant added can be adjusted appropriately so that the resulting sintered magnet contains an Ag molar fraction within the range of 0.005 to 0.20 atomic percent when the Ag content is determined.
[0045] The lubricant described above is solid at room temperature and therefore does not need to be mixed as a powder. The particle size of the lubricant can be adjusted, for example, to be in the range of 1 to 50 µm. Fine pulverization process
[0046] The coarsely pulverized powder is then finely pulverized using a jet mill pulverizer. For use in this preferred embodiment, a cyclone classifier is connected to the jet mill pulverizer. The jet mill pulverizer is fed with the rare-earth metal alloy that has been coarsely pulverized in the initial pulverization process (i.e., with the coarsely pulverized powder), and the powder is further pulverized by the pulverizer. The powder pulverized in the pulverizer is then collected in a collection tank by means of the cyclone classifier. In this way, a finely pulverized powder with particle sizes of approximately 0.1 to approximately 20 µm can be obtained. The pulverizer used in such a fine pulverization process need not be a jet mill, but can also be a friction mill or a ball mill. Press compaction process
[0047] In this embodiment, 0.3 wt% lubricant was added and mixed in a vibrating mixer with the magnetic powder produced according to the above-described method, thereby coating the surface of the alloy powder particles with the lubricant. The magnetic powder produced according to the above-described method is then compacted under an aligning magnetic field using a known pressing device. The aligning magnetic field to be applied can have a strength of, for example, 1 Tesla (T).
[0048] If Ag is added, a lubricant containing the silver carboxylate described above can be added after the fine pulverization process. Alternatively, the lubricant described above can be added only after the fine pulverization process, without adding any lubricant before the fine pulverization process. As a further alternative, only a known lubricant can be added before the fine pulverization process, and then a lubricant containing an aliphatic silver carboxylate or an aromatic silver carboxylate can be added after the fine pulverization process. Sintering process
[0049] The powder pellet described above is preferably subjected successively to a process in which the pellet is exposed to a temperature of 650 to 1000 °C for 10 to 240 minutes, and then to a process in which the pellet is further sintered at a higher temperature (e.g., 1000 to 1100 °C) than in the preceding process. Particularly when a liquid phase forms during the sintering process (i.e., when the temperature is in the range of 650 to 1000 °C), the rhodium-rich phase at the grain boundary begins to melt, forming the liquid phase. The sintering process then continues, potentially resulting in the formation of a sintered magnet. The sintered magnet can be subjected to an aging treatment if necessary.
[0050] If necessary, before being subjected to the sintering process, the powder compact can be subjected to a binder removal process in which the compact is held for approximately 30 to 300 minutes within a hydrogen atmosphere at a temperature of 200 to 500 °C (hereinafter referred to as the "hydrogen binder removal process"). By carrying out such a process, the carbon in the lubricant reacts with hydrogen, and the lubricant is removed as a hydrocarbon. As a result, the amount of carbon that was contained in the lubricant and remains in the sintered magnet can be reduced. When such a hydrogen binder removal process is carried out, a larger quantity of lubricant can be added.
[0051] Specific examples of the present invention are described in more detail below. Example 1 (not according to the invention)
[0052] An alloy was produced consisting essentially of 14.1 atomic percent Nd, 6.1 atomic percent B, 0.05 to 0.6 atomic percent Ag, 0.05 atomic percent Al, and Fe as the remainder. As Example 1, a sintered magnet was produced from this alloy using the manufacturing process already described in the preferred embodiments. Furthermore, as Comparative Example 1, a parent alloy with the same composition as in Example 1, except that no Ag was added, was also produced using the same process as in Example 1.
[0053] Before pressing and compaction, the powder had an average particle size of 4.4 µm. The compaction process was carried out under a magnetic field of 1.0 T. The resulting compact was subjected to a sintering process at a temperature of 1000 to 1100 °C for 4 h and then to an aging treatment for 2 h at a temperature of 620 °C. The resulting sintered body had a rectangular, parallelepiped (cuboid) shape with dimensions of 11 mm x 10 mm x 18 mm.
[0054] The Fig. Figure 1 shows a diagram illustrating how the magnetic power changes with the amount of Ag added, with the ordinate on the left side representing the coercive force H. cJ (kA / m), represented by O, indicates, and the ordinate on the right side indicates the remanence B. r (T), represented by +, indicates.
[0055] As from the Fig. As can be seen, the coercivity H can be increased by adding only 0.05 atomic percent Ag. cJ more than doubled compared to a value of 340 kA / m in the reference example (to which no Ag had been added), reaching approximately 930 kA / m. In the Fig. In the example shown, the coercive force H is reached cJ Its peak value is reached when approximately 0.1 atomic percent Ag has been added. Once the added amount of Ag exceeds 0.3 atomic percent, further additions of Ag produce virtually no effect. On the other hand, the remanence B changes. r Hardly any effect occurs if the amount of Ag added is 0.3 atomic percent or less. However, if the amount of Ag added exceeds the upper limit, the remanence B increases. r gradually decreases.
[0056] According to the results of more detailed experiments, it was found that the effects to be achieved by adding Ag occurred when the amount of Ag added was at least 0.005 atomic percent. This is why, according to the invention, the amount of Ag added is adjusted to a value within the range of 0.005 to 0.3 atomic percent. Example 2 (not according to the invention)
[0057] An alloy was produced consisting essentially of 14.1 atomic percent Nd, 6.1 atomic percent B, and Fe as the remainder. In Example 2 and Comparative Example 2, sintered magnets were produced from the alloy using the manufacturing process already described with reference to the preferred embodiments. In Example 2, 0.02 to 0.5 atomic percent Ag powder was added to the alloy powder before it was pressed and compacted. In Comparative Example 2, on the other hand, no Ag powder was added. The Ag was mixed with the alloy powder either as Ag metal powder or as Ag₂O powder.
[0058] Before pressing and compaction, the powder had an average particle size of 4.6 µm. The compaction process was carried out under a magnetic field of 1.0 T. The resulting compact was subjected to a sintering process at a temperature of 1000 to 1100 °C for 4 hours and then to an aging treatment at a temperature of 620 °C for 2 hours. The resulting sintered body had a rectangular parallelepiped shape with dimensions of 11 mm x 10 mm x 18 mm.
[0059] The Fig. 2 represents a diagram showing how the coercive force H cJ changes with the amount of Ag added, where O indicates the results obtained when Ag metal powder was added, and X indicates the results obtained when Ag2O powder was added.
[0060] If you look at the ones in the Fig. 1 and Fig. Comparing the two results shown, it can be seen that the same effects can be achieved by adding a very small amount of Ag, regardless of when the Ag is added. That is, the Ag can be added either to the alloy that is yet to be pulverized or to the pulverized powder. As also shown in the Fig. As is easily seen in Figure 2, the Ag can be added either in the form of an Ag compound, for example as Ag oxide, or in the form of Ag metal. Example 3 (not according to the invention)
[0061] An alloy was produced consisting essentially of 14.1 atomic% Nd, 6.1 atomic% B, 0.1 atomic% Ag, 0.05 to 0.5 atomic% Al and Fe as the remainder, and sintered magnets were produced from the alloy as Example 3 and as Comparative Example 3 using the manufacturing process as already described in connection with preferred embodiments.
[0062] Before pressing and compaction, the powder had a mean particle size of 4.6 µm. The compaction process was carried out under a magnetic field of 1.0 T. The resulting compact was subjected to a sintering process for 4 hours at a temperature of 1000 to 1060 °C and then to an aging treatment for 2 hours at a temperature of 600 to 640 °C. The resulting sintered body had a rectangular parallelepiped shape with dimensions of 11 mm x 10 mm x 18 mm.
[0063] The Fig. Figure 3 presents a diagram showing how the remanence B r The magnetization changes with the amount of Al added. It can be seen that when the amount of Al added exceeds 0.40 atomic percent, the saturation magnetization decreases too much to achieve the effects expected when a very small amount of Ag is added. Example 4 (not according to the invention)
[0064] An alloy was prepared consisting essentially of 11.4 atomic percent Nd, 2.8 atomic percent Pr, 6.1 atomic percent B, 0.1 atomic percent Ag, and Fe as the remainder, and a sintered magnet was produced from this alloy as Example 4 using the same procedure as applied in Example 1. The magnetic properties of Example 4 included a coercive force H cJ of 1.035 kA / m and a Br remanence of 1.39 T. This confirmed that the present invention was also effective when another rare earth element, such as Pr, was additionally added together with Nd. Example 5 (not according to the invention)
[0065] An alloy was produced consisting essentially of 14.1 atomic percent Nd, 6.1 atomic percent B, 0.005 to 0.30 atomic percent Ag, 0.4 atomic percent Mo, and Fe as the remainder. A sintered magnet was produced from this alloy, as described in Example 5, using the manufacturing process already described in connection with preferred embodiments. Simultaneously, a comparative example 4 was also produced from a parent alloy with the same composition as in Example 5, except that no Ag or element M was added, using the same process as applied to Example 5.
[0066] Before pressing and compaction, the powder had an average particle size of 4.4 µm. The compaction process was carried out under a magnetic field of 1.0 T. The resulting compact was subjected to a sintering process for 4 hours at a temperature of 1000 to 1100 °C and then to an aging treatment for 2 hours at a temperature of 620 °C. The resulting sintered body had a rectangular parallelepiped shape with dimensions of 11 mm x 10 mm x 18 mm.
[0067] The Fig. Figure 4 shows a diagram illustrating how the coercive force H changes. cJ (kA / m) changes with the amount of Ag added, where the data for the example to which 0.4 atomic % Mo had been added are represented in the diagram by ■, and the data relating to the comparison example to which no Mo had been added are represented by ◊.
[0068] From the Fig. 4 shows that by adding only 0.05 atomic percent Ag the coercive force H cJ The value can be more than doubled compared to approximately 340 kA / m (when no Ag was added), reaching approximately 930 kA / m in both the example and the comparison example. In the example in Fig. In the example shown, the coercive force H is reached. cJ Its peak value is reached when approximately 0.1 atomic percent Ag has been added. However, once the added amount of Ag exceeds 0.3 atomic percent, virtually no effects can be achieved, even with further additions of Ag.
[0069] From the Fig. 4 It is also evident that the coercive force can be further increased by adding not only Ag, but also 0.4 atomic % Mo.
[0070] According to the results of more detailed experiments, it was found that the increase in coercivity achieved by adding a very small amount of Ag was further enhanced by the addition not only of Mo, but also of at least one element selected from the group consisting of Ti, V, Nb, and W. It was also confirmed that the effects achieved by adding these elements M occurred when the molar fraction of Ag was in the range of 0.005 to 0.30 atomic percent. Example 6 (not according to the invention)
[0071] An alloy was produced consisting essentially of 14.1 atomic percent Nd, 6.1 atomic percent B, 0.1 atomic percent Ag, 0.05 to 1.0 atomic percent of element M (which is at least one element selected from the group consisting of Ti, V, Nb, Mo, and W), and iron as the remainder. A sintered magnet, Example 6, was produced from this alloy using the manufacturing process already described, for example, in connection with preferred embodiments. Simultaneously, a comparative example 5 was also produced from a parent alloy with the same composition as in Example 6, but without the addition of element M, using the same process as applied to Example 6.
[0072] Before pressing and compaction, the powder had an average particle size of 4.4 µm. The compaction process was carried out under a magnetic field of 1.0 T. The resulting compact was subjected to a sintering process for 4 hours at a temperature of 1000 to 1100 °C and then to an aging treatment for 2 hours at a temperature of 620 °C. The sintered body obtained in this way had a rectangular parallelepiped shape with dimensions of 11 mm x 10 mm x 18 mm.
[0073] The Fig. Figure 5 shows a diagram illustrating how the coercive force H changes. cJ (kA / m) changes with the added quantity of the element M. In the Fig. 5 represents the ordinate, the coercive force H cJ (kA / m) represents.
[0074] As from the Fig. As can be seen in section 5, the coercivity H can be increased by adding only about 0.1 atomic % Ti, V, Nb, Mo or W. cJfrom approximately 950 kA / m of comparison example 5, to which 0.1 atomic percent Ag was added. In the Fig. In the example shown in Figure 5, the coercive force H also increased with increasing amount of the added element M. cJ to.
[0075] According to the results of more detailed experiments, it was found that the effects that can be achieved by adding element M were evident when the amount of element M added was in the range of 0.05 to 1.0 atomic percent.
[0076] As far as remanence is concerned, the rare earth metal magnets of Examples 5 and 6 of the present invention were comparable to a conventional rare earth metal magnet based on R-Fe-B to which Cu or Al had been added.
[0077] The inventors have also confirmed that the same effects were achieved not only by adding element M in the examples given above, but also by using Cr, Zr, Hf or Ta as an alternative element M. Example 7
[0078] An alloy was produced consisting essentially of 14.1 atomic percent Nd, 6.1 atomic percent B, 0.05 atomic percent Al, and iron as the remainder. A sintered magnet, known as Example 7, was produced from this alloy using the manufacturing process already described in connection with the preferred embodiments. In Example 7, 0.12 to 0.3 wt. percent silver stearate was added as a lubricant. In contrast, zinc stearate was added to Comparative Example 6 instead of silver stearate.
[0079] Before pressing and compaction, the powder had a mean particle size of 4.4 ± 0.2 µm. The compaction process was carried out under a magnetic field of 1.7 T. The resulting compact was subjected to a sintering process for 4 hours at a temperature of 1000 to 1100 °C and then to an aging treatment for 2 hours at a temperature of 500 to 700 °C. The resulting sintered body had a rectangular parallelepiped shape with dimensions of 20 mm x 50 mm x 12 mm.
[0080] The Fig. Figure 6 presents a diagram showing how the magnetic power changes with the amount of Ag added, with the coercive force H on the left side of the ordinate. cJ (kA / m), represented by +, is given, and on the ordinate on the right-hand side is the remanence B. r (T), represented by □, is specified.
[0081] As from the Fig. As can be seen in section 6, the coercivity H can be increased by adding only 0.02 atomic percent Ag. cJ more than double the value of approximately 340 kA / m in the comparison example (to which no Ag was added), reaching approximately 880 kA / m. Although not in the Fig. As shown in Figure 6, the magnetic power decreases when the amount of Ag added exceeds 0.2 atomic % and virtually no effects are achieved if more Ag is added.
[0082] According to the results of more detailed tests, it was found that the desired effects of adding silver were achieved when the amount of silver added was at least 0.005 atomic percent. This is why the amount of silver added is adjusted to a range of 0.005 to 0.2 atomic percent. The amount of silver added is also controlled by adjusting the amount of lubricant added. Therefore, if the amount of silver added is increased, the carbon content in the lubricant also increases. However, the higher the carbon content, the greater the likelihood that the performance of the sintered magnet will decrease (deteriorate). For this reason, when the amount of lubricant added is increased, a step is preferably carried out before the sintering process in which the lubricant is sufficiently evaporated.When the binder removal procedure described above is carried out, the lubricant may be added in such a way that the amount of Ag added may be 0.2 atomic percent. Example 8
[0083] An alloy was produced consisting essentially of 14.1 atomic percent Nd, 6.1 atomic percent B, 0.02 to 0.5 atomic percent Al, and Fe as the remainder. A sintered magnet was then produced from this alloy using the manufacturing process already described in connection with preferred embodiments. Prior to fine pulverization and the use of a jet mill, 0.12 wt. percent silver stearate was added to Example 8 as a lubricant. The total amount of Ag added was thus 0.02 atomic percent of the entire sintered magnet.
[0084] Before pressing and compaction, the powder had a mean particle size of 4.4 ± 0.2 µm. The compaction process was carried out under a magnetic field of 1.7 T. The resulting compact was subjected to a sintering process for 4 h at a temperature of 1000 to 1100 °C and then to an aging treatment for 2 h at a temperature of 500 to 650 °C. The resulting sintered body had a rectangular parallelepiped shape with dimensions of 20 mm x 50 mm x 12 mm.
[0085] The Fig. Figure 7 presents a diagram showing how the remanence B r with the amount of Al added. It can be seen from this that when the amount of Al added exceeds 0.40 atomic percent, the remanence B r decreases, which may destroy the effects achieved by adding a very small amount of Ag. Example 9
[0086] An alloy was produced consisting essentially of 14.1 atomic percent Nd, 6.1 atomic percent B, 0.05 to 0.6 atomic percent Ni, 0.05 atomic percent Al, and Fe as the remainder. A sintered magnet, Example 9, was produced from this alloy using the manufacturing process already described in connection with preferred embodiments. Simultaneously, a comparative example 7 was also produced from a parent alloy having the same composition as in Example 9, except that no Ni was added, using the same process as in Example 9.
[0087] Before pressing and compaction, the powder had an average particle size of 4.4 to 4.6 µm. The compaction process was carried out under a magnetic field of 1.0 T. The resulting compact was subjected to a sintering process for 4 hours at a temperature of 1000 to 1100 °C and then to an aging treatment for 2 hours at a temperature of 580 to 660 °C. The resulting sintered body had a rectangular parallelepiped shape with dimensions of 11 mm x 10 mm x 18 mm.
[0088] The Fig. Figure 8 shows a diagram illustrating how the magnetic power changes with the amount of Ni added, with the coercive force H on the left side of the ordinate. cJ (kA / m), represented by O, is given, and on the ordinate on the right-hand side the remanence with B r (T), represented by ◆, is specified.
[0089] As from the Fig. As can be seen in Figure 8, the coercivity H can be increased by adding only 0.05 atomic percent Ni. cJ more than double the value of approximately 340 kA / m in comparison example 7 (to which no Ni had been added), reaching approximately 800 kA / m. In the Fig. In the example shown, the coercive force H is achieved. cJ Its peak value is reached when approximately 0.05 atomic percent of Ni has been added. However, if the added amount of Ni exceeds 0.4 atomic percent, the effect achieved by adding Ni gradually decreases. On the other hand, the remanence B changes. r hardly at all if the amount of Ni added is 0.4 atomic percent or less.
[0090] Based on the results of more detailed experiments, it was found that the effects achievable by adding Ni are obtained when the added amount of Ni is at least 0.005 atomic percent. This is why the added amount of Ni is adjusted to a value within the range of 0.005 to 0.4 atomic percent. Example 10
[0091] An alloy was produced consisting essentially of 14.1 atomic percent Nd, 6.1 atomic percent B, and iron as the remainder. Sintered bodies were produced from this alloy using the manufacturing process described in connection with preferred embodiments, as shown in Example 10 and Comparative Example 8. In Example 10, 0.02 to 0.5 atomic percent Ni powder was added to the alloy powder before pressing and compaction. In Comparative Example 8, on the other hand, no Ni powder was added at all. The Ni was mixed with the alloy powder either as Ni-metal powder or as NiO powder.
[0092] Before pressing and compaction, the powder had an average particle size of 4.6 µm. Pressing and compaction were carried out under a magnetic field of 1.0 T. The resulting compact was subjected to a sintering process for 4 hours at a temperature of 1000 to 1100 °C and then to an aging treatment for 2 hours at a temperature of 580 to 620 °C. The resulting sintered body had a rectangular, parallelepiped shape with dimensions of 11 mm x 10 mm x 18 mm.
[0093] The Fig. Figure 9 shows a diagram illustrating how the coercive force H changes. cJ with the amount of Ni added, where O shows the results obtained when Ni metal powder was added, and X shows the results obtained when NiO powder was added.
[0094] From a comparison of the in the Fig. 8 and Fig. The results presented in Figure 9 show that the same effects are achieved by adding a very small amount of Ni, regardless of when it is added. That is, Ni can either be added to the alloy yet to be pulverized or it can be added to the pulverized powder. From the Fig. 9 It is also easily evident that Ni can be added either in the form of a Ni compound, such as Ni oxide, or in the form of Ni metal. Example 11
[0095] An alloy was produced which essentially consisted of 14.1 atomic% Nd, 6.1 atomic% B, 0.05 atomic% Ni, 0.05 to 0.5 atomic% Al and Fe as the remainder, and sintered magnets were produced from the alloy using the manufacturing process as already described in connection with preferred embodiments, as Example 11 and as Comparative Example 9.
[0096] Before pressing and compaction, the powder had an average particle size of 4.5 to 4.7 µm. The compaction process was carried out under a magnetic field of 1.0 T. The resulting compact was subjected to a sintering process for 4 hours at a temperature of 1000 to 1060 °C and then to an aging treatment for 2 hours at a temperature of 600 to 620 °C. The resulting sintered body had a rectangular, parallelepiped shape with dimensions of 11 mm x 10 mm x 18 mm.
[0097] The Fig. Figure 10 presents a diagram showing how the remanence B r The magnetization changes with the amount of Al added. It can be seen that if the amount of Al added exceeds 0.40 atomic percent, the saturation magnetization decreases too much to achieve the expected effects when a very small amount of Ni is added. Example 12
[0098] An alloy was prepared consisting essentially of 11.4 atomic percent Nd, 2.8 atomic percent Pr, 6.1 atomic percent B, 0.05 atomic percent Ni, and Fe as the remainder. A sintered magnet was then produced from this alloy, as Example 12, using the same procedure as in Example 9. The magnetic properties of Example 12 include a coercive force H cJ of 855 kA / m and a remanence B r of 1.39 T. It was thus confirmed that the invention is sufficiently effective even when another rare earth element, such as Pr, is added in addition to Nd. Example 13 (not according to the invention)
[0099] An alloy was produced consisting essentially of 14.0 atomic percent Nd, 6.0 atomic percent B, 0.01 to 0.3 atomic percent Au, 0.05 atomic percent Al, and Fe as the remainder. A sintered magnet, designated Example 13, was produced from this alloy using the manufacturing process already described in connection with preferred embodiments. Simultaneously, a comparative example 10 was produced from a parent alloy having the same composition as Example 13, except that no Au was added, using the same process as had been used to produce Example 13.
[0100] Before pressing and compaction, the powder had an average particle size of 4.4 to 4.6 µm. The compaction process was carried out under a magnetic field of 1.5 T. The resulting compact was subjected to a sintering process for 4 hours at a temperature of 1000 to 1100 °C and then to an aging treatment for 2 hours at a temperature of 500 to 700 °C. The resulting sintered body had a rectangular, parallelepiped shape with dimensions of 20 mm x 50 mm x 15 mm.
[0101] Fig. Figure 11 presents a diagram showing how the magnetic power changes with the amount of Au added, with the coercive force H on the ordinate on the left side. cJ (kA / m), represented by O, is given, and on the ordinate on the right-hand side the remanence B r (T), represented by +, is specified.
[0102] As from the Fig. As can be seen in section 11, the coercivity H can be increased by adding only 0.01 atomic percent Au. cJ more than doubled from approximately 340 kA / m in comparison example 10 (to which no Au was added) to approximately 890 kA / m. In the Fig. In the example shown, the coercive force H is reached cJ Its peak value is reached when approximately 0.01 atomic percent of Au has been added. However, if the added amount of Au exceeds 0.3 atomic percent, virtually no effects are achieved, even with further additions of Au. On the other hand, the remanence B decreases with increasing amount of added Au. r gradually decreases.
[0103] According to the results of more detailed experiments, it was found that the effects achieved by adding Au were observed when the molar fraction of Au was at least 0.005 atomic percent. This is why, according to the invention, the amount of Au added is adjusted to a value within the range of 0.005 to 0.2 atomic percent. Example 14 (not according to the invention)
[0104] An alloy was produced which essentially consisted of 14.0 atomic% Nd, 6.0 atomic% B, 0.05 atomic% Au, 0.05 to 0.5 atomic% Al and Fe as the remainder, and sintered magnets were produced from the alloy using the manufacturing process as already described in connection with preferred embodiments, as Example 14 and as Comparative Example 11.
[0105] Before pressing and compaction, the powder had an average particle size of 4.4 to 4.6 µm. The compaction process was carried out under a magnetic field of 1.5 T. The resulting compact was subjected to a sintering process for 4 hours at a temperature of 1000 to 1060 °C and then to an aging treatment for 2 hours at a temperature of 550 to 650 °C. The resulting sintered body had a rectangular, parallelepiped shape with dimensions of 20 mm x 50 mm x 15 mm.
[0106] The Fig. 12 presents a diagram showing how the remanence B rwith the amount of Al added. It can be seen that when the amount of Al added exceeds 0.4 atomic percent, the saturation magnetization becomes almost equal to that of a magnet with a conventional composition containing the additives Al and Cu, thereby possibly negating the effects caused by the addition of a very small amount of Au. Example 15 (not according to the invention)
[0107] An alloy was prepared consisting essentially of 11.2 atomic percent Nd, 2.8 atomic percent Pr, 6.0 atomic percent B, 0.05 atomic percent Au, and Fe as the remainder. A sintered magnet was then produced from this alloy, as Example 15, using the same manufacturing process as Example 14. The magnetic properties of Example 15 included a coercive force H cJ of 929 kA / m and a remanence B rof 1.41 T. It was thus confirmed that the present invention was sufficiently effective even when another rare earth element, such as Pr, was added together with Nd.
[0108] The results of the specific examples described above show that even more pronounced effects were achieved with the addition of Ag than with any other additive metal A. The effects increase in the order Ni, Au and Ag. Industrial applicability
[0109] A rare-earth metal sintered magnet according to the invention exhibits a coercivity as high as that of a conventional rare-earth metal sintered magnet based on R-Fe-B to which Cu and / or Al have been added, and it exhibits a higher remanence than the conventional sintered magnet. The rare-earth metal sintered magnet according to the invention can therefore be effectively used in various applications where both coercivity and remanence are required.
Claims
[1] Rare earth metal sintered magnet comprising: 12.0 to 15.0 atomic% of one or more rare earth elements, which is at least one element selected from the group consisting of Nd, Pr, Gd, Tb, Dy and Ho, and which comprises at least 50% Nd and / or Pr; 5.5 to 8.5 atomic% boron (B); a predetermined percentage of an additive metal A; and Iron (Fe) and unavoidable impurities contained therein as residue, wherein the specified percentage of additive metal A comprises 0.005 to 0.20 atomic% nickel (Ni), in which the unavoidable impurities contained therein include Al whose content is 0.4 atomic% or less. [2] A rare earth metal sintered magnet according to claim 1, further comprising 0.05 to 1.0 atomic% of an element M which is at least one element selected from the group consisting of Ti, V, Cr, Zr, Nb, Mo, Hf, Ta and W. [3] A process for producing a rare earth sintered magnet comprising the following steps: Providing (manufacturing) an alloy containing 12.0 to 15.0 atomic % of one or more rare earth elements, which is at least one element selected from the group consisting of Nd, Pr, Gd, Tb, Dy and Ho, and which comprises at least 50% Nd and / or Pr; 5.5 to 8.5 atomic% boron (B); a predetermined percentage of an additive metal A and iron (Fe) and unavoidable impurities contained therein as the remainder, wherein the predetermined percentage of additive metal A comprises 0.005 to 0.20 atomic% nickel (Ni); pulverising the alloy to produce a powder and Sintering of the powder, in which the unavoidable impurities contained therein include Al whose content is 0.4 atomic% or less. [4] The method of claim 3, wherein the alloy further contains 0.05 to 1.0 atomic% of an element M, which is at least one element selected from the group consisting of Ti, V, Cr, Zr, Nb, Mo, Hf, Ta and W. [5] A process for producing a rare earth sintered magnet comprising the following steps: Production (provision) of an alloy containing 12.0 to 15.0 atomic% of one or more rare earth elements, which is at least one element selected from the group consisting of Nd, Pr, Gd, Tb, Dy and Ho, and which comprises at least 50% Nd and / or Pr; 5.5 to 8.5 atomic% boron (B) and iron (Fe) and the remainder of any unavoidable impurities contained therein; pulverizing the alloy to produce a powder; Adding 0.005 to 0.20 atomic% of nickel (Ni) to the powder to thereby produce a powder containing a very small amount of the additive element, and Sintering the powder containing the very small amount of the additive element, in which the unavoidable impurities contained therein include Al whose content is 0.4 atomic% or less. [6] The method according to claim 5, wherein 0.05 to 1.0 atomic% of the element M, which is at least one element selected from the group consisting of Ti, V, Cr, Zr, Nb, Mo, Hf, Ta and W, is further added to the powder containing the very small amount of an additive element. [7] A process for producing a rare earth sintered magnet comprising the following steps: (A) Producing (providing) an alloy powder for producing a rare earth magnet, the powder containing 12.0 to 15.0 atomic % of one or more rare earth elements, which is at least one element selected from the group consisting of Nd, Pr, Gd, Tb, Dy and Ho, and comprising 50% Nd and / or Pr; 5.5 to 8.5 atomic % boron (B) and iron (Fe) and unavoidable impurities contained therein as the remainder, wherein a lubricant is added to the powder, and (B) preparing a compact from the alloy powder and sintering the compact, wherein the lubricant comprises an aliphatic silver carboxylate or an aromatic silver carboxylate. [8] The method according to claim 7, wherein the amount of the aliphatic silver carboxylate or the aromatic silver carboxylate added is adjusted so that the rare earth sintered magnet contains 0.005 to 0.20 atomic% of Ag. [9] A method according to claim 7, wherein step (A) of preparing (providing) the alloy powder comprises the following steps: (a1) Providing an alloy for producing a rare earth magnet, the alloy containing 12.0 to 15.0 atomic % of one or more rare earth elements, which is at least one element selected from the group consisting of Nd, Pr, Gd, Tb, Dy and Ho, and comprising 50% Nd and / or Pr; 5.5 to 8.5 atomic % boron (B); and iron (Fe) with inevitable impurities contained therein as the balance; (a2) producing a coarsely pulverised powder from the alloy; (a3) producing a finely pulverized powder from the coarsely pulverized powder of the alloy; and (a4) Addition of a lubricant to the powder between steps (a2) and (a3) or after step (a3). [10] The process according to claim 7, wherein the aliphatic silver carboxylate or the aromatic silver carboxylate contains 6 to 20 carbon atoms. [11] A method according to claim 7, wherein the unavoidable impurities contained therein include Al whose content is 0.4 atomic% or less.
Citation Information
Patent Citations
Permanent magnet
JP1984132104A
Material for sintered magnet
JP1985138056A
Magnetic anisotropic sintered magnet and manufacture thereof
JP1989220803A
Ag containing sintered magnet excellent in corrosion resistance
JP1992217302A
Rare earth element transition metal base permanent magnet and manufacturing method thereof
JP1993205927A