Titanium alloys exhibiting low anisotropy

Alloying titanium with rare earths to induce a peritectic reaction and subsequent heat treatment addresses anisotropy issues in titanium alloys, resulting in isotropic structures with enhanced mechanical properties for additive manufacturing.

FR3148040A1Pending Publication Date: 2024-10-25DEUTSCHES ZENTRUM FÜR LUFT UND RAUMFAHRT E V
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2024003885
Authority / Receiving Office
FR · FR
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-18
Filing Date
2024-04-15
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Titanium alloys used in additive manufacturing exhibit significant anisotropic properties due to high oriented cooling gradients, leading to non-uniform microstructures and mechanical instability, which complicates part design and limits the achievement of desired mechanical properties.

Method used

Alloying titanium with rare earths to create a peritectic reaction with a peritectic temperature higher than the allotropic transformation temperature, followed by a heat treatment at a specific temperature to achieve a globular or bimodal structure with reduced anisotropy.

Benefits of technology

The resulting titanium alloys exhibit more isotropic properties, enabling improved mechanical stability and uniform microstructures without the need for thermomechanical deformation, suitable for complex part manufacturing in aerospace and other applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The present invention relates to a material obtained by combining titanium or a titanium alloy with a mixture of lanthanides, where the transformation temperature (peritectic temperature) is higher than the allotropic transformation temperature of the titanium alloy, such that the resulting alloy undergoes a peritectic transformation upon cooling. Figure for the abstract: Fig. 1
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Titanium alloys exhibiting low anisotropy. Technical field

[0001] The present invention relates to titanium alloys used in primary processing or coating processes that exhibit improved properties with respect to crystallographic texture and anisotropy. The invention further relates to a method for adjusting structures during the manufacture of metallic materials. Technological background

[0002] Metal-based additive manufacturing (AM), commonly referred to as metal 3D printing, forms an important subgroup of primary processing methods. It is currently generating a paradigm shift in various sectors, such as the aerospace, automotive, and biomedical industries. One of the main advantages of additive manufacturing is the production of metal parts with complex geometries and virtually any final contour, which until now could only be produced at great expense, using a combination of existing processes (e.g., 5-axis point milling, using a casting method and bonded structures for the various components) or could not be produced at all.For example, it allows for internal channels for cooling fluids or bionic and load-optimized structures with reduced weight. Additive or generative ("layer-by-layer") manufacturing of components from a computer-aided 3D design model offers significantly greater design freedom, increased flexibility in adapting products to specific customer needs, and reduced time to market.

[0003] In primary processing, particularly in additive manufacturing, many different materials based on titanium, nickel, iron, or aluminum are used, among others. Titanium materials offer very high potential for lightweight construction due to their very good specific strengths for a lower density.

[0004] For the manufacture of parts made of titanium or titanium alloys (hereinafter referred to simply as "titanium") or for their repair, additive manufacturing promises considerable reductions in production costs, given that machining costs and material loss (chip removal, energy expenditure, etc.) can be reduced. In aeronautics and astronautics, additive manufacturing is therefore being considered, particularly for titanium components with a high buy-to-fly ratio (cost savings). For example, manufacturing a powertrain mounting element in Ti-6A1-4V using additive manufacturing resulted in a 50% cost reduction compared to conventional forging.

[0005] It is therefore essential to accelerate the capabilities of 3D printing and support the paradigm shift. To this end, new materials will be needed in the future, defined by the process properties of additive manufacturing using laser or electron beam sources, and which, during their transformation, generate parts with targeted properties. Among the processes particularly under consideration for this purpose are laser powder bed fusion (LBPF), direct energy deposition (DED), electron beam melting (EBM), and wire-arc additive manufacturing (WAAM).

[0006] In primary processing, the titanium materials used, particularly in additive manufacturing, are not specifically designed for the additive manufacturing process but rather derive from developments made for processing using conventional casting or forging processes. Additive and generative processes, however, are all characterized by specific metallurgical process conditions, which, depending on the process, process parameters, part properties, and construction strategy, exhibit high to extremely high cooling rates. These differ significantly from conventional processes and consequently result in different material properties despite an identical chemical composition.

[0007] Under the cooling conditions of additive manufacturing, these known alloys, for example titanium-6-aluminum-4-vanadium (Ti-6A1-4V, therefore a titanium alloy containing 6 wt% aluminum and 4 wt% vanadium), exhibit anisotropic properties, meaning that the material behavior is a function of orientation [Shunyu Liu, Yung C. Shin, Additive manufacturing of Ti6A14V alloy: A review, Material & Design, 2019, 164, 107552]. This occurs in cubic crystal systems based on the physical metallurgy of an additive process, which is characterized by high oriented cooling gradients. In titanium alloys, this generates typical "columnar crystalline" microstructures exhibiting very coarse columnar B grains with a strong texture type <100> B along the direction of additive construction. A A schematic representation is shown in Figure 1a of [Fig. 1]. These highly anisotropic material properties (e.g., elongation limits, stability, etc.) pose a problem for the parts and their design. Microstructures also form which, upon subsequent heat treatment, become much less refined and do not generate the desired mechanical properties.

[0008] Thermomechanical deformation / recovery treatments, which can be used in conventional manufacturing, are also not, in additive manufacturing close to the final contours, a possibility for breaking textures, generating recrystallization and adapting grain sizes and morphologies.

[0009] However, to design new parts optimally, a material with nearly isotropic properties is often required. New materials for metal-based additive manufacturing (AM materials) are also desired to exhibit other targeted properties, such as a globular or bimodal structure, with a particle size distribution specifically adapted to each application scenario (static stability, fatigue stresses, finishing loads, etc.). Consequently, there is a need for an additive manufacturing process using titanium alloys that avoid the drawbacks associated with the prior art and, in particular, exhibit anisotropic properties and the most homogeneous crystallographic texture possible. Detailed description of the invention

[0010] It has been surprisingly discovered that titanium alloys which form a miscibility gap with rare earth elements undergo a peritectic reaction with a peritectic temperature higher than the allotropic transformation temperature [3 -> a (882 °C for pure titanium; transus |3). These alloys can be used in various manufacturing processes according to DIN 8580:2003-09, in particular for primary processing and / or coating. The primary processing methods are therefore, in accordance with the present invention, casting or additive manufacturing (3D printing) according to DIN EN ISO / ASTM 52900.

[0011] In a first embodiment, the object at the basis of the present invention is solved by a material which is obtained by combining titanium or a titanium alloy with several lanthanides, the transformation temperature (peritectic temperature) being higher than the allotropic transformation temperature of the titanium alloy, so that a peritectic transformation occurs in the alloy obtained during cooling.

[0012] Surprisingly, it has turned out that it is possible, through alloying with rare earths, to exploit a peritectic transformation in such a way that new alloys with tunable structures and properties can be manufactured. considerably more isotropic than the corresponding original alloys without lanthanides. Furthermore, it has been surprisingly found that the use of several lanthanides can achieve adaptation to different alloy compositions, for example, critical temperatures. The peritectic pathway generated by the modification, (L1 + B -> a), which leads to the desired texture reduction through the formation of globular grains, must therefore be characterized by a critical temperature (peritectic temperature) higher than the allotropic transformation temperature. For this to occur, the lanthanide phase (L1) must be in a liquid state during manufacturing. The melting zone of the lanthanide mixture can be adapted by selecting the lanthanides and their composition.The peritectic reaction should be close to the allotropic transformation temperature, since further heat treatment must be possible at the lowest possible temperature. The fraction of globular and lamellar zones is adjusted by adding at least one other alloying element.

[0013] The preparation of the material involves heating and subsequent cooling under the conditions described, these occurring, for example, within the framework of an additive manufacturing process (3D printing). The processes are characterized by rapid to very rapid cooling rates. In accordance with the invention, this cooling may be followed by heat treatment. During this heat treatment, the material is heated to a temperature T that is higher than the peritectic temperature (PTT) of the material, and therefore remains between 600 °C and 1000 °C, preferably between 750 °C and 900 °C. The heating is preferably carried out at temperatures higher than the peritectic temperature of the respective alloy, which is known to those skilled in the art, and is carried out over a period of between 1 second and 200 hours, preferably from more than 1 minute to up to 10 hours, and particularly preferably from 1 minute to up to 1 hour.The material is then cooled to room temperature. This heat treatment in L + [3] further reduces the texture and anisotropy. In particular, the anisotropy can preferably be completely eliminated.

[0014] Heat treatment to eliminate internal stresses after the actual manufacturing process is known for metallic materials. However, these do not lead to a reduction in texture and anisotropy, at least not to the extent that is the case for the material according to the invention. If common alloys with rapid cooling rates are used in the process, post-heat treatment is only possible to a very limited extent, since the output texture, after rapid solidification, is still too large and the new grains that form still possess orientation information. grains from the high-temperature phase (Burgers equation) that the new grains resulting from peritectic solidification no longer have.

[0015] In a preferred embodiment, the resulting material contains at least 0.01% by weight or more of a lanthanide mixture. In particular, the lanthanide fraction is 20% or less. A higher fraction unduly affects the mechanical properties of the material. Moreover, lanthanides are expensive, so the price of the material is not attractive if they are used. In a particularly preferred embodiment, the fraction of the lanthanide mixture is between 0.05% by weight and 15% by weight, preferably between 0.1% by weight and 10% by weight, and in particular between 0.5% by weight and 5% by weight, preferably between 1% by weight and 3% by weight. The quantity indications refer respectively to the total weight of the titanium alloy.

[0016] The lanthanide mixture content is specifically selected such that, after heat treatment in the range L + 3, the geometry of the parts manufactured from the material by additive manufacturing remains unchanged. The exact quantity depends on the choice of the lanthanide mixture, as well as the titanium or titanium alloy. However, the fraction is specifically within the aforementioned range.

[0017] In the additive manufacturing of conventional titanium alloys, strong epitaxial growth occurs, resulting in the formation of structures with a marked crystallographic texture and strong anisotropic properties of the material, as shown in Figure 1a. By using the titanium alloy according to the invention, or a titanium alloy with a lanthanide mixture, it is possible to achieve a globular, low-texture, or even textureless structure, as shown in Figure 1b. Beyond the fraction of stabilizing alloying elements [3], it is possible to obtain a bimodal structure, as shown in Figure 1a.

[0018] There is a possible application of the invention in the 3D printing of structural parts, particularly for the aerospace industry (e.g., chassis parts, turbines for turbopumps, satellite structures, etc.). Titanium alloys are used, among other things, for high-performance corrosion-resistant applications. In addition to structural applications, such metals are also used in other sectors, such as energy and biomedical applications.

[0019] The material according to the present invention is therefore used to manufacture a part, the material being formed during the manufacturing of the part. In another embodiment of the present invention, it relates to a method for manufacturing a part from a titanium alloy during a production process comprising the steps of:

[0020] a) supply titanium or a titanium alloy which is / are free of lanthanide,

[0021] b) provide a mixture of lanthanides / mischmetal,

[0022] c) combine components a) and b),

[0023] d) use the alloy obtained in c) to manufacture a material in a manufacturing process, preferably a primary processing and / or coating process,

[0024] e) optionally determine experimentally the peritectic temperature of the part, and

[0025] f) then proceed with a heat treatment, at a temperature T which is higher than the peritectic temperature.

[0026] The lanthanide mixture may consist of two, three, or more lanthanides. It is also possible, in accordance with the present invention, for the lanthanide mixture to be made available in a mixture with another metal and then for the lanthanide / lanthanide mixture to be alloyed together with this metal with titanium / titanium alloy.

[0027] Lanthanides are, according to the invention, rare earths which consist of the group of elements following: lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium and lutetium.

[0028] When ranges of quantities are specified to describe the alloy, the intermediate ranges are always considered disclosed. It is possible to combine features of each embodiment in any way, and also to combine them with other embodiments as long as this combination is not explicitly excluded.

[0029] In accordance with the invention, the material provided can be used in manufacturing processes, particularly during coating and / or primary processing. For the purposes of this invention, coating means the application of an adherent layer of an amorphous substance to the surface of a part. The part to be coated may be produced by another manufacturing process. The coating applied from the material provided in accordance with the invention can be a thin or thick layer. Furthermore, the coating can be used, for example, as corrosion protection.

[0030] Primary transformation, in accordance with the invention, refers to the process of manufacturing a solid body with a defined geometric shape from an amorphous substance. In accordance with the invention, this preferably includes casting, as well as additive manufacturing (AM), i.e., 3D printing, using the provided material.

[0031] Examples of implementation:

[0032] In the following embodiment example, the object underlying the present invention is better explained in a non-limiting manner.

[0033] A titanium alloy was manufactured. For this purpose, a mischmetal alloy containing 85% by weight of cerium, 10% by weight of lanthanum and 5% by weight of neodymium was used. A titanium-molybdenum alloy containing 96% by weight of titanium and 4% by weight of molybdenum (Ti-4Mo) was also used.

[0034] This Ti-4Mo alloy composition was alloyed with mischmetal (MM) in a weight ratio of 99% by weight of Ti-4Mo alloy and 1% by weight of mischmetal, by melting in a crucible at a temperature of 1900 °C. The allotropic transformation (TA) temperature was 832 °C, and the solidus temperature of the mischmetal was approximately 822 °C.

[0035] From the alloy thus obtained, a powder having the composition Ti-4Mo-1MM was produced by gas atomization. This powder was used in an additive manufacturing process (laser powder bed fusion, FLLP) to manufacture a part.

[0036] An experimental determination of the peritectic temperature (TPT) was carried out using in situ X-ray diffraction, preferably performed with high-energy synchrotron radiation, here at 100 keV, to obtain particularly accurate results.

[0037] The part was then subjected to a post-heat treatment at a temperature of 850 °C, which was above the peritectic temperature, resulting in a micro-structure adaptation of the Ti-4Mo-1MM alloy. The material exhibited a bimodal structure, as shown in Figure 1.

[0038] Materials exhibiting a bimodal structure possess exceptional mechanical properties, lower anisotropy, and superior structural refining annealing without the need for thermomechanical machining containing deformation steps, which are generally not feasible during a manufacturing process, particularly during coating or primary processing.

Claims

Claims

1. Process for obtaining a material characterized in that titanium or a titanium alloy is alloyed with a mixture of lanthanides, where the transformation temperature (peritectic temperature) is higher than the allotropic transformation temperature of the titanium alloy, so that the alloy obtained undergoes a peritectic transformation during cooling.

2. A method of obtaining a material according to claim 1, characterized in that the material is further subjected to a heat treatment which occurs at a temperature T which is higher than the peritectic temperature (TPT) of the material.

3. Method for obtaining a material according to claim 2, characterized in that the heat treatment is carried out over a period of up to several hours (< 200 h).

4. Method for obtaining a material according to claim 2, characterized in that the heat treatment is carried out over a period ranging from 1 minute to 10 hours.

5. Method for obtaining a material according to claim 2, characterized in that the heat treatment is carried out over a period ranging from 1 minute to 1 hour.

6. Material obtained according to a production process according to at least one of claims 1 to 5, characterized in that the material has at least 0.01% by weight of a mixture of lanthanides.

7. Material obtained according to a production process according to at least one of claims 1 to 6, characterized in that the material has a lanthanide fraction of 20% by weight.

8. A method for manufacturing a part from a titanium alloy in an additive process, comprising the steps of: a) providing titanium or a titanium alloy which is / are free of lanthanides, b) providing a mixture of lanthanides, c) alloying components a) and b), d) using the alloy obtained in c) to manufacture a part in a manufacturing process, preferably a primary transformation and / or a coating, e) optionally experimentally determining the peritectic temperature of the part, and (f) carry out a subsequent heat treatment at a temperature T which is higher than the peritectic temperature.