glove

A glove with a balanced composition of anionic polyurethane and specific additives achieves both wear resistance and flexibility, addressing the limitations of existing rubber-based gloves, suitable for industrial use.

DE112016004944B4Active Publication Date: 2024-12-05DIC CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
DE112016004944
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2015-10-30
Filing Date
2016-09-06
Publication Date
2024-12-05
Estimated Expiration
2036-09-06

AI Technical Summary

Technical Problem

Existing gloves made from synthetic or natural rubber materials with elasticity often cause allergies and lack both wear resistance and flexibility, while aqueous polyurethane compositions that enhance wear resistance through increased aromatic ring concentration or urea bonds compromise flexibility.

Method used

A glove made from a coagulated film of an aqueous polyurethane composition containing anionic polyurethane with specific oxyalkylene and urea bond contents, formulated to balance wear resistance and flexibility, using a composition of polyol, glycol, chain extender, and polyisocyanate, and adjusted with a neutralizing agent for optimal properties.

Benefits of technology

The resulting glove exhibits excellent wear resistance and flexibility, suitable for various industrial applications, including chemical and food industries, with improved durability and comfort.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Glove comprising a coagulated film of an aqueous polyurethane composition containing anionic polyurethane (A) having an oxyalkylene group content in the range of 4 to 12 mol / kg and a urea binding content of 0.2 mol / kg or less, and an aqueous medium (B), wherein the anionic polyurethane (A) is the reaction product of a polyol containing polyoxyalkylene polyol, a glycol with a carboxyl group, a chain extender and a polyisocyanate and the acid value of the aqueous polyurethane composition is in the range of 5 to 19 mg KOH / g.
Need to check novelty before this filing date? Find Prior Art

Description

Technical area

[0001] The present invention relates to a glove that satisfies both wear resistance and flexibility. Background of the invention

[0002] Synthetic rubber and natural rubber such as cis-1,4-polypropylene and the like, which are generally used as materials with elasticity, have the risk of causing allergy by contact, and thus relatively flexible urethane resins with rubber elasticity are widely used for application on gloves.

[0003] On the other hand, with the recent influence of the increasing social tendency to demand environmentally conscious products, the change from solvent-type urethane resins to aqueous urethane resins is also required in the application to gloves.

[0004] Gloves are used in various chemical industry applications and therefore require high wear resistance, not to mention rubber elasticity. It has been disclosed that, to improve wear resistance, the aromatic ring concentration of waterborne polyurethane is increased or a urea bond is incorporated into waterborne polyurethane by chain extension with a diamine compound (see, for example, Patent Literature 1). However, it is noted that this method cures films and thus exhibits poor flexibility.

[0005] WO 2004 / 041892 A1 describes the preparation of stable aqueous poly(urea / urethane) polymers and dispersions that do not require chain extenders, curing agents, or crosslinking agents. The disclosed poly(urea / urethane) dispersions can be used to manufacture articles such as films and gloves that reduce the likelihood of chemical and biological allergic reactions on the skin and exhibit improved puncture and tear resistance compared to articles made from other materials.

[0006] WO 2015 / 012117 A1 relates to a glove characterized in that it is produced using a water-based urethane resin composition which forms a solidified film having a 100% modulus of 5 MPa or less in a tensile strength test carried out under the conditions of a temperature of 23°C, a humidity of 60% and a crosshead speed of 300 mm / min, and having an area swelling ratio of 160% or less when immersed in toluene for 24 hours under the conditions of a temperature of 23°C. Citation listPatent literature

[0007] PTL 1: International Publication No. 2013 / 018478 Summary of the inventionTechnical problem

[0008] A problem to be solved by the present invention is to provide a glove that satisfies both wear resistance and flexibility. Solution to the problem

[0009] The present invention provides a glove having a coagulated film of an aqueous polyurethane composition comprising: an anionic polyurethane (A) having an oxyalkylene group content in a range of 4 to 12 mol / kg and a urea bond content of 0.2 mol / kg or less, and an aqueous medium (B), wherein the anionic polyurethane (A) is the reaction product of a polyol containing polyoxyalkylene polyol, a glycol having a carboxyl group, a chain extender and a polyisocyanate and wherein the acid number of the aqueous polyurethane composition is in a range of 5 to 19 mg KOH / g. Advantageous effects of the invention

[0010] A glove of the present invention has excellent wear resistance and flexibility and can therefore be preferably used in various fields such as chemical industry, food industry, etc. Description of embodiments

[0011] An aqueous polyurethane composition used in the present invention contains an anionic polyurethane (A) having an oxyalkylene group content in a range of 4 to 12 mol / kg and a urea bond content of 0.2 mol / kg or less, and an aqueous medium (B), wherein the anionic polyurethane (A) is the reaction product of a polyol containing polyoxyalkylene polyol, a glycol having a carboxyl group, a chain extender and a polyisocyanate and wherein the acid number of the aqueous polyurethane composition is in a range of 5 to 19 mg KOH / g.

[0012] From the viewpoint of achieving excellent wear resistance and flexibility, the anionic polyurethane (A) must have an oxyalkylene group content in a range of 4 to 12 mol / kg, and preferably in a range of 5 to 11.5 mol / kg. An oxyalkylene group content of more than 12 mol / kg reduces the strength of a film and thus causes poor wear resistance, while an oxyalkylene group content of less than 4 mol / kg hardens a film and thus causes poor flexibility.

[0013] The oxyalkylene group is supplied by a polyoxyalkylene polyol used as the starting material for the anionic polyurethane (A). The oxyalkylene group content of the anionic polyurethane (A) refers to the content of the oxyalkylene group supplied by the polyoxyalkylene polyol relative to the total mass of the raw materials constituting the anionic polyurethane (A).

[0014] From the perspective of achieving excellent wear resistance and flexibility, the anionic polyurethane (A) must have a urea bond content of 0.2 mol / kg or less, and preferably 0.15 mol / kg or less. A urea bond content exceeding 0.2 mol / kg will harden the film due to the strengthening of hydrogen bonds, thus causing poor wear resistance and flexibility.

[0015] The urea bond is generated by reaction with a polyisocyanate when a chain extender having an amino group is used as the starting material of the anionic polyurethane (A), and by reaction of the polyisocyanate with an amino group generated by reacting an isocyanate group with water. Therefore, the urea bond content in the anionic polyurethane (A) can be adjusted by adjusting the amount of the chain extender having an amino group used and by completely urethanizing the isocyanate before an emulsification process. The urea bond content refers to a value calculated by the following general formula (1). [Math. 1] Urea binding content (mol / kg) = (number of moles of amino group) + (number of moles of isocyanate group−number of moles of hydroxyl group−number of moles of amino group) / 2 mass of polyol + mass of glycol with carboxyl group + mass of polyisocyanate + mass of chain extender

[0016] In particular, the anionic polyurethane (A) is the reaction product of a polyol containing polyoxyalkylene polyol, a glycol having a carboxyl group, a chain extender and a polyisocyanate.

[0017] Usable examples of the polyoxyalkylene polyol include polyoxyethylene glycol, polyoxypropylene glycol, polyoxytetramethylene glycol, polyoxyethylene polyoxypropylene glycol, polyoxyethylene polyoxytetramethylene glycol, polyoxypropylene polyoxytetramethylene glycol, and the like. These polyoxyalkylene polyols can be used alone or in combination with two or more. Among them, polyoxytetramethylene glycol is preferred in view of achieving good wear resistance due to its high strength.

[0018] In view of flexibility and ease of production, the number-average molecular weight of the polyoxyalkylene polyol is preferably in a range of 500 to 5,000, and more preferably in a range of 700 to 4,000. The number-average molecular weight of the polyoxyalkylene polyol refers to a value measured by gel permeation chromatography (GPC) under the following conditions. Measuring device: High-speed GPC device (“HLC-8220GPC”, manufactured by Tosoh Corporation)

[0019] Column: The following columns manufactured by Tosoh Corporation were connected in series and used. "TSKgel G5000" (7.8m ID × 30cm)×1 "TSKgel G4000" (7.8m ID × 30cm)×1 "TSKgel G3000" (7.8m ID × 30cm)×1 "TSKgel G2000" (7.8m ID × 30cm)×1 Detector: RI (Differential Refractometer) Column temperature: 40 °C Eluent: Tetrahydrofuran (THF) Flow rate: 1.0 ml / min Injection volume: 100 µl (tetrahydrofuran solution at a sample concentration of 0.4 mass%) Standard sample: A calibration curve was constructed using the following standard polystyrene. (Standard polystyrene) “TSKgel Standard Polystyrene A-500”, manufactured by Tosoh Corporation “TSKgel Standard Polystyrene A-1000”, manufactured by Tosoh Corporation “TSKgel Standard Polystyrene A-2500”, manufactured by Tosoh Corporation “TSKgel Standard Polystyrene A-5000”, manufactured by Tosoh Corporation “TSKgel Standard Polystyrene F-1”, manufactured by Tosoh Corporation “TSKgel Standard Polystyrene F-2”, manufactured by Tosoh Corporation “TSKgel Standard Polystyrene F-4”, manufactured by Tosoh Corporation “TSKgel Standard Polystyrene F-10”, manufactured by Tosoh Corporation “TSKgel Standard Polystyrene F-20”, manufactured by Tosoh Corporation “TSKgel Standard Polystyrene F-40”, manufactured by Tosoh Corporation “TSKgel Standard Polystyrene F-80”, manufactured by Tosoh Corporation “TSKgel Standard Polystyrene F-128”, manufactured by Tosoh Corporation “TSKgel Standard Polystyrene F-288”, manufactured by Tosoh Corporation “TSKgel Standard Polystyrene F-550”, manufactured by Tosoh Corporation

[0020] If necessary, the polyoxyalkylene polyol can be used in combination with a polyol other than the polyol. Examples of the other polyol include polyester polyol, polycarbonate polyol, polyacrylic polyol, polybutadiene polyol, and the like. These polyols can be used alone or in combination with two or more. When the other polyol is used, polyester polyol and / or polycarbonate polyol are preferably used in view of good mechanical-physical properties.

[0021] The glycol with a carboxyl group imparts an anionic group to the urethane, and usable examples include 2,2'-dimethylolpropionic acid, 2,2'-dimethylolbutanoic acid, 2,2'-dimethylolbutyric acid, 2,2'-dimethylolbutanoic acid, 2,2'-dimethylolbutanoic acid, valeric acid, and the like. These compounds can be used alone or in combination of two or more.

[0022] The carboxyl group may be partially or completely neutralized with a basic compound in the aqueous polyurethane composition. Examples of the basic compound include organic amines such as ammonia, trimethylamine, pyridine, morpholine, and the like; alkanolamines such as monoethanolamine and the like; metal-basic compounds containing sodium, potassium, lithium, calcium, or the like; and the like.

[0023] The chain extender has a number-average molecular weight within a range of 50 to 450, and usable examples thereof include chain extenders each having an amino group, such as ethylenediamine, 1,2-propanediamine, 1,6-hexamethylenediamine, piperazine, 2,5-dimethylpiperazine, isophoronediamine, 1,2-cyclohexanediamine, 1,3-cyclohexanediamine, 1,4-cyclohexanediamine, 4,4'-dicyclohexylmethanediamine, 3,3'-dimethyl-4,4'-dicyclohexylmethanediamine, hydrazine, and the like; Chain extenders each having a hydroxyl group, such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, hexamethylene glycol, sucrose, methylene glycol, glycerin, sorbitol, bisphenol A, 4,4'-dihydroxydiphenyl, 4,4'-dihydroxydiphenyl ether, trimethylolpropane, and the like; and the like. These chain extenders can be used alone or in combination of two or more.Among them, a chain extender having a hydroxyl group is preferably used to prevent the curing of a coagulated film and achieve excellent wear resistance and flexibility, and ethylene glycol or butanediol is more preferably used from the viewpoint of forming a hard segment with a suitable chain length and achieving excellent wear resistance and flexibility. From the viewpoint of achieving better wear resistance by crystallization, the amount of the chain extender used is preferably in a range of 0.01 to 8 mass%, and more preferably in a range of 0.01 to 5 mass%, of the total mass of the raw materials of the anionic polyurethane (A).

[0024] Usable examples of the polyisocyanate include aromatic polyisocyanates such as phenylene diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, naphthalene diisocyanate, polymethylene polyphenyl polyisocyanate, carbodiimidized diphenylmethane polyisocyanate, and the like; aliphatic or alicyclic polyisocyanates such as hexamethylene diisocyanate, lysine diisocyanate, cyclohexane diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, xylylene diisocyanate, tetramethylxylylene diisocyanate, dimer acid diisocyanate, norbornene diisocyanate, and the like; and the like. These polyisocyanates can be used alone or in combination of two or more.Among them, an aromatic polyisocyanate is preferably used from the viewpoint of achieving excellent wear resistance and flexibility, and diphenylmethane diisocyanate or toluene diisocyanate is more preferably used, and diphenylmethane diisocyanate is still more preferably used from the viewpoint of forming a hard segment having an appropriate chain length and achieving excellent wear resistance and flexibility.

[0025] The anionic polyurethane (A) can be prepared by, for example, mixing the polyol, the glycol having a carboxyl group, the chain extender and the polyisocyanate without solvent or in the presence of an organic solvent and carrying out the urethanization reaction at a reaction temperature of, for example, 50 °C to 100 °C for 3 to 10 hours.

[0026] The anionic polyurethane (A) can also be prepared by, for example, mixing the polyol, the glycol having a carboxyl group and the polyisocyanate without a solvent or in the presence of an organic solvent, conducting a reaction at a reaction temperature of 50 °C to 100 °C for 3 to 10 hours to produce a urethane prepolymer having an isocyanate group at its molecular terminal and then reacting the urethane prepolymer with the chain extender.

[0027] The [isocyanate group / hydroxyl group] (molar ratio) in the reaction of the polyol, the glycol having a carboxyl group, the chain extender and the polyisocyanate is preferably within a range of 0.9 to 1.1, and more preferably within a range of 0.93 to 1.05.

[0028] Examples of an organic solvent that can be used for preparing the anionic polyurethane (A) include ketone solvents such as acetone, methyl ethyl ketone, and the like; ether solvents such as tetrahydrofuran, dioxane, and the like; ester solvents such as ethyl acetate, butyl acetate, and the like; nitrile solvents such as acetonitrile, and the like; amide solvents such as dimethylformamide, N-methylpyrrolidone, and the like; and the like. The organic solvents can be used alone or in combination of two or more.

[0029] From the viewpoint of preventing the formation of precipitates and thus achieving excellent product stability, the average particle diameter of the anionic polyurethane (A) is preferably in a range of 0.01 to 1 µm, and more preferably in a range of 0.05 to 1 µm 0.9 µm. A method for measuring the average particle diameter of the anionic polyurethane (A) will be described later in Examples.

[0030] From the viewpoint of achieving excellent flexibility and wear resistance, the weight-average molecular weight of the anionic polyurethane (A) is preferably in a range of 10,000 to 1,000,000, and more preferably in a range of 30,000 to 500,000. The weight-average molecular weight of the anionic polyurethane (A) refers to a value measured by the same method as for the number-average molecular weight of the polyoxyalkylene polyol.

[0031] From the viewpoint of achieving excellent flexibility and wear resistance, the urethane bond content in the anionic polyurethane (A) is preferably in a range of 500 mmol / kg to 3,500 mmol / kg, and more preferably in a range of 700 mmol / kg to 3,000 mmol / kg, based on the total anionic polyurethane (A). The urethane bond content in the anionic polyurethane (A) refers to the content of a urethane bond structure in raw materials relative to the total mass of the raw materials constituting the anionic polyurethane (A).

[0032] From the viewpoint of achieving excellent wear resistance, the aromatic ring content in the anionic polyurethane (A) is preferably in a range of 550 mmol / kg to 2500 mmol / kg, and more preferably in a range of 800 mmol / kg to 2200 mmol / kg, based on the total anionic polyurethane (A). The aromatic ring content in the anionic polyurethane (A) refers to the content of an aromatic ring in the raw materials relative to the total mass of the raw materials constituting the anionic polyurethane (A). In the calculation, the molecular weight of each of a benzene ring and a naphthalene ring, excluding an organic group, is used as the molecular weight of an aromatic ring.For example, in the case of toluene, the molecular weight of a benzene ring with 5 hydrogen atoms without a methyl group is used; in the case of diphenylmethane diisocyanate, the molecular weight of a benzene ring with four hydrogen atoms without an isocyanate group and a methylene group is used; and in the case of toluene diisocyanate, the molecular weight of a benzene ring with four hydrogen atoms without two methyl groups is used.

[0033] From the viewpoint of achieving good viscosity and coating processability, the content of the anionic polyurethane (A) in the aqueous polyurethane composition is preferably in a range of 10% to 60% by mass, and more preferably in a range of 20% to 50% by mass in the aqueous polyurethane composition.

[0034] For example, water, a water-miscible organic solvent, and a mixture thereof can be used as the aqueous medium (B). Examples of the water-miscible organic solvent include alcohol solvents such as methanol, ethanol, n-propanol, isopropanol, and the like; ketone solvents such as acetone, methyl ethyl ketone, and the like; polyalkylene glycol such as ethylene glycol, diethylene glycol, propylene glycol, and the like; polyalkylene polyol alkyl ether solvents; lactam solvents such as N-methyl-2-pyrrolidone, and the like; and the like. Among them, water is preferably used in view of environmental friendliness.

[0035] A method for preparing the aqueous polyurethane composition is, for example, a method of preparing the anionic polyurethane (A) without solvent or in the presence of the organic solvent, then neutralizing carboxyl groups in the anionic polyurethane (A) if necessary, supplying the aqueous medium (B) and dispersing the anionic polyurethane (A) in the aqueous medium (B).

[0036] When mixing the anionic polyurethane (A) with the aqueous medium (B), a machine such as a homogenizer or the like may be used if necessary.

[0037] In the preparation of the aqueous polyurethane composition, an emulsifier may also be used from the viewpoint of improving the dispersion stability of the anionic polyurethane (A) in the aqueous medium (B).

[0038] Usable examples of the emulsifier include nonionic emulsifiers such as polyoxyethylene nonylphenyl ether, polyoxyethylene lauryl ether, polyoxyethylene styrylphenyl ether, polyoxyethylene sorbitol tetraolate, polyoxyethylene-polyoxypropylene copolymer, and the like; anionic emulsifiers such as fatty acid salts such as sodium oleate, and the like; alkyl sulfate ester salts, alkylbenzenesulfonic acid salts, alkylsulfosuccinic acid salts, naphthalenesulfonic acid salts, polyoxyethylene alkylsulfuric acid salts, alkanesulfonate sodium salts, alkyldiphenyl ethersulfonate sodium salt, and the like; cationic emulsifiers such as alkylamine salts, alkyltrimethylammonium salts, alkyldimethylbenzylammonium salts, and the like; and the like. These emulsifiers can be used alone or in combination of two or more.

[0039] From the viewpoint of obtaining excellent manufacturing stability, the acid value of the aqueous polyurethane composition is in a range of 5 to 19 mg KOH / g, and more preferably in a range of 7 to 14 mg KOH / g. A method for measuring the acid value of the aqueous polyurethane composition is described in the examples described later.

[0040] The aqueous polyurethane composition contains the anionic polyurethane (A) and the aqueous medium (B) and may optionally contain further additives.

[0041] Usable examples of the additives include an associative thickener, a defoaming agent, a urethanization catalyst, a silane coupling agent, a filler, a thixotropy-imparting agent, a coupling agent, a wax, a heat stabilizer, a light-resistant stabilizer, a fluorescent brightener, a foaming agent, a pigment, a dye, an antistatic agent, a moisture permeability improver, a water repellent, an oil repellent, a flame retardant, an anti-blocking agent, a hydrolysis inhibitor, and the like. These additives can be used alone or in combination of two or more.

[0042] The associative thickener can be preferably used to adjust the viscosity of the aqueous polyurethane composition and facilitate the work of salt coagulation. Usable examples thereof include cellulose derivatives such as hydroxyethylcellulose, methylcellulose, carboxymethylcellulose, and the like; polyacrylic acid salts; polyvinylpyrrolidone; urethane compounds; polyether compounds; and the like. When the associative emulsifier is used, the use amount is, for example, in a range of 0.5 to 5 parts by mass based on 100 parts by mass of the anionic polyurethane (A).

[0043] Usable examples of the defoaming agent include defoaming agents such as silicone compounds, mineral oil compounds, polyglycol ether compounds, fatty acid ester compounds, metallic soaps, fluorine compounds, and the like. These defoaming agents can be used alone or in combination with two or more.

[0044] The aqueous polyurethane composition used in the present invention can be used for producing medical tubes, particularly tubes such as a catheter and the like, and contraceptive devices such as a condom and the like, besides gloves.

[0045] A method for producing a coagulated film using the aqueous polyurethane composition is, for example, a method of applying the aqueous polyurethane composition to a surface of a mold release film, then immersing the coated material in a predetermined coagulant, and then drying the coated material.

[0046] Examples of the method for applying the aqueous polyurethane composition to a mold release film or the like include a blade coating method, a spraying method, a curtain coating method, a flow coating method, a roll coating method, a brushing method, and the like. During coating, the viscosity of the aqueous polyurethane composition is preferably in a range of 50 to 10,000 mPa s, and more preferably in a range of 1,000 to 3,000 mPa s. The viscosity of the aqueous polyurethane composition refers to a value measured with a B-type viscometer (40P cone) at 25°C.

[0047] Usable examples of the coagulant in which the coated material of the aqueous polyurethane composition is immersed include metal salt solutions of calcium nitrate, calcium chloride, zinc nitrate, zinc chloride, magnesium acetate, aluminum sulfate, sodium chloride, and the like; acidic solutions of formic acid, acetic acid, and the like; and the like. Usable examples of a solvent capable of dissolving the metal salts and acids include water, methanol, ethanol, isopropanol, and the like. The metal salt contained in the coagulant is preferably contained in a range of 1% to 50% by mass based on the total amount of the coagulant. Furthermore, the time required for immersing the coated material in the coagulant is preferably 1 to 10 minutes, and the coagulant is preferably used at a temperature of 5°C to 60°C.

[0048] After immersion, the coated material is dried at a temperature of, for example, 50 °C to 150 °C for 1 minute to 1 hour to form the coagulated film coagulated on the surface of the mold release film.

[0049] The 100% modulus obtained by a tensile test of the coagulated film under the condition of a crosshead speed of 300 mm / min is preferably 6 MPa or less, and more preferably in a range of 0.1 to 4 MPa from the viewpoint of achieving excellent flexibility.

[0050] The 300% modulus obtained by a tensile test of the coagulated film under the condition of a crosshead speed of 300 mm / min is preferably 14 MPa or less, and more preferably in a range of 0.1 to 12 MPa from the viewpoint of achieving excellent flexibility.

[0051] When producing a glove using the coagulated film, first, a hand mold, a tubular mold, or the like is immersed in the coagulant and then dried if necessary, whereby a metal salt or the like in the coagulant adheres to the surface of the hand mold or the like. Next, the hand mold or the like is immersed in the aqueous polyurethane composition, and then its surface is washed with water and dried to form the coagulated film on the hand mold or the like. Next, a glove with the coagulated film having the same shape as the hand mold can be produced by separating the coagulated film from the hand mold. When producing a tubular mold, it can also be produced by the same method as described above except for using the tubular mold.

[0052] The hand mold or tubular mold may be at room temperature or may be heated to, for example, 30°C to 70°C before being immersed in the coagulant. Just as with the hand mold or the like, the coagulant may be at room temperature, but if the hand mold or the like is heated, the coagulant may be heated to, for example, 30°C to 70°C.

[0053] Furthermore, the hand mold or the tubular mold may be previously provided with a glove-shaped material or a tubular material made of a knitted fabric made of nylon fibers or the like. Specifically, the hand mold or the like provided with the glove-shaped material or the like made of a knitted fabric is first immersed in the coagulant, and then the glove-shaped material or the like is impregnated with the coagulant by drying as needed. Next, the hand mold or the like is immersed in the aqueous polyurethane composition, and its surface is washed with water and dried to form a glove or the like consisting of a film coagulated on the surface of the glove material or the like.The glove including the coagulated film having a shape corresponding to the hand mold or the like can be manufactured by separating the glove or the like from the hand mold and the glove-shaped material or the like. When manufacturing the tubular shape, the tubular shape can be manufactured by the same method as described above, except that the tubular shape and the tubular material are made of a knitted fabric made of nylon fibers or the like.

[0054] The knitted fabric is not limited to one made of nylon fibers; a knitted fabric made of polyester fibers, aramid fibers, cotton, or the like can also be used. A woven fabric made of these fibers can also be used instead of the knitted fabric. In addition, a glove-shaped material or a tubular material made of vinyl chloride, natural rubber, synthetic rubber, or the like can be used instead of the knitted fabric.

[0055] From the viewpoint of achieving excellent wear resistance, the number of times of abrasion performed on the glove according to EN388: 2004 is preferably in a range of 2,000 or more, more preferably in a range of 5,000 to 20,000, and even more preferably in a range of 8,000 to 10,000.

[0056] From the foregoing, it is understood that the glove of the present invention has excellent wear resistance and flexibility and thus can be preferably used in various fields such as chemical industry, food industry, etc. EXAMPLES

[0057] The present invention will be described below in further detail using examples. [Preparation Example 1] Preparation of an aqueous polyurethane composition (X-1)

[0058] In a nitrogen-purged vessel equipped with a thermometer, a nitrogen gas introduction tube, and a stirrer, the reaction was carried out at 70 °C in the presence of 895.3 mass parts of polyoxytetramethylene glycol (number average molecular weight: 2,000, hereinafter abbreviated as "PTMG2000"), 18 mass parts of ethylene glycol (hereinafter abbreviated as "EG"), 25.5 mass parts of 2,2'-dimethylolpropanoic acid (hereinafter abbreviated as "DMPA"), 224 mass parts of diphenylmethane diisocyanate (hereinafter abbreviated as "MDI"), and 487 mass parts of methyl ethyl ketone.

[0059] When the reaction product reached a specified viscosity, 2.9 parts by mass of methanol was added and stirred for 1 hour, and then the reaction was terminated. Further, 1257 parts by mass of methyl ethyl ketone was added as a diluent to prepare an organic solvent solution of anionic polyurethane.

[0060] Next, 19.2 parts by mass of triethylamine as a neutralizing agent was added to the organic solvent solution of the anionic polyurethane and stirred, and another 3638 parts by mass of water were added and stirred to prepare a water dispersion of the anionic polyurethane. Next, the solvent was removed from the water dispersion to prepare an aqueous polyurethane composition (X-1) with a nonvolatile content of 40 mass% and an acid value of 9.2 mg KOH / g. The anionic polyurethane had an oxyalkylene group content of 10.7 mol / kg and an average particle diameter of 0.25 µm. [Preparation Example 2] Preparation of an aqueous polyurethane composition (X-2)

[0061] In a nitrogen-purged vessel equipped with a thermometer, a nitrogen gas inlet tube, and a stirrer, the reaction was carried out at 70 °C in the presence of 764.5 parts by mass of PTMG2000, 18.9 parts by mass of butanediol (hereinafter abbreviated as "BG"), 23.1 parts by mass of DMPA, 190.8 parts by mass of MDI, and 417.5 parts by mass of methyl ethyl ketone.

[0062] When the reaction product reached a specified viscosity, 2.5 parts by mass of methanol was added and stirred for 1 hour, and then the reaction was terminated. Further, 1078.4 parts by mass of methyl ethyl ketone was added as a diluting solvent to prepare an organic solvent solution of anionic polyurethane.

[0063] Next, 17.4 parts by mass of triethylamine was added as a neutralizing agent to the anionic organic polyurethane solution and stirred, and another 3200 parts by mass of water was added and stirred to prepare a water dispersion of anionic polyurethane. Next, the solvent was removed from the water dispersion to prepare an aqueous polyurethane composition (X-2) with a nonvolatile content of 40 mass% and an acid value of 9.7 mg KOH / g. The anionic polyurethane had an oxyalkylene group content of 10.6 mol / kg and an average particle diameter of 0.14 µm. [Preparation Example 3] Preparation of an aqueous polyurethane composition (X-3)

[0064] In a nitrogen-purged container equipped with a thermometer, a nitrogen gas inlet tube, and a stirrer, the reaction was carried out at 70°C in the presence of 354.3 parts by mass of polyoxytetramethylene glycol (number average molecular weight: 700, hereinafter abbreviated as “PTMG700”), 8.6 parts by mass of EG, 16.7 parts by mass of DMPA, 190.8 parts by mass of MDI, and 237.3 parts by mass of methyl ethyl ketone.

[0065] When the reaction product reached a specified viscosity, 2.7 parts by mass of methanol was added and stirred for 1 hour, and then the reaction was terminated. Further, 618 parts by mass of methyl ethyl ketone was added as a diluting solvent to prepare an organic solvent solution of anionic polyurethane.

[0066] Next, 12.6 parts by mass of triethylamine as a neutralizing agent was added to the organic solvent solution of the anionic organic polyurethane and stirred, and another 1785 parts by mass of water was added and stirred to prepare a water dispersion of the anionic polyurethane. Next, the solvent was removed from the water dispersion to prepare an aqueous polyurethane composition (X-3) with a nonvolatile content of 40 mass% and an acid value of 12.3 mg KOH / g. The anionic polyurethane had an oxyalkylene group content of 8.6 mol / kg and an average particle diameter of 0.39 μm. [Preparation Example 4] Preparation of an aqueous polyurethane composition (X-4)

[0067] In a nitrogen-purged container equipped with a thermometer, a nitrogen gas introduction tube, and a stirrer, the reaction was carried out at 70 °C in the presence of 1127.3 mass parts of polyoxytetramethylene glycol (number average molecular weight: 4000, hereinafter abbreviated as "PTMG4000"), 10.3 mass parts of EG, 44.5 mass parts of DMPA, 190.8 mass parts of MDI, and 569 mass parts of methyl ethyl ketone.

[0068] When the reaction product reached a specified viscosity, 2.6 parts by mass of methanol was added and stirred for 1 hour, and then the reaction was terminated. Further, 1490 parts by mass of methyl ethyl ketone was added as a diluting solvent to prepare an organic solvent solution of anionic polyurethane. Next, 33.5 parts by mass of triethylamine was added as a neutralizing agent to the organic solvent solution of anionic polyurethane and stirred, and another 4293 parts by mass of water was added and stirred to prepare a water dispersion of anionic polyurethane. Next, the solvent was removed from the water dispersion to prepare an aqueous polyurethane composition (X-4) with a nonvolatile content of 40 mass% and an acid value of 13.5 mg KOH / g. The anionic polyurethane had an oxyalkylene group content of 11.4 mol / kg and an average particle diameter of 0.43 μm. [Preparation Example 5] Preparation of an aqueous polyurethane composition (X-5)

[0069] In a nitrogen-purged vessel equipped with a thermometer, a nitrogen gas inlet tube and a stirrer, the reaction was carried out at 70°C in the presence of 391.1 parts by mass of PTMG2000, 26.7 parts by mass of EG, 15.7 parts by mass of DMPA, 190.8 parts by mass of MDI and 261 parts by mass of methyl ethyl ketone.

[0070] When the reaction product reached a specified viscosity, 2.1 parts by mass of methanol was added and stirred for 1 hour, and then the reaction was terminated. Further, 675.6 parts by mass of methyl ethyl ketone was added as a diluting solvent to prepare an organic solvent solution of anionic polyurethane.

[0071] Next, 11.8 parts by mass of triethylamine as a neutralizing agent was added to the organic solvent solution of the anionic polyurethane and stirred, and another 1953.4 parts by mass of water was added and stirred to prepare a water dispersion of the anionic polyurethane. Next, the solvent was removed from the water dispersion to prepare an aqueous polyurethane composition (X-5) with a nonvolatile content of 40 mass% and an acid value of 10.5 mg KOH / g. The anionic polyurethane had an oxyalkylene group content of 8.7 mol / kg and an average particle diameter of 0.42 μm. [Preparation Example 6] Preparation of an aqueous polyurethane composition (X-6)

[0072] In a nitrogen-purged container equipped with a thermometer, a nitrogen gas inlet tube, and a stirrer, the reaction was carried out at 70 °C in the presence of 458.7 mass parts of PTMG2000, 305.8 mass parts of polyester polyol (prepared by reacting 1,6-hexanediol, neopentyl glycol, and adipic acid, number-average molecular weight: 2,000, hereinafter abbreviated as “PES”), 11.8 mass parts of EG, 28.2 mass parts of DMPA, 190.8 mass parts of MDI, and 414.5 mass parts of methyl ethyl ketone.

[0073] When the reaction product reached a specified viscosity, 2.2 parts by mass of methanol was added and stirred for 1 hour, and then the reaction was terminated. Further, 1078.5 parts by mass of methyl ethyl ketone was added as a diluting solvent to prepare an organic solvent solution of anionic polyurethane.

[0074] Next, 21.3 mass parts of triethylamine as a neutralizing agent was added to the organic solvent solution of the anionic polyurethane and stirred, and another 3113.2 mass parts of water were added and stirred to prepare a water dispersion of the anionic polyurethane. Next, the solvent was removed from the water dispersion to prepare an aqueous polyurethane composition (X-6) with a nonvolatile content of 40 mass% and an acid value of 11.8 mg KOH / g. The anionic polyurethane had an oxyalkylene group content of 6.4 mol / kg and an average particle diameter of 0.13 µm. [Preparation Example 7] Preparation of an aqueous polyurethane composition (X-7)

[0075] In a nitrogen-purged vessel equipped with a thermometer, a nitrogen gas inlet tube, and a stirrer, the reaction was carried out at 70 °C in the presence of 1151 parts by mass of PTMG2000, 17.8 parts by mass of EG, 42.4 parts by mass of DMPA, 200 parts by mass of toluene diisocyanate (hereinafter abbreviated as “TDI”), and 586.6 parts by mass of methyl ethyl ketone.

[0076] When the reaction product reached a specified viscosity, 3.9 parts by mass of methanol was added and stirred for 1 hour, and then the reaction was terminated. Further, 1530.3 parts by mass of methyl ethyl ketone was added as a diluting solvent to prepare an organic solvent solution of anionic polyurethane.

[0077] Next, 32 parts by mass of triethylamine as a neutralizing agent was added to the organic solvent solution of the anionic polyurethane and stirred, and another 4415 parts by mass of water was added and stirred to prepare a water dispersion of the anionic polyurethane. Next, the solvent was removed from the water dispersion to prepare an aqueous polyurethane composition (X-7) with a nonvolatile content of 40 mass% and an acid value of 12.6 mg KOH / g. The anionic polyurethane had an oxyalkylene group content of 11.3 mol / kg and an average particle diameter of 0.19 µm. [Preparation Example 8] Preparation of an aqueous polyurethane composition (X-8)

[0078] In a nitrogen-purged vessel equipped with a thermometer, a nitrogen gas introduction tube, and a stirrer, the reaction was carried out at 70 °C in the presence of 601 parts by mass of PTMG2000, 200 parts by mass of polycarbonate polyol ("UH-200", manufactured by Ube Industries, Ltd., hereinafter abbreviated as "PC"), 9.9 parts by mass of EG, 32.2 parts by mass of DMPA, 200 parts by mass of MDI, and 433.4 parts by mass of methyl ethyl ketone.

[0079] When the reaction product reached a specified viscosity, 2.2 parts by mass of methanol was added and stirred for 1 hour, and then the reaction was terminated. Further, 1131.9 parts by mass of methyl ethyl ketone was added as a diluting solvent to prepare an organic solvent solution of anionic polyurethane.

[0080] Next, 24.3 parts by mass of triethylamine was added as a neutralizing agent to the organic solvent solution of the anionic polyurethane and stirred, and further, 3263.8 parts by mass of water was added and stirred to prepare a water dispersion of the anionic polyurethane. Next, the solvent was removed from the water dispersion to prepare an aqueous polyurethane composition (X-8) with a nonvolatile content of 40 mass% and an acid value of 12.9 mg KOH / g. The anionic polyurethane had an oxyalkylene group content of 8.0 mol / kg and an average particle diameter of 0.32 μm. [Preparation Example 9] Preparation of an aqueous polyurethane composition (X-9)

[0081] In a nitrogen-purged vessel equipped with a thermometer, a nitrogen gas inlet tube, and a stirrer, the reaction was carried out at 70 °C in the presence of 863.2 mass parts of PTMG2000, 287.7 mass parts of PEs, 25.9 mass parts of BG, 42.4 mass parts of DMPA, 200 mass parts of TDI, and 590.1 mass parts of methyl ethyl ketone.

[0082] When the reaction product reached a specified viscosity, 3.1 parts by mass of methanol was added and stirred for 1 hour, and then the reaction was terminated. Further, 1538.9 parts by mass of methyl ethyl ketone was added as a diluting solvent to prepare an organic solvent solution of anionic polyurethane.

[0083] Next, 32.0 parts by mass of triethylamine as a neutralizing agent was added to the organic solvent solution of the anionic polyurethane and stirred, and another 4439.3 parts by mass of water was added and stirred to prepare a water dispersion of the anionic polyurethane. Next, the solvent was removed from the water dispersion to prepare an aqueous polyurethane composition (X-9) with a nonvolatile content of 40 mass% and an acid value of 12.5 mg KOH / g. The anionic polyurethane had an oxyalkylene group content of 8.4 mol / kg and an average particle diameter of 0.24 μm. [Comparative Preparation Example 1] Preparation of an aqueous polyurethane composition (X'-1)

[0084] In a nitrogen-purged vessel equipped with a thermometer, a nitrogen gas inlet tube, and a stirrer, the reaction was carried out at 70 °C in the presence of 1836.8 mass parts of PTMG4000, 1.9 mass parts of EG, 34.9 mass parts of DMPA, 180 mass parts of MDI, and 865.2 mass parts of methyl ethyl ketone.

[0085] When the reaction product reached a specified viscosity, 2.8 parts by mass of methanol was added and stirred for 1 hour, and then the reaction was terminated. Further, 2215.3 parts by mass of methyl ethyl ketone was added as a diluting solvent to prepare an organic solvent solution of anionic polyurethane.

[0086] Next, 26.3 mass parts of triethylamine as a neutralizing agent was added to the organic solvent solution of the anionic polyurethane and stirred, and another 6421 mass parts of water were added and stirred to prepare a water dispersion of the anionic polyurethane. Next, the solvent was removed from the water dispersion to prepare an aqueous polyurethane composition (X'-1) with a nonvolatile content of 40 mass% and an acid value of 7.1 mg KOH / g. The anionic polyurethane had an oxyalkylene group content of 12.4 mol / kg and an average particle diameter of 0.57 µm. [Comparative Preparation Example 2] Preparation of an aqueous polyurethane composition (X'-2)

[0087] In a nitrogen-purged vessel equipped with a thermometer, a nitrogen gas inlet tube, and a stirrer, the reaction was carried out at 70 °C in the presence of 179.9 mass parts of PTMG2000, 539.6 mass parts of PEs, 11.2 mass parts of EG, 26.5 mass parts of DMPA, 180 mass parts of MDI, and 390.2 mass parts of methyl ethyl ketone.

[0088] When the reaction product reached a specified viscosity, 2.3 parts by mass of methanol was added and stirred for 1 hour, and then the reaction was terminated. Further, 1015.4 parts by mass of methyl ethyl ketone was added as a diluting solvent to prepare an organic solvent solution of anionic polyurethane.

[0089] Next, 20.0 parts by mass of triethylamine as a neutralizing agent was added to the organic solvent solution of the anionic polyurethane and stirred, and another 2931.3 parts by mass of water was added and stirred to prepare a water dispersion of the anionic polyurethane. Next, the solvent was removed from the water dispersion to prepare an aqueous polyurethane composition (X'-2) with a nonvolatile content of 40 mass% and an acid value of 11.84 mg KOH / g. The anionic polyurethane had an oxyalkylene group content of 2.7 mol / kg and an average particle diameter of 0.67 µm. [Comparative Preparation Example 3] Preparation of an aqueous polyurethane composition (X'-3)

[0090] In a nitrogen-purged vessel equipped with a thermometer, a nitrogen gas inlet tube, and a stirrer, the reaction was carried out at 70 °C in the presence of 581.4 parts by mass of PTMG2000, 9.0 parts by mass of EG, 21.4 parts by mass of DMPA, 200 parts by mass of MDI, and 1243.7 parts by mass of methyl ethyl ketone. When the reaction product reached a specified NCO content, the reaction was terminated to prepare an organic solvent solution of anionic polyurethane. Next, 16.2 parts by mass of triethylamine as a neutralizing agent was added to the organic solvent solution of the anionic polyurethane and stirred, and another 2572.4 parts by mass of water and 17.4 parts by mass of piperazine (hereinafter abbreviated as "PZ") were added and stirred to prepare a water dispersion of anionic polyurethane.Next, the solvent was removed from the water dispersion to prepare an aqueous polyurethane composition (X'-3) with a non-volatile content of 40 mass% and an acid value of 10.8 mg KOH / g. The anionic polyurethane had an oxyalkylene group content of 9.7 mol / kg, a urea bond content of 0.24 mol / kg, and an average particle diameter of 0.83 µm. [Example 1]

[0091] A knitted glove made of nylon fibers was placed on a hand mold, immersed in an aqueous potassium nitrate solution adjusted to a concentration of 5 mass% at room temperature for 10 seconds, and then withdrawn. Next, the hand mold was immersed in the aqueous polyurethane composition (X-1) for 2 seconds to form a coagulated film of the anionic polyurethane on the surface of the knitted glove, and then withdrawn. Next, the hand mold was immersed in water for 180 minutes and then withdrawn. Further, the hand mold was dried in an environment of 70°C for 20 minutes and further dried in an environment of 120°C for 30 minutes. Then, the knitted glove was separated from the hand mold to produce a glove coated with the coagulated film. [Examples 2 to 9 and Comparative Examples 1 to 3]

[0092] Gloves were prepared by the same procedure as in Example 1, except that the aqueous polyurethane composition used was changed as shown in Tables 1 and 2. [Method for measuring the average particle diameter of anionic polyurethane (A)]

[0093] The area-based average particle diameter of the aqueous polyurethane composition prepared in each of the preparation examples was measured with a relative refractive index = 1.10 using a laser diffraction / scattering particle size distribution analyzer ("LA-910", manufactured by HORIBA, Ltd.) and water as a dispersing liquid. [Method for measuring the acid number of an aqueous polyurethane composition]

[0094] The aqueous polyurethane composition prepared in each of the preparation examples was dried, and 0.05 g to 0.5 g of dry solidified resin particles were weighed into a 300 ml conical flask. Then, approximately 80 ml of a mixed solvent of tetrahydrofuran and ion-exchange water in a mass ratio [tetrahydrofuran / ion-exchange water] of 80 / 20 was added to the resin particles to form a mixed solution.

[0095] Next, the mixed solution was mixed with a phenolphthalein indicator and titrated with a 0.1 mol / L aqueous potassium hydroxide solution that had been previously standardized. The acid value (mgKOH / g) of the aqueous polyurethane composition was determined from the amount of aqueous potassium hydroxide solution used in the titration according to the following calculation formula (2). Calculation formula A=(B×f×5.611) / s

[0096] In the formula, A is the acid value (mgKOH / g) of the resin solid content, B is the amount (ml) of the 0.1 mol / L aqueous potassium hydroxide solution used in the titration, f is the factor of the 0.1 mol / L aqueous potassium hydroxide solution, S is the mass (g) of the resin particles, and 5.611 is the formula weight (56.11 / 10) of potassium hydroxide. [Method for assessing flexibility]

[0097] Flexibility was evaluated using a coagulated film.

[0098] An associative thickener “Hydran Assister T10” (manufactured by DIC Corporation) was mixed with 100 parts by mass of the aqueous polyurethane composition prepared in each of the preparation examples, and the resulting mixture was adjusted so that the viscosity was 1,000 to 3,000 mPa s. Then, 150 g / cm 2The mixture was applied at room temperature using a doctor blade coating method onto the surface of a polypropylene film treated with a mold release agent.

[0099] The coated material was immersed in an aqueous calcium nitrate solution at room temperature, adjusted to a concentration of 5 mass%, for 3 minutes and then immersed in water for 18 hours. Next, the coated material was dried in an environment of 70°C for 20 minutes and further dried in an environment of 120°C for 2 minutes, forming a coagulated film on the surface of the polypropylene film. After drying, the coagulated film was separated from the surface of the polypropylene film to prepare the coagulated film with a thickness of 50 μm.

[0100] The resulting coagulated film was cut into a length of 100 mm and a width of 5 mm to form a test piece. The test piece was held between jigs at both ends and stretched using a tensile tester [Autograph AG-1] (manufactured by Shimadzu Corporation) in an atmosphere of 23 °C and 60% humidity at a crosshead speed of 300 mm / min, while measuring the 100% modulus and 300% modulus (MPa) of the test piece. In this test, the distance between the reference lines was 20 mm, and the initial distance between the chucks was 20 mm.

[0101] The flexibility was evaluated from the obtained 100% modulus value and the 300% modulus value according to the following criteria “A”: The 100% modulus is 6 MPa or less and the 300% modulus is 14 MPa or less. “B”: These criteria are not met. [Method for evaluating wear resistance]

[0102] A wear test of the palm portion of the glove prepared in each of the Examples and Comparative Examples was conducted using a Martindale Abrasion Tester manufactured by Intec Inc. in accordance with EN388:2004 and the following criteria. “A”: Number of abrasion tests is 5,000 or more and less than 20,000. “B”: Number of abrasion tests is 2,000 or more and less than 5,000. “C”: Number of abrasions is less than 2,000. [Table 1] Table 1 Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Aqueous polyurethane composition (X-1) (X-2) (X-3) (X-4) (X-5) (X-6) Acid number (mgKOH / g) 9, 2 9,7 12,3 13,5 10,5 11, 8 Anionic polyurethane (A) composition PTMG2000 PTMG2000 PTMG700 PTMG4000 PTMG2000 PTMG2000 PEs DMPA DMPA DMPA DMPA DMPA DMPA EC BG EC EC EC EC MDI MDI MDI MDI MDI MDI Oxyalkylene group content (mol / kg) 10, 7 10, 6 8, 6 11, 4 8, 7 6, 4 Urea binding content (mol / kg) 0 0 0 0 0 0 Average particle diameter (µm) 0,25 0, 14 0,39 0,43 0,42 0,13 Aqueous medium (B) Water Water Water Water Water Water Assessment of wear resistance A A A A A A Assessment of flexibility A A A A A A [Table 2] Table 2 Example 7 Example 8 Example 9 Comparison example 1 Comparison example 2 Comparison example 3 Aqueous polyurethane composition (X-7) (X-8) (X-9) (X'-1) (X'-2) (X'-3) Acid number (mgKOH / g) 12, 6 12, 9 12,5 7, 1 11, 8 10, 8 Anionic polyurethane (A) composition PTMG2000 PTMG2000 PTMG2000 PTMG4000 PTMG2000 PTMG4000 PC PEs PEs DMPA DMPA DMPA DMPA DMPA DMPA EC EC BG EC EC EC PZ TDI MDI TDI MDI MDI MDI Oxyalkylene group content (mol / kg) 11,3 8,0 8, 4 12, 4 2, 7 9, 7 Urea binding content (mol / kg) 0 0 0 0 0 0,24 Average particle diameter (µm) 0,19 0,32 0,24 0,57 0,67 0,83 Aqueous medium (B) Water Water Water Water Water Water Assessment of wear resistance A A A C A A Assessment of flexibility A A A A B B

[0103] It has been found that the glove of the present invention has excellent wear resistance and flexibility.

[0104] On the other hand, Comparative Example 1 has conditions in which the content of oxyalkylene groups exceeds the range specified in the present invention and low wear resistance is exhibited.

[0105] Comparative Example 2 has conditions in which the oxyalkylene group content is lower than the range specified in the present invention, and low flexibility is exhibited.

[0106] Comparative Example 3 has conditions in which the urea bond content exceeds the range specified in the present invention and exhibits low flexibility.

Claims

[1] A glove comprising a coagulated film of an aqueous polyurethane composition containing anionic polyurethane (A) having an oxyalkylene group content in a range of 4 to 12 mol / kg and a urea bond content of 0.2 mol / kg or less, and an aqueous medium (B), wherein the anionic polyurethane (A) is the reaction product of a polyol containing polyoxyalkylene polyol, a glycol having a carboxyl group, a chain extender and a polyisocyanate and wherein the acid number of the aqueous polyurethane composition is in a range of 5 to 19 mg KOH / g. [2] The glove according to claim 1, wherein the amount of the chain extender used is in a range of 0.01 to 8 mass% of the total mass of the starting materials of the anionic polyurethane (A). [3] The glove of claim 1, wherein the chain extender is ethylene glycol or butanediol. [4] A glove according to claim 1, wherein the polyisocyanate is diphenylmethane diisocyanate or toluene diisocyanate. [5] The glove according to claim 1, wherein the average particle diameter of the anionic polyurethane (A) is in a range of 0.01 to 1 µm.

Citation Information

Patent Citations

  • Articles comprising aqueous dispersions using poly(urea / urethanes)

    WO2004041892A1

  • glove

    WO2015012117A1