COMBUSTION-RESISTANT THERMOPLASTIC COMPOSITION
By integrating a lignin-based filler treated with hydrothermal carbonization into thermoplastic compositions, the combustion resistance and thermal stability are enhanced, addressing the need for environmentally friendly materials with reduced combustion rates.
Patent Information
- Application Number
- FR2022010767
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-10-21
- Filing Date
- 2022-10-18
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-10-18
AI Technical Summary
Existing thermoplastic compositions lack sufficient combustion resistance, and there is a need for environmentally friendly materials that enhance thermal stability while reducing combustion rates.
Incorporating a lignin-based filler prepared through hydrothermal carbonization treatment into thermoplastic compositions, which comprises 62-70% carbon and up to 3% ash by weight, to create a combustion-resistant thermoplastic composition with a reduced combustion rate of at least 20% compared to untreated lignin-based compositions.
The lignin-based filler significantly improves the combustion resistance of thermoplastic compositions, achieving a minimum 20% reduction in combustion rate, while maintaining thermal stability and environmental sustainability.
Abstract
Description
Title of the invention: COMBUSTION-RESISTANT THERMOPLASTIC COMPOSITION Technical field
[0001] The present disclosure relates to a combustion-resistant thermoplastic composition. The present disclosure further relates to the use of a lignin-based filler for improving the combustion resistance of a thermoplastic composition. The present disclosure further relates to a method for producing a combustion-resistant thermoplastic composition. The present disclosure further relates to an article and use of the combustion-resistant thermoplastic composition. BACKGROUND
[0002] From a sustainability and circular economy perspective, it is desired to use bio-based materials in thermoplastic compositions or materials, such as packaging materials. The thermal stability of thermoplastic compositions is also an important property for the processing of these materials. Providing environmentally friendly solutions with regard to the thermoplastic composition must be achieved. SUMMARY
[0003] A combustion resistant thermoplastic composition is disclosed.The combustion-resistant thermoplastic composition comprises at least one polymer and a lignin-based filler, wherein the lignin-based filler is prepared from a lignin material subjected to a hydrothermal carbonization treatment, and wherein the lignin-based filler comprises carbon in a total amount of from 62 to 70% by weight and ash in a total amount of at most 3% by weight, and wherein the burning rate of the combustion-resistant thermoplastic composition is at least 20 percent lower than the burning rate of a corresponding thermoplastic composition, wherein the corresponding thermoplastic composition is prepared in a manner otherwise similar to the combustion-resistant thermoplastic composition but wherein the lignin material used to prepare the lignin-based filler has not been subjected to a hydrothermal carbonization treatment.
[0004] Further disclosed is the use of a lignin-based filler for improving the combustion resistance of a thermoplastic composition. The combustion-resistant thermoplastic composition comprises at least one polymer and the lignin-based filler, wherein the lignin-based filler is prepared from of a lignin material subjected to a hydrothermal carbonization treatment, and wherein the lignin-based filler comprises carbon in a total amount of from 62 to 70% by weight and ash in a total amount of not more than 3% by weight, and wherein the burning rate of the combustion-resistant thermoplastic composition is at least 20 percent lower than the burning rate of a corresponding thermoplastic composition, wherein the corresponding thermoplastic composition is prepared in a manner otherwise similar to the combustion-resistant thermoplastic composition but wherein the lignin material used to prepare the lignin-based filler has not been subjected to a hydrothermal carbonization treatment.
[0005] A method of producing a combustion-resistant thermoplastic composition comprising at least one polymer and a lignin-based filler is further disclosed, wherein the method comprises:
[0006] - providing at least one polymer and a lignin-based filler, wherein the lignin-based feedstock is prepared from a lignin material subjected to a hydrothermal carbonization treatment, wherein the lignin-based feedstock comprises carbon in a total amount of from 62 to 70% by weight and ash in a total amount of not more than 3% by weight; and
[0007] - the combination of at least one polymer and the lignin-based filler for form the combustion-resistant thermoplastic composition, where
[0008] the burning rate of the combustion-resistant thermoplastic composition is at least 20 percent lower than the burning rate of a corresponding thermoplastic composition, wherein the corresponding thermoplastic composition is prepared in a manner otherwise similar to the combustion-resistant thermoplastic composition but wherein the lignin material used to prepare the lignin-based filler has not been subjected to a hydrothermal carbonization treatment.
[0009] An article comprising the combustion-resistant thermoplastic composition as defined in the present description is further disclosed.
[0010] The use of the thermoplastic composition as defined in the present description in a package, a housing, an automobile part, an aeronautical part, a marine part, a machine part, a sports equipment, a sports equipment part, a leisure equipment, a leisure equipment part, a tool, a tool part, a pipe, a membrane, a tube, a fitting, a bottle, a film, a sachet, a bag, a textile, a rope, a container, a tank, an electrical component, an electronic component, a part for the production of energy, a toy, a household appliance, a kitchen utensil, a tableware, a floor covering, a fabric, a medical application, a material in contact with food, a building material, a drinking water application and / or furniture is further disclosed. DETAILED DESCRIPTION
[0011] A combustion resistant thermoplastic composition is disclosed.The combustion-resistant thermoplastic composition comprises at least one polymer and a lignin-based filler, wherein the lignin-based filler is prepared from a lignin material subjected to a hydrothermal carbonization treatment, and wherein the lignin-based filler comprises carbon in a total amount of from 62 to 70% by weight and ash in a total amount of at most 3% by weight, and wherein the burning rate of the combustion-resistant thermoplastic composition is at least 20 percent lower than the burning rate of a corresponding thermoplastic composition, wherein the corresponding thermoplastic composition is prepared in a manner otherwise similar to the combustion-resistant thermoplastic composition but wherein the lignin material used to prepare the lignin-based filler has not been subjected to a hydrothermal carbonization treatment.
[0012] The use of a lignin-based filler to improve the combustion resistance of a thermoplastic composition is further disclosed.The combustion-resistant thermoplastic composition comprises at least one polymer and the lignin-based filler, wherein the lignin-based filler is prepared from a lignin material subjected to a hydrothermal carbonization treatment, and wherein the lignin-based filler comprises carbon in a total amount of from 62 to 70% by weight and ash in a total amount of at most 3% by weight, and wherein the burning rate of the combustion-resistant thermoplastic composition is at least 20 percent lower than the burning rate of a corresponding thermoplastic composition, wherein the corresponding thermoplastic composition is prepared in a manner otherwise similar to the combustion-resistant thermoplastic composition but wherein the lignin material used to prepare the lignin-based filler has not been subjected to a hydrothermal carbonization treatment.
[0013] A method of producing a combustion-resistant thermoplastic composition comprising at least one polymer and a lignin-based filler is further disclosed, wherein the method comprises:
[0014] - providing at least one polymer and a lignin-based filler, wherein the lignin-based feedstock is prepared from a lignin material subjected to a hydrothermal carbonization treatment, wherein the lignin-based feedstock comprises carbon in a total amount ranging from 62 to 70% by weight and ash in a total quantity of not more than 3% by weight; and
[0015] - the combination of at least one polymer and the lignin-based filler for form the combustion-resistant thermoplastic composition, where
[0016] the burning rate of the combustion-resistant thermoplastic composition is at least 20 percent lower than the burning rate of a corresponding thermoplastic composition, wherein the corresponding thermoplastic composition is prepared in a manner otherwise similar to the combustion-resistant thermoplastic composition but wherein the lignin material used to prepare the lignin-based filler has not been subjected to a hydrothermal carbonization treatment.
[0017] An article comprising the combustion-resistant thermoplastic composition as defined in the present specification is further disclosed. In one embodiment, the thermoplastic composition has been formed into an article by extrusion, injection molding, compression molding, blow molding, injection blow molding, injection stretch blow molding, thermoforming, vacuum forming, melt spinning, electrospinning, melt blowing, film blowing, film casting, extrusion coating, rotational molding, coextrusion, lamination, calendering, fused deposition, or any combination thereof.
[0018] The use of the thermoplastic composition as defined in the present description in a package, a housing, an automotive part, an aeronautical part, a marine part, a machine part, a sports equipment, a sports equipment part, a leisure equipment, a leisure equipment part, a tool, a part of a tool, a pipe, a membrane, a tube, a fitting, a bottle, a film, a sachet, a bag, a textile, a rope, a container, a tank, an electrical component, an electronic component, a part for energy production, a toy, a household appliance, a kitchen utensil, tableware, a floor covering, a fabric, a medical application, a food contact material, a building material, a drinking water application and / or furniture is further disclosed.
[0019] Thus, the term "corresponding thermoplastic composition" is to be understood as referring to a thermoplastic composition that has been prepared in a manner otherwise similar to the combustion-resistant thermoplastic composition but where the hydrothermal carbonization treatment has not been used to prepare the lignin-based filler. That is, all other components and their amounts as well as the process steps used to prepare the corresponding thermoplastic composition have remained the same as in the preparation of the combustion-resistant thermoplastic composition but the step of using the hydrothermal carbonization treatment of the lignin material is omitted when preparing the lignin-based filler for the corresponding thermoplastic composition.
[0020] The burning rate can be determined according to ISO 3795:1989 (Road vehicles, tractors and agricultural and forestry machinery - Determination of the burning behaviour of interior materials (Horizontal combustion test); conditioning: 23°C and 50% relative humidity (RH), sample size: 147 mm x 100 mm x 2 mm).
[0021] In one embodiment, the burning rate of the combustion-resistant thermoplastic composition is at least 30 percent, or at least 40 percent, or at least 50 percent, or at least 60 percent, or at least 70 percent, lower than the burning rate of the corresponding thermoplastic composition.
[0022] The thermoplastic composition may contain 0.1 to 65% by weight, or 0.3 to 60% by weight, or 0.5 to 50% by weight, or 1 to 40% by weight, or 1.2 to 30% by weight, or 1.5 to 20% by weight, or 2 to 10% by weight, or 2.5 to 5% by weight, of the lignin-based filler relative to the total weight of the combustion-resistant thermoplastic composition. In one embodiment, the combustion-resistant thermoplastic composition comprises the lignin-based filler in a total amount ranging from 0.1 to 60% by weight, or from 0.5 to 50% by weight, or from 1 to 45% by weight, relative to the total weight of the combustion-resistant thermoplastic composition.
[0023] "Total weight" is to be understood in this description, unless otherwise indicated, as the weight of all components of the combustion-resistant thermoplastic composition, including any moisture.
[0024] A thermoplastic composition, or a thermo-softenable plastic composition as it may also be called, is a plastic polymer material that becomes pliable or moldable at a certain elevated temperature and solidifies upon cooling.
[0025] The thermoplastic composition may be prepared using at least one polymer and a lignin-based filler. In the thermoplastic composition, the at least one polymer and the lignin-based filler may be mixed together but may not have reacted with each other. Other components or materials, such as additives, lubricants, stabilizers, antioxidants, other fillers, etc., may also be used to prepare the thermoplastic composition.
[0026] In one embodiment, combining the at least one polymer and the lignin-based filler comprises preparing a masterbatch and then composing the polymer and the lignin-based filler. In one embodiment, combining the at least one polymer and the lignin-based filler comprises combining the at least one polymer, the lignin-based filler, and additives and molding the formed combustion-resistant thermoplastic composition. In one embodiment, combining the at least one polymer and the lignin-based filler comprises directly compounding the at least one polymer and the lignin-based filler at processing temperatures appropriate for each polymer type. The processing temperatures are elevated temperatures and are defined by the polymer supplier for each polymer.
[0027] In preparing the combustion-resistant thermoplastic composition, a so-called masterbatch may first be prepared using a polymer and the lignin-based filler. The masterbatch may be prepared by mixing the polymer and the lignin-based filler at an elevated temperature. Also other additives, lubricants, stabilizers, antioxidants, other fillers, etc., as required may be included in the masterbatch. A masterbatch is generally considered to be a solid product (normally plastic, rubber, or elastomer) in which pigments or fillers are optimally dispersed at a high concentration in a carrier material.The carrier material is compatible with the main plastic material into which it will be mixed during molding, whereby the final plastic product, i.e. the thermoplastic composition, obtains the color or properties of the masterbatch.
[0028] Alternatively, the thermoplastic composition is directly compounded at an elevated temperature from the polymer(s) and the lignin-based filler. In addition, other additives, lubricants, stabilizers, antioxidants, other fillers, etc., as required, may be directly compounded with the polymer and the lignin-based filler.
[0029] The temperature used when combining the at least one polymer and the lignin-based filler may vary depending on the type of polymer used. The appropriate temperature to be used for each polymer is readily available to those skilled in the art. In addition, polymer suppliers define appropriate processing temperatures for different polymers. Generally, temperatures ranging, for example, from 150 to 440°C, or from 180 to 350°C, or from 200 to 300°C, may be used.
[0030] The thermoplastic composition may comprise at least one polymer, for example at least two different polymers, at least three different polymers, at least four different polymers, etc. The polymer may be any polymer selected from the group consisting of thermoplastic polymers or a combination of different thermoplastic polymers. The polymer may be selected from one or more of the following: polyethylene, polypropylene, polystyrene, ethylene vinyl acetate (EVA), polybutylene adipate terephthalate (PBAT), polyamide, polyacrylate, polyester, acrylonitrile butadiene styrene (ABS), polycarbonate, polylactic acid (PLA), polyvinyl chloride (PVC) etc. In one embodiment, the polymer is selected from polypropylene and / or polystyrene. That is, one type of polymer may be used to produce the flame-resistant thermoplastic composition or a combination of two or more different polymers may be used.
[0031] The term "lignin-based filler" is to be understood in this specification, unless otherwise indicated, as referring to a filler that has been prepared from lignin material subjected to a hydrothermal carbonization (HTC) treatment.
[0032] Hydrothermal carbonization (HTC) treatment may also be referred to as "high temperature and pressure aqueous carbonization". Hydrothermal carbonization treatment of a lignin material refers to a thermochemical conversion process of a lignin-containing material in an aqueous suspension. Hydrothermal carbonization treatment of lignin produces lignin derivatives having a high carbon content and functional groups. It is therefore a chemical process for the conversion of organic compounds into structured carbons.
[0033] The lignin material used to prepare the lignin-based feedstock may be selected from a group consisting of kraft lignin, steam explosion lignin, biorefinery lignin, supercritical separation lignin, hydrolysis lignin, flash precipitated lignin, lignin from biomass, lignin from an alkaline pulping process, lignin from a soda process, lignin from organosolv pulping, lignin from an alkali process, lignin from an enzymatic hydrolysis process, and any combination thereof. In one embodiment, the lignin is wood-derived lignin. The lignin may be derived from softwood, hardwood, annual plants, or any combination thereof.
[0034] In this specification, unless otherwise indicated, the term "kraft lignin" means lignin that originates from kraft black liquor. Black liquor is an alkaline aqueous solution of lignin residues, hemicellulose, and inorganic chemicals used in a kraft pulping process. The black liquor from the pulping process comprises components from different softwood and hardwood species in various proportions. Lignin can be separated from the black liquor by various techniques, including, for example, precipitation and filtration. Lignin generally begins to precipitate at pH values below 11 - 12. Different pH values can be used to precipitate lignin fractions with different properties. These lignin fractions differ from each other in molecular weight distribution, e.g., e.g., Mw and Mn, polydispersity, hemicellulose and extractive contents. The molar mass of lignin precipitated at a higher pH value is greater than the molar mass of lignin precipitated at a lower pH value. In addition, the molecular weight distribution of the lignin fraction precipitated at a lower pH value is broader than that of the lignin fraction precipitated at a higher pH value. Precipitated lignin can be purified from inorganic impurities, hemicellulose and wood extractives using acid washing steps. Further purification can be achieved by filtration.
[0035] The term "flash-precipitated lignin" is to be understood in this specification as lignin that has been precipitated from black liquor in a continuous process by decreasing the pH of a black liquor stream, under the influence of an overpressure ranging from 200 to 1000 kPa, to the lignin precipitation level using a carbon dioxide-based acidifying agent, preferably carbon dioxide, and abruptly releasing the pressure to precipitate the lignin. The process for producing flash-precipitated lignin is disclosed in patent application FI 20106073. The residence time in the above process is less than 300 s. Flash-precipitated lignin particles, having a particle diameter of less than 2 μm, form agglomerates, which can be separated from the black liquor using, for example, filtration.The advantage of flash-precipitated lignin is its greater reactivity compared to normal kraft lignin. Flash-precipitated lignin can be purified and / or activated if necessary for further processing.
[0036] Lignin can be derived from an alkali process. The alkali process can begin with the liquefaction of biomass with a strong alkali followed by a neutralization process. After the alkali treatment, the lignin can be precipitated in a manner similar to that presented above.
[0037] Lignin can be derived from steam explosion. Steam explosion is a pulping and extraction technique that can be applied to wood and other fibrous organic material.
[0038] In this specification, unless otherwise indicated, "biorefinery lignin" means lignin that can be recovered from a refining facility or process where biomass is converted into fuel, chemicals, and other materials.
[0039] In this specification, unless otherwise indicated, the term "supercritical separation lignin" means lignin that can be recovered from biomass using a supercritical fluid separation or extraction technique. Supercritical conditions correspond to the temperature and pressure above the critical point for a given substance. Under supercritical conditions, separate liquid and gas phases do not exist. Supercritical water or liquid extraction is a process of breaking down and converting biomass into cellulosic sugar using water or a liquid under supercritical conditions. The water or liquid, acting as a solvent, extracts the sugars from the cellulosic plant material, and the lignin remains as a solid particle.
[0040] Lignin can be derived from a hydrolysis process. Lignin derived from the hydrolysis process can be recovered from chemical processes on paper pulp or wood.
[0041] Lignin can be derived from an organosolv process. Organosolv is a pulping technique that uses an organic solvent to solubilize lignin and hemicellulose.
[0042] In one embodiment, the lignin-based feedstock is prepared from lignin material derived from an enzymatic hydrolysis process and / or a Kraft process and subjected to the hydrothermal carbonization treatment. In one embodiment, the lignin-based feedstock is prepared from lignin material derived from an enzymatic hydrolysis process and subjected to the hydrothermal carbonization treatment. In one embodiment, the lignin-based feedstock is prepared from lignin material derived from a Kraft process and subjected to the hydrothermal carbonization treatment.
[0043] In one embodiment, the starting material for preparing the lignin-based feedstock is a lignin material derived from an enzymatic hydrolysis process. In one embodiment, the enzymatic hydrolysis comprises the enzymatic hydrolysis of a plant-derived feedstock, such as a wood-based feedstock. In one embodiment, the enzymatic hydrolysis comprises the enzymatic hydrolysis of cellulose. Enzymatic hydrolysis is a process in which an enzyme(s) helps cleave bonds in molecules with the addition of water elements. In one embodiment, the enzymatic hydrolysis comprises the enzymatic hydrolysis of cellulose. In one embodiment, the lignin-based feedstock is prepared from a lignin material derived from an enzymatic hydrolysis process that is subjected to a hydrothermal carbonization treatment.
[0044] In one embodiment, the lignin-based feedstock is prepared from lignin derived from wood pulping, e.g., kraft lignin.
[0045] The lignin-based feedstock as disclosed in the present specification may be prepared as disclosed below. The lignin material to be used may be derived, for example, from a process in which lignin is formed upon enzymatic hydrolysis of a lignocellulosic feedstock or the lignin may be derived from a Kraft process. Also, other sources of lignin may be used as disclosed in the present description.
[0046] The derived lignin material may be dissolved in an alkaline solution, such as NaOH. Dissolution may be accomplished by heating the mixture of lignin and alkaline solution to about 80°C, adjusting the pH to a value above 7, such as 9 to 11, and mixing the mixture of lignin and alkaline solution for a predetermined time. The mixing time may be continued for about 2 to 3 hours. The exact pH value is determined based on the target product quality.
[0047] The dissolved lignin material can then be subjected to a hydrothermal carbonization (HTC) treatment.
[0048] The hydrothermal carbonization treatment may take place in one reactor (HTC reactor), or if necessary, in several parallel reactors, operating discontinuously. The dissolved lignin material may be preheated before being introduced into the HTC reactor(s). The temperature in the HTC reactor(s) may be between 150 and 250°C and the pressure may be between 20 and 30 bar. The residence time in the HTC reactor(s) may be between about three and six hours. In the HTC reactor, the lignin is carbonized, whereby a stabilized lignin derivative with a high specific surface area may be precipitated. The formed pasty suspension comprising the carbonized lignin may then be removed and cooled. As a result, a pasty suspension comprising a lignin-based feedstock is formed.
[0049] The pasty suspension comprising a lignin-based feedstock may be introduced into a separation unit, in which the precipitated lignin-based feedstock may be separated from the pasty suspension. The separated lignin-based feedstock may be dried and recovered. Before drying, the lignin-based feedstock may be washed, if necessary. The ground lignin particles may be dried and used as the lignin-based feedstock.
[0050] During the process described above, the lignin polymers are linked to each other. Thus, the lignin-based filler can be considered to comprise or consist of the lignin polymers that are linked together. The lignin polymers that are linked or linked together may no longer be soluble. However, smaller lignin polymer chains still remain soluble and can therefore be subjected to standard analytical techniques such as size exclusion chromatography or nuclear magnetic resonance spectroscopy (NMR spectroscopy), which require the analyte to be dissolved in a solvent. Thus, different properties of the soluble fraction of the lignin-based filler can be determined.
[0051] In one embodiment, the lignin-based filler comprises ash in a total amount ranging from 0.1 to 3% by weight, or from 0.1 to 2.5% by weight, or from 0.2 to 2.0% by weight, or from 0.3 to 1.5% by weight, or from 0.4 to 1.0% by weight. The ash content can be determined according to DIN 51719.
[0052] The inventors have surprisingly discovered that when, for example, the lignin material from the enzymatic hydrolysis process is used to produce the lignin-based feedstock, it is possible to reduce the ash content of the lignin-based feedstock. The lower ash content has the additional advantage of, for example, higher purity of the lignin-based feedstock.
[0053] The lignin-based filler may comprise carbon in a total amount ranging from 62 to 70% by weight. In one embodiment, the lignin-based filler comprises carbon in a total amount ranging from 63 to 69% by weight or from 64 to 68% by weight. The amount of carbon in the lignin-based filler may be determined according to DIN 51732 (1997). The inventors have surprisingly discovered that the amount of carbon in the lignin-based filler has the additional utility of advantageously affecting the combustion resistance of the thermoplastic composition compared to other lignin-containing fillers with a lesser amount of carbon. The amount of carbon in the lignin-based filler may thus contribute to preventing combustion from occurring.
[0054] In one embodiment, the solubility of the lignin-based filler in 0.1 M NaOH is between 1 and 40 wt%, or 3 and 35 wt%, or 5 and 30 wt%. The solubility can be measured as follows: first, a sample is dried at a temperature of 60°C for four hours. A sample mass of 0.5 grams is weighed and suspended in 50 ml of 0.1 M NaOH at a concentration of 1% having a temperature of 22°C. Mixing is continued for 1 hour, after which the sample is placed on a glass microfiber paper (1.6 qm) and the filter paper with the sample is dried at a temperature of 60°C for 2 hours. The portion of the sample that has dissolved can be determined gravimetrically.
[0055] In one embodiment, the lignin-based filler has a weight average molecular weight (Mw) ranging from 1000 to 4000 Da, or from 1300 to 3700 Da, or from 1700 to 3200 Da, or from 2500 to 3000 Da, or from 2600 to 2900 Da, or from 2650 to 2850 Da, when determined based on the soluble fraction of the lignin-based filler. The weight average molecular weight can be determined by size exclusion chromatography (SEC) using 0.1 M NaOH as the eluent and a sample amount of about 1 mg / ml, which is dissolved in 0.1 M NaOH. The molecular weights are measured relative to polystyrenesulfonate standards. A UV detector with a wavelength of 280 nm is used.
[0056] The polydispersity index (PDI) of the lignin-based filler can be understood between 1.5 and 5.0, or 1.8 and 4.5, or 1.9 and 4.3, or 2.1 and 4.0, or 2.4 and 3.5, or 2.6 and 3.2, when determined based on the soluble fraction of the lignin-based filler. The polydispersity index can be determined by size exclusion chromatography (SEC). PDI is a measure of the molecular weight distribution in a given polymer sample. PDI is calculated as the weight average molecular weight (Mw) divided by the number average molecular weight (Mn). PDI indicates the distribution of individual molecular weights in a batch of polymers.
[0057] The lignin-based filler may have an STSA value ranging from 3 to 150 m2 / g, or from 5 to 100 m2 / g, or from 7 to 60 m2 / g. The STSA value may be determined according to ASTM D6556.
[0058] In one embodiment, the lignin-based filler has a density of at most 1.5 g / cm3. In one embodiment, the lignin-based filler has a density ranging from 1.0 to 1.5 g / cm3, or from 1.15 to 1.35 g / cm3, or from 1.1 to 1.4 g / cm3. The density can be determined according to ISO 21687.
[0059] The combustion-resistant thermoplastic composition as disclosed in the present specification has the additional utility of exhibiting improved combustion resistance. The thermoplastic composition thus has the additional utility of being thermally stable. The inventors have surprisingly discovered that the lignin-based filler has a carbon content that beneficially affects the ability of the thermoplastic composition to resist combustion.
[0060] The combustion resistant thermoplastic composition as disclosed herein has the additional utility of exhibiting good stability compared to, for example, compositions prepared using carbon black as a filler. EXAMPLES
[0061] Reference will now be made in detail to various embodiments.
[0062] The description below discloses certain embodiments in sufficient detail that a person skilled in the art will be able to use the embodiments based on the disclosure. Not all steps or features of the embodiments are discussed in detail, as many steps or features will be obvious to those skilled in the art based on this description.
[0063] Example 1 - Combustion Resistance Test of Thermoplastic Compositions
[0064] In this example, the purpose was to evaluate the combustion resistance of the combustion-resistant thermoplastic composition by comparing it with the combustion resistance of corresponding thermoplastic compositions. As indicated above, the corresponding thermoplastic composition was prepared in a manner otherwise similar to the combustion-resistant thermoplastic composition but the lignin material was not subjected to a hydrothermal carbonization treatment during the preparation of the lignin-based filler. The filler used in the corresponding thermoplastic composition is referred to as virgin lignin in this example.
[0065] As comparative examples, a native thermoplastic composition, which did not contain any filler, and a thermoplastic composition using carbon black as a filler were also prepared.
[0066] The lignin-based feedstock was prepared following the description provided above in this specification using lignin material from enzymatic hydrolysis subjected to hydrothermal carbonization treatment. The virgin lignin was lignin from enzymatic hydrolysis but which had not been subjected to the hydrothermal carbonization treatment. The carbon black used was MONARCH®800 supplied by Cabot. The properties of the lignin-based feedstock and virgin lignin were measured and are shown in Table 1 below:
[0067] [Tables 1] Measured value Measurement method Unit Lignin-based filler Virgin lignin STSA ASTM D6556 m2 / g 45.5 9.3 Density ISO 21687 g / cm3 1.3-1.4 1.3-1.4 C content DIN51732 % 65.93 60.3 H content DIN51732 % 5.57 5.90 N content DIN51732 % 0.11 0.76 S content DIN51732 % 0.03 <0.05 Ash content DIN51719 % 2.3 0.4 Solubility in NaOH at 0.1 M As described in this specification % 26.2 40.8 PH ASTMD1512 - 8.4 6-7 Moisture content ASTM DI509 % 0.7 2.4
[0068] The carbon content of the carbon black was > 95% and the density was 1.8 g / cm3.
[0069] First, the following thermoplastic compositions were prepared:
[0070] [Tables2] Filler Type Polypropylene (PP) Polystyrene (PS) 40% by weight of carbon black XX 40% by weight of virgin lignin XX 40% by weight of lignin-based filler XX
[0071] The thermoplastic compositions were prepared by combining the following components at the appropriate processing temperatures for each polymer type: 40% by weight of filler, 52% by weight of the polymer and a total of 8% by weight of an additive package (consisting of 2% of calcium stearate (lubricant), 2% of the antioxidant Irganox 1010, 4% of polyethylene wax (lubricant)).
[0072] 3 kg of each type of thermoplastic composition was manufactured, and this was made at a loading of 40% by weight of filler. The fire behavior was tested on the basis of the horizontal combustion test ISO 3795:1989. The tests were carried out on molded masterbatches of PP and PS and their unfilled counterpart (comparative example). The results of the combustion test are presented in the table below:
[0073] [Tables3] Sample Burning rate mm / min Pure PP, unfilled 52 PP 40% carbon black 14 PP 40% lignin-based filler 19 PP 40% virgin lignin 79 Pure PS, unfilled 47 PS 40% carbon black 23 PS 40% lignin-based filler 47 PS 40% virgin lignin 129
[0074] Results of combustion tests
[0075] From the test results it can be seen that the fire behavior of the com combustion-resistant thermoplastic position is considerably better than that of the corresponding thermoplastic composition. The result is quite close to the thermoplastic composition where carbon black was used as a filler.
[0076] It will be apparent to those skilled in the art that with advances in technology, the basic idea can be implemented in various ways. The embodiments are therefore not limited to the examples described above; rather, they may vary within the scope of the claims.
[0077] The embodiments described above may be used in any combination with each other. Several of the embodiments may be combined together to form another embodiment. A thermoplastic composition, use, or method disclosed herein may include at least one of the embodiments described above. It will be understood that the benefits and advantages described above may relate to one embodiment or may relate to several embodiments. Embodiments are not limited to those that solve any or all of the stated problems or those that exhibit any or all of the stated benefits and advantages.The term "comprising" is used in this description to mean the inclusion of the following feature(s) or act(s), without excluding the presence of one or more additional features or acts.
Claims
Claims
1. Use of a lignin-based filler for improving the combustion resistance of a thermoplastic composition comprising at least one polymer and the lignin-based filler, wherein the thermoplastic composition contains 0.3 to 65% by weight of the lignin-based filler relative to the total weight of the combustion-resistant thermoplastic composition, wherein the lignin-based filler is prepared from a lignin material subjected to a hydrothermal carbonization treatment, and wherein the lignin-based filler comprises carbon in a total amount of 62 to 70% by weight and ash in a total amount of not more than 3% by weight, and wherein the combustion rate of the combustion-resistant thermoplastic composition is at least 20 percent lower than the combustion rate of a corresponding thermoplastic composition,wherein the corresponding thermoplastic composition is prepared in a manner otherwise similar to the combustion-resistant thermoplastic composition but wherein the lignin material used to prepare the lignin-based filler has not been subjected to a hydrothermal carbonization treatment.,
2. The use of claim 1, wherein the burning rate of the combustion-resistant thermoplastic composition is at least 30 percent, or at least 40 percent, or at least 50 percent, or at least 60 percent lower than the burning rate of the corresponding thermoplastic composition.
3. Use of any one of claims 1 and 2, wherein the combustion-resistant thermoplastic composition comprises the lignin-based filler in a total amount ranging from 0.5 to 50% by weight, or from 1 to 45% by weight, based on the total weight of the combustion-resistant thermoplastic composition.
4. The use of any one of claims 1 to 3, wherein the lignin material used to prepare the lignin-based feedstock is derived from an enzymatic hydrolysis process and / or a Kraft process.
5. Use of any one of claims 1 to 4, wherein the lignin-based filler comprises ash in a total amount of from 0.1 to 2.5% by weight, or from 0.2 to 2.0% by weight, or from 0.3 to 1.5% by weight, or 0.4 to 1.0% by weight
6. Use of any one of claims 1 to 5, wherein the solubility of the lignin-based filler in 0.1 M NaOH is 1 to 40 wt%, or 3 to 35 wt%, or 5 to 30 wt%.
7. The use of any one of claims 1 to 6, wherein the lignin-based filler has a weight average molecular weight (Mw) of from 1000 to 4000 Da, or from 1300 to 3700 Da, or from 1700 to 3200 Da, or from 2500 to 3000 Da, or from 2600 to 2900 Da, or from 2650 to 2850 Da, when determined based on the soluble fraction of the lignin-based filler.
8. Use of any one of claims 1 to 7, wherein the polydispersity index of the lignin-based filler is between 1.5 and 5.0, or 1.8 and 4.5, or 1.9 and 4.3, or 2.1 and 4.0, or 2.4 and 3.5, or 2.6 and 3.2, when determined on the basis of the soluble fraction of the lignin-based filler.