PLASMA CURRENT COLLECTOR TREATMENT METHOD

Low temperature atmospheric plasma treatment with arcing effectively cleans and modifies current collectors, addressing the limitations of conventional methods by enhancing adhesion, wettability, and reducing resistance for improved battery performance.

FR3148323A1Pending Publication Date: 2024-11-01SAFT GRP SA
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
FR2023004217
Authority / Receiving Office
FR · FR
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-26
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Conventional cleaning processes for current collectors in batteries are expensive, introduce pollutants, and do not effectively improve the surface condition or interface properties, which are crucial for enhancing energy density and performance.

Method used

A low temperature atmospheric plasma treatment with electric arc is applied to current collectors to clean and modify their surface, removing organic pollutants and improving adhesion, wettability, and reducing interface resistance.

Benefits of technology

The plasma treatment with arcing effectively cleans the surface, enhances adhesion and wettability, and reduces electronic resistance, leading to improved performance and durability of the current collectors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000012_0000
    Figure 00000012_0000
  • Figure 00000013_0000
    Figure 00000013_0000
  • Figure 00000014_0000
    Figure 00000014_0000
Patent Text Reader

Abstract

PLASMA TREATMENT METHOD FOR CURRENT COLLECTORS This application relates to a treatment method for improving the surface condition of a current collector by applying a low-temperature atmospheric plasma with arcing, as well as the collectors that can be obtained by said method. Figure for abstract: none
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: METHOD FOR TREATING A CURRENT COLLECTOR BY PLASMA

[0001] The present invention relates to the field of batteries consisting of primary or secondary type electrochemical elements, in particular lithium, and more particularly the current collectors of these electrochemical elements.

[0002] Current collectors used in the battery field contain deposits on the surface linked to their manufacture, in particular organic deposits such as grease or solvents.

[0003] It is important to clean the surface of the collector because these species affect the quality and / or quantity of ink deposits in particular, negatively impacting the operation of the accumulator.

[0004] Conventionally used decontamination / cleaning processes are expensive and involve the use of solvents (e.g. acetone, ethanol, etc.). However, the use of these solvents is increasingly regulated. Furthermore, these solvents can in turn introduce additional pollutants into the battery.

[0005] Avoiding such a solvent decontamination step is therefore becoming increasingly necessary for battery manufacturers.

[0006] Furthermore, the trend towards increasing energy densities and performances implies on the one hand improving the collector / active materials interfaces and on the other hand reducing the quantities of adhesion / cohesion materials and percolation materials.

[0007] Thus, plasma treatment has been considered for electrochemical applications.

[0008] US 2019 / 0237758 describes a current collector surface on which a lithium layer is deposited by means of a plasma in a reducing atmosphere. This application does not, however, concern the cleaning or improvement of the surface condition of the collector.

[0009] WO 2015 / 009867 describes a treatment of a surface of an electrochemical element, by plasma.

[0010] It remains desirable to provide an improved collector treatment method making it possible in particular to decontaminate and / or improve the properties of the surface of the current collectors.

[0011] Plasma processing may involve the formation of an electric arc ("arcing") when an electrical contact is created between the substrate to be treated and the plasma forming device. Generally, users seek to avoid the formation of an electric arc, particularly when treating fragile surfaces, because the arc causes generally a deterioration of the substrates.

[0012] It has now been discovered that current collector processing can be improved by the low temperature atmospheric plasma technique with electric arc ("with arcing").

[0013] According to a first object, the present application therefore relates to a method for treating a current collector suitable for electrochemical use, such that the treatment is carried out by plasma and characterized in that said plasma is a low temperature atmospheric plasma with arcing.

[0014] The low-temperature atmospheric plasma treatment process with electric arc makes it possible to clean the surface of the collector and also makes it possible to improve its surface condition for the purposes of its electrochemical use, within an electrochemical element.

[0015] Here, cleaning is understood to mean the elimination or degradation, for example by carbonization, of various pollutants, in particular organic pollutants, which could be present on the surface of the collector.

[0016] The improvement of the surface condition is understood here as any modification making it possible to improve the chemical and electrochemical properties of the collector.

[0017] Among these modifications, we can notably cite the modification of the surface chemistry; the increase of the adhesion properties with a view to the subsequent deposition of materials, such as an ink; the reduction of the interface resistance; etc.

[0018] These modifications can in particular be illustrated by the micro-structuring on the surface of the collector, the modification of the roughness, the modification of the surface composition for example by the creation of chemical species on the surface, and / or the increase in wettability.

[0019] These properties are particularly beneficial for improving the affinity of the collector with the inks comprising the active material(s), binder(s), conductive material(s), additive(s) and possible solvent(s), as well as the quality of their coating.

[0020] More particularly, it has been unexpectedly observed that arcing makes it possible to obtain better interface performances, in particular in terms of durability, compared to conventional treatments such as corona treatment or plasma treatment alone, and thus to improve the performances of the accumulator.

[0021] The term "current collector" designates a metallic collector, suitable for use as an electrode support and / or accumulator current collector.

[0022] Said collector is generally in the form of a strip of conductive material, such as a metal. As metal, mention may in particular be made of materials such as aluminum, copper, tin, nickel, iron, molybdenum, zinc, manganese, steels (including stainless steel), and their alloys and / or mixtures. According to one embodiment, the current collector is made of copper or aluminum.

[0023] It is further understood that the collectors may also be coated. Indeed, before the current collector is coated with the layer of active material composition, it may be coated, on one of its faces or on both of its faces, with a coating intended to improve the electronic conductivity between the layer of active material composition and the strip and / or to improve the adhesion of the layer of active material composition to the strip. The coating material may be chosen from the group consisting of carbon, graphite, carbon fibers, carbon nanotubes and mixtures thereof. The coating material may be obtained by coating the strip with a dispersion of the material and then evaporating the solvent from the dispersion, or it may be obtained by cathode sputtering. Only certain parts of the strip may be coated with the coating material.The coated parts may be separated from each other by predetermined or periodic intervals ("intermittent coating"). The intermittent coating is preferably present on both sides of the strip. It facilitates the processing of the electrodes.

[0024] Typically, the coating may be a carbon coating.

[0025] In the case where the collector is coated, the treatment according to the invention can be carried out on the face of the collector which has been coated.

[0026] The concept of atmospheric plasma as used herein refers to a technique in which the plasma can be generated directly in ambient air without the need for a controlled atmosphere enclosure. These plasmas are therefore distinguished from reducing plasmas conducted in a reducing atmosphere.

[0027] These plasmas are also called low temperature because the temperatures of the plasma thus generated are typically between 20°C and 75°C, and are therefore much lower than the temperatures of conventional plasmas (of the order of several thousand degrees).

[0028] The arcing or electric arc technique consists of electrically connecting the substrate to be treated (here the collector) to the plasma torch which will generate electric arcs between the torch and the substrate / collector during the plasma treatment.

[0029] Typically, said arc can be made by electrical contact between the collector and the torch, when applying the plasma to said collector. This contact can in particular be made by connecting the mass of the collector to the mass of the plasma apparatus, or by maintaining the plasma source at an appropriate distance from the sample, typically less than 100 mm, preferably between 5 mm and 25 mm, the distance being able to be adjusted according to the type of torch used or the material constituting the collector.

[0030] According to one embodiment, the plasma may be a plasma of a gas chosen from air, nitrogen, oxygen, hydrogen, helium, argon, halides such as than hydrogen halides, and their mixtures.

[0031] According to one embodiment, the method according to the invention may comprise the steps of:

[0032] Generation of a gas plasma by means of a plasma torch, at atmospheric pressure;

[0033] Creation of an electric arc between said collector and said torch; and

[0034] Submitting at least a portion of at least one surface of said collector to said plasma.

[0035] Typically, the plasma can thus be applied for a variable duration, at a speed typically between 5 and 100 mm.s', which a person skilled in the art can adapt according to the nature of the collector and the conditions for producing the plasma. Generally, the treatment can be carried out for a duration sufficient to obtain the desired surface condition of the collector, preferably without degrading its integrity.

[0036] According to one embodiment, the method may comprise directing a plasma source to the surface of said collector at a temperature between about 20°C and 75°C, and under atmospheric pressure.

[0037] Devices for plasma application are generally commercially available. Examples include the low-temperature OpenAir device.

[0038] For example, the plasma may be a dry air plasma.

[0039] One or more parameters of the plasma treatment process may be adjusted to facilitate the desired surface modification (e.g., treatment gas selection, treatment duration, and / or distance from the plasma source). For example, one or more parameters of the plasma treatment process may be selected to optimize surface adhesion and / or wettability.

[0040] According to another object, the present application also relates to a current collector capable of being obtained by the method according to the invention.

[0041] A collector capable of being obtained by the method according to the invention can be identified by its surface state, and in particular according to its wettability and roughness parameters and also its electrochemical characteristics.

[0042] According to one embodiment, said current collector has, after treatment, a resistance less than 30% of the resistance before treatment, the resistance being measured by impedance spectrometry, for example over a frequency range of 103 to 104 Hz, typically 10 to 10000 Hz.

[0043] According to one embodiment, the surface of said collector has a wettability defined by a contact angle of less than 50°, in particular less than 10°, and particularly less than 5°, in a contact angle test using a goniometer with a drop of water.

[0044] According to one embodiment, the collector according to the invention has a state of surface that can be characterized visually, for example in terms of surface irregularity or roughness. Thus, in particular, impacts created by arcing can be visualized by scanning electron microscopy (SEM) and are characterized by a spherical shape with a diameter of a few microns. Roughness can be analyzed by profilometry, and defined by the surface roughness parameter Sq. Thus, the impacts created can multiply by a factor of 4 the peak height parameter Sq measured by profilometry.

[0045] According to another of its objects, the present application also relates to an electrode comprising the collector according to the invention, on which is coated on at least one of its faces a composition comprising one or more active material(s), conductive material(s), and optionally binder(s), additive(s) and / or solvent(s).

[0046] Said electrode may be a positive electrode or a negative electrode.

[0047] According to another object, the present invention also relates to an electrochemical element comprising a current collector coated according to the invention and a solid electrolyte of sulfide type.

[0048] The term "electrochemical element" means an elementary electrochemical cell consisting of the positive electrode / electrolyte / negative electrode assembly, making it possible to store the electrical energy supplied by a chemical reaction and to restore it in the form of current.

[0049] Said element may be a non-rechargeable battery, called primary or rechargeable, also called secondary.

[0050] According to one embodiment, said element is an electrochemical element of the lithium-ion type, the electrolyte being able to be liquid, polymeric or solid.

[0051] Said element can be prepared from at least one current collector according to the invention. Thus, the method according to the invention can be applied to at least one face of at least one collector, before assembling the other constituents of the electrochemical element on said face.

[0052] According to another object, the present invention also relates to an electrochemical module comprising the stack of at least two elements according to the invention, each element being electrically connected with one or more other element(s).

[0053] The term “module” therefore designates here the assembly of several electrochemical elements, said assemblies being able to be in series and / or parallel.

[0054] According to another of these objects, the invention also relates to a battery comprising one or more modules according to the invention.

[0055] The term “battery” means the assembly of several modules according to the invention.

[0056] The invention may be illustrated with reference to the following Figures: Figures

[0057] [Fig.l] [Fig.l] schematically represents the application of a plasma to a substrate.

[0058] As shown in [Fig.l], the application of a plasma to a collector (4) comprises feeding gas (1) into a plasma torch. An electric arc (arcing) (3) is typically obtained for example when the sample being treated is close to the torch (of the order of about 5 mm to about 25 mm), or when the substrate to be treated is electrically connected to the torch, so as to be at the same potential. The electric arc (3) causes an electric discharge (2).

[0059] The energy provided by the plasma and the arc causes the change of state of the surface of the collector (4) by ionization of the atoms and formation of the corresponding ions (6) and radicals (5) and electrons (7).

[0060] [Fig.2] [Fig.2] represents the variation of the contact angle between the surface of a collector and a drop of water in the wettability test (goniometer) for an untreated aluminum collector (continuous curve, for comparison) and a plasma-treated collector with arcing (dotted curve, according to the invention), as a function of time.

[0061] [Fig.3] [Fig.3] visually illustrates the improvement in water wettability on a plasma-treated aluminum collector with arcing according to the invention (right), compared to the same untreated collector (left).

[0062] [Fig.4] [Fig.4] represents the variation of absorbance as a function of length waveform for an untreated aluminum collector (curve 1), treated by plasma without arcing (curve 2), treated by plasma with arcing according to the invention (curve 3), respectively.

[0063] [Fig 5] [Fig 5] illustrates the analysis of the surface by scanning electron microscopy (SEM) on untreated aluminum collector (A) or treated by plasma with arcing (B), and with a lower magnification on untreated aluminum collector (C) or treated by plasma with arcing (D).

[0064] [Fig.6] [Fig.6] represents the measurements in optical profilometry (in confocal mode) with roughness measurement for an untreated aluminum collector (left, height parameter: 2.245 pm) and for a plasma-treated aluminum collector with arcing (right, height parameter: 0.4863 pm).

[0065] [Fig.7] [Fig.7] represents the measurement of the contact angle of a drop of water on an untreated aluminum collector (A), treated by Corona treatment (B) and treated by plasma with arcing (C).

[0066] [Fig.8] [Fig.8] represents the variation of the contact angle formed by a drop of water as a function of time on an untreated aluminum collector (1), treated by Corona treatment (2) and treated by plasma with arcing (3).

[0067] [Fig.9] [Fig.9] represents the parameters involved in the angle measurement of contact by goniometry.

[0068] The following examples are given by way of illustration and not limitation of the invention: Examples

[0069] An OpenAir plasma device with a rotary type torch (with a scanning speed between 5 and 80 mm / s) was used.

[0070] The sample is an aluminum foil, such as an A4 sheet, about 15 pm thick. It was used as is (untreated, control) or can be subjected to one of the following treatments: Plasma, plasma with arcing, corona.

[0071] Plasma treatment with arcing is carried out by keeping the torch at a distance of less than 10 cm, typically between approximately 5 and 25 mm from the sample.

[0072] The untreated and treated samples were subjected to various tests and characterizations: Infrared absorbance measurement

[0073] The industrial and non-degreased aluminum strip was tested by plasma treatment with and without arcing. The results are illustrated in [Fig.4] and show that the plasma treatment (curve 2) allows to attenuate the solvent peaks obtained for the untreated sample (curve 1). This degreasing effect is even more pronounced by plasma treatment with arcing (curve 3). Thus, the infrared analysis presented in [Fig.4] shows the cleaning of the collector surface after passage under the plasma: the plasma allows to reduce the functional groups linked to the presence of grease on the surface, and this is accentuated if the arcing is activated. Goniometer

[0074] The contact angle 0 formed by a drop of liquid placed on the sample is defined by the Young-Dupré law:

[0075] cos 0 = (ysv-Ysl) / Ylv

[0076] where Ysv- Ysl, and Ylv denote respectively the surface tension of the solid / vapor, solid / liquid and liquid / vapor interfaces considered, as illustrated in [Fig.9].

[0077] The measured angle therefore depends on the parameter Ysl-

[0078] The results are illustrated in Figures 2, 3, 7 and 8.

[0079] Contact angle analyses showed that the collector treatment Plasma aluminum generates better wettability when depositing a drop of electrolyte on the treated collector (reduction of the contact angle from 90° to 30°). The additional arcing treatment accentuates the improvement in wettability: the contact angle between the collector and the drop decreases more sharply (17°). Scanning electron microscopy

[0080] Analysis of the surface by high magnification electron microscope shows with evidence (illustrated in [Fig 5] (AD)) the impact of plasma treatment with arcing on an aluminum collector. Indeed, many impacts are visible and significant post-treatment.

[0081] Measurement in optical profilometry (in confocal mode) with roughness measurement

[0082] The effect identified by SEM is also measurable and quantifiable as illustrated in [Fig.6], at lower magnification by analysis of roughness by optical profilometry (in confocal mode).

[0083] Thus the roughness Sq (root mean square height) goes from 2.24 to 0.48pm. The surface layers, pollution, oxidation, protective greases, etc. on the surface of the aluminum have been removed. Impedance measurement

[0084] The tests were carried out on button batteries comprising a treated or untreated collector as a positive electrode, and lithium iron phosphate (LFP) and a lithium nickel, cobalt and aluminium (NCA) oxide as active material (88% LFP / NCA active material + 7% carbon black + 5% PVdF binder).

[0085] The same ink based on LFP+NCA material was coated on two collectors, one without treatment and the other with plasma treatment with arcing. The electrodes were formed in buttons versus a Lithium electrode, recovered and then mounted in a symmetrical button (without transfer) in order to evaluate the electronic resistance (semicircle at high frequencies).

[0086] The impact of the surface treatment on the collector was evaluated in terms of power weight.

[0087] The impedance measurement leads to the following results:

[0088] [Tableauxl] Electronic resistance (Q.cm2) on new electrode Collector Untreated aluminum 31.8 Collector Plasma-treated aluminum with arcing 22.9

[0089] The measurement of the impedance clearly shows that the plasma treatment with arcing induces a reduction in the electronic resistance of the electrode:

[0090] Plasma treatment with arcing leads to a 27% reduction in the electronic resistance of the positive electrode.

[0091] Thus, the tests carried out demonstrate that the treatment of an aluminum collector with plasma with arcing makes it possible to clean the strip, improve the surface wettability and reduce the electronic resistance of the positive electrode thus manufactured. after ink coating.

Claims

Claims

1. A method of treating a current collector suitable for electrochemical use, such that the treatment is carried out by plasma and characterized in that said plasma is a low temperature atmospheric plasma with arcing.

2. A method according to claim 1 comprising the steps of: - generating a gas plasma by means of a plasma torch, at atmospheric pressure; - creating an electric arc between said collector and said torch; and - subjecting at least a portion of at least one surface of said collector to said plasma.

3. A method according to claim 1 or 2 such that the current collector is a metal strip.

4. A method according to any preceding claim, such that the current collector is an aluminum or copper foil.

5. A method according to any one of the preceding claims such that the plasma is a plasma of a gas chosen from air, nitrogen, oxygen, hydrogen, helium, and mixtures thereof.

6. A method according to any preceding claim, wherein said arc is produced by electrical contact between the collector and the torch.

7. Current collector obtainable by the method according to any one of the preceding claims.

8. Current collector according to claim 7 such that it has after treatment a resistance less than 30% of the resistance before treatment, the resistance being measured by impedance spectrometry.

9. Current collector such that it has a surface having a wettability defined by a contact angle of less than 50°, in particular less than 10°, and particularly less than 5°, in a contact angle test using a goniometer with a drop of water.

10. Electrode comprising the collector according to any one of claims 7, 8 or 9 on which is coated on at least one of its faces a coating comprising one or more active material(s), at least one binder and at least one additive.

11. An electrochemical element comprising a current collector according to claim 7, 8 or 9 or an electrode according to claim 10.

12. An electrochemical element according to claim 11 as a primary or secondary battery.

13. An electrochemical element according to claim 11 or 12 such that it is a lithium battery.

Citation Information

Patent Citations

  • Printed silver oxide batteries

    WO2015009867A1

  • Negative electrode for lithium secondary battery and method for manufacturing same

    EP4207352A1

  • Plasma pretreatment on current collectors for thin film lithium metallization

    US20190237758A1

  • Method for manufacturing spiral-wound battery

    US20190296386A1

  • Pretreatment and post-treatment of electrode surfaces

    WO2022216897A1