METHOD FOR MANUFACTURING A PIEZOELECTRIC LAYER ON A SUBSTRATE
The method of forming a seed layer on a donor substrate and transferring it to a recipient substrate for monocrystalline piezoelectric layer growth addresses the issues of non-uniformity and precision, enabling high-quality piezoelectric layers for advanced devices.
Patent Information
- Application Number
- FR2022010858
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-10-20
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-10-20
AI Technical Summary
Existing methods for manufacturing piezoelectric layers on substrates result in non-uniform thickness and low precision, with limitations on diameter, particularly when transferring from smaller ingots to larger substrates like silicon.
A method involving the formation of a seed layer on a donor substrate through epitaxy, followed by transfer to a recipient substrate using an insulating or conductive layer, and subsequent growth of a monocrystalline piezoelectric layer, allowing for uniform and high-quality piezoelectric layers of large diameter and thickness.
Enables the production of thick, uniform, and high-quality piezoelectric layers on large-diameter substrates, suitable for applications in microelectronic, photonic, and optical devices, with improved crystalline quality and reduced attenuation of surface waves.
Smart Images

Figure 00000018_0000 
Figure 00000018_0001 
Figure 00000018_0002
Abstract
Description
Title of the invention: METHOD FOR MANUFACTURING A PIEZOELECTRIC LAYER ON A SUBSTRATE Technical field
[0001] The invention relates to a method for manufacturing a piezoelectric layer on a substrate. STATE OF THE ART
[0002] Various acoustic components are used for filtering in the radio frequency domain, including surface acoustic wave (SAW) filters, which typically comprise a thick piezoelectric layer (i.e., generally several tens of nanometers to several tens of millimeters thick) and two electrodes in the form of two interlocking metal combs deposited on the surface of said piezoelectric layer. An electrical signal, typically a change in voltage, applied to one electrode is converted into an elastic wave that propagates across the surface of the piezoelectric layer. The propagation of this elastic wave is favored if the wave frequency corresponds to the frequency band of the filter. This wave is again converted into an electrical signal upon reaching the other electrode.The piezoelectric layer must have excellent crystalline quality to avoid attenuating the surface wave. Therefore, a single-crystal layer is preferred. Currently, suitable materials for industrial use are quartz, LiNbO3, or LiTaO3.
[0003] Currently, the piezoelectric layer is obtained by cutting an ingot of one of said materials, which results in low precision for the thickness of said layer as well as a non-uniform thickness over the whole of the layer.
[0004] Furthermore, the diameters of the piezoelectric material ingots are smaller than the diameters of the substrate material ingots, such as silicon. However, to achieve a direct transfer, particularly a Smart Cut™ type layer transfer, it is necessary that the donor and recipient substrates have the same diameter.
[0005] There remains to this day a need for methods enabling the formation of a high-quality, uniform, thick piezoelectric layer on a large-diameter substrate. BRIEF DESCRIPTION OF THE INVENTION
[0006] An object of the invention is to design a method for manufacturing a substrate for a microelectronic, photonic or optical device, in particular but not limited to a surface acoustic wave device, in particular by enabling
[0007]
[0008]
[0009]
[0010]
[0011]
[0012]
[0013]
[0014]
[0015]
[0016]
[0017]
[0018]
[0019]
[0020] to obtain thick (i.e., thicker than 5 pm, or even greater than 15 pm), uniform, high-quality and large-diameter (i.e., larger than 15 or 20 cm in diameter) layers. According to the invention, a method for manufacturing a piezoelectric layer on a substrate is proposed, characterized in that it comprises; - the formation, through initial epitaxy, of a germ layer of a first piezoelectric material on a donor substrate, - the transfer of the seed layer and a portion of the donor substrate onto a recipient substrate via at least one electrically insulating layer and / or at least one electrically conductive layer adapted to allow relaxation of the seed layer, - the removal of the transferred portion of the donor substrate so as to expose a surface of the germ layer, - the formation of a single-crystal layer of a second piezoelectric material on the seed layer. According to a first embodiment, the transfer of the germ layer and the portion of the donor substrate comprises the following steps: - the formation of a weakened zone in the donor substrate in order to delimit the portion to be transferred, - the assembly of the donor substrate onto the recipient substrate, with the seed layer at the assembly interface, - the detachment of the donor substrate along the weakening zone, and the formation of the germ layer on the donor substrate is carried out before the formation of the weakening zone. According to a second embodiment, the transfer of the seed layer and the portion of the donor substrate comprises the following steps: - the formation of a weakened zone in the donor substrate in order to delimit the portion to be transferred, - the assembly of the donor substrate onto the recipient substrate, with the seed layer at the assembly interface, - the detachment of the donor substrate along the weakening zone, and the formation of the germ layer on the donor substrate is carried out after the formation of the weakening zone. The embrittlement zone can be formed by ion implantation, in particular of hydrogen and / or helium, in the donor substrate. Preferably, the formation of the seed layer on the donor substrate is achieved by atomic layer deposition. Alternatively, the formation of the seed layer on the donor substrate is achieved by molecular beam epitaxy.
[0021] Preferably, the formation of the single-crystal layer of the second piezoelectric material is carried out by a second epitaxy.
[0022] Preferably, the second epitaxy of the second piezoelectric material on the seed layer is a chemical vapor deposition with organometallics.
[0023] Alternatively, the formation of the single-crystal layer on the seed layer is achieved by deposition of the second piezoelectric material in amorphous form followed by recrystallization of said second material.
[0024] Advantageously, the thickness of the germ layer is between 2 nm and 20 nm.
[0025] Advantageously, the portion of the donor substrate transferred onto the receiving substrate has a thickness of less than 2 pm, preferably less than 1 pm.
[0026] Advantageously, the thickness of the layer of the second piezoelectric material at the end of the second epitaxy is between 20 nm and 15 pm.
[0027] According to a particular embodiment, the process comprises, after the formation of the single-crystal layer of the second piezoelectric material, the transfer of at least a part of the layer of the second piezoelectric material onto a final substrate.
[0028] Advantageously, the portion of the second piezoelectric material layer transferred to the final substrate has a thickness of less than 2 pm, preferably less than 1 pm.
[0029] The receiving substrate or the final substrate may include at least one electronic device or interconnection.
[0030] The receiving substrate or final substrate may include a charge trapping layer.
[0031] The first piezoelectric material and the second piezoelectric material may be identical. Alternatively, the first piezoelectric material and the second piezoelectric material may be different.
[0032] According to one embodiment, an intermediate layer adapted for the epitaxial growth of the germ layer on the donor substrate can be formed on the donor substrate before the formation of the germ layer.
[0033] Another object relates to a method for manufacturing a surface acoustic wave device, comprising the formation of two interdigitated electrodes on the surface of a piezoelectric layer, characterized in that it comprises the fabrication of the piezoelectric layer by a method such as described above.
[0034] Another object relates to a method for manufacturing a photonic device, comprising the formation of at least one photonic component, such as a laser or a light-emitting diode, at least partially in a piezoelectric layer, characterized in that it comprises the fabrication of the piezoelectric layer by a process as described above.
[0035] Another object relates to a surface acoustic wave device, characterized in that it comprises a piezoelectric layer that can be obtained by a process as described above, and two interdigitated electrodes on one face of the piezoelectric layer.
[0036] Another object relates to a photonic device, characterized in that it comprises a piezoelectric layer capable of being obtained by a process as described above, and at least one photonic component, such as a laser, a modulator, a waveguide or a multiplexer, formed at least in part in said piezoelectric layer.
[0037] The invention also relates to a structure comprising at least one such surface acoustic wave device and one such photonic device, comprising the same piezoelectric layer in which said surface acoustic wave device and said photonic device are arranged. Brief description of the drawings
[0038] Other features and advantages of the invention will become apparent from the detailed description that follows, with reference to the accompanying drawings in which: - Figure 1 is a schematic cross-sectional view of a surface acoustic wave filter, - Figures 2A and 2B illustrate two successive first steps in the manufacturing process of a single-crystal piezoelectric layer according to a first embodiment of the invention, - Figures 3A and 3B illustrate two successive first steps of said process according to a second embodiment of the invention, - Figures 4 to 8 illustrate successive stages of said process according to the first or second embodiment of the invention, - Figures 9 to 11 illustrate optional subsequent steps of said process.
[0039] For reasons of legibility of the figures, the illustrated elements are not necessarily shown to scale. Furthermore, elements designated by the same reference numerals in different figures are identical. DETAILED DESCRIPTION OF IMPLEMENTATION METHODS
[0040] Fig. 1 is a schematic view of a surface acoustic wave filter.
[0041] Said filter comprises a piezoelectric layer 10 and two electrodes 12, 13 in the form of two interlocking metal combs deposited on the surface of said piezoelectric layer. On the side opposite the electrodes 12, 13, the piezoelectric layer rests on a substrate 11. The piezoelectric layer 10 is single-crystal, excellent crystalline quality being preferable in order to avoid attenuation. of the surface wave.
[0042] In general, the invention proposes the formation of a single-crystal piezoelectric layer by means of transferring a seed layer produced by epitaxy of a first piezoelectric material onto a donor substrate, said transfer being carried out from the donor substrate to a receiving substrate. Subsequently, a layer of a second piezoelectric material is formed on the seed layer so as to obtain the desired thickness for the single-crystal layer of the second piezoelectric material.
[0043] The donor substrate may be a single-crystal bulk substrate of the first piezoelectric material or of another material. Alternatively, the donor substrate may be a composite substrate, that is, formed from a stack of at least two layers of different materials, the surface layer of which is made of the first single-crystal piezoelectric material or of another single-crystal material. Said single-crystal material is suitable for the epitaxial growth of the seed layer; in particular, it has a lattice parameter sufficiently close to the lattice parameter of the seed layer so as not to generate crystal defects during the growth of the seed layer.
[0044] Advantageously, the seed layer is pseudomorphic, meaning that the actual lattice parameter of the seed layer material is forced, for example by atomic forces, to correspond substantially to the lattice parameter of the donor substrate on which it is formed. To this end, the thickness of the seed layer must not exceed a critical thickness beyond which stress relaxation and the generation of defects in the seed layer would occur. This critical thickness depends on the seed layer material. For example, the critical thickness is typically less than 5 nm for a germanium seed layer formed on a silicon substrate. Generally, the critical thickness is between 2 nm and 20 nm depending on the materials chosen for the seed layer and the substrate.
[0045] In some embodiments, an intermediate layer (called an "epitaxial intermediate layer") of a material suitable for the growth of the germ layer on the donor substrate can be formed on the donor substrate before the formation of the germ layer. The usefulness of such an intermediate layer depends in particular on the chemical stability between the germ layer and the donor substrate. Thus, if the growth of the germ layer directly on the donor substrate is not hindered by chemical interactions or reactions between the material of the germ layer and that of the donor substrate, it is not necessary to use an intermediate layer. On the other hand, if chemical interactions or reactions between the material of the germ layer and that of the donor substrate are likely to prevent the growth of the For the seed layer, it is desirable to use an intermediate layer made of a material stable with respect to both the donor substrate material and the seed layer material. For example, a single-crystal germanium layer can be formed on a silicon donor substrate to promote the growth of the seed layer of the first piezoelectric material. In other embodiments, the intermediate layer can be made of single-crystal strontium titanate (SrTiO3), single-crystal aluminum oxide (Al2O3), single-crystal lanthanum aluminate (LaAl3), or a single-crystal metal such as aluminum.
[0046] The receiving substrate provides mechanical support for the seed layer. It can be of any type suitable for carrying out epitaxy (particularly in terms of temperature resistance) and, advantageously but not necessarily, adapted to the intended application. It can be solid or composite. Advantageously, the receiving substrate may include at least one electronic device or interconnection.
[0047] At least one intermediate layer (called the "relaxation intermediate layer") is interposed between the receiving substrate and the seed layer. For example, such an intermediate layer may be electrically conductive or electrically insulating. Those skilled in the art can choose the material and thickness of this layer according to the properties they wish to impart to the radiofrequency device intended to understand the piezoelectric layer. This intermediate layer allows the free relaxation of the seed layer. The transferred pseudomorphic seed layer can thus freely recover its lattice parameter during the transfer, or between the transfer and the formation of the second layer of the second piezoelectric material, or even during the formation of the second layer of the second piezoelectric material.
[0048] The material of the intermediate layer can advantageously be chosen from silicon oxide (SiO2), a nitride or a metal.
[0049] Said intermediate layer can be formed on the donor substrate (on the germ layer) or on the receiving substrate.
[0050] As an intermediate layer of silicon oxide, it can be deposited or obtained by thermal oxidation. The technique for forming said layer is chosen in particular according to the substrate on which it is to be formed and any limitations (for example, thermal) to be respected. For example, if the intermediate layer is formed on the receiving substrate and this substrate contains electronic components, a technique with a thermal budget that will not risk damaging said components will be chosen.
[0051] Advantageously, the receiving substrate can be made of a semiconductor material. It can be, for example, a silicon substrate.
[0052] In certain embodiments, particularly when the receiving substrate constitutes The final support for the piezoelectric layer, the receiving substrate, includes a "trap-rich" layer (which can be translated into French as a charge-trapping layer), which can be formed either on the receiving substrate itself or in a surface region of the receiving substrate. This "trap-rich" layer is thus located between the seed layer and the receiving substrate and improves the electrical insulation performance of the receiving substrate. This "trap-rich" layer can be formed from at least one polycrystalline semiconductor material, amorphous or porous, in particular polycrystalline silicon, amorphous silicon, or porous silicon, but is not limited to these materials.Furthermore, depending on the temperature resistance of the "trap-rich" layer used for epitaxy, it may be advantageous to introduce an additional layer between the receiving substrate and said "trap-rich" layer, in order to prevent the recrystallization of the latter during heat treatment.
[0053] The seed layer has a negligible thickness compared to the thickness of the final single-crystal piezoelectric layer. Consequently, it is considered not to significantly affect the operation of the radio frequency device incorporating the single-crystal piezoelectric layer.
[0054] The germ layer typically has a thickness between 1 nm and 20 nm.
[0055] The thickness of the layer of the second piezoelectric material formed on the layer The thickness of the seed layer depends on the specifications of the device intended to incorporate the single-crystal piezoelectric layer. In this respect, the thickness of the layer formed on the seed layer is not limited in terms of either a minimum or maximum value. The thickness of the final piezoelectric layer is typically between 20 nm and 15 pm.
[0056] The first piezoelectric material is advantageously chosen from a compound of formula ABO3, where A is chosen from barium and lithium and B is chosen from titanium and niobium. However, the interest in these materials is not limited to their piezoelectric character. Particularly for other applications, for example related to integrated optics, they may also be of interest, where appropriate, for their dielectric permittivity, their refractive indices, or even for their pyroelectric, ferroelectric, or ferromagnetic properties, for example, and depending on the case.
[0057] The first epitaxy can be carried out by any suitable technique to obtain high crystalline quality, in particular by atomic layer deposition (ALD) or molecular beam epitaxy (MBE), etc. These techniques are characterized by a very slow growth rate. However, since the seed layer has a small thickness, the use of one of these techniques Growing the seed layer has a low economic impact on the process but allows obtaining a crystalline quality of the seed layer, which will promote the crystalline quality of the single-crystal layer of the second piezoelectric material.
[0058] According to a first alternative, the formation of the layer of the second piezoelectric material on the seed layer can be achieved by a second epitaxy.
[0059] The second epitaxy can be carried out by any technique providing a higher growth rate than the first epitaxy, in particular by metal-organic chemical vapor deposition (MOCVD). Although providing a lower crystalline quality than ALD or MBE techniques, this second epitaxy is more economical for growing a relatively thick single-crystal layer.
[0060] According to a second alternative, the formation of the layer of the second piezoelectric material can be achieved by depositing said piezoelectric material in amorphous form followed by recrystallizing said material to give it a single-crystal structure. Optionally, this can be carried out in several successive cycles, each comprising deposition of the amorphous piezoelectric material to a certain thickness, followed by recrystallization of the material to said thickness, until the desired total thickness of the layer of the second piezoelectric material is obtained.
[0061] The deposition of amorphous material can be carried out by any technique known to those skilled in the art, and advantageously by MOCVD, by low-pressure chemical vapor deposition (LPCVD), by plasma-enhanced chemical vapor deposition (PECVD), or by spraying.
[0062] A person skilled in the art is able to determine the reagents and operating conditions according to the piezoelectric material to be grown and the technique chosen.
[0063] The transfer of the germ layer typically involves a step of gluing the donor substrate and the recipient substrate, the germ layer and the intermediate relaxation layer being at the gluing interface, then a step of thinning the recipient substrate so as to expose the germ layer for subsequent epitaxy.
[0064] The bonding step can be carried out for example by direct molecular bonding of the "wafer bonding" type according to Anglo-Saxon terminology, with or without an additional intermediate layer.
[0065] In a particularly advantageous way, the transfer is carried out according to the Smart Cut™ process which is well known for the transfer of semiconductor thin films, in particular silicon.
[0066] To this end, with reference to [Fig. 2A], according to a first embodiment, one A donor substrate 100 is provided, and a layer of a first single-crystal piezoelectric material, called the seed layer 102, is grown by initial epitaxy. The first piezoelectric material has a lattice parameter close to that of the donor substrate. Thus, the donor substrate 100 imposes its lattice parameter and allows the growth of a good-quality single-crystal material. Growth is stopped when the desired thickness of the seed layer is reached. In this figure, the donor substrate 100 is shown as a solid, but, as mentioned above, it could potentially be a composite.
[0067] Advantageously but optionally, an intermediate epitaxial layer 106 can be formed on the donor substrate 100 before the epitaxy of the germ layer 102. For the sake of simplicity of the figures, said layer 106 has not been shown in the following figures.
[0068] With reference to [Fig. 2B], a weakening zone 101 is formed by ion implantation (schematized by the arrows) through the seed layer in the donor substrate. This zone delimits a single-crystal layer 103 to be transferred, comprising the seed layer and a portion of the donor substrate. Advantageously, and depending on the piezoelectric material considered, the implanted species are hydrogen or helium, alone or in combination. A person skilled in the art is able to determine the dose and implantation energy of these species to form the embrittlement zone at a determined depth, which is preferably between 0.2 pm and 0.6 pm: typically and always depending on the piezoelectric material and the implanted species considered, the dose is in the range of 2 E+16 to 2 E+17 ionic species / cm2, and the implantation energy is from 30keV to 500keV.The buried weakened layer can also be obtained by any other means known to those skilled in the art, for example by porosification of the material, or by laser irradiation. However, as explained below, there are transfer methods that do not require the use of ion implantation, and the present invention can be implemented using these methods.
[0069] Figures 3A and 3B illustrate a second embodiment of the process for manufacturing a single-crystal piezoelectric layer. The second embodiment is an alternative to the first embodiment, illustrated in Figures 2A and 2B, in which implantation into the donor substrate is carried out before the formation of the seed layer by a first epitaxy.
[0070] With reference to [Fig.3A], a donor substrate 100 is provided and a weakening zone 101 is formed by ion implantation (schematized by the arrows) in the donor substrate 100, which delimits a single-crystal layer 103 to be transferred.
[0071] With reference to [Fig. 3B], a layer of a first single-crystal piezoelectric material, called the seed layer 102, is grown by a first epitaxy on the Transfer layer 103. As previously explained, the donor substrate 100 imposes its lattice parameter and allows the growth of a good quality single-crystal material. The first piezoelectric material has a lattice parameter close to that of the donor substrate. Growth is stopped when the desired thickness of the seed layer is reached. In this figure, the donor substrate 100 is shown as a solid, but, as mentioned above, it could potentially be a composite.
[0072] Advantageously, the thermal budget of the first epitaxy is lower than the thermal budget likely to cause fracture of the donor substrate along the weakening zone. Thus, the donor substrate retains its mechanical cohesion until the end of the growth of the seed layer.
[0073] Following the steps illustrated in figures 2A and 2B or 3A and 3B, a seed layer 102 is obtained on the donor substrate 100 in which a weakening zone has been formed by implantation and which defines a transfer layer 103 which includes the seed layer 102.
[0074] With reference to [Fig.4], at least one intermediate relaxation layer 105, electrically insulating or electrically conductive, is formed on the surface of the receiving substrate 110. The receiving substrate 110 may further include a charge trapping layer 107. For the sake of simplification, the layer 107 has not been shown in the following figures.
[0075] With reference to [Fig.5], the donor substrate 100, thus weakened, is glued onto the recipient substrate 110, the germ layer 102 and the intermediate relaxation layer 105 being at the glue interface.
[0076] With reference to [Fig. 6], the donor substrate 100 is detached along the embrittlement zone 101. Such detachment can be caused by any means known to those skilled in the art, for example, thermal, mechanical, chemical, etc. The layer 103 is thus transferred onto the receiving substrate 110. Advantageously, the remaining portion of the donor substrate can then be recovered and potentially recycled.
[0077] With reference to [Fig. 7], a superficial portion of the transferred layer is removed, for example by mechanical polishing and / or chemical etching. This material removal aims to expose the seed layer 102. Following this removal, a thinned layer 102 is obtained on the receiving substrate 110, which will serve as the seed layer in the next step.
[0078] With reference to [Fig. 8], a layer of a second piezoelectric material 104 is formed on the seed layer 102. The material of layer 104 has a lattice parameter close to or identical to that of the seed layer 102. Thus, the seed layer 102 imposes its lattice parameter and allows the growth of a good quality single-crystal material. Layer 104 may be of a leucine nature The process differs from that of the seed layer 102, notably through the controlled introduction of slight levels of impurities for various purposes (doping, adjustment of piezoelectric properties, optimization of crystal defect / dislocation densities, surfactant, etc.). Growth is stopped when the desired thickness of the single-crystal piezoelectric layer is reached. The final piezoelectric layer 10 is formed by stacking the seed layer 102 and the layer 104.
[0079] The first piezoelectric material and the second piezoelectric material may be identical.
[0080] Alternatively, the first piezoelectric material and the second piezoelectric material may be different.
[0081] As mentioned above, the seed layer is considered to have no effect or a second-order effect on the operation of a radio frequency device incorporating the piezoelectric layer formed on the seed layer. Therefore, even if the implantation carried out for the implementation of the Smart Cut™ process damages the seed layer and disrupts its piezoelectric properties, these defects are not, or only slightly, detrimental.
[0082] In an embodiment not illustrated, no embrittlement zone is formed in the donor substrate. In this case, the transfer of the seed layer to the receiving substrate is achieved by assembling the donor substrate onto the receiving substrate and then etching the donor substrate until the seed layer is exposed. This embodiment is, however, less preferred than the one involving the formation of an embrittlement zone in the donor substrate, because it results in a greater loss of material.
[0083] In another embodiment not illustrated, a weakening zone is not formed in the donor substrate, but a detachable interface is formed by a chemical or thermal reaction. In this case, the transfer of the seed layer to the receiving substrate is achieved by assembling the donor substrate onto the receiving substrate and then detaching the interface following a chemical or thermal reaction in order to expose the seed layer.
[0084] As can be seen in [Fig.8], at the end of the process, a substrate is obtained for a surface acoustic wave device which comprises a receiving substrate 110 and a single-crystal piezoelectric layer 10 on said substrate 110. Such a substrate may also prove useful for other applications, for example for photonics and integrated optics.
[0085] Layer 10 is characterized by the presence of two portions with different characteristics:
[0086] - a first portion 102 located at the interface with the receiving substrate 110, cor corresponding to the germ layer,
[0087] - a second portion 104 extending from the first portion 102, cor- corresponding to the layer formed on portion 102, which may have a different crystalline quality than that of the first portion (said quality can be adjusted and optimized during the second epitaxy step for example) and / or a different composition (especially if impurities, such as dopants, have been introduced during the epitaxy), possibly conferring particular properties to the layer formed on portion 102.
[0088] This substrate is advantageously used to manufacture a surface acoustic wave device as illustrated in [Fig.1] and / or any other microelectronic, photonic or optical device comprising a piezoelectric layer.
[0089] In some cases, the receiving substrate onto which the seed layer is transferred may not be optimal for the intended application. Indeed, in certain embodiments, the receiving substrate must undergo the operating conditions of epitaxy, thus limiting the choice of suitable materials. In particular, the receiving substrate must not contain layers or elements that could be damaged by the epitaxy temperature. It may then be advantageous to transfer the piezoelectric layer 10 onto a final substrate 120 whose properties are chosen according to the intended application, by adhering it to said substrate 120 via the surface of the layer 104 formed on the seed layer 102 (see [Fig. 9]), and removing the receiving substrate (see [Fig. 10]). This transfer can be carried out by any of the transfer techniques mentioned above.Another advantage of this transfer onto a final substrate is that the seed layer 102, which was buried in the structure resulting from the formation of the second piezoelectric material layer, is then exposed and can optionally be removed (see [Fig. 11]), particularly in the case where it presents defects. Only the second piezoelectric material layer 104 then remains on the final substrate 120.
[0090] The final substrate can be solid or composite.
[0091] Advantageously, the final substrate may include at least one electronic device or interconnection.
[0092] In certain embodiments, the final substrate comprises a charge-trapping layer (designated by reference numeral 121 in [Fig. 9]), which may be formed either on said final substrate or in a surface region of said final substrate. This charge-trapping layer is thus located between the piezoelectric layer and the final substrate and improves the electrical insulation performance of the final substrate. This charge-trapping layer may be formed from at least one polycrystalline, amorphous, or porous semiconductor material, in particular polycrystalline silicon, amorphous silicon, or porous silicon, but not limited to these materials.
[0093] In the case where it is desired to manufacture a surface acoustic wave device, a piezoelectric layer 10 is deposited on the surface opposite the receiving substrate. or, where appropriate, to the final substrate (whether it is the receiving substrate 110 or the final substrate 120, said substrate forms the support substrate noted 11 on the [Fig. 1]), the metallic electrodes 12, 13 in the form of two interdigitated combs.
[0094] In other applications, at least one photonic component, such as a laser, a modulator, a waveguide or a multiplexer, can be formed in the piezoelectric layer, or in a stack of layers comprising said piezoelectric layer.
[0095] Advantageously, it is possible to integrate a surface acoustic wave device and a photonic device within the same substrate. To this end, at least one surface acoustic wave device and one photonic device, such as a laser, modulator, waveguide, or multiplexer, are formed within the same piezoelectric layer. It is also possible to combine these devices, as described, with other devices present in the receiving or final substrate, thus aiming at co-integration approaches for known 2D, 2.5D, and 3D devices.
Claims
Claims
1. Method for manufacturing a piezoelectric layer (10) on a substrate (11), characterized in that it comprises: - the formation by a first epitaxy of a pseudomorphic seed layer (102) of a first piezoelectric material on a donor substrate (100), - the transfer of the seed layer (102) and a portion (103) of the donor substrate (100) onto a receiving substrate (110) via at least one electrically insulating layer and / or at least one electrically conductive layer (105) adapted to allow relaxation of the seed layer, - the removal of the portion (103) of the donor substrate (100) transferred so as to expose a surface of the seed layer (102), - the formation of a monocrystalline layer (104) of a second piezoelectric material on the seed layer (102).
2. The method of claim 1, wherein the transfer of the seed layer (102) and the portion (102) of the donor substrate (100) comprises the following steps: - forming a weakening zone (101) in the donor substrate (100) so as to delimit the portion (103) to be transferred, - assembling the donor substrate (100) on the recipient substrate (110), the seed layer (102) being at the assembly interface, - detaching the donor substrate (100) along the weakening zone (101), and wherein the formation of the seed layer (102) on the donor substrate (100) is carried out after the formation of the weakening zone (101).
3. The method of claim 1, wherein transferring the seed layer (102) and the portion (103) of the donor substrate (100) comprises the following steps: the formation of a weakening zone (101) in the donor substrate (100) so as to delimit the portion to be transferred (103), - the assembly of the donor substrate (100) on the recipient substrate (110), the seed layer (102) being at the assembly interface, - the detachment of the donor substrate (100) along the weakening zone (101), and in which the formation of the seed layer (102) on the donor substrate (100) is carried out before the formation of the weakening zone (101).
4. Method according to one of claims 2 or 3, in which the weakening zone (101) is formed by ion implantation of hydrogen and / or helium in the donor substrate (100).
5. Method according to one of claims 1 to 4, in which the formation of the seed layer (102) on the donor substrate (100) is carried out by atomic layer deposition.
6. Method according to one of claims 1 to 4, in which the formation of the seed layer (102) on the donor substrate (100) is carried out by molecular beam epitaxy.
7. Method according to one of claims 1 to 6, in which the formation of the monocrystalline layer (104) on the seed layer (102) is carried out by a second epitaxy.
8. The method of claim 7, wherein the second epitaxy of the second piezoelectric material on the seed layer (102) is organometallic chemical vapor deposition.
9. Method according to one of claims 1 to 6, in which the formation of the monocrystalline layer (104) on the seed layer (102) is carried out by deposition of the second piezoelectric material in amorphous form followed by recrystallization of said second material.
10. Method according to one of the preceding claims, in which the thickness of the seed layer (102) is between 2 nm and 20 nm.
11. Method according to one of the preceding claims, in which the portion (103) of the donor substrate (100) transferred onto the recipient substrate (110) has a thickness of less than 2 μm, preferably less than 1 μm.
12. Method according to one of the preceding claims, in which the thickness of the layer (104) of the second piezoelectric material at the end of the second epitaxy is between 20 nm and 15 pm.
13. Method according to one of claims 1 to 12, in which the receiving substrate (110) comprises at least one electronic device or an interconnection.
14. Method according to one of the preceding claims, in which the receiving substrate (110) comprises a charge trapping layer (107).
15. Method according to one of claims 1 to 12, comprising, after the formation of the monocrystalline layer of the second piezoelectric material, the transfer of at least a portion of the layer (104) of the second piezoelectric material onto a final substrate (120).
16. Method according to claim 15, wherein the portion of the layer (104) of the second piezoelectric material transferred onto the final substrate (120) has a thickness of less than 2 pm, preferably less than 1 pm.
17. A method according to one of claims 15 or 16, wherein the final substrate (120) comprises at least one electronic device or interconnection.
18. Method according to one of claims 15 to 17, in which the final substrate (120) comprises a charge trapping layer (121).
19. A method according to one of claims 1 to 18, wherein the first piezoelectric material and the second piezoelectric material are identical.
20. A method according to one of claims 1 to 18, wherein the first piezoelectric material and the second piezoelectric material are different.
21. A method according to one of the preceding claims, comprising, before the formation of the seed layer (102), the formation of an intermediate layer (106) on the donor substrate (100), said intermediate layer being adapted for the epitaxial growth of the seed layer (102) on the donor substrate (100).
22. A method of manufacturing a surface acoustic wave device, comprising forming two interdigitated electrodes (12, 13) on the surface of a piezoelectric layer (10), characterized in that it comprises manufacturing the piezoelectric layer (10) by a method according to one of claims 1 to 21.
23. A method of manufacturing a photonic device, comprising forming at least one photonic component, such as a laser, a modulator, a waveguide or a multiplexer, at least in part in a piezoelectric layer, characterized in that it comprises the manufacture of the piezoelectric layer (10) by a method according to one of claims 1 to 21.
24. Surface acoustic wave device, characterized in that it comprises a piezoelectric layer (10) capable of being obtained by a method according to one of claims 1 to 21, and two electrodes (12, 13) interdigitated on one face of the piezoelectric layer (10).
25. Photonic device, characterized in that it comprises a piezoelectric layer obtainable by a method according to one of claims 1 to 21, and at least one photonic component, such as a laser, a modulator, a waveguide or a multiplexer, formed at least in part in said piezoelectric layer.