Carbon nanotube composite wire and methods for its production

The carbon nanotube composite wire addresses conductivity limitations by optimizing CNT alignment and crystallinity, achieving higher conductivity than conventional metals through reduced CNT content and synergistic metal interaction.

DE112023000559T5Pending Publication Date: 2024-11-28YAZAKI CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
DE112023000559
Authority / Receiving Office
DE · DE
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-01-11
Filing Date
2023-01-11
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing carbon nanotube (CNT) metal composite materials do not provide higher conductivity than conventional metal materials, and high CNT content leads to increased costs and potential degradation of CNT properties, such as a decrease in the G/D ratio, affecting conductive properties.

Method used

A carbon nanotube composite wire with a CNT occupancy area ratio of 10% or less and a G/D ratio of 5 to 30, combined with a metal thin film, is produced through steps including dispersion, metal film formation, positioning, masking, and heat treatment, to enhance conductivity while reducing CNT amount.

Benefits of technology

The composite wire achieves higher conductivity than conventional metals by optimizing CNT alignment and crystallinity, reducing CNT content, and utilizing a synergistic effect with the metal film, resulting in improved conductivity and reduced resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

A carbon nanotube composite wire (10) is provided, comprising: a substrate (3); a carbon nanotube (1); and a thin metal film (2) formed on the carbon nanotubes (1), wherein the carbon nanotube (1) has a peak ratio (G / D) of a G band to a D band in a Raman spectrum of 5 or more and 30 or less, and a carbon nanotube area coverage ratio, which is a ratio of a cross-sectional area of ​​the carbon nanotube (1) to a sum of the cross-sectional area of ​​the carbon nanotube (1) and a cross-sectional area of ​​the thin metal film (2), is 10% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical area

[0001] The present invention relates to a carbon nanotube composite wire and a method for producing the carbon nanotube composite wire. State of the art

[0002] To reduce the size and power consumption of electronic devices, the resistance of wiring materials must be reduced and the allowable current density increased. Because carbon nanotubes (CNTs) are lightweight and highly conductive, they are being used as composite wires combining CNTs and metals.

[0003] As a CNT composite wire, for example, Patent Literature 1 proposes a CNT-metal composite material containing a CNT assembly in which a metal is deposited on the surface of CNTs to be mixed. It is further described that the metal in the CNT-metal composite material has a volume content of 20% or more and less than 70% or less, and the minimum volume resistivity of the CNT-metal composite material is 1.8 × 10 -5 Ω·cm. Citation listPatent literature

[0004] Patent Document 1: Japanese Patent No. 5 896 422 Summary of the invention

[0005] However, the CNT-metal composite described in Patent Literature 1 does not offer higher conductivity than wiring using only conventional metal materials. Since CNT is more expensive than metal, a high CNT volume content, as described in Patent Literature 1, results in high costs. Furthermore, in the coating method described in Patent Literature 1, when CNT is immersed in an electrolytic solution such as an acid, the properties of CNT itself may change, such as a decrease in the intensity ratio of the G band to the D band (G / D ratio), which is a measure of the crystallinity of CNT. As a result, the conductive properties of the composite may decrease.

[0006] Therefore, it is an object of the present invention to provide a CNT composite wire having higher conductivity than conventional metal materials, wherein the amount of CNT in the CNT composite wire is reduced, and a method for producing the CNT composite wire.

[0007] A carbon nanotube composite wire according to one aspect of the present invention comprises a substrate, a carbon nanotube, and a thin metal film formed on the carbon nanotubes, wherein the carbon nanotube has a peak ratio (G / D) of a G band to a D band in a Raman spectrum of 5 or more and 30 or less, and a carbon nanotube occupation area ratio, which is a ratio of a cross-sectional area of ​​the carbon nanotube to a sum of the cross-sectional area of ​​the carbon nanotube and a cross-sectional area of ​​the thin metal film, is 10% or less.

[0008] A method for producing a carbon nanotube composite wire according to one aspect of the present invention comprises (a) a step of spreading a carbon nanotube dispersion on a substrate; (b) a step of forming the thin metal film on the carbon nanotube after step (a); (c) a step of determining a position of the carbon nanotube on the thin metal film after step (b); (d) a step of forming a mask on the thin metal film after step (c) and then removing by etching a part not protected by the mask; and (e) a step of heat-treating in a reducing atmosphere after step (d).

[0009] The present invention provides a CNT composite wire having higher conductivity than conventional metal materials while reducing the amount of CNT in the CNT composite wire, and a method for producing the CNT composite wire. Short description of the drawings [ Fig. 1] Fig. Figure 1 is a schematic diagram showing a CNT composite wire and electrodes for evaluating electrical properties. [ Fig. 2] Fig. 2 is a cross-sectional view of the Fig. 1 shown CNT composite wire along the line AA. [ Fig. 3A] Fig. Figure 3A is a schematic diagram for explaining a method for manufacturing the CNT composite wire. [ Fig. 3B] Fig. Figure 3B is a schematic diagram for explaining the process for manufacturing the CNT composite wire. [ Fig. 3C] Fig. Figure 3C is a schematic diagram for explaining the manufacturing process of the CNT composite wire. [ Fig. 4] Fig. Figure 4 is a graph showing the relationship between the ratio of the resistivity of the CNT composite wire and that of the wiring using only aluminum and the G / D ratio of the CNT. [ Fig. 5] Fig. Figure 5 is a graph showing the relationship between the ratio of the resistivity of the CNT composite wire and that of the wiring using only aluminum and the CNT occupation area ratio. [ Fig. 6A] Fig. Figure 6A is a transmission electron microscope (TEM) image of a cross-section of the CNT composite wire. [ Fig. 6B] Fig. Figure 6B is a transmission electron microscope (TEM) image of a cross-section of the CNT composite wire. [ Fig. 6C] Fig. Figure 6C is a transmission electron microscope (TEM) image of a cross-section of the CNT composite wire. Description of the embodiments

[0010] With reference to the drawings, a CNT composite wire and a method for manufacturing the CNT composite wire according to the present embodiment will be described in detail below.

[0011] A CNT composite wire 10 according to the present embodiment comprises a CNT 1 arranged on a substrate 3 and a thin metal film 2 formed on the CNT 1. In Fig. 1 and Fig. 2, metal films 4 and 5 are formed on the thin metal film 2 as electrode 6 for evaluating the electrical properties of the CNT composite wire 10.

[0012] As the CNT 1 constituting the CNT composite wire 10, known CNTs can be used. The CNT 1 can be a single-walled nanotube (SWNT) with a single wall, a double-walled carbon nanotube (DWCNT), or a multi-walled nanotube (MWNT) with multiple walls, with an MWNT with three or more walls being preferable from the aspect of conductivity. The diameter of the CNT is preferably in a range between 0.4 and 50 nm, and the average length of the CNT 1 is preferably 10 μm or more. Note that the diameter and average length of the CNT 1 are measured using a known method such as electron microscopy.

[0013] The CNTs 1 constituting the CNT composite wire 10 form a conductive path that conducts electricity in the longitudinal direction of the CNT composite wire 10. Thus, the CNTs 1 are aligned along the longitudinal direction (conduction direction) of the CNT composite wire 10. Since the CNT composite wire 10 according to the present embodiment is manufactured using a semiconductor process, it should be noted that the alignment state of the CNTs 1 can be optionally controlled.

[0014] In the CNT composite wire 10, the conductive pattern is formed using one or more CNTs 1. Furthermore, one or more CNTs may be in a spread state or aggregated into a mass to form the CNT 1. Furthermore, the terminal portion of the CNT 1 may be in an open or closed state.

[0015] When measuring CNT 1 with Raman spectroscopy, characteristic peaks appear in the Raman spectrum, which are due to lattice vibrations: D-band around 1,300 cm -1 , G-band around 1,590 cm -1 and G' band around 2,700 cm -1 The G band originates from the in-plane stretching vibration of a six-membered ring structure in a graphite structure, and the D band originates from its defect structure. The intensity ratio of the G band to the D band (G / D ratio) is an index indicating the degree of crystallinity in the CNT 1. In the CNT 1, the G / D ratio is preferably in a range of 5 or more and 30 or less, more preferably 12 or more and 20 or less. When the G / D ratio of the CNT 1 is 5 or more and 30 or less, the CNT surface has few defects and high crystallinity, so the CNT has excellent conductivity.

[0016] The CNT coverage area ratio in the CNT composite wire 10 is preferably 10% or less, more preferably in a range of 0.01% or more and 1% or less, and even more preferably 0.01% or more and 0.1% or less. A CNT coverage area ratio of 10% or less allows the CNT composite wire 10 to have higher conductivity than conventional metal materials while reducing the amount of CNT 1 in the CNT composite wire 10. The CNT coverage area ratio indicates the ratio of the cross-sectional area of ​​the CNT 1 to the sum of the cross-sectional area of ​​the CNT 1 and the cross-sectional area of ​​the thin metal film 2.

[0017] As described above, the CNT occupancy area ratio in the CNT composite wire 10 is preferably 10% or less. Here, the CNT occupancy area ratio is preferably the ratio of the cross-sectional area of ​​the CNT 1 to the sum of the cross-sectional area of ​​the CNT 1 and the cross-sectional area of ​​the thin metal film 2 in the cross section perpendicular to the longitudinal direction of the CNT composite wire 10. In this case, since the proportion of the CNT 1 oriented along the longitudinal direction of the CNT composite wire 10 increases, it is possible to obtain the CNT composite wire 10 with higher conductivity than conventional metal materials while further reducing the amount of the CNT 1.

[0018] As the metal used to form the thin metal film 2, a highly conductive metal is preferably used, for example, at least one selected from the group consisting of copper, a copper alloy, aluminum, and an aluminum alloy. The metal used to form the thin metal film need not be a pure metal but may be an alloy of two or more elements. The thin metal film may be formed from a single layer or multiple layers of two or more metals. The thickness of the thin metal film is not particularly limited and may be, for example, between 30 and 100 nm.

[0019] In the CNT composite wire 10, an amorphous layer of a metal oxide is preferably present at the interface between the CNT 1 and the thin metal film 2. The thickness of the amorphous layer is preferably in a range of 1 nm or more to 5 nm or less. The presence of the amorphous layer relaxes the lattice mismatch between the thin metal film 2 and the CNT 1, and the CNT composite wire 10 with high conductivity can be obtained.

[0020] Any known substrate can be used as the substrate 3 constituting the CNT composite wire 10. For example, a semiconductor substrate (a silicon substrate such as SiO2 / Si or a compound semiconductor substrate), a ceramic substrate, a glass substrate, and the like can be used as long as the insulating properties are ensured.

[0021] Known metal films can be used as metal films 4 and 5 for the electrode 6 for evaluating the electrical properties of the CNT composite wire 10. Metal films made of at least one metal selected from the group consisting of Au, Ti, Ag, Cu, Al, Fe, Ni, Co, Cr, Mo, Nb, and W can be used as metal films 4 and 5. The electrode 6 can be an alloy of two or more previously described metal types or a laminate of two or more previously described metal types, as shown in Fig. 2. The thickness of the electrode 6 is not particularly limited.

[0022] In the CNT composite wire 10 according to the present embodiment, the CNT 1 is aligned along the longitudinal direction (conduction direction) of the CNT composite wire 10 to form a conductive pattern. Even if the CNT 1 has a low concentration, the conductive pattern is formed efficiently. By adding the conductive pattern formed by the CNT 1 to a conductive pattern formed by the thin metal film 2, the CNT composite wire 10 has higher conductivity than conventional metal materials due to the synergistic effect between the conductive pattern of the thin metal film 2 and the conductive pattern of the CNT 1.

[0023] In the CNT composite wire 10 according to the present embodiment, the presence of an amorphous metal oxide layer at the interface between the CNT 1 and the thin metal film 2 relaxes the lattice mismatch between the CNT 1 and the thin metal film 2, thereby increasing the affinity between the CNT 1 and the thin metal film 2. This facilitates the conductive connection between the CNT 1 and the thin metal film 2. Consequently, the CNT composite wire 10 effectively utilizes the conductivity of the CNT 1.

[0024] As described above, the CNT composite wire 10 according to the present embodiment includes the substrate 3, the CNT 1, and the thin metal film 2 formed on the CNT 1. In the CNT 1, the peak ratio (G / D) of the G band to the D band in the Raman spectrum is in a range of 5 or more and 30 or less, and the CNT occupation area ratio, which is the ratio of the cross-sectional area of ​​the CNT 1 to the sum of the cross-sectional area of ​​the CNT 1 and the cross-sectional area of ​​the thin metal film 2, is 10% or less. Therefore, the CNT composite wire 10 has higher conductivity than conventional metal materials even though the amount of CNT 1 in the CNT composite wire 10 has been reduced. <Verfahren zur Herstellung eines CNT-Verbunddrahtes>

[0025] A method for manufacturing the CNT composite wire according to the present embodiment includes a step of spreading a CNT dispersion on a substrate (step (a)), a step of forming a thin metal film on the CNT after step (a) (step (b)), a step of determining the position of the CNT on the thin metal film after step (b) (step (c)), a step of forming a mask on the thin metal film after step (c) and then removing the part not protected by the mask by etching (step (d)), and a step of performing a heat treatment in a reducing atmosphere after step (d) (step (e)). Each step is described below. [Step (a)]

[0026] In step (a), a CNT dispersion is distributed on the substrate 3 ( Fig. 3A).

[0027] The CNT dispersion to be coated on the substrate is prepared by highly dispersing a CNT 1 in a solvent. The solvent for dispersing the CNT 1 is not particularly limited, but an organic solvent is preferably used.

[0028] As the organic solvent, any of the following can be used: an alcohol-based solvent, an amide-based solvent, a ketone-based solvent, and a mixed solvent optionally prepared by combining an alcohol-based solvent, a ketone-based solvent, and an amide-based solvent. As the alcohol-based solvent, at least one selected from the group consisting of methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-methyl-1-propanol, 2-butanol, and 1-methyl-2-propanol can be used. As the amide-based solvent, at least one selected from the group consisting of N,N-dimethylformamide, N-methylpyrrolidone, dimethyl sulfoxide, and dimethylacetamide can be used. As the ketone-based solvent, acetone and / or methyl ethyl ketone can be used.

[0029] A previously described CNT 1 can be used. Furthermore, the CNT 1 can be prepared by removing a metal catalyst such as platinum or amorphous carbon by pre-washing with an acid, or it can be pre-treated with graphitization by heating. Such pretreatment of the CNT 1 can result in highly purified or highly crystallized CNT 1.

[0030] The heating temperature for graphitization is preferably in the range between 500 and 3,500 °C. The heating time is determined taking the heating temperature into account, but is preferably in the range of 10 minutes to 5 hours. The rate of temperature rise to 1,500 °C is preferably in the range of 5 to 30 °C / min.

[0031] Examples of inert gases used to create an inert gas atmosphere during heating include noble gases such as helium and argon gas, and nitrogen.

[0032] In CNT 1, the defects on the CNT surface are reduced by the heat treatment in this step, and the peak ratio (G / D ratio) of the G band to the D band, which is an index of crystallinity in the Raman spectrum, becomes 5 or more, thereby improving the crystallinity.

[0033] The method for highly dispersing the CNT 1 in the solvent is not particularly limited, and the CNT 1 can be dispersed by high-speed stirring after adding the CNT 1 to the solvent. To efficiently disperse the CNT 1, an external force can be applied after adding the CNT 1 to the solvent using an ultrasonic disperser or the like. By performing such a step, a CNT dispersion can be obtained in which the CNT 1 dissolves and is highly dispersed in the solvent.

[0034] The resulting CNT dispersion is dropped and spread onto the substrate 3. The method for spreading the CNT dispersion is not particularly limited, and known methods such as spin coating, casting, and dipping can be used. Furthermore, the CNTs 1 can be purified by annealing after spreading the CNTs and before forming a thin metal film. [Step (b)]

[0035] In step (b), the thin metal film 2 is formed on the CNT 1 ( Fig. 3A).

[0036] The thin metal film 2 is formed on the substrate 3 to which the CNT dispersion was applied in step (a). A previously described metal can be used as the metal for forming the thin metal film 2. The method for forming the thin metal film 2 is not particularly limited and can be appropriately selected according to the type and thickness of the thin film. For example, known methods such as vacuum deposition by resistance heating, chemical vapor deposition (CVD), electron beam deposition, sputtering, and ion plating can be used.

[0037] A thin metal film can be formed after the CNT dispersion has been spread on the substrate on which the mask has been applied. Furthermore, the CNTs can be applied to a substrate on which a thin metal film has previously been formed, and another thin metal film can be formed on top of it. [Step (c)]

[0038] In step (c), the position of the CNT 1 on the thin metal film 2 is determined ( Fig. 3A).

[0039] The position of the CNT 1 can be determined by observing the substrate 3 on which the thin metal film 2 was formed in step (b) using a scanning electron microscope (SEM). Specifically, the position of the CNT 1 can be measured using relative coordinates based on an alignment mark previously formed on the substrate 3. Through this step (c), the alignment state of the CNT 1 in the CNT composite wire 10 can be confirmed and used as a mark for determining the position of the mask formation and etching to be performed in step (d). [Step (d)]

[0040] In step (d), a mask is formed on the thin metal film 2 and then a part not protected by the mask is removed by etching ( Fig. 3B and Fig. 3C).

[0041] As in Fig. As shown in Figure 3B, patterning is performed by forming a resist layer 15 on the surface of the substrate 3 on which the thin metal film 2 was formed, and this resist pattern is used as a mask. After developing the resist pattern, the parts not protected by the mask are selectively etched away. Then, the thin metal film 2 is removed by peeling off the resist layer 15, as shown in Fig. 3C, into a predetermined shape, thereby forming a conductive wiring on the substrate 3.

[0042] Methods for patterning the thin metal film 2 include electron beam lithography, which involves direct drawing with an electron beam, photolithography using a short-wavelength light source, and direct laser drawing. Furthermore, the patterning of the thin metal film 2 can be performed by forming a thin metal film through a mask, such as a stencil mask.

[0043] A well-known varnish can be used. For example, a thermosetting varnish or a UV-curing varnish. For example, an epoxy-based varnish or a urethane-based varnish is used as a thermosetting varnish.

[0044] A known method can be used as the etching method. For example, dry etching or wet etching can be used. In wet etching, a mixed acid such as hydrofluoric acid, nitric acid, acetic acid, phosphoric acid, sulfuric acid, and the like can be used as the etching solution, and the processing can be performed using a dipping method in which the etching solution is immersed or a spin etching method in which the etching solution is sprayed. [Step (e)]

[0045] Step (e) is a step of performing a heat treatment in a reducing atmosphere.

[0046] The substrate 3, on which the thin metal film 2 was patterned in step (d), is subjected to heat treatment in an inert gas atmosphere such as argon and a reducing atmosphere such as hydrogen. This heat treatment enables grain growth while simultaneously removing the oxide layer at the grain boundary formed during the formation of the thin metal film. The heating temperature and heating time during the heat treatment in a reducing atmosphere are not particularly limited.

[0047] It is possible to prepare an electrode by forming a metal film of the above electrode for evaluating electrical properties on the entire substrate obtained in step (e), for example, by a vacuum deposition method.

[0048] As described above, the method for manufacturing a CNT composite wire according to the present embodiment includes: (a) a step of spreading a CNT dispersion on a substrate; (b) a step of forming a thin metal film on the CNT after step (a); (c) a step of determining the position of the CNT on the thin metal film after step (b); (d) a step of forming a mask on the thin metal film after step (c) and then removing the part not protected by the mask by etching; and (e) a step of performing a heat treatment in a reducing atmosphere after step (d). Therefore, according to the manufacturing method according to the present embodiment, it is possible to provide a CNT composite wire having higher conductivity than conventional metal materials while reducing the amount of CNT in the CNT composite wire. Examples

[0049] The present embodiment will be described in more detail below using examples, but is not limited to these examples. [Example 1]

[0050] MWNTs (manufactured by TAIYO NIPPON SANSO CORPORATION, Grade S product) were used for the CNTs. The initial G / D ratio was in the range of 1 to 2, the average diameter was 13 nm, and the length was approximately 150 µm. (Distribution of CNT dispersion (step (a)>)

[0051] A graphite crucible encapsulated with powdered CNTs was placed in a heating furnace (SCC-220 from KURATA GIKEN). The furnace was maintained at a negative pressure of 10 Pa for 30 minutes, and the residual gas in the crucible and the gas adsorbed on the CNT surface were vented (venting step). Subsequently, the power supply to the heater was turned on, and the temperature was increased at a rate of 20 °C / min (heating step). When the temperature in the furnace reached 2,200 °C, argon gas (99.9999%) was supplied to achieve a positive pressure of +40 kPa. When the temperature in the furnace reached the peak temperature of 2,800 °C, the temperature was held constant (holding step). After 2 to 12 hours, the power supply to the heater was turned off, and the interior of the furnace was gradually cooled.

[0052] The CNT dispersion was prepared by immersing the heat-treated CNTs in 2-propanol and dispersing them for 30 minutes using an ultrasonic disperser (PR-1 from THINKY CORPORATION). The CNT concentration in the dispersion was 1 × 10 -5 Mass%. The dispersion was drop-coated onto a SiO2 / Si substrate and spin-coated at 1,000 rpm. (Formation of a thin metal film (step b))

[0053] A thin aluminum film with a thickness of 50 nm was deposited on the substrate on which the CNT dispersion was dispersed using an electron beam evaporation method with a vacuum evaporator (VT-43N, manufactured by CANON A-NELVA CORPORATION). Pure aluminum pellets with a purity of 99.9% or more were used as the deposition source, and the deposition rate was set to approximately 2 Å / s, and deposition was performed. (Positioning of the CNT (step (c))

[0054] After the position of the CNT was determined using a scanning electron microscope (SEM) (MERLIN from Carl Zeiss Co., Ltd.), the position of the CNT was measured using relative coordinates based on an alignment mark prefabricated on the substrate. (Mask formation, etching<Schritt (d)> )

[0055] An electron beam lithography negative resist (OEBR-CAN40, manufactured by TOKYO OHKA KOGYO CO., LTD.) was applied at 3,000 rpm to the surface of the substrate on which the thin aluminum film was formed and prebaked at 110 °C for 1 minute. Subsequently, an electron beam was irradiated at a dose of 25 µC / cm 2The resist pattern was irradiated with an electron beam lithography system (F7000S from ADVANTEST CORPORATION) and, after exposure, baked (PEB) at 110°C for 1 minute. The resist pattern was then developed by immersing it in a developer (NMD-3W, manufactured by TOKYO OHKA KOGYO CO., LTD.) for 50 seconds. After development, the resist pattern was etched by immersing it in a mixed acidic aluminum etching solution (thin metal film, KANTO CHEMICAL CO., INC.) for 1 to 2 minutes at room temperature and then stripped by immersing it in Stripping Solution 104 (manufactured by TOKYO OHKA KOGYO CO., LTD.) for 20 minutes at 60°C. (Heat treatment in a reducing atmosphere<Schritt (e)> )

[0056] An H2 annealing step was performed in a 3.2 vol% H2 / Ar formation gas at 350 °C for 60 minutes to facilitate grain growth while simultaneously removing the grain boundary oxide layer formed during aluminum deposition. Thus, the CNT composite wire according to the present embodiment was obtained. (Formation of an electrode to evaluate electrical properties)

[0057] A positive resist (ZEP-520A from Zeon Corporation) was applied at 6,000 rpm to the surface of the substrate on which the thin aluminum film was formed, and an electron beam was irradiated at a dose of 100 µC / cm 2 with an electron beam lithography system. Then, the pattern was formed by immersing it in a developer (ZED-N50, manufactured by Zeon Corporation) and a rinse (ZMD-B, manufactured by Zeon Corporation) at room temperature. Subsequently, a thin titanium film (metal film 4 in Fig. 2) at 5 nm and a thin gold film (metal film 5 in Fig. 2) at 50 nm by vacuum evaporation, and then an electrode was formed by immersing it in a stripping solution (ZDMAC, manufactured by Zeon Corporation) at 60 °C for 20 minutes. [Evaluation procedure]

[0058] The sample from Example 1 was evaluated according to the following procedure. The results are shown in Fig. 4 to 6. (Sample confirmation)

[0059] The pattern shape of the formed aluminum / CNT composite was examined using a scanning electron microscope (SEM) (MERLIN from Carl Zeiss Co., Ltd.). The thickness of the thin aluminum film was also examined using a scanning probe microscope (AFM5000 from Hitachi High-Tech Corporation) with dynamic force mode. (Evaluation of electrical properties)

[0060] The electrical properties were evaluated by measuring the electrical resistance using a four-terminal method. As described in Fig. As shown in Figure 1, a sample of Example 1, in which four electrodes were formed for evaluating electrical properties, was placed. A constant current was passed between the two outer probes, and the electrical resistance was measured by measuring the potential difference between the two inner probes. A vacuum probe (CPX-4K, manufactured by TOYO Corporation) was used as the measuring device. (Evaluation of the CNT coverage area ratio and the metal-CNT interface)

[0061] The CNT coverage ratio and the state of the aluminum-CNT interface in the CNT composite wire were evaluated by observing the cross-section of the CNT composite wire with a transmission electron microscope (TEM) (JEM-2100F from JEOL Ltd.). The sample was cut to 100 nm or less using a focused ion beam (FIB) system (manufactured by FEI Company Japan Ltd.) and then examined with a TEM. The accelerating voltage at the time of observation was 200 kV, and a TEM and a scanning transmission electron microscope (STEM) were used as observation methods.

[0062] Fig. 6A to 6C show photographs of cross sections of the CNT composite wire, showing the CNT 1, the substrate 3, the thin metal film (aluminum) 2, the electrode (gold / titanium) 6, the protective layer 7, the crystalline aluminum 20, and an amorphous layer 30, respectively. For the CNT coverage ratio in the CNT composite wire, the ratio of the cross-sectional area of ​​the CNT 1 to the sum of the cross-sectional area of ​​the CNT 1 and the cross-sectional area of ​​the thin metal film 2 was calculated based on the obtained photographs.

[0063] Fig. Figure 4 shows the relationship between the specific resistance ratio (resistance ratio) of the CNT composite wire and the specific resistance of the wiring using only aluminum (aluminum wiring), and the G / D ratio of the CNTs contained in the CNT composite wire. When the resistance ratio is less than 1, the resistance of the CNT composite wire was lower than that of the aluminum wiring, indicating that the CNT composite wire was more conductive than the aluminum wiring. As shown in Fig. As shown in Figure 4, it is obvious that at a G / D ratio of less than 12, the resistivity of the CNT composite wire was higher than that of the aluminum wire, and at a G / D ratio of 12 or more, the resistivity of the CNT composite wire was lower than that of the aluminum wire. Therefore, it is obvious that at a G / D ratio of 12 or more, the CNT composite wire had higher conductivity than the aluminum wire, and the resistivity of the CNT composite wire was reduced by 10% or more compared to that of the aluminum wire.

[0064] Fig. Figure 5 shows the relationship between the ratio of the specific resistance of the CNT composite wire to that of the aluminum wire (resistivity ratio) and the CNT coverage area ratio in the CNT composite wire. It is obvious that the resistance ratio decreases with increasing CNT coverage area ratio. As shown in Fig. As shown in Figure 5, it is obvious that even when the CNT coverage area ratio is 0.1% or less, the CNT composite wire has higher conductivity than the aluminum wire because the resistance ratio is less than 1 and the resistance of the CNT composite wire is reduced by 10% or more compared with the aluminum wire.

[0065] It is known that the mean free path of CNTs increases with increasing crystallinity, and the mean free path of CNTs with sufficiently high crystallinity is longer than that of aluminum. As the results in Fig. 4 and Fig. 5, it is therefore assumed that the presence of high crystallinity CNT in aluminum increases the apparent mean free path as a composite wire and decreases the resistivity.

[0066] The aluminum-CNT interface state was then determined using the Fig. Rated 6A to 6C. As in Fig. 6A to 6C, it is obvious that the CNT 1 with a diameter of about 10 nm is present in the thin metal film (aluminum) 2. In Fig. 6C, the highest magnification photograph, it can be confirmed that the amorphous layer 30 with a diameter of about several nm exists at the interface between the crystalline aluminum 20 and the CNT 1. The amorphous layer 30 is composed of a metal oxide (aluminum oxide), and it is believed that the lattice mismatch between the thin metal film (aluminum) 2 and the CNT 1 is relaxed by the amorphous layer 30, thereby achieving high conductivity.

[0067] Although the present embodiment has been described with reference to the above-described examples, the present embodiment is not limited thereto, and various modifications are possible according to the scope of the content of the present embodiment.

[0068] The entire contents of Japanese Patent Application No. 2022-002308 (filed on January 11, 2022) are incorporated herein by reference. List of reference symbols 1 CNT 2 Thin metal film 3 Substrat 6 Electrode 10 CNT composite wire 15 coats of paint 30 Amorphous layer QUOTES CONTAINED IN THE DESCRIPTION

[0000] This list of documents submitted by the applicant was generated automatically and is included solely for the convenience of the reader. This list is not part of the German patent or utility model application. The DPMA assumes no liability for any errors or omissions. Cited patent literature

[0000] 5 896 422

[0004] Japanese Patent Application No. 2022-002308

[0068]

Claims

[1] Carbon nanotube composite wire comprising: a substrate; a carbon nanotube; and a thin metal film formed on the carbon nanotube, wherein the carbon nanotubes have a peak ratio (G / D) of a G band to a D band in a Raman spectrum of 5 or more and 30 or less, and a carbon nanotube coverage area ratio, which is a ratio of a cross-sectional area of ​​the carbon nanotube to a sum of the cross-sectional area of ​​the carbon nanotube and a cross-sectional area of ​​the thin metal film, is 10% or less. [2] The carbon nanotube composite wire according to claim 1, wherein a metal constituting the thin metal film is at least one selected from the group consisting of copper, a copper alloy, aluminum, and an aluminum alloy. [3] The carbon nanotube composite wire according to claim 1 or 2, wherein an amorphous layer of a metal oxide is present at an interface between the carbon nanotube and the thin metal film, and a thickness of the amorphous layer is in a range of 1 nm or more and 5 nm or less. [4] The carbon nanotube composite wire according to any one of claims 1 to 3, wherein the carbon nanotube occupation area ratio is in a range of 0.01% or more and 1% or less. [5] The carbon nanotube composite wire according to any one of claims 1 to 4, wherein the carbon nanotube occupation area ratio is in a range of 0.01% or more and 0.1% or less. [6] The carbon nanotube composite wire according to any one of claims 1 to 5, wherein the peak ratio (G / D) of the G band to the D band in the Raman spectrum is in a range of 12 or more and 20 or less. [7] A method for producing the carbon nanotube composite wire according to any one of claims 1 to 6, the method comprising: (a) a step of spreading a carbon nanotube dispersion on a substrate; (b) a step of forming the thin metal film on the carbon nanotube after step (a); (c) a step of determining a position of the carbon nanotube on the thin metal film after step (b); (d) a step of forming a mask on the thin metal film after step (c) and then removing by etching a part not protected by the mask; and (e) a step of performing a heat treatment in a reducing atmosphere after step (d).

Citation Information

Patent Citations

  • Floor heating system

    JP1983096422U

  • High power mmic devices having bypassed gate transistors

    JP2022002308A