METHOD FOR MANUFACTURING A SILICON CARBIDE-BASED SEMICONDUCTIVE STRUCTURE AND AN INTERMEDIATE COMPOSITE STRUCTURE

FR3120737B1Active Publication Date: 2024-11-15SOITEC SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2021002307
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-09
Publication Date
2024-11-15
Estimated Expiration
2041-03-09

Smart Images

  • Figure 00000019_0000
    Figure 00000019_0000
  • Figure 00000019_0001
    Figure 00000019_0001
  • Figure 00000019_0002
    Figure 00000019_0002
Patent Text Reader

Abstract

The invention relates to a method for manufacturing a semiconducting structure, comprising: a) a step of supplying a temporary substrate made of a material whose coefficient of thermal expansion is close to that of silicon carbide; b) a step of forming an intermediate graphite layer on a front face of the temporary substrate;c) a step of depositing, onto the intermediate layer, a polycrystalline silicon carbide support layer having a thickness between 10 microns and 200 microns, d) a step of transferring a monocrystalline silicon carbide useful layer onto the support layer, directly or via an additional layer, to form a composite structure, said transfer employing molecular adhesion, e) a step of forming an active layer on the useful layer, f) a step of dismantling at an interface of or within the intermediate layer, to form, on the one hand, the semiconductor structure including the active layer, the useful layer, and the support layer, and on the other hand, the temporary substrate. The invention also relates to a composite structure obtained in an intermediate step of the process. Figure to be published with the abstract: No figure;
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: METHOD FOR MANUFACTURING A SEMICONDUCTOR STRUCTURE BASED ON CARBIDE SILICON AND INTERMEDIATE COMPOSITE STRUCTURE FIELD OF THE INVENTION

[0001] The present invention relates to the field of semiconductor materials for microelectronic components. It relates in particular to a method for manufacturing a semiconductor structure comprising an active layer of high-quality monocrystalline silicon carbide comprising or intended to accommodate electronic components, said active layer being arranged on a support layer of polycrystalline silicon carbide. The invention also relates to an intermediate composite structure obtained during said method. TECHNOLOGICAL BACKGROUND OF THE INVENTION

[0002] Interest in silicon carbide (SiC) has increased significantly in recent years because this semiconductor material can increase power handling capacity. SiC is increasingly widely used for the manufacture of innovative power devices to meet the needs of emerging fields of electronics, such as electric vehicles.

[0003] Power devices and integrated power systems based on monocrystalline silicon carbide can handle much higher power density compared to their traditional silicon counterparts, and with smaller active area dimensions. To further limit the dimensions of power devices on SiC, it is advantageous to manufacture vertical rather than lateral components. For this, vertical electrical conduction, between an electrode arranged on the front face of the assembly of components and an electrode arranged on the rear face, must be allowed by said assembly.

[0004] Massive monocrystalline SiC substrates intended for the microelectronics industry nevertheless remain expensive and difficult to supply in large sizes. In addition, when produced on a massive substrate, the set of electronic components often requires the substrate to be thinned on the rear face, typically around 100 microns, to reduce the vertical electrical resistivity and / or to meet size and miniaturization specifications.

[0005] It is therefore advantageous to use thin film transfer solutions to develop composite structures typically comprising a thin film of monocrystalline SiC on a lower cost support substrate, the thin film being used to form the electronic components. A thin film transfer solution A well-known method is the Smart Cut™ process, based on light ion implantation and direct bonding. Such a process makes it possible, for example, to manufacture a composite structure comprising a thin layer of monocrystalline SiC (c-SiC), taken from a c-SiC donor substrate, in direct contact with a polycrystalline SiC (p-SiC) support substrate, and allowing vertical electrical conduction. The support substrate, which must be of sufficient thickness to be compatible with the formation of the components, is finally thinned to obtain the set of electronic components ready for integration. Even if said support substrate is of lower quality, the thinning steps and the loss of material remain cost contributors that one would like to eliminate.

[0006] Also known is document US8436363, which describes a method for manufacturing a composite structure comprising a thin layer of c-SiC arranged on a metal support substrate whose coefficient of thermal expansion is matched with that of the thin layer. This manufacturing method comprises the following steps:

[0007] - the formation of a fragile plane buried in a c-SiC donor substrate, delimiting a thin layer between said buried fragile plane and a front surface of the donor substrate,

[0008] - the deposition of a metallic layer, for example tungsten or molybdenum, on the front surface of the donor substrate to form the support substrate of sufficient thickness to fulfill the role of stiffener,

[0009] - the separation along the buried fragile plane, to form on the one hand, the structure composite comprising the metal support substrate and the thin c-SiC layer, and on the other hand, the rest of the donor substrate in c-SiC.

[0010] The disadvantage of this approach is that a metal support substrate is not always compatible with electronic component manufacturing lines. It may also be necessary to thin the support substrate, depending on the applications. SUBJECT OF THE INVENTION

[0011] The present invention relates to an alternative solution to those of the state of the art, and aims to overcome all or part of the aforementioned drawbacks. It relates in particular to a method for manufacturing a semiconductor structure for electronic components, advantageously vertical, produced on and / or in an active layer of high-quality monocrystalline silicon carbide, which is arranged on a support layer of polycrystalline silicon carbide. The invention also relates to a composite structure obtained at an intermediate stage of said manufacturing method. BRIEF DESCRIPTION OF THE INVENTION

[0012] The invention relates to a method of manufacturing a semiconductor structure, including:

[0013] a) a step of providing a temporary substrate made of a material whose coefficient of thermal expansion is between 3.5.106 / °C and 5.10 6 / °C;

[0014] b) a step of forming an intermediate graphite layer, on a front face of the temporary substrate;

[0015] c) a step of depositing, on the intermediate layer, a support layer of polycrystalline silicon carbide having a thickness of between 10 microns and 200 microns,

[0016] d) a step of transferring a useful layer of monocrystalline silicon carbide onto the support layer, directly or via an additional layer, to form a composite structure, said transfer implementing bonding by molecular adhesion,

[0017] e) a step of forming an active layer on the useful layer,

[0018] f) a disassembly step at an interface of the intermediate layer or in the intermediate layer, to obtain, on the one hand the semiconductor structure including the active layer, the useful layer and the support layer, and on the other hand the temporary substrate.

[0019] According to other advantageous and non-limiting characteristics of the invention, taken alone or in any technically feasible combination:

[0020] • the intermediate layer has a thickness of between 1 micron and 100 microns; • the graphite of the intermediate layer has a grain size between 1 micron and 50 microns; • the graphite of the intermediate layer has a porosity of between 6 and 17%; • the graphite of the intermediate layer has a coefficient of thermal expansion between 4.10 6 / °C and 5.10 6 / °C; • in step b), the intermediate layer is also formed on a peripheral edge of the temporary substrate, and / or a second intermediate layer is formed on a rear face of the temporary substrate; • in step c), the support layer is also deposited on the intermediate layer present on the peripheral edge of the temporary substrate and / or directly on the peripheral edge of the temporary substrate; • step d) of transfer includes: • the introduction of light species into a monocrystalline silicon carbide donor substrate, to form a buried fragile plane defining with the front face of the donor substrate, the useful layer, • assembly of the front face of the donor substrate on the layer support, directly or via an additional layer, by molecular adhesion bonding, • separation along the buried fragile plane to transfer the useful layer onto the support layer; separation takes place during heat treatment at a temperature between 800°C and 1200°C; step e) comprises epitaxial growth of at least one additional layer of doped monocrystalline silicon carbide, on the useful layer, said additional layer forming all or part of the active layer; step e) comprises a heat treatment at a temperature greater than or equal to 1600°C, aimed at activating dopants in the active layer; the method comprises a step e') of producing all or part of electronic components on and / or in the active layer, step e') being interposed between step e) and step f); a removable handle is assembled on the free face of the active layer or of all or part of the electronic components if they are present, prior to step f) of disassembly; the disassembly of step f) is carried out by the propagation of a crack at an interface of the intermediate layer or in the intermediate layer, following the application of a mechanical stress; the disassembly of step f) comprises a lateral chemical etching of all or part of the intermediate layer; the disassembly of step f) includes thermal damage to the graphite of the intermediate layer; the method comprises a step of recycling the temporary substrate from step f); step c) comprises the deposition, on the second intermediate layer present on the rear face of the temporary substrate, of a second support layer of polycrystalline silicon carbide having a thickness of between 10 microns and 200 microns, step d) comprises the transfer of a second useful layer of monocrystalline silicon carbide onto the second support layer, directly or via an additional layer, said transfer implementing bonding by molecular adhesion, step e) comprises the formation of a second active layer on the second useful layer, step f) comprises disassembling at an interface of the second interlayer intermediate or in the second intermediate layer, to obtain another semiconductor structure including the second active layer, the second useful layer and the second support layer.

[0021] The invention also relates to a composite structure comprising:

[0022] - a temporary substrate made of a material whose coefficient of thermal expansion is close to that of silicon carbide,

[0023] - an intermediate layer of graphite, at least arranged on the front face of the temporary substrate,

[0024] - a support layer of polycrystalline silicon carbide having a thickness between 10 microns and 200 microns, arranged on the intermediate layer,

[0025] - a useful layer of monocrystalline silicon carbide, arranged on the layer support.

[0026] According to other advantageous and non-limiting characteristics of the invention, taken alone or in any technically feasible combination:

[0027] • the temporary substrate is made of monocrystalline or polycrystalline silicon carbide; • the useful layer has a thickness between 100nm and 1500nm. BRIEF DESCRIPTION OF THE FIGURES

[0028] Other characteristics and advantages of the invention will emerge from the detailed description of the invention which follows with reference to the appended figures in which:

[0029] [fig. 1] [fig.l] shows a set of electronic components produced according to a manufacturing method in accordance with the invention;

[0030] [fig.2a]

[0031] [fig.2b]

[0032] [fig.2c]

[0033] [fig.2d]

[0034] [fig.2e]

[0035] [fig.2e']

[0036] [fig.2f] Figures 2a, 2b, 2c, 2d, 2e, 2e' and 2f show steps of a manufacturing method according to the invention;

[0037] [fig.3a]

[0038] [fig.3b]

[0039] [fig.3c]

[0040] [fig.3d] Figures 3a to 3d show steps of a particular embodiment of the manufacturing method according to the invention;

[0041] [fig.4a]

[0042] [fig.4b]

[0043] [fig.4c] Figures 4a to 4c show a step d) of transfer of the manufacturing method according to the invention.

[0044] The same references in the figures may be used for elements of the same type. The figures are schematic representations which, for the sake of readability, are not to scale. In particular, the thicknesses of the layers along the z axis are not to scale relative to the lateral dimensions along the x and y axes; and the relative thicknesses of the layers to each other are not necessarily respected in the figures. DETAILED DESCRIPTION OF THE INVENTION

[0045] The present invention relates to a method for manufacturing a semiconductor structure 100 ([fig.l]). By semiconductor structure 100, we mean at least a stack of layers 4,3,2 intended to accommodate a plurality of microelectronic components; we also mean the stack of layers 4,3,2 with said electronic components 40, resulting from a collective manufacturing on and / or in the active layer 4 held in the form of a wafer by a support layer 2, and ready to undergo the steps of singularization prior to packaging.

[0046] The manufacturing method advantageously applies to vertical microelectronic components, which require vertical electrical conduction through the support layer 2, which forms the mechanical support of said components 40.

[0047] The manufacturing method firstly comprises a step a) of providing a temporary substrate 1 made of a material whose coefficient of thermal expansion is close to that of silicon carbide (SiC), namely between 3.5.106 / °C and 5.106 / °C, having a front face 1a, a rear face 1b and a peripheral edge 1c ([fig.2a]). Preferably, the temporary substrate 1 is therefore made of polycrystalline or monocrystalline SiC of low crystalline quality, the role of the temporary substrate 1 being essentially mechanical.

[0048] Other materials compatible with the stated thermal expansion coefficient constraint may be used. It is also required that these materials be compatible with very high temperatures, namely up to approximately 1850°C, taking into account the heat treatments subsequently provided in the process.

[0049] The manufacturing method then comprises a step b) of forming an intermediate layer 12 of graphite.

[0050] Advantageously, certain physical properties of graphite, set out below, are chosen to provide an excellent seed for the deposition of a layer of polycrystalline silicon carbide (p-SiC), called support layer 2 hereinafter, and which will be described with reference to step c) of the method. In particular, the graphite has a grain size of between 1 micron and 50 microns, i.e. falling in the same order of magnitude as the expected grain size for the support layer 2, in the plane of the faces 1a, 1b. The thermal conductivity of the support layer 2 is thus ensured, because the grains of said layer will not be too small; moreover, even if the grain size is caused to increase during the deposition of the support layer 2, we remain within a controlled size range, due to the defined range of grain sizes of the graphite, which limits the roughness at the level of the free surface of the deposited support layer 2. The porosity of the graphite is between 6 and 17%, a restricted range which makes it possible to control the surface roughness of the support layer 2 after its deposition. Typically, it will be possible to limit the surface roughness to less than 1 micron RMS, or even less than 10m RMS, so as to reduce the smoothing treatments after the deposition of the support layer 2. The coefficient of thermal expansion of the intermediate layer 12 is between 4.10 6 / °C and 5.10 6 / °C so as to match the thermal expansion coefficient of silicon carbide, to limit mechanical stresses during treatments (described later in the process) involving high temperatures.

[0051] The temporary substrate 1 provided with the intermediate layer 12 is compatible with temperatures up to 1450°C, when the atmosphere is controlled, i.e. without oxygen. Indeed, if it is exposed to air, the graphite of the intermediate layer 12 begins to burn in a low temperature range, typically 400°C - 600°C. Protected by a protective layer completely encapsulating it, the graphite intermediate layer 12 is compatible with very high temperatures, even above 1450°C.

[0052] According to a particular embodiment of the method, step b) also comprises the formation of the intermediate layer 12 on the peripheral edges 1c of the temporary substrate 1 ([fig.3b]). Step b) may also comprise a second intermediate layer 12' made of graphite, on a rear face 1b of the temporary substrate 1 ([fig.3a], [fig.3b]), with or without an intermediate layer 12 on the peripheral edges 1c.

[0053] Returning to the general description of the method, a step c) of depositing, on the intermediate layer 12, a support layer 2 made of polycrystalline silicon carbide (p-SiC) is then carried out ([fig.2c]). Advantageously, the deposition of the support layer 2 is also carried out on the peripheral edges 1c of the temporary substrate 1, so as to encapsulate and protect the intermediate layer 12 for the subsequent steps of the method.

[0054] The deposition can be carried out by any known technique, in particular by chemical vapor deposition (CVD), at a temperature of the order of 1100°C to 1400°C. For example, a thermal CVD technique such as atmospheric pressure deposition (APCVD for “atmospheric pressure CVD) or low pressure deposition (LPCVD for “low pressure CVD”) can be cited, the precursors being able to be chosen from the me- ethylsilane, dimethyldichlorosilane or dichlorosilane + i-butane. A plasma-enhanced CVD (PECVD) technique can also be used, for example with silicon tetrachloride and methane as precursors; preferably, the frequency of the source used to generate the electrical discharge creating the plasma is around 3.3 MHz, and more generally between 10 kHz and 100 GHz.

[0055] Prior to deposition, conventional cleaning sequences may be applied to the temporary substrate 1 provided with the intermediate layer 12, to eliminate all or part of the particulate, metallic or organic contaminants potentially present on its free faces 1a, 1b.

[0056] The support layer 2 made of p-SiC has a thickness of between 10 microns and 200 microns. This thickness is chosen according to the thickness specifications expected for the semiconductor structure 100. The support layer 2 will, in this structure 100, have the role of mechanical substrate and will potentially have to ensure vertical electrical conduction. To guarantee this latter electrical conduction property (low resistivity), the support layer 2 is advantageously doped with n or p type as required.

[0057] According to the particular embodiment stated above, the deposition of step c) can also be carried out on the second intermediate layer 12', to form a second support layer 2', and / or on the peripheral edge 1c of the temporary substrate 1, as illustrated in [fig.3c]. The role of the second support layer 2', deposited on the rear face 1b of the temporary substrate 1 is to allow the following steps of the method to be carried out on the two faces 1a, 1b of said substrate 1.

[0058] In general, after deposition of the support layer 2 (and potentially of the second support layer 2'), a surface treatment is carried out to improve the surface roughness of the support layer 2 and / or the quality of the edges of the structure, with a view to the following thin layer transfer step.

[0059] Conventional techniques of chemical etching (wet or dry) and / or mechanical grinding and / or chemical-mechanical polishing can be implemented to achieve a surface roughness of the p-SiC of the order of 0.5 nm RMS, preferably less than 0.3 nm RMS (roughness measurement by atomic force microscopy - AFM, on a scan of 20 microns x 20 microns for example). The aforementioned characteristics of the graphite of the intermediate layer 12 nevertheless make it possible to limit the surface treatments to be applied.

[0060] Then, the manufacturing method according to the invention comprises a step d) of transferring a useful layer 3 of monocrystalline silicon carbide (c-SiC) directly onto the support layer 2 or via an additional layer, to form a composite structure 10 ([fig.2d]). The transfer implements bonding by molecular adhesion, and by consequently a bonding interface 5. The additional layer can be formed on the side of the useful layer 3 and / or on the side of the support layer 2, to promote said bonding.

[0061] Advantageously, and as is known with reference to the Smart Cut™ process, transfer step d) comprises:

[0062] - the introduction of light species into a donor substrate 30 made of silicon carbide monocrystalline, to form a buried fragile plane 31, defining with the front face 30a of the donor substrate 30, the useful layer 3 ([fig.4a]),

[0063] - the assembly of the front face 30a of the donor substrate 30 on the support layer 2, directly or via an additional layer, by molecular adhesion bonding, along a bonding interface 5 ([fig.4b]),

[0064] - separation along the buried fragile plane 31 to transfer the useful layer 3 onto support layer 2 ([fig.4c]).

[0065] The light species are preferably hydrogen, helium or a co-implantation of these two species, and are implanted at a determined depth in the donor substrate 30, consistent with the thickness of the targeted useful layer 3 ([fig.4a]). These light species will form, around the determined depth, microcavities distributed in a thin layer parallel to the free surface 30a of the donor substrate 30, i.e. parallel to the plane (x,y) in the figures. This thin layer is called the buried fragile plane 31, for the sake of simplification.

[0066] The implantation energy of the light species is chosen so as to reach the determined depth. For example, hydrogen ions will be implanted at an energy between 10 keV and 250 keV, and at a dose between 5E16 / cm2 and Ie 17 / cm2, to delimit a useful layer 3 having a thickness of the order of 100 to 1500 nm. Note that a protective layer may be deposited on the front face 30a of the donor substrate 30, prior to the ion implantation step. This protective layer may be composed of a material such as silicon oxide or silicon nitride for example. It may be kept for the following step, or removed.

[0067] The assembly of the donor substrate 30 on the support layer 2 takes place at their respective front / free faces and forms a bonded stack, along the bonding interface 5 ([fig.4b]). As is well known per se, bonding by molecular adhesion does not require an adhesive material, bonds being established at the atomic scale between the assembled surfaces. Several types of bonding by molecular adhesion exist, which differ in particular by the conditions of temperature, pressure, atmosphere or treatments prior to bringing the surfaces into contact. We can cite bonding at room temperature with or without prior plasma activation of the surfaces to be assembled, bonding by atomic diffusion ("Atomic diffusion bonding” or ADB according to Anglo-Saxon terminology), surface-activated bonding (“SAB”), etc.

[0068] The assembly step may comprise, prior to bringing the faces to be assembled into contact, conventional cleaning sequences, surface activation or other surface preparations, capable of promoting the quality of the bonding interface 5 (low defectivity, high adhesion energy).

[0069] As already mentioned, the front face 30a of the donor substrate 30 and / or the free face of the support layer 2 may possibly comprise an additional layer, for example metallic (tungsten, etc.) or doped semi-conductor (silicon, etc.) to promote vertical electrical conduction, or insulating (silicon oxide, silicon nitride, etc.) for applications not requiring vertical electrical conduction. The additional layer is capable of promoting bonding by molecular adhesion, in particular by erasing residual roughness or surface defects present on the faces to be assembled. It may undergo planarization or smoothing treatments, to achieve a roughness lower than 1 nm RMS, or even lower than 0.5 nm RMS, favorable to bonding.

[0070] The separation along the buried fragile plane 31 is usually carried out by applying a heat treatment at a temperature between 800°C and 1200°C ([fig.4c]). Such a heat treatment induces the development of cavities and microcracks in the buried fragile plane 31, and their pressurization by the light species present in gaseous form, until the propagation of a fracture along said fragile plane 31. Alternatively or jointly, a mechanical stress can be applied to the bonded assembly and in particular at the buried fragile plane 31, so as to propagate or help to propagate mechanically the fracture leading to the separation. At the end of this separation, we obtain on the one hand the composite structure 10 comprising the temporary substrate 1, the intermediate layer 12 in graphite, the support layer 2 in p-SiC and the useful layer 3 transferred in c-SiC, and on the other hand, the remainder 30' of the donor substrate.The useful layer 3 typically has a thickness between 100nm and 1500nm. The level and type of doping of the useful layer 3 is defined by the choice of the properties of the donor substrate 30 or can be adjusted subsequently via known techniques for doping semiconductor layers.

[0071] The free surface of the useful layer 3 is usually rough after separation: for example, it has a roughness of between 5nm and 100nm RMS (AFM, 20 micron x 20 micron scan). Cleaning and / or smoothing steps can be applied to restore a good surface condition (typically, a roughness of less than a few angstroms RMS on a 20 micron x 20 micron scan by AFM).

[0072] Alternatively, the free surface of the useful layer 3 may remain rough, as separated, when the following step of the method tolerates this roughness.

[0073] In the particular embodiment implementing a second intermediate layer 12' and a second support layer 2' arranged on the rear face 1b of the temporary substrate 1, step d) may also comprise the transfer of a second useful layer 3' in c-SiC onto the second support layer 2', via a second bonding interface 5' ([fig.3d]).

[0074] The manufacturing method according to the invention then comprises a step e) of forming an active layer 4 on the useful layer 3 ([fig.2e]).

[0075] Advantageously, the active layer 4 is produced by epitaxial growth of an additional layer of doped monocrystalline silicon carbide, on the useful layer 3. This epitaxial growth is carried out in the conventional temperature range, namely between 1500°C and 1900°C and forms an additional layer with a thickness of the order of 1 micron to a few tens of microns, depending on the electronic components targeted.

[0076] The presence of a protective layer on the edges of the intermediate graphite layer 12, in the composite structure 10, is required so that the aforementioned very high temperature treatments do not damage the graphite. As mentioned previously, this protective layer may, for example, consist of a layer of polycrystalline silicon carbide (deposited, for example, at the same time as the support layer 2) or amorphous silicon carbide.

[0077] The manufacturing method according to the invention may further comprise a step e') of producing all or part of the electronic components 40 on and / or in the active layer 4 ([fig.2e]'). The electronic components 40 may for example consist of transistors or other high voltage and / or high frequency components.

[0078] For their manufacture on and / or in the active layer 4, conventional steps of cleaning, deposition, lithography, implantation, etching, planarization and heat treatment are carried out. In particular, among the heat treatments mentioned, some aim to activate dopants introduced locally into the active layer 4 (or the useful layer 3), and are typically carried out at a temperature greater than or equal to 1600°C.

[0079] Note that in the particular embodiment implementing a second support layer 2' on the rear face of the temporary substrate 1, step e) may also comprise the formation of a second active layer on the second useful layer 3'; and step e') may comprise the development of all or part of second electronic components on and / or in said second active layer.

[0080] Finally, the manufacturing method according to the invention comprises a step f) of disassembly at an interface of the intermediate layer 12 and / or in the intermediate layer 12 to form on the one hand the semiconductor structure 100 including the active layer 4, the useful layer 3 and the support layer 2, and on the other hand the substrate temporary 1 (figure 2f (i)), and potentially the electronic components 40 (figure 2f (ii)), if a step e' has been carried out.

[0081] Several disassembly variants, at the level of the intermediate layer 12 (and potentially at the level of the second intermediate layer 12', in the particular embodiment) can be implemented for this step.

[0082] According to a first variant, step f) comprises mechanical disassembly by propagation of a crack in the intermediate layer 12, and / or at the interface between the intermediate layer 12 and the support layer 2, and / or between the intermediate layer 12 and the temporary substrate 1. The crack propagates substantially parallel to the plane of the intermediate layer 12, following the application of a mechanical stress. For example, the insertion of a beveled tool opposite the intermediate layer 12 makes it possible to initiate and propagate an opening at a fragile interface: since graphite has a lower cohesion energy along the z axis, the cracking will preferentially occur in the intermediate layer 12 or at interfaces, until the complete separation between the semiconductor structure 100 and the temporary substrate 1.Advantageously, the protective layer present on the edges of the temporary substrate 1 is removed, by dry or wet etching for example, to promote the initiation of the crack in the graphite.

[0083] According to a second variant, step f) comprises a chemical disassembly between the semiconductor structure 100 and the temporary substrate 1, by lateral chemical etching. The protective layer (p-SiC) located on the peripheral edges 1c of the temporary substrate 1 (and in particular on the edges of the intermediate layer 12) in the composite structure 10 must be removed chemically or mechanically, to allow access to the graphite. Then, the lateral chemical etching of the intermediate layer 12 can use a solution based on nitric acid and / or sulfuric acid, for example a solution of concentrated sulfuric acid and potassium dichromate or a solution of sulfuric acid, nitric acid and potassium chlorate. A chemical etching using an alkaline solution (of the potassium hydroxide (KOH) or sodium hydroxide (NaOH) type) can also be applied.

[0084] Of course, care will be taken to protect the free face and the edges of the active layer 4 and the electronic components 40 if they are present, and / or to limit the time of contact with the etching solution, to avoid damaging them during this chemical disassembly.

[0085] According to a third variant, step f) comprises mechanical disassembly by thermal damage to the graphite making up the intermediate layer 12. Here again, it is required to remove the protective layer present at least on the edges of the temporary substrate 1 to provide access to the intermediate layer 12.

[0086] Disassembly by thermal damage can be carried out at a temperature between 600°C and 1000°C, in the presence of oxygen: the graphite of the intermediate layer 12 is then burnt and crumbles, thus separating the semiconductor structure 100 from the temporary substrate 1.

[0087] Of course, in the case where the electronic components 40 were produced during step e'), this disassembly variant can only be applied if said components 40 are compatible with the temperature applied.

[0088] Note that the aforementioned variants may possibly be combined with each other, according to all technically feasible combinations.

[0089] Whatever the variant implemented, the dismantling of the temporary substrate 1 may leave residues 12r of the intermediate layer 12, on the rear face 2b of the support layer 2 and / or on the front face of the temporary substrate 1. These residues may be eliminated by mechanical grinding, by chemical-mechanical polishing, by chemical etching and / or by thermal damage.

[0090] Chemical-mechanical polishing or chemical etching techniques may also be used to reduce the roughness of the rear face 2b of the support layer 2, if necessary, after removal of the residues 12r.

[0091] In the particular embodiment mentioned above, for which a second active layer is present on the side of the rear face 1b of the temporary substrate 1, step f) of dismantling the temporary substrate 1 also makes it possible to form a second semiconductor structure including the second active layer, the second useful layer 3' and the second support layer 2'.

[0092] If the semiconductor structure 100 must be handled during and after the removal of the temporary substrate 1, and its total thickness is insufficient for its mechanical maintenance during this handling, it is possible to use a removable handle: the latter is arranged on the active layer 4 or on the components 40, and temporarily secured to them, to carry out the handling up to the singulation step for example.

[0093] The semiconductor structure 100 obtained at the end of the manufacturing method according to the invention comprises an active layer 4 advantageously finalized with electronic components 40 and arranged on a support layer 2 having the thickness targeted for the application. No mechanical thinning involving a significant loss of material is required. The support layer 2 is made of good quality p-SiC (because it is deposited at relatively high temperatures) but at low cost compared to a solid substrate of monocrystalline or polycrystalline SiC which would have had to be significantly thinned before singulating the components 40. The temporary substrate 1, after disassembly, is recovered for recycling, which also constitutes an economic advantage.

[0094] The intermediate graphite layer 12 allows simple disassembly of the composite structure 10 after the active layer 4 (and preferably all or part of the components) has been formed, while ensuring mechanical stability for the composite structure 10 during the very high temperature heat treatments applied for the production of the active layer 4.

[0095] The choice of the physical characteristics of the intermediate graphite layer 12 (grain size, porosity, coefficient of thermal expansion) ensures the formation of a support layer 2 allowing a robust and high-quality composite structure 10 to be obtained, and allowing a reliable and high-performance semiconductor structure 100 to be obtained. The performance of the components 40 comes in particular from the fact that the composite structure 10 allows treatments at very high temperatures for the formation of the active layer 4.

[0096] The invention also relates to a composite structure 10, described previously with reference to the manufacturing method, and corresponding to an intermediate structure obtained during said method (figures 2d, 3d).

[0097] The composite structure 10 comprises:

[0098] - a temporary substrate 1 made of a material whose coefficient of thermal expansion is close to that of silicon carbide,

[0099] - an intermediate layer 12 made of graphite, at least arranged on the front face of the temporary substrate 1,

[0100] - a support layer 2 made of polycrystalline silicon carbide having a thickness between 10 microns and 200 microns, arranged on the intermediate layer 12,

[0101] - a useful layer 3 of monocrystalline silicon carbide, arranged on the layer support 2.

[0102] Preferably, the graphite of the intermediate layer 12 has a grain size of between 1 micron and 50 microns, a porosity of between 6 and 17%, and / or a coefficient of thermal expansion of between 4.10 6 / °C and 5.10 6 / °C. The advantages linked to these characteristics have been previously stated.

[0103] Preferably, the useful layer 3 has a thickness of between 100 nm and 1500 nm. The intermediate layer 12 has a thickness of between 1 micron and 100 microns, or between 10 microns and 100 microns; the temporary substrate 1 has a thickness of between 300 microns and 800 microns.

[0104] For applications for vertical microelectronic components, the support layer 2 advantageously has good electrical conductivity, i.e. between 0.015 and 0.03 ohm.cm, high thermal conductivity, i.e. greater than or equal to 200 Wm *.K1 and a coefficient of thermal expansion similar to that of the useful layer 3, i.e. typically between 3.8.10 6 / °C and 4.2.10 6 / °C at room temperature.

[0105] The intermediate layer 12 and / or the temporary substrate 1 can advantageously have a thermal conductivity of between 5 Wm *.K1 and 500 Wm *.K so as to ensure a uniform temperature on the temporary substrate 1 during the very high temperature heat treatment stages of the manufacturing process. This improves in particular the uniformity of the deposited layers and the reproducibility of the physical properties of the layers and components produced.

[0106] Finally, as has been described with reference to the manufacturing method according to the invention, the composite structure 10 may be “double-sided”, that is to say comprise:

[0107] - a second intermediate layer 12' in graphite, arranged on the rear face 1b of temporary substrate 1,

[0108] - a second support layer 2' made of polycrystalline silicon carbide having a thickness of between 10 microns and 200 microns, arranged on the second intermediate layer 12, - a second useful layer 3' of monocrystalline silicon carbide, arranged on the second support layer 2' ([fig.3d]).

[0109] Such a composite structure 10 allows the formation of two active layers 40, on the first 3 and the second 3' useful layer, and at the end of the manufacturing method according to the invention, the obtaining of two semiconductor structures 100, from a single temporary substrate 1.

[0110] Of course, the invention is not limited to the embodiments and examples described, and variant embodiments may be made without departing from the scope of the invention as defined by the claims.

Claims

Claims

1. Method for manufacturing a semiconductor structure (100), comprising: a) a step of providing a temporary substrate (1) made of a material whose coefficient of thermal expansion is between 3.5.10 6 / °C and 5.106 / °C; b) a step of forming an intermediate layer (12) of graphite, on a front face (la) of the temporary substrate (1); c) a step of depositing, on the intermediate layer (12), a support layer (2) of polycrystalline silicon carbide having a thickness of between 10 microns and 200 microns, d) a step of transferring a useful layer (3) of monocrystalline silicon carbide onto the support layer (2), directly or via an additional layer, to form a composite structure (10), said transfer implementing bonding by molecular adhesion, e) a step of forming an active layer (4) on the useful layer (3), f) a step of dismantling at an interface of the intermediate layer (12) or in the intermediate layer (12), to obtain, on the one hand, the semiconductor structure (100) including the active layer (4), the useful layer (3) and the support layer (2), and on the other hand, the temporary substrate (D-.

2. Manufacturing method according to the preceding claim, in which the intermediate layer (12) has a thickness of between 1 micron and 100 microns.

3. Manufacturing method according to one of the preceding claims, in which the graphite of the intermediate layer (12) has a grain size of between 1 micron and 50 microns.

4. Manufacturing method according to one of the preceding claims, in which the graphite of the intermediate layer (12) has a porosity of between 6 and 17%.

5. Manufacturing method according to one of the preceding claims, in which the graphite of the intermediate layer (12) has a coefficient of thermal expansion of between 4.10 6 / °C and 5.10 6 / °C.

6. Manufacturing method according to one of the preceding claims, wherein, in step b), the intermediate layer (12) is also formed on a peripheral edge (le) of the temporary substrate (1), and / or a second intermediate layer (12') is formed on a rear face (1b) of the temporary substrate (1).

7. Manufacturing method according to one of the preceding claims, wherein, in step c), the support layer (2) is also deposited on an intermediate layer (12) present on the peripheral edge (le) of the temporary substrate (1) and / or directly on the peripheral edge (le) of the temporary substrate (1).

8. Manufacturing method according to one of the preceding claims, in which the transfer step d) comprises: - the introduction of light species into a donor substrate (30) made of monocrystalline silicon carbide, to form a buried fragile plane (31) defining with the front face (30a) of the donor substrate (30), the useful layer (3), - the assembly of the front face (30a) of the donor substrate (30) on the support layer (2), directly or via an additional layer, by bonding by molecular adhesion, - the separation along the buried fragile plane (31) to transfer the useful layer (3) onto the support layer (2).

9. Manufacturing method according to one of the preceding claims, in which step e) comprises epitaxial growth of at least one additional layer of doped monocrystalline silicon carbide, on the useful layer (3), said additional layer forming all or part of the active layer (4).

10. Manufacturing method according to the preceding claim, in which step e) comprises a heat treatment at a temperature greater than or equal to 1600°C, aimed at activating dopants in the active layer (4).

11. Manufacturing method according to one of the preceding claims, comprising a step e') of producing all or part of electronic components (40) on and / or in the active layer (4), step e') being interposed between step e) and step f).

12. Manufacturing method according to one of the preceding claims, in which a removable handle is assembled on the free face of the active layer (4) or of all or part of the electronic components (40) if they are present, prior to step f) of disassembly.

13. Manufacturing method according to one of the preceding claims, in which: - the disassembly of step f) is carried out by the propagation of a crack at an interface of the intermediate layer (12) or in the inter- intermediate layer (12), following the application of mechanical stress, and / or - the disassembly of step f) comprises lateral chemical etching of all or part of the intermediate layer (12), and / or - the disassembly of step f) comprises thermal damage to the graphite of the intermediate layer (12).

14. Manufacturing method according to claim 6, wherein: - step c) comprises the deposition, on the second intermediate layer (12') present on the rear face (1b) of the temporary substrate (1), of a second support layer (2') of polycrystalline silicon carbide having a thickness of between 10 microns and 200 microns, - step d) comprises the transfer of a second useful layer (3') of monocrystalline silicon carbide onto the second support layer (2'), directly or via an additional layer, said transfer implementing bonding by molecular adhesion, - step e) comprises the formation of a second active layer on the second useful layer (3'), and - step f) comprises the disassembly at an interface of the second intermediate layer (12') or in the second intermediate layer (12'), to obtain another semiconductor structure (100) including the second active layer,the second useful layer (3') and the second support layer (2').,

15. Composite structure (10) comprising: - a temporary substrate (1) made of a material whose coefficient of thermal expansion is close to that of silicon carbide, - an intermediate layer (12) made of graphite, at least arranged on the front face of the temporary substrate (1), - a support layer (2) made of polycrystalline silicon carbide having a thickness of between 10 microns and 200 microns, arranged on the intermediate layer (12), - a useful layer (3) made of monocrystalline silicon carbide, arranged on the support layer (2).

16. Composite structure (10) according to the preceding claim, in which the temporary substrate (1) is made of monocrystalline or polycrystalline silicon carbide, and the useful layer (3) has a thickness of between 100 nm and 1500 nm.