Insulation material and process for its production

A popcorn-based insulation material with carbon black and silicate binder addresses the flammability and toxicity issues of existing panels, offering high fire and water resistance, vapor permeability, and environmental sustainability.

FR3140569B3Inactive Publication Date: 2024-11-01SPANIEL PETR +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2023010637
Authority / Receiving Office
FR · FR
Patent Type
Utility models
Current Assignee / Owner
Priority Date
2022-10-05
Filing Date
2023-10-05
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing insulation panels made from wood chips, glass fibers, and other materials are highly flammable, have low water resistance, poor vapor permeability, and release toxic substances, while being susceptible to external and biological attacks, and are not environmentally friendly.

Method used

A non-flammable, water-resistant insulation material composed of popcorn, aluminum hydroxide, and an aqueous silicate solution, coated with carbon black, which is mixed with a water glass stabilizer and hardener to form a binder, providing excellent thermal and acoustic insulation, resistance to external influences, and environmental friendliness.

Benefits of technology

The material achieves high fire resistance, water resistance, vapor permeability, and environmental sustainability, while being non-toxic and resistant to biological attacks, with improved thermal and acoustic insulation properties.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Title: Insulating material and process for its production. Insulating material made from popcorn, in particular a non-flammable, water-resistant and vapor-permeable material made from popcorn, in particular a non-flammable, water-resistant and vapor-permeable material made from popcorn for the manufacture of insulating panels, which is composed of a mixture comprising 23 to 38% by weight of popcorn, 55.9 to 68% by weight of an aqueous silicate solution, 2 to 6% by weight of aluminum hydroxide, 1 to 3% by weight of water, and 0.1 to 1% by weight of a soluble glass stabilizer. Process for the production of a material, in particular a process for the production of a non-flammable, water-resistant and vapor-permeable material, in particular a non-flammable material.Water-resistant and vapor-permeable for the manufacture of lightweight thermal and acoustic insulation panels, the process involves first mixing aluminum hydroxide with water, then mixing popcorn with a carbon black solution so that its entire surface is coated with carbon black, then adding this to the aluminum hydroxide solution, and all the components are mixed together. Next, a soluble glass stabilizer is added to an aqueous silicate solution, then a soluble glass hardener is mixed into this solution, which is then stirred for 1 to 10 minutes to form a binder solution. Finally, the wood chip mixture is added to the binder solution, stirring continuously, and all the components are mixed together. The resulting mixture is then poured onto the application site. The resulting mixture is then left to stand until it hardens. Figure for summary: none.
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Insulation material and method for its production Technical field

[0001] The present invention relates to popcorn, in particular to a non-flammable, water-resistant and vapor-permeable material made from popcorn, in particular to a non-flammable, water-resistant and vapor-permeable material made from popcorn for the manufacture of panels, and to a method for its production. Prior art

[0002] A number of models of panels made from wood chips, glass fibers, basalt and other fibers, glass granules, ceramic and basalt, fly ash, cement, etc. are known in the current state of the art.

[0003] Polyurethane binders or synthetic resins, for example phenol-formaldehyde or urea-formaldehyde resins, are used as binders, for example.

[0004] Patent EP2081743 discloses a wood fiberboard to which popcorn of a size of 2 to 10 mm has been added, with phenol-formaldehyde resins as binders. The disadvantage of the board is that the binder is of organic nature and the mixture is highly flammable, not permeable to vapor and not resistant to external influences.

[0005] Patent WO2008128589 discloses a wood chip panel design in which crushed popcorn of a maximum size of 10 mm is added to retain the released formaldehyde. A formaldehyde resin is used as a binder. The disadvantages of the panel are its high flammability, very low vapor permeability and low resistance to external influences.

[0006] Patent WO2014131801 discloses a composite material in which a layer of popcorn is inserted between two layers of wood. A disadvantage is the high flammability of the panel.

[0007] It is clear from the above-mentioned state of the art that the main disadvantage of the prior art is that the known panels are almost always flammable or highly flammable. Another problem is their low water resistance. The use of volatile organic binders that begin to release toxic substances, especially formaldehyde, from the material is also problematic. The fact that the materials are not vapor permeable is also a disadvantage. Another disadvantage is that the The panels are not resistant to external influences and biological attacks. They are not recyclable and represent a burden on the environment.

[0008] The aim of the invention is to provide a thermal and acoustic insulation material which is water-resistant, has high fire resistance and is permeable to vapour, is environmentally friendly, is not harmful to health, is recyclable and is resistant to external influences as well as to biological attacks. Summary of the invention

[0009] The above-mentioned disadvantages are eliminated to a large extent and the objectives of the invention are achieved by means of a material made from popcorn, in particular a non-flammable and water-resistant material made from popcorn, in particular a non-flammable and water-resistant material for the manufacture of panels from popcorn, the characteristics of which lie in the fact that it is composed of a mixture comprising 23 to 28% by weight of popcorn, 55.9 to 68% by weight of an aqueous silicate solution, 2 to 5% by weight of aluminum hydroxide, 1 to 3% by weight of water, and 0.1 to 1% by weight of a water glass stabilizer. The advantages of this material are its lightness, strength, high vapor permeability, high fire resistance as well as high water resistance.At the same time, the material has excellent thermal and acoustic insulation properties, anti-mold effects and resistance to external influences. It is environmentally friendly and does not harm health. It is able to resist the effects of heat released by a burning object by delaying and significantly reducing heat release.

[0010] The aluminum hydroxide used preferably acts as a flame retardant. It is Advantageously, the mixture of water glass and aluminum hydroxide is incorporated deep into the material in a very tight and stable manner.

[0011] Preferably, the size of the popcorn is between 10 and 50 mm. Most preferably, the surface of the popcorn is covered with carbon black, the pure carbon black representing 0.025 to 0.25% by weight of the total weight. The advantage is that the carbon black thus arranged reduces flammability because the carbon black is preferably absorbed by the popcorn, to a certain extent, which stabilizes its bond to the carbon black. Another advantage is that the carbon black acts as a flame retardant.

[0012] Preferably, the aqueous silicate solution is an aqueous sodium silicate solution.

[0013] Preferably, the water glass stabilizer is a (hydroxyalkyl)ethylenediamine.

[0014] Preferably, the aqueous sodium silicate solution has a density between 1,370 and 1,400 kg / m3 and a molar ratio between SiO2 and Na2O between 3.2 and 3.4. It is advantageous that this water glass is partially flexible after hardening.

[0015] Preferably, the material made from popcorn further comprises a water glass hardener.

[0016] Furthermore, the above-mentioned disadvantages are eliminated to a large extent and the objectives of the invention are achieved by means of a method for producing an insulating material, in particular a method for producing a non-flammable, water-resistant and vapor-permeable material based on popcorn, in particular a non-flammable, water-resistant and vapor-permeable material based on popcorn for the manufacture of thermal and acoustic insulation panels, the characteristics of which lie in the fact that, firstly, aluminum hydroxide is mixed with water, then the popcorn is mixed with a carbon black solution so that its entire surface is covered by the carbon black, then it is added to the aluminum hydroxide solution, and all the components are mixed to form a popcorn mixture, then a water glass stabilizer is added to an aqueous silicate solution,and finally a water glass hardener is mixed into this solution. This solution is then stirred for 1 to 10 minutes to form a binder solution, then the popcorn mixture is added to the binder solution with continuous stirring, and all the components are mixed and the resulting mixture is poured onto the application site.

[0017] Preferably, the mixture obtained is finally left to stand until it hardens.

[0018] The main advantage of the insulating material and its production method according to the invention is that it is highly non-flammable. The popcorn is covered over its entire surface with carbon black and aluminum hydroxide, which act as flame retardants. It is very advantageous to use water glass as a binder, which, after drying, resembles standard glass in its composition and properties. It is very hard, abrasion-resistant, heat-resistant up to temperatures around 1000 °C, water-resistant and vapor-permeable. At the same time, it is environmentally friendly and does not harm health. It reflects UV rays well. It does not release any toxic organic substances. This binder has excellent adhesive and bonding effects, as well as good adhesion to usual substrates. This binder allows the popcorn to be bonded very effectively.At the same time, the popcorn is covered with this binder over its entire surface, which protects it from the effects of water, flames and UV rays, which slows down the decomposition of the popcorn, for example due to humidification. Insulation boards containing this binder are hard, strong, abrasion-resistant, non-flammable and resistant to . heat, water resistant, vapor permeable, resistant to biological attack, environmentally friendly and not harmful to health, without emissions of organic substances. Examples of embodiments of the invention

[0019] Example 1

[0020] The non-flammable, water-resistant material made from popcorn is composed of a mixture comprising 28% by weight of popcorn, 68% by weight of an aqueous solution of sodium silicate, 2% by weight of aluminum hydroxide, 1% by weight of water and 0.1% by weight of a water glass stabilizer.

[0021] The water glass stabilizer is a hydrophilic (hydroxyalkyl)ethylenediamine, in the form of a 98% aqueous solution of N,N,N',N'-Tetrakis(2-hydroxypropyl)ethylenediamine.

[0022] The aqueous solution of sodium silicate has a density of 1380 kg / m3, and its molar ratio between SiO2 and Na2O is 3.3.

[0023] The material made from popcorn further comprises a water glass hardener, which is a mixture of pure glycerol diacetate / triacetate in a ratio of 7:3 parts by volume, with a concentration of 0.5 to 5% by weight, relative to the pure water glass.

[0024] According to the method for producing the non-flammable and water-resistant material made from popcorn, aluminum hydroxide is first mixed with water, the popcorn is mixed with a carbon black solution so that its entire surface is covered with carbon black, then it is added to the aluminum hydroxide solution, and all the components are mixed to form a corn mixture, then the water glass stabilizer is added to the aqueous silicate solution, and then the water glass hardener is mixed with this solution. This solution is then stirred for 5 minutes to form a binder solution, then the corn mixture is added to the binder solution with continuous stirring, and all the components are mixed, and finally the resulting mixture is poured into the application site, which is a panel-shaped silicone mold.

[0025] Finally, the mixture obtained is left to stand until it hardens.

[0026] Example 2

[0027] The non-flammable, water-resistant material made from popcorn is composed of a mixture comprising 36% by weight of popcorn, 55.9% by weight of an aqueous solution of sodium silicate, 5% by weight of aluminum hydroxide, 3% by weight of water and 0.1% by weight of a water glass stabilizer.

[0028] The stabilizer of the water glass is a (hydroxyalkyl)ethylenediamine, in the form of a 98% aqueous solution of N,N,N',N'-Tetrakis(2-hydroxypropyl)ethylenediamine.

[0029] The aqueous solution of sodium silicate has a density of 1370 kg / m3, and its molar ratio between SiO2 and Na2O is 3.2.

[0030] The material made from popcorn further comprises a water glass hardener, which is a mixture of pure glycerol diacetate / triacetate in a ratio of 7:3 parts by volume, with a concentration of 0.5 to 5% by weight, relative to the pure water glass.

[0031] According to the method for producing the non-flammable and water-resistant material made from popcorn, aluminum hydroxide is first mixed with water, the popcorn is mixed with a carbon black solution so that its entire surface is covered with carbon black, then it is added to the aluminum hydroxide solution, and all the components are mixed to form a corn mixture, then the water glass stabilizer is added to the aqueous silicate solution, and then the water glass hardener is mixed with this solution. This solution is then stirred for 5 minutes to form a binder solution, then the corn mixture is added to the binder solution with continuous stirring, and all the components are mixed, and finally the resulting mixture is poured into the application site, which is a panel-shaped silicone mold.

[0032] Finally, the mixture obtained is left to stand until it hardens.

[0033] Example 3

[0034] The non-flammable, water-resistant material made from popcorn is composed of a mixture comprising 31% by weight of popcorn, 63% by weight of an aqueous solution of sodium silicate, 3% by weight of aluminum hydroxide, 2% by weight of water and 1% by weight of a water glass stabilizer.

[0035] The stabilizer of the water glass is a (hydroxyalkyl)ethylenediamine, in the form of a 98% aqueous solution of N,N,N',N'-Tetrakis(2-hydroxypropyl)ethylenediamine.

[0036] The aqueous solution of sodium silicate has a density of 1400 kg / m3, and its molar ratio between SiO2 and Na2O is 3.4.

[0037] The material made from popcorn further comprises a water glass hardener, which is a mixture of pure glycerol diacetate / triacetate in a ratio of 7:3 parts by volume, with a concentration of 0.5 to 5% by weight, relative to the pure water glass.

[0038] According to the method for producing the non-flammable and water-resistant material made from popcorn, aluminum hydroxide is first mixed with water, the popcorn is mixed with a carbon black solution so that its entire surface is covered with carbon black, then it is added to the aluminum hydroxide solution, and all the components are mixed to form a corn mixture, and then the water glass stabilizer is added to the aqueous solution of silicate, then the water glass hardener is mixed into this solution. This solution is then stirred for 5 minutes to form a binder solution, then the corn mixture is added to the binder solution with continuous stirring, and all the components are mixed, and finally the resulting mixture is poured into the application site, which is a panel-shaped silicone mold.

[0039] Finally, the mixture obtained is left to stand until it hardens. Industrial applicability

[0040] The thermal and acoustic insulation material made from popcorn according to the invention can be used to manufacture shaped articles or flat panels, which are usable in particular in the construction industry.

Claims

Claims

1. Insulating material made from popcorn, in particular non-flammable, water-resistant and vapor-permeable material made from popcorn, in particular non-flammable, water-resistant and vapor-permeable material made from popcorn for the manufacture of insulating panels, characterized in that it is composed of a mixture comprising from 23 to 38% by weight of popcorn, from 55.9 to 68% by weight of an aqueous silicate solution, 2 to 5% by weight of aluminum hydroxide, 1 to 3% by weight of water, and 0.1 to 1% by weight of a water glass stabilizer.

2. An insulating material made from popcorn according to claim 1, characterized in that the surface of the popcorn is covered with carbon black, the carbon black representing from 0.025% to 0.25% by weight of the total weight.

3. A popcorn-based insulating material according to any preceding claim, characterized in that the aqueous silicate solution is an aqueous sodium silicate solution.

4. A popcorn-based insulating material according to any preceding claim, characterized in that the water glass stabilizer is a hydrophilic (hydroxyalkyl)ethylenediamine.

5. Insulating material made from popcorn according to claim 3, characterized in that the aqueous sodium silicate solution has a density between 1370 and 1400 kg / m3.

6. Insulating material made from popcorn according to claims 3 or 5, characterized in that the aqueous sodium silicate solution has a molar ratio of SiO2 and Na2O of between 3.2 and

7. 3,H-. Popcorn-based insulating material according to any one of the preceding claims, characterized in that it further comprises a hardener for water glass.

8. A method for producing a material, in particular a non-flammable, water-resistant and vapour-permeable material, in particular a non-flammable, water-resistant and vapour-permeable material for the production of lightweight thermal and acoustic insulation panels according to claim 7, characterized in that firstly aluminium hydroxide is mixed with water, then popcorn is mixed with a carbon black solution so as to that its entire surface is covered with carbon black, and, then, it is added to the aluminum hydroxide solution, and all the components are mixed to form a mixture, then a water glass stabilizer is added to an aqueous silicate solution, then a water glass hardener is mixed into this solution, which is then stirred for 1 to 10 minutes to form a binder solution, then the popcorn mixture is added to the binder solution, stirring continuously, and all the components are mixed, and then the resulting mixture is poured onto the application site.

9. A method of producing an insulating material according to claim 8, characterized in that the mixture obtained is finally left to stand until it hardens.