A HIGH-PERFORMANCE CURRENT COLLECTOR FOR LITHIUM BATTERIES, A CONDUCTIVE PASTE AND ITS MANUFACTURING PROCESS
The high-performance lithium battery current collector addresses the instability of existing network structures by using modified carbon nanotubes to form a three-dimensional, magnetically aligned network, enhancing adhesion and conductivity, thereby improving battery performance and lifespan.
Patent Information
- Application Number
- FR2024004806
- Authority / Receiving Office
- FR · FR
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-09
- Filing Date
- 2024-05-07
- Publication Date
- 2024-11-15
AI Technical Summary
Current lithium-ion battery current collectors face issues with random network structures of carbon nanotubes leading to poor adhesion, high internal resistance, and difficulty in maintaining a stable connection network during charge and discharge cycles, which affects battery performance and lifespan.
A high-performance current collector with a functional coating using modified multi-walled carbon nanotubes in a dumbbell-shaped structure, forming a double-anchored island bridge network that aligns under a magnetic field, creating a three-dimensional network with improved adhesion and conductivity, capable of adapting to volume changes.
The solution enhances the stability of the connection network, reduces internal resistance, and improves the battery's cycle life and energy density by maintaining a reliable spatial distribution of conductive substances, ensuring durable adhesion and efficient electron transfer.
Abstract
Description
Title of the invention: A HIGH-PERFORMANCE CURRENT COLLECTOR FOR LITHIUM BATTERY, A CONDUCTIVE PASTE AND ITS MANUFACTURING METHOD REFERENCE TO OTHER RELATED DOCUMENTS
[0001] The present invention claims priority from Chinese Patent Application No. 202310512566.1, entitled "A high-performance current collector for lithium battery, a conductive paste and a manufacturing method therefor", filed on May 9, 2023, with the Chinese Patent Office, the contents of which are fully incorporated by reference herein. Technical field
[0002] The technical field of the invention is that of the production of lithium batteries, the present invention relates in particular to a high-performance current collector for lithium-ion batteries, a conductive paste and its manufacturing method. TECHNOLOGICAL BACKGROUND
[0003] Lithium-ion power batteries, among others, are already widely used in certain growing sectors, such as electric vehicles or energy storage systems. A current collector of lithium-ion batteries and other rechargeable batteries refers to a structure or part that can collect current. For lithium-ion batteries, this structure is mainly made of copper or aluminum metal foils. This structure may also include connecting tabs. The main role of a current collector is to collect the current generated by the active material of the battery to form a larger current intended for the outside. Therefore, the current collector must be in full contact with the active material and have the lowest possible internal resistance.
[0004] In current technology, the use of functional coatings for the surface treatment of conductive substrates of batteries represents a significant technical innovation. Carbon coating on aluminum or copper foils is achieved by uniformly and meticulously applying conductive materials such as nanoscale conductive graphite, carbon-coated particles or carbon nanotubes. Not only can carbon-coated copper or aluminum foils provide excellent static conductivity and collect microcurrents from active materials, thereby significantly reducing the contact resistance between the materials of the positive electrode / negative and the current collector, but they also improve the adhesion between the latter two, thus reducing the amount of binder required, and resulting in a significant improvement in the overall performance of the battery.
[0005] Currently, LiFePO4, which is safer and cheaper, has considerable potential as an anode material. However, its electronic and ionic conductivities are low in nature, and its mass and volume density are also relatively low, which impairs conductivity and adhesion (bonding). Other defects such as flaking may also be observed during use. Applying carbon-coated aluminum foils to the anode collectors can reduce the contact impedance at the interface, decrease the internal resistance of the battery, alleviate the internal planning of the battery, and partially improve the discharge rate of the battery.In terms of the anode of lithium-ion batteries, the requirements for high surface area density of electrodes for high energy density batteries, the use of silicon-carbon materials prone to expansion, as well as the specific needs of stacked-layer batteries to prevent spalling, can all be addressed by using carbon-coated copper foils.
[0006] Current carbon sheets use conductive materials such as graphite, carbon black, and multi-layer carbon nanotubes, mixed with different ratios of dispersants and binders to form a uniformly dispersed conductive paste, which is then applied to aluminum or copper sheets. The carbon layer is applied at a thickness of between 2 and 50 μm, and is therefore relatively thick, but has low resistance to chipping during repeated charging cycles. Depending on the proportions of the conductive materials, the carbon layer exhibits some visual variation but generally remains black or gray in color with various shades of depth.However, when using different material systems for lithium batteries, simple observation based on color differences with current coating equipment cannot accurately determine the density and thickness of electrode layers to ensure the stability of current collector product quality. This limitation hinders the accuracy of coating rate measurement during high-speed production quality management, ultimately limiting production efficiency.
[0007] To optimize the performance of the conductive coating of current collectors, current technology presents, in Chinese patent application number 201610410998.1, an innovative method for manufacturing a current collector with a conductive coating based on carbon nanotubes. This method includes applying a carbon nanotube coating to a current collector metallic, with a thickness ranging from 1 to 50 qm. This coating has a network structure of microcracks and a porous and rough surface. The carbon nanotube coating creates an effective conductivity network for the electrode by forming dense microcracks after drying, which strengthens adhesion to the current collector and reduces the internal resistance of the battery. However, this process requires the use of several conductive materials and has a relatively high thickness, in the order of microns, which can lead to detachment of the coating after several charge and discharge cycles. This detachment exposes the metallic layer of the current collector to active substances, thus increasing the risk of corrosion and oxidation of the current collector electrodes and reducing the battery life.In addition, the formed conductive coating has poor realignment capability, manifested by a black or gray color, which complicates the accurate assessment of the coating thickness and coverage rate during the application process. This lack of an effective method for monitoring coating quality during application negatively impacts the subsequent steps of coating and welding of battery electrodes. The inability to accurately determine the coating color can have adverse consequences during these steps.
[0008] Chinese invention patent application number 201610522526.5 discloses a method for forming a thermally and electrically conductive network from a conductive gel material. This material is composed of the following weight proportions: carbon nanotubes (4-6 parts), conductive carbon black (8-12 parts), flake graphite (1-3 parts), polyvinyl alcohol (15-25 parts). This invention uses carbon materials with high thermal and electrical conductivity, at least one dimension of one nanometer, to form network materials, such as carbon nanotubes and graphene. Integrated with conventional conductive carbon black, they form a continuous, thermally and electrically conductive network coating on the collector.This not only improves high-power cooling during charging and discharging, but also meets the electrical conductivity requirements, thus avoiding thermal aging of the system and increasing its service life. However, this method requires the use of more than two types of conductive materials, which leads to a relatively large thickness of the conductive network coating as well as poor shrinkage quality and an uncontrollable gray-black color. In addition, the spatial structure of the network material is random, without specific orientation. This limits its effectiveness in reducing interfacial resistance, and improving electrical and thermal conductivity as well as adhesion.
[0009] During the charging and discharging process of lithium batteries, the relative position, contact area and contact points of various internal components (especially active materials, conductive materials and collectors) vary periodically due to electrochemical reactions and physical volume changes. During these variations (especially during volume expansion) the distances between the components increase, the contact points decrease and the contact resistance increases, which results in an increase in the internal resistance of the battery and a rapid drop in its efficiency. In addition, it is difficult to ensure that each material can accurately return to its initial position and that the original connection network and its resistance are restored after each cycle.The spatial distribution of the components then gradually becomes disordered, which deteriorates the connection performance (electrical and thermal conductivity). Therefore, after several cycles, some aspects of the battery's performance may deteriorate. To overcome this defect, it is essential to ensure that the internal components of the lithium-ion battery maintain a strong and durable connection network during charge and discharge cycles, as well as after many cycles. This helps reduce the loss of the connection network due to physicochemical reactions, this loss leading to an increase in the internal resistance of the battery and a decrease in its capacity.
[0010] In the above-mentioned existing technologies, the randomly and disorderly arranged carbon nanotubes cannot fully exploit the mechanical, electrical and thermal potential of each individual nanotube and their assemblies. In addition, this disordered distribution can easily cause agglomeration of the carbon nanotubes and increase the contact resistance between them. Therefore, the lithium-ion battery anode materials made with this type of conductive coating exhibit performance far below expectations. However, it is difficult to control and construct a specific three-dimensional structure by arranging the carbon nanotubes in an orderly manner with the techniques.Therefore, it is necessary to simultaneously improve the carbon nanotubes, conductive paste, coating structure and manufacturing process of the current collector to significantly improve the overall performance of the current collector. CONTENT OF THE INVENTION
[0011] The present invention aims to overcome the shortcomings presented by current techniques by providing a high-performance current collector for lithium batteries. The functional coating of this collector uses a modified conductive agent as a conductive material. Based on the dumbbell-shaped structure of the modified conductive agent, a double-anchored bridge-island structure network is formed in the coating, which is capable of automatically adapting to deformations due to volume changes. Under the effect of an external magnetic field, the modified conductive agent aligns obliquely and parallel to a specific angle of 15-45° in the thickness direction, thereby forming a reinforced, conductive, thermal, and high-resilience three-dimensional network. This solves the problem of random network structures in current techniques, which fail to simultaneously reconcile the reinforcement, conductivity, and thermal conductivity properties of the coating. When applied to lithium batteries, the current collector of the invention can establish a reliable spatial network structure with the active components.During the charging and discharging cycles, as well as during the expansion and contraction of the battery coating and active substances, the modified conductive agent can, through its angle changes and anchoring effect, maintain the order of the spatial distribution of the internal conductive substances of the lithium battery. This can preserve the relative stability of the connection network and the electrical connection strength, thereby solving the problem of decreased adhesion and coating peeling after multiple charging and discharging cycles in lithium battery applications.
[0012] The present invention also provides a method for preparing the modified conductive agent with a dumbbell-shaped structure. This method involves oxidizing the multi-walled carbon nanotubes, chemically modifying their ends, and preconnecting larger-sized nano-conductive agent particles at their ends to form a dumbbell-shaped structure. In the coating, this structure forms a double-anchored bridge-island network capable of automatically adapting to a regular arrangement and automatically adjusting the tilt angle to compensate for deformations due to volume changes. During the oxidation process, the single-layer carbon nanotubes exhibit vacancy defects due to the oxidation of local C-C bonds. The presence of these defects results in the appearance of magnetic moments in the vicinity, thus giving the modified conductive agents of the carbon nanotubes weak magnetization.
[0013] In addition, the present invention also provides a conductive paste and its preparation method for preparing the above-mentioned functional coating. By simultaneously improving the formulation and the manufacturing process of the coating, it is possible to reduce the amount of modified conductive agent added and to obtain a coating with an average thickness of not more than 800 nm after drying. This conductive paste uses a slightly modified conductive agent magnetic to form an oblique arrangement structure of 15 to 45° in the direction of the coating thickness, thereby increasing the specific contact area with the active substances. This can significantly improve the adhesion of the coating after many charge and discharge cycles, solving the problems of excess thickness and poor adhesion of current coatings, thereby improving the service life and high-power performance of rechargeable batteries (such as lithium-ion batteries).
[0014] The present invention also provides a preparation method for the aforementioned current collector, which solves the problems of formation and process complexity for creating an adaptive three-dimensional connection structure in the coating. By using a constant magnetic field, a network alignment of the magnetic modified conductive agents is achieved, which enhances the conductive performance and adhesion of the functional coating, while reducing the amount of modified conductive agent and the thickness of the functional coating. During the conductive paste coating process, the three-dimensional structuring of the modified conductive agent and the substrate is facilitated and controlled. Thus, the structuring can be carried out simultaneously with the coating and drying processes, decreasing the manufacturing steps and obtaining a coating where the oriented modified conductive agent is intertwined with the substrate.
[0015] To achieve the above-mentioned objectives, the present invention proposes the following technical solutions:
[0016] A high-performance current collector for a lithium battery, comprising a metal foil and a functional coating formed by applying a conductive paste to one or both surfaces of the metal foil, forming after drying a functional layered covering structure with a thickness of not more than 800 nm;the functional coating comprises several strip-shaped modified conductive agents which are multi-walled carbon nanotubes modified by magnetic orientation, after curing, these modified conductive agents are parallel to each other in the coating and form an angle of 15-45° with the surface of the metal foil, orienting obliquely, they are interwoven with modified nanofibers, a binder and other modified conductive agents to form an oriented three-dimensional network connection structure, strengthening the fixation, electrical and thermal conductivity, and making uniform deformation and automatic return to the initial position possible. ;
[0017] The magnetically oriented modified multi-walled carbon nanotubes in the functional coating should have a dumbbell-shaped structure, with an inner diameter of at least 5 nm, an outer diameter of not more than 20 nm, and a length of not more than 1200 nm. After oxidation and chemical modification, they have a fiber structure with wider ends and a narrower center, once aligned, the wider lower ends connect respectively to the surface of the metal foil while the upper ends connect to each other, now binding the other conductive nanoparticles of different sizes and the modified nanofibers to the narrower center of the fiber, which forms a three-dimensional island-bridge structure anchored at both ends and aligned, where the elastic three-dimensional network limits the deformation and displacement of the modified multi-walled carbon nanotubes and conductive nanoparticles during battery operation;This structure automatically adapts and compensates for internal volume variations, as well as deformations and displacements of the conductive nanoparticles during the charging and discharging cycles of the lithium battery, ensuring the connection between the functional coating, the surface of the metal foil and the active material.
[0018] A conductive paste for the current collector of a high-performance lithium battery characterized by being an aqueous dispersion prepared from modified multi-walled carbon nanotubes, conductive nanoparticles, modified nanofibers, a dispersant, a binder, and a solvent. This paste has a solids content of 0.1 to 10%, a viscosity of 200 to 1000 mPa-s (25°C), and a pH of 8 to 11;
[0019] The proportions by weight of the components of this conductive paste are respectively as follows: modified multi-walled carbon nanotubes: conductive nanoparticles: modified nanofibers: dispersant: binder: solvent = (0.01-1.8): (0.01-0.2): (0.02-2): (0.02-20): (0.05-20): (56-99.89).
[0020] The preparation method of the conductive paste for high-performance lithium battery current collector is characterized by the following steps:
[0021] El: Preparation of materials:
[0022] The modified multi-walled carbon nanotubes, the conductive nanoparticles, the modified nanofibers, the dispersant, the binder, and the solvent are prepared according to the indicated proportions.
[0023] E2: Preparation of the high concentration modified conductor suspension:
[0024] The modified nanofibers and the dispersant are weighed according to the proportions, then added to 1 / 3 of the solvent and dissolved completely by mechanical stirring, the required modified conductor is then weighed and then added to the mixed solution to be ultrasonicated for 30 minutes to obtain a suspension of modified conductor (specifically a suspension of high concentration modified multi-walled carbon nanotubes).
[0025] E3: Magnetic loading:
[0026] The dispersed solution of modified multi-walled carbon nanotubes and nanoscale conductive agents is placed in a strong external magnetic field to activate magnetic charging to further stimulate the magnetic anisotropy of the modified multi-walled carbon nanotubes, thereby obtaining a suspension of high-concentration magnetic modified multi-walled carbon nanotubes.
[0027] E4: Initial dispersion:
[0028] the binder is added in the corresponding proportion to the suspension of high-concentration magnetic modified multi-walled carbon nanotubes, the solvent is then added up to the required amount; a preliminary dispersion is carried out using first a high-speed vacuum disperser, then a ball mill; the shear rate of the vacuum disperser should be 10-25 m / s, with a vacuum pressure of at least 0.085 MPa, and a dispersion time of 1-5 hours while in the ball mill, the diameter of the balls should be 0.2-2 mm, with a proportion of 30-90%, a rotation speed of 600-10000 rpm, and a grinding time of 0.1-5 hours.
[0029] E5: Secondary dispersion:
[0030] Secondary dispersion is carried out using ultrasonic processing equipment for ultrasonic resonance; an alternating magnetic field on both sides is applied to make the modified multi-walled carbon nanotubes and conductive nanoparticles disperse uniformly and align in the same direction under the induction of the magnetic field, thereby obtaining a conductive paste with a magnetic orientation.
[0031] The manufacturing process of the high-performance current collector for lithium battery is characterized by the following steps:
[0032] (Al) A current collector metal foil, a dispersed conductive paste are prepared, and coating equipment, ultrasonic equipment, constant magnetic field generating equipment, and drying equipment are set up.
[0033] (A2) The already dispersed conductive paste is applied to the surface of the sheet metallic to form on this surface a liquid colloidal layer with a viscosity of 200-1000 mPa-s (25°C) and a thickness of 500-1200 nm.
[0034] (A3) A constant magnetic field is applied perpendicular to the surface of the metal foil on the liquid colloidal layer, so that the oriented modified conductive agent aligns in an orderly manner under the induction of the applied magnetic field, and gradually unfolds, forming a parallel network, intertwined with the matrix.
[0035] (A4) By continuing to apply the magnetic field, the layer dries, the solvent and volatile components evaporate, the modified conductive agent maintains its alignment and posture while the viscosity of the layer increases and quickly sets, aligning parallel in the thickness direction with an inclination of 15-45° until the solidified components of the conductive paste attach to the surface of the metal foil, forming a dense functional coating with a thickness of not more than 800 nm, which thus creates on the surface of the metal foil a three-dimensional network structure with enhanced fixation, electrical and thermal conductivity and can be easily retracted.
[0036] BENEFICIAL EFFECTS
[0037] Compared with existing techniques, the present invention has the following advantages:
[0038] (1) The functional coating and conductive paste of this invention use Modified conductive agents as a conductive material. Thanks to their unique dumbbell-shaped structure, they form a bridge-island structure within the coating, anchored at both ends, which can automatically adapt and compensate for deformations caused by volume variations. In addition, these modified conductive agents possess magnetic anisotropy, allowing them to align in a specific orientation under the effect of a magnetic field. When used in lithium batteries, these modified conductive agents can automatically adjust their tilt angle according to the internal volume variations of the battery, establish a better spatial network structure with the active components, and ensure a reliable connection.During charge and discharge cycles, as well as during expansion and contraction of battery coatings and active substances, they maintain an orderly spatial distribution, thus ensuring the relative stability of the connection network and the electrical connection strength. This solves the problem of rapid decrease in coating adhesion after many charge and discharge cycles in lithium batteries, and prevents coating detachment.
[0039] (2) Modified conductive agents, modified nanocelluloses and agents dispersants are combined in the preparation of the conductive paste provided by this invention. The dispersing agents modify the surface of the modified conductive agents non-covalently, thereby reducing the Van der Waals force between the molecules and lowering their surface energy, which allows for better dispersion in an aqueous solution. The modified nanocelluloses provide a porous three-dimensional network structure to the modified conductive agents as well as other components in the functional coating, and the negatively charged groups create electrostatic repulsion forces between the fibers, forming a Stable colloid. This allows the modified conductive agents to remain stable in the pores, acting as a dispersion aid. Under the combined effect of the two, the magnetic modified conductive agents disperse normally in the conductive paste, preventing agglomeration and facilitating their alignment under the effect of the magnetic field in subsequent processes.
[0040] (3) The functional coating of this invention continuously applies a field external magnetic field during the conductive paste preparation and coating process. Under the influence of a strong magnetic field, the magnetically modified conductive agents are induced to form magnetic moments, which allows their organization. Eventually, this leads to the formation of a specific alignment of 15 to 45 degrees relative to the thickness direction, with a parallel arrangement in the coating.
[0041] (4) In the functional coating of this invention, the conductive agents modified are composed of carbon nanotubes, which, thanks to their relatively large inner diameter, can serve as ion diffusion channels. This allows Li+ ions to quickly penetrate through the coating along the internal cavity of the carbon nanotubes, thereby increasing the diffusion rate of Li+ ions and shortening their migration path. This improves electron transfer efficiency and reduces impedance. Applied to lithium batteries, this improves performance in terms of charge and discharge rates as well as low-temperature performance.
[0042] (5) In the functional coating of this invention, the oriented parallel alignment magnetic modified conductive agents impart magnetic anisotropy to the functional coating. By using a combination of magnetic current collectors with positive and negative poles for the battery, a stable magnetic field is formed between the positive and negative current collectors of the battery. This constrained magnetic field makes the migration of lithium ions more regular. On the other hand, by passing through the membrane of the lithium battery, the regular movement of lithium ions also increases the permeability efficiency of the membrane, thereby reducing its impedance. A lithium battery assembled with the polarized magnetic current collectors manufactured according to this invention has its capacity significantly increased, its impedance reduced, and its cyclic performance improved.In addition, the ability to adapt to volume changes and maintain a reliable connection increases the safety of lithium batteries during high-power discharges, improving the efficiency of energy use during charging and discharging, improving charging efficiency and reducing charging time.
[0043] (6) The functional coating of this invention constructs a network structure three-dimensional where modified conductive agents are interwoven with the materials of the flexible adhesive matrix. This provides a high-strength connection layer, high conductive efficiency and good flexibility, which improves the contact area between the rigid metal current collector and the conductive paste and the adhesion of the coating. In addition, it also reduces the interfacial resistance between the current collector and the battery active materials, increases the electrochemical stability of the current collector and prevents the increase in the internal resistance of the battery, thus minimizing the negative impact on battery performance, especially during high-current charging and discharging conditions.By using the three-dimensional network anchored at both ends of the modified conductive agents, volume changes during charge and discharge cycles are damped, improving the reliability of the electrical connection and avoiding separation between the conductive paste and the current collector. This strengthens the lasting adhesion between the metal foil material of the current collector and the active materials of the battery during repeated charge and discharge cycles, thereby improving the stability of the electrode, and avoiding cycle failures. This increases the specific capacity, cyclic stability and rate performance of the electrode. Therefore, the functional coating and lithium batteries prepared according to this invention have the advantages of high capacity, long cyclic life and good rate performance.
[0044] (7) Introduction of modified carbon nanotubes and construction of a network The three-dimensional structures presented in this invention provide more contact points for the active particles, thereby increasing the specific surface area of contact with the active materials. This greatly improves the adhesion of the positive and negative electrode materials to the current collector. Therefore, with the current collector of this invention, the proportion of binder in the pastes of the positive and negative electrodes can be reduced. This further reduces the internal resistance and improves the energy density of the battery. By using the current collector of this invention to prepare the positive electrode, the resistance is reduced to only one-third that of the pure metal foil, while the peel strength is increased more than fourfold.Lithium-ion batteries prepared with this current collector exhibit a reduction of more than 42% in internal AC resistance compared to batteries prepared with a pure metal foil current collector.
[0045] (8) The current collector provided by this invention can significantly increase the battery energy density, improve cycle life and rate performance. Under IC charge and 2C discharge regime, after 2000 cycles at room temperature, lithium-ion batteries prepared with The current collector of this invention retains 93% capacity, much higher than the 80% capacity retained by batteries with a pure metal foil current collector. In addition, their battery cycles show much better consistency.
[0046] (9) The steps of preparation method of high performance current collector for lithium-ion batteries and the conductive paste proposed by this invention are simple and the necessary materials are easy to obtain. In addition, this method has strong controllability and low preparation cost. The prepared current collector functional coating has a unique internal double-layer aggregation structure and excellent mechanical performance, offering high potential for development and use in fields such as the manufacture of lithium-ion batteries for power applications. METHOD OF IMPLEMENTATION
[0047] The exemplary embodiments below make it possible to explain the present invention in more detail.
[0048] Example of realization
[0049] The present invention provides a current collector, a conductive paste and their preparation method for a high-performance lithium-ion battery. This invention can be applied to lithium batteries using technologies such as lithium cobaltate (LCO), lithium manganate (LMO), lithium iron phosphate (LFP), ternary materials (nickel cobalt manganese lithium (NCM) and nickel cobalt aluminum lithium (NCA)), and it is compatible with various types of membranes and electrolytes, thus offering many application possibilities.
[0050] A high-performance current collector for a lithium battery, comprising a metal foil and a functional coating formed by applying a conductive paste to one or both surfaces of the metal foil, forming after drying a functional layered covering structure with a thickness of not more than 800 nm;the functional coating comprises several strip-shaped modified conductive agents which are multi-walled carbon nanotubes modified by magnetic orientation, after curing, these modified conductive agents are parallel to each other in the coating and form an angle of 15-45° with the surface of the metal foil, orienting obliquely, they are interwoven with modified nanofibers, a binder and other modified conductive agents to form an oriented three-dimensional network connection structure, strengthening the fixation, electrical and thermal conductivity, and making uniform deformation and automatic return to the initial position possible. ;
[0051] The modified conductive agent in the functional coating is a magnetically oriented modified multi-walled carbon nanotube having a shaped structure dumbbell, with an inner diameter of at least 5 nm, an outer diameter not exceeding 20 nm, and a length not exceeding 1200 nm. After oxidation and chemical modification, it has a fiber structure with wider ends and a narrower center, once aligned, the wider lower ends connect respectively to the surface of the metal foil while the upper ends connect to each other, now binding the other conductive nanoparticles of different sizes and the modified nanofibers to the narrower center of the fiber, which forms a three-dimensional island-bridge structure anchored at both ends and aligned, where the elastic three-dimensional network limits the deformation and displacement of the modified multi-walled carbon nanotubes and the conductive nanoparticles during battery operation;This structure automatically adapts and compensates for internal volume variations, as well as deformations and displacements of the conductive nanoparticles during the charging and discharging cycles of the lithium battery, ensuring the connection between the functional coating, the surface of the metal foil and the active material.
[0052] A conductive paste for the current collector of a high-performance lithium battery, characterized by being an aqueous dispersion prepared from a modified conductor (modified multi-walled carbon nanotubes), conductive nanoparticles, modified nanofibers, a dispersant, a binder, and a solvent. This paste has a solids content of 0.1 to 10%, a viscosity of 200 to 1000 mPa-s (25°C), and a pH of 8 to 11;
[0053] The proportions by weight of the components of this conductive paste are respectively as follows: modified conductor (modified multi-walled carbon nanotubes): conductive nanoparticles: modified nanofibers: dispersant: binder: solvent = (0.01-1.8): (0.01-0.2): (0.02-2): (0.02-20): (0.05-20): (56-99.89).
[0054] The preparation method of the conductive paste for high-performance lithium battery current collector is characterized by the following steps:
[0055] El: Preparation of materials:
[0056] The modified conductor (modified multi-walled carbon nanotubes), the conductive nanoparticles, the modified nanofibers, the dispersant, the binder, and the solvent are prepared according to the indicated proportions.
[0057] E2: Preparation of the high concentration modified conductor suspension:
[0058] The modified nanofibers and the dispersant are weighed according to the proportions, then added to 1 / 3 of the solvent and dissolved completely by mechanical stirring, the required modified conductor is then weighed and then added to the mixed solution to be ultrasonicated for 30 minutes to obtain a suspension of modified conductor (specifically a suspension of high concentration modified multi-walled carbon nanotubes).
[0059] E3: Magnetic loading:
[0060] The dispersed solution of modified multi-walled carbon nanotubes and nanoscale conductive agents is placed in a strong external magnetic field to activate magnetic charging to further stimulate the magnetic anisotropy of the modified multi-walled carbon nanotubes, thereby obtaining a suspension of high-concentration magnetic modified multi-walled carbon nanotubes.
[0061] E4: Initial dispersion:
[0062] the binder is added in the corresponding proportion to the suspension of high-concentration magnetic modified multi-walled carbon nanotubes, the solvent is then added up to the required amount; a preliminary dispersion is carried out using first a high-speed vacuum disperser, then a ball mill; the shear rate of the vacuum disperser should be 10-25 m / s, with a vacuum pressure of at least 0.085 MPa, and a dispersion time of 1-5 hours while in the ball mill, the diameter of the balls should be 0.2-2 mm, with a proportion of 30-90%, a rotation speed of 600-10000 rpm, and a grinding time of 0.1-5 hours.
[0063] E5: Secondary dispersion:
[0064] Secondary dispersion is carried out using ultrasonic processing equipment for ultrasonic resonance; an alternating magnetic field on both sides is applied to make the modified multi-walled carbon nanotubes and conductive nanoparticles disperse uniformly and align in the same direction under the induction of the magnetic field, thereby obtaining a conductive paste with a magnetic orientation.
[0065] The manufacturing process of the high-performance current collector for lithium battery is characterized by the following steps:
[0066] (Al) A current collector metal foil, a dispersed conductive paste are prepared, and coating equipment, ultrasonic equipment, constant magnetic field generating equipment, and drying equipment are set up.
[0067] (A2) The already dispersed conductive paste is applied to the surface of the sheet metallic to form on this surface a liquid colloidal layer with a viscosity of 200-1000 mPa-s at 25°C and a thickness of 500-1200 nm.
[0068] (A3) A constant magnetic field is applied perpendicular to the surface of the metal foil on the liquid colloidal layer, so that the oriented modified conductive agent aligns in an orderly manner under the induction of the applied magnetic field, and gradually unfolds, forming a parallel network, intertwined with the matrix.
[0069] (A4) By continuing to apply the magnetic field, the layer dries, the solvent and volatile components evaporate, the modified conductive agent maintains its alignment and posture while the viscosity of the layer increases and quickly sets, aligning parallel in the thickness direction with an inclination of 15-45° until the solidified components of the conductive paste attach to the surface of the metal foil, forming a dense functional coating with a thickness of not more than 800 nm, which thus creates on the surface of the metal foil a three-dimensional network structure with enhanced fixation, electrical and thermal conductivity and can be easily retracted.
[0070] Example 1
[0071] This example is a concrete application case. In example 1 of this implementation, the metal foil substrate used is an aluminum foil, with a thickness of 10 to 15 qm.
[0072] The high-performance current collector for lithium-ion batteries provided by this The invention comprises a metallic aluminum foil and a functional coating; the functional coating is a functional covering structure with a thickness of 700 nm, formed after conductive paste is applied and dried on both surfaces of the metallic aluminum foil; the functional coating has a magnetic orientation.
[0073] In Example 1, the modified conductive agent in the functional coating as well as each modified multi-walled carbon nanotube axis, is arranged inclined with a specific angle of 15 to 45° relative to the surface of the aluminum foil in the thickness direction, and interlaced with matrix materials such as adhesives, thereby forming a reinforced three-dimensional network structure for attachment, conduction and heat dissipation.
[0074] The magnetic modified conductive agent used in this invention forms a parallel distributed network, allowing charge carriers to move along the network direction of the modified conductive agent. This increases the propagation speed of the charge carriers and prevents the recombination of the charge carriers during their transmission, thereby providing good directional conduction performance, thus quickly conducting the charge carriers to the metal foil.
[0075] In this example 1, the preparation of the modified conductive agent comprises the following steps:
[0076] (1) Oxidation of carbon nanotubes: 2g of multi-walled carbon nanotubes and a mixture of 200 mL of concentrated sulfuric acid and concentrated nitric acid [V (concentrated HNO3): V (concentrated H2SO4) = 1:3] are placed in a 500 mL Erlenmeyer flask. The whole is then treated with ultrasound for 2 hours to dispersecarbon nanotubes in the acid solution. The resulting mixture is placed on a temperature-controlled magnetic stirrer and stirred at 55°C for 6 hours to oxidize the carbon nanotubes and cut them into short tubes of 150 to 400 nm (in this example, the specific length is 150 to 300 nm). Then, the mixture is diluted with deionized water and vacuum filtered using a 0.22 µm filter membrane. Washing and filtration with deionized water is repeated until the pH of the filtrate is close to 7. The black substance on the filter membrane is then collected and dried in a vacuum box at 60°C for 24 hours. It is then crushed and sieved through a 200-mesh sieve to obtain short, oxidized, and purified carbon nanotubes.During the oxidation process, cavities form in the internal lattice of short carbon nanotubes, giving them a local magnetic moment and weak magnetization to short multi-walled carbon nanotubes.
[0077] (2) Amination of carbon nanotubes: 1g of oxidized carbon nanotubes and 6g of 1,6-hexamethylenediamine was weighed into 30 mL of acetone and then treated with ultrasound for 1 hour. 0.4g of condensing agent DCC (dicyclohexylcarbodiimide) was then added to mix everything and heated under reflux at 70°C for 32 hours. Anhydrous ethanol was added to ultrasonically remove excess 1,3-hexamethylenediamine, DCC and reaction by-products. Vacuum filtration was then performed using a 0.22 µm filter membrane and a membrane filter. After several washes with anhydrous ethanol, the black substance on the filter membrane was collected and then dried in a vacuum box at 65°C for 24 hours. It was then ground and sieved through a 200-mesh sieve to obtain amine-modified magnetic carbon nanotubes.
[0078] (3) Dumbbell-shaped structuring: 0.5 g of magnetic carbon nanotubes modified with amine groups 0.7 g of nanoscale conductive carbon black is weighed, added into 30 mL of acetone and then dispersed by ultrasound for 1 hour. The condensation agent DCC is added to heat under reflux at 70°C for 24 hours. Anhydrous ethanol is used to ultrasonically remove DCC and reaction by-products. Vacuum filtration using a 0.45 µm filter membrane and a membrane filter is carried out before washing several times with anhydrous ethanol to collect the black substance on the filter membrane. The latter is then dried in a vacuum box at 65°C for 24 hours and then ground and sieved through a 200 mesh sieve to obtain the modified conductive agent in the shape of a dumbbell, with thick ends and a thin center.
[0079] In Example 1 of this invention, the multi-walled carbon nanotubes used have an inner diameter of at least 5 nm and an outer diameter not exceeding 20 nm, as well as a length before cutting not exceeding 1200 nm.
[0080] In this example, the oxidation step uses the oxidizing effect of a mixture of acids. Due to their large length-to-diameter ratio, this oxidation causes the unstable five- and seven-atom carbon rings located at the helical twist points of the carbon nanotubes to break. This cuts the nanotubes to form short nanotubes with open ends. Continued oxidation of the carbon atoms at the ends forms carboxyl groups, thus providing numerous contact sites for grafting reactions. In addition, the shortened carbon nanotubes have cavities created by the oxidation of the local CC bonds, giving the carbon nanotubes a weak magnetization due to the magnetic moments around them.The cavities or curvatures on the structure of carbon nanoparticles, amorphous carbon, and graphite fragments make impurities highly reactive and selectively remove them by oxidation with concentrated acid.
[0081] In this example of the invention, the diamine compound may be selected from 1,6-hexamethylenediamine, 1,4-butylenediamine, paraphenylenediamine, or other similar diamine compounds. Its main function is to react via its amine groups with the carboxyl groups at the ends of the single-layer carbon nanotubes to form amide bonds, with the other amine group remaining exposed, thus completing the amine modification of the carbon nanotubes. The grafted diamines separate adjacent carbon nanotubes and increase the spacing between them. In addition, the presence of the steric hindrance of the diamines reduces the hydrogen bonds formed between the multi-walled carbon nanotubes during the oxidation process, which improves the dispersion of the carbon nanotubes after amination. This facilitates the subsequent grafting of conductive nanoparticles containing many carboxyl groups.Specifically in Example 1, 1,6-hexanediamine is used.
[0082] In this example of the invention, the condensing agent may be selected from dicyclohexylcarbodiimide (DCC), diisopropylcarbodiimide (DIC) or EDC (1-(3-dimethylaminopropyl)-3-ethylcarbodiimide). Its function is to serve as a dehydrating agent to promote the reaction between the amine and carboxyl groups, thereby forming an amide bond. In Example 1, dicyclohexylcarbodiimide (DCC) is used.
[0083] The inert solvent in this example of the invention may be chosen from acetone, xylene, etc. In Example 1, acetone is used.
[0084] The particles of the nanoscale conductive agent may be made of carbon black, with a particle diameter ranging from 20 to 250 nm. The surface of these particles contains numerous carboxyl groups capable of reacting with the amine groups of the modified carbon nanotubes to form amide bonds. In Example 1, nanoscale conductive carbon black with an average diameter of 120 nm is used.
[0085] The conductive paste in the preparation method for the high-performance current collector for lithium-ion batteries mentioned above is an aqueous dispersion composed of a modified conductive agent, a nano-sized conductive agent, modified nanofibers, a dispersant, a binder, and a solvent. The solid content of this paste is 0.1 to 10%, its viscosity is 200 to 1000 mPa-s (at 25°C), and its pH is 8 to 10. Technicians in the field can adjust these parameters according to specific needs. In Example 1, the solid content of the paste is 8.5%, the viscosity is 500 mPa-s (at 25°C), and the pH is 9.
[0086] The functional coating, after application and before drying, has a thickness of about 800 to 1200 nm, providing sufficient space for unwinding, stretching and directional alignment of the modified conductive agents. By controlling the viscosity within a specific range, the unwinding, stretching and directional alignment of the modified conductive agents under the effect of a magnetic field is facilitated, while preventing them from sliding and floating to the surface. With the evaporation of the volatile components of the paste, the modified conductive agents are captured in the grid structure of the matrix and intertwine with it to form a three-dimensional network structure.
[0087] In example 1, the weight composition of the different components of the conductive paste is as follows: modified multi-walled carbon nanotubes: nanometric conductive agent: modified nanofibers: dispersant: binder: solvent = 0.3: 0.05: 5: 20: 17: 57.65.
[0088] In this example of the invention, the modified nanofibers may be cellulose or chitin nanofibers (ChNF) modified by carboxylation, sulfonation, phosphorylation, or ammonium quaternization. These nanofibers are dispersed in a deionized aqueous medium with a solids content of 0.1 to 3.0 wt.%. The modified nanofibers are suitable for aqueous media and provide a porous three-dimensional cross-linked structure. The negatively charged groups present on the fibers induce electrostatic repulsion forces between the fibers, forming a stable colloid that allows the magnetic modified conductive agents to remain stable in their developed pores, aiding in dispersion. In the functional coating, these nanofibers intertwine with the carbon nanotubes to form a three-dimensional network structure, thereby improving the overall performance of the current collector.In Example 1, carboxylated cellulose nanofibers are used.
[0089] In this invention, the dispersant may be selected from polyvinylpyrrolidone (PVP), polyvinyl alcohol (PVA) or poly(N-vinylacetamide) (PNVA), alone or mixed with a binder resin. The amount of dispersant used (whether single-component or multi-component) is typically 20 to 1000 times the weight of the dry powdered carbon nanotube. This dispersant is suitable for aqueous media and its main function is to ensure uniform dispersion of the modified conductive agent in the conductive paste system. In Example 1, polyvinylpyrrolidone (PVP) is used.
[0090] In this example of the invention, the binder may be a resin resistant to the electrolyte of lithium-ion batteries and to high voltages. This resin may be polyacrylate (PAA) with a wide molecular weight distribution and its salts, a modified acrylic resin, or a modified polyacrylonitrile (PAN) resin. It is dispersed in a deionized aqueous medium with a solids content of 5 to 30% by weight. This binder is suitable for aqueous media and its main function is to ensure the adhesion of the conductive paste between the current collector and the materials of the positive / negative electrodes, while improving the fixing capacity between them. In Example 1, polyacrylate (PAA) is used.
[0091] In Example 1 of the invention, the solvent used is deionized water.
[0092] The method of preparing the conductive paste for the high-performance current collector of lithium-ion batteries is characterized by the following steps:
[0093] (1) Preparation of materials: Modified multi-walled carbon nanotubes, The nanoscale conductive agent, modified cellulose nanofibers, dispersant, binder and solvent are prepared in the following proportions: 0.3:0.05:5:20:17:57.65.
[0094] (2) Preparation of the suspension of the modified conductive agent at high concentration: The modified nanofibers and the dispersant are weighed and then added at 1 / 3 of the amount of the solvent and then mixed until completely dissolved. The modified conductive agents are then added to this solution and the whole is treated with ultrasound for 30 minutes to obtain a suspension of modified multi-walled carbon nanotubes at high concentration.
[0095] (3) Magnetic loading: The suspension of the modified conductive agent is placed in a strong external magnetic field to induce magnetic moments in the defects of the carbon nanotubes, thereby enhancing the magnetic anisotropy of the conducting agent. This results in a suspension of high-concentration modified magnetic multi-walled carbon nanotubes.
[0096] (4) Initial dispersion: The binder is added into the suspension of the conductive agent modified to high concentration and then supplemented with the solvent to the required amount. First, a high-speed vacuum disperser and then a ball mill is used for initial dispersion. During vacuum dispersion, the shear rate should be 10-25 m / s, the vacuum should not be less than 0.085 MPa and The dispersion time should be 1-5 hours. In the mill, the diameter of the balls should be 0.2-2 mm, representing 30-90% of the volume, with a rotation speed of 600-10000 rpm and a grinding time of 0.1-5 hours.
[0097] (5) Secondary dispersion: Using an ultrasonic treatment device, a Ultrasonic resonance dispersion is performed while applying an alternating magnetic field on both sides. This allows the magnetic modified conductive agents to be uniformly dispersed and aligned in the direction induced by the magnetic field. The ultrasonic frequency should be 20-40 kHz with a power of 1-3 kW per unit, and the magnetic field strength should be 0.1-5 T with a frequency of 40-60 Hz.
[0098] During steps (4) and (5) of the dispersion process, it is also necessary to maintain the pH of the conductive paste between 8 and 11 with ammonia, in order to guarantee the stability of the paste.
[0099] In Example 1 of the invention, the components and preparation steps of the conductive paste are as follows: 20g of 10% polyvinylpyrrolidone (PVP K30) solution and 5g of 1% carboxylated cellulose nanofiber solution are added to 13g of deionized water and then mixed thoroughly. Then, 0.3g of modified multi-walled carbon nanotubes and 0.05g of conductive nanomaterials are added to the mixture and subjected to ultrasonic treatment for 30 minutes to obtain a suspension of modified magnetic conductive material. This suspension is then placed in a strong external magnetic field to magnetize the material. Then, 17g of PAA (polyacrylic acid) and 44.65g of deionized water are added to the magnetized modified conductive magnetic suspension, and pre-dispersed for 30 minutes using a high-speed mixer (first at low speed, then accelerated).After uniform basic mixing, the dispersion is continued under vacuum at 2400 RPM for 120 minutes (with a pressure below 0.08 MPa), followed by a grinding step. Grinding is carried out at 3000 rpm for 10 minutes. The thus treated paste is then subjected to further ultrasonic dispersion, with the application of an alternating magnetic field on the sides, to obtain an oriented aqueous conductive paste. By adjusting the amounts of modified magnetic conductive material, modified cellulose nanofibers, dispersant and binder based on the above formula, it is also possible to produce an aqueous conductive paste with a solid content of 0.1 to 6%.
[0100] The above-mentioned method for preparing the high-performance lithium battery current collector comprises the following steps:
[0101] (1) The metal film of the current collector and the dispersed conductive paste are prepared, and coating equipment, ultrasonic equipment, devices constant magnetic field generation and drying equipment are installed.
[0102] (2) The dispersed conductive paste is applied on the surface of the metal film of the current collector, to form a liquid gel layer with a viscosity of 200-1000 mPa-s (at 25°C) and a thickness of 800-1000 nm. This liquid gel layer has a thickness of approximately 800-1200 nm before drying, to provide sufficient space for the magnetic field-induced directional alignment of the magnetically modified conductive agents, control The viscosity is controlled within a specific range to allow the magnetic field-induced alignment without the modified conductive agents floating on the surface. As the volatile components of the paste evaporate, they are captured in the lattice structure of the matrix and intertwine with it to form a three-dimensional network structure.
[0103] (3) A stable magnetic field perpendicular to the surface of the metal film of the current collector is continuously applied to the liquid gel layer, so that the magnetic modified conductive agents form an oriented network under the effect of the induced magnetic field.
[0104] The specific steps of the magnetic field-induced orientation are as follows: at the first third of the coating production line, a magnetic field oriented at an angle of 45 degrees to the surface of the metal film is applied with an intensity of 200mT to 1000mT, to complete the first orientation of the magnetic modified conductive agents and reorient the magnetic monolayer carbon nanotubes disturbed by the coating. Then, at the second third of the coating production line, a uniform magnetic field oriented at an angle of 45 to 90 degrees to the surface of the metal film is applied with a field intensity of 500mT to 1000mT, to complete the second orientation, so that the modified magnetic conductive agents finally form a specific inclined network of 15 to 45 degrees to the thickness direction.
[0105] (4) The gel layer is dried so that the solvent evaporates completely, while by continuing to apply a constant magnetic field. As the viscosity of the layer increases, the alignment and shape are rapidly maintained until the solid components of the conductive paste are attached to the surface of the metal film, forming a compact functional cover with a thickness not exceeding 800 nm, including a three-dimensional network layer strengthening the attachment as well as the electrical and thermal conduction on the surface of the metal film.
[0106] The above-mentioned step (3) also includes the following steps:
[0107] (31) In the first third of the coating production line, the temperature of The already applied conductive paste or coating layer is heated to 45-65°C for pre-drying, which helps to extend the condensation time, reduce the viscosity of the liquid gel layer, and increase the kinetic energy required for unfolding, alignment, and orientation of the single-layer carbon nanotubes.
[0108] The high-performance current collector for lithium battery prepared according to Example 1 is used in the manufacture of lithium-ion batteries and subjected to performance tests. The electrodes are manufactured according to the following parameters:
[0109] The positive electrode sheet comprises the current collector and a positive active material layer coated on the current collector. The current collector is the high-performance current collector for lithium battery prepared according to the above example. The positive active material layer is composed of the following raw materials: 93 parts of cathode material (LFP), 4 parts of cathode conductive agent (SP), and 3 parts of cathode binder (PVDF-5130).
[0110] The negative electrode foil comprises the current collector and a negative active material layer applied to the current collector. The current collector is a shiny copper foil. The negative active material layer is composed of the following raw materials: 96 parts of anode material (artificial graphite), 1 part of anode conductive agent (SP), 1 part of anode binder 1 (sodium carboxymethylcellulose, CMC), and 2 parts of anode binder 2 (styrene-butadiene rubber, SBR).
[0111] An 18650 battery is assembled using the above-mentioned positive and negative electrode sheets, a 20 pm polypropylene (PP) membrane, and a LiPF6 electrolyte. The performances of the electrodes and the battery are shown in Tables 1 and 2.
[0112] Comparison 1
[0113] In comparison 1, the current collector of the positive electrode is fabricated using a shiny aluminum foil, the other preparation conditions remain the same.
[0114] Using the high-performance current collector for lithium battery prepared according to Example 1, and directly using a bright aluminum foil as the current collector for the positive electrode, an 18650 battery is prepared according to the same formulation and process for the positive and negative electrodes. The performances of the electrodes and batteries are tested, the test results being shown in Tables 1 and 2 below, respectively.
[0115] [Table 1]: Comparative test data of positive electrodes using the high-performance current collector for lithium battery of the invention Electrode Type N. Positive Electrode Resistance (Q) Positive Electrode Peeling Force (N) Positive Electrode Peeling Force after 2000 IC Charge and 2C Discharge Cycles (N) Example 1 1 3.31 17.313 15.413 2 3.35 17.521 15.230 3 3.32 17.446 15.331 Average 3.34 17.427 15.325 Comparison 1 1 11.81 4.516 3.210 2 11.60 4.874 3.455 3 11.47 4.450 3.107 Average 11.63 4.613 3,257
[0116] [Table 2]: Comparative test data applied to the lithium-ion battery for the high-performance current collector in the examples of the present invention. Battery Type N. Internal Battery Resistance (mQ) Battery Capacity after Division (mAh) Battery Capacity after 2000 IC Charge and 2C Discharge Cycles (mAh) Battery Retention Rate after 2000 IC Charge and 2C Discharge Cycles (%) Example 1 1 14.4 1620.2 1505.7 92.9 2 14.6 1618.4 1500.0 92.7 3 14.7 1617.9 1504.1 93.0 Average 14.6 1618.8 1503.3 92.8 Comparison 1 1 25.1 1616.3 1263.9 78.2 2 26.2 1615.5 1316.6 81.5 3 24.8 1615.8 1295.8 80.2 Average 25.4 1615.8 1292.1 80.0
[0117] From the test results, it is easy to conclude that when applied to the manufacture of lithium batteries, the high-performance current collector for lithium batteries provided by this invention exhibits superior performance to that of the pure copper foil current collector used in Comparison 1, and this in all aspects, from the electrode to the battery. The resistance of the electrode prepared according to Example 1 is only one-third that of the pure copper foil current collector in Comparison 1, while its peel strength is more than four times higher. In addition, the internal resistance of the battery measured in Example 1 is reduced by 42% compared to that of the copper foil. At room temperature, after 2000 cycles of charging at IC and discharging at 2C, the retention rate of the lithium-ion battery manufactured according to Example 1 can reach 93%, which is much higher than the 80% retention rate of the pure copper foil current collector in Comparison 1. The cycle consistency of the battery is also significantly better than that of the pure copper foil current collector.
[0118] Example 2
[0119] The present example provides a current collector for a high-performance lithium battery, a conductive paste, and a method for preparing the same. This example is similar to Example 1 except for the following few differences:
[0120] The modified conductive agent for preparing the above-mentioned high-performance current collector is composed of multi-walled carbon nanotubes, modified by oxidation and chemical modification, and then connected to other larger conductive nanomaterial particles to form a dumbbell-shaped island-bridge structure with anchored ends. In this second example, 1,4-butylenediamine is used as the modifying agent and diisopropylcarbodiimide (DIC) is used as the condensing agent.
[0121] The conductive paste for preparing the above-mentioned high-performance lithium battery current collector is an aqueous paste obtained by dispersing and mixing a modified conductive agent, conductive nanomaterials, modified nanofibers, a dispersant, a binder, and a solvent. The solid content of this paste is 4 to 6%, its viscosity is 300 to 1000 mPa-s (25°C), and its pH is 8 to 9.
[0122] In this example 2, the weight ratio of the components of the conductive paste is as follows: modified multi-walled carbon nanotubes: nano conductive agent: modified nanofibers: dispersant: binder: solvent = 0.6: 0.1: 6: 20: 20: 53.3.
[0123] In this example 2, the modified nanofibers are carboxylated chitin nanofibers, the binder is a modified acrylic resin, and the dispersant used is polyvinyl alcohol (PVA).
[0124] In this example 2, when the conductive paste is coated on a copper foil, it makes it possible to manufacture a current collector for a high-performance lithium battery.
[0125] The preparation parameters of the negative electrode for the comparative test of the lithium battery manufactured from the current collector of this example 2 are the following: the negative electrode comprises the current collector and a negative active material layer coated on the current collector. The current collector is the high-performance current collector for lithium battery manufactured in this Example 2. The negative active material layer is composed of the following raw materials in weight parts: 96 parts of negative material (artificial graphite); 1 part of negative conductive agent (SP); 1 part of negative binder 1 (sodium carboxymethylcellulose, CMC); 2 parts of negative binder 2 (styrene-butadiene rubber, SBR). An electronic tensile machine is used to test the peeling force of the electrode, and a dual-probe test method is used to measure the electrode resistance. The obtained electrode performances are shown in Table 3.
[0126] Example 3
[0127] The present example provides a current collector for a high-performance lithium battery, a conductive paste, and a method for preparing the same. This example is similar to Examples 1 and 2 except for the following few differences:
[0128] In this Example 3, to prepare the modified conductive agent of the above-mentioned high-performance current collector, 1,6-hexanediamine is used as the modifying agent and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide (EDCI) is used as the condensing agent.
[0129] The conductive paste of the above-mentioned high-performance current collector for lithium battery is an aqueous paste obtained by dispersing and mixing a modified conductive agent, conductive nanomaterials, modified nanofibers, a dispersant, a binder and a solvent. The solid content of this paste is 3 to 4%, its viscosity is 200 to 800 mPa-s (25°C) and its pH is 9 to 10.
[0130] In this example 3, the weight ratio of the components of the conductive paste is as follows: modified multi-walled carbon nanotubes: nano conductive agent: modified nanofibers: dispersant: binder: solvent = 0.3: 0.1: 4: 12: 14: 69.6.
[0131] In this example 3, the modified nanofibers are carboxylated chitin nanofibers, the binder is modified polyacrylonitrile (PAN), and the dispersant used is poly(N-vinylacetamide) (PNVA).
[0132] When Example 3 is coated on a copper foil, it makes it possible to manufacture a current collector for a high-performance lithium battery.
[0133] The preparation parameters of the negative electrode for the comparative test of the lithium battery manufactured from the current collector of this Example 3 are as follows: the negative electrode comprises the current collector and a negative active material layer coated on the current collector. The current collector is the high-performance current collector for lithium battery manufactured in this Example 2. The negative active material layer is composed of the raw materials following in weight parts: 97 parts of negative material (artificial graphite); 1 part of negative conductive agent (SP); 1 part of negative binder 1 (sodium carboxymethylcellulose, CMC); 1 part of negative binder 2 (styrene-butadiene rubber, SBR). An electronic tensile machine is used to test the peel strength of the electrode, and a dual-probe test method is used to measure the electrode resistance. The electrode performances obtained are shown in Table 3 (comparative test data for the application of the high-performance current collector of the present invention on the negative electrode).
[0134] Comparison 2
[0135] The preparation parameters of the negative electrode for the comparative test of the lithium battery, manufactured according to Example 2, are as follows: the material of the negative electrode (artificial graphite): conductive agent (SP): binder 1 (CMC): binder 2 (SBR) = 96: 1: 1: 2. The only difference lies in the choice of the current collector, which is a smooth copper foil. The performance of the electrode is shown in Table 3.
[0136] Comparison 3
[0137] For Comparison 3, the preparation parameters of the negative electrode are the same as those of Example 3: the material of the negative electrode (artificial graphite): conductive agent (SP): binder 1 (CMC): binder 2 (SBR) = 97: 1: 1: 1. The only difference lies in the choice of the current collector, which is a smooth copper foil. The performances of the electrode are also shown in Table 3.
[0138] [Table 3]: Comparative test data for the application of the high-performance current collector of the present invention on the negative electrode Electrode Type Negative Electrode Resistance (Q) Negative Electrode Peeling Force (N) Example 2 0.13 7.533 Example 3 0.12 5.158 Comparison 2 0.14 4.385 Comparison 3 0.13 3.314
[0139] From the test results, it is easy to conclude that the negative electrodes prepared with the high-performance current collector for lithium battery of the present invention show higher adhesion with the same amount of negative binder, while having lower resistance than the electrodes made with smooth copper foil. This indicates that the high-performance current collector for lithium battery of the present invention can reduce the proportion of binder in the paste of the positive and negative electrodes, which further reduces the internal resistance and promotes the increase of the energy density of the battery.
[0140] In summary, the high-performance current collector for a lithium battery of the present invention uses a magnetic modified conductive agent to form a distributed parallel network in the functional coating. This three-dimensional network interconnected between the modified conductive agent and the flexible substrate provides a high-strength, efficient electrical conduction, and flexible connection layer. It effectively improves the contact area between the rigid metal current collector and the conductive paste, strengthens the adhesion of the coating, reduces the interface resistance between the current collector and the active material of the battery, and uses the interwoven network to dampen volume changes during charge and discharge cycles.This prevents the separation of the conductive paste from the current collector, improves the durability of the adhesion between the metal foil current collector and the battery active material during repeated charge and discharge cycles, thereby increasing the stability of the electrode, avoiding cycle failures, and improving the specific capacity, cycle stability and rate performance of the battery, greatly improving the overall performance of the lithium battery.
[0141] In other embodiments of this invention, the metal foil used as the metal substrate of the current collector may also be copper, iron, or stainless steel. In addition, under the conditions of the proportion of components, process steps, and working conditions described in this invention, an expert in the field can select the specific components, proportions, processes, and conditions required by using conventional techniques to achieve the technical effects described in this invention. The various embodiments of this invention set forth above will not be listed one by one.
[0142] The foregoing is only a preferred example of the present invention and does not constitute a limitation on the scope of protection of this invention. All modifications, equivalent substitutions, improvements, etc., made in the spirit and principles of this invention are to be included within the scope of protection of this invention.
Claims
1. Claims A high-performance current collector for a lithium battery, comprising a metal foil and a functional coating formed by applying a conductive paste to one or both surfaces of the metal foil, forming after drying a functional layered covering structure with a thickness of not more than 800 nm; the functional coating comprises several strip-shaped modified conductive agents which are multi-walled carbon nanotubes modified by magnetic orientation, after curing, these modified conductive agents are parallel to each other in the coating and form an angle of 15 to 45° with the surface of the metal foil, orienting obliquely, they are interwoven with modified nanofibers, a binder and other modified conductive agents to form an oriented three-dimensional network connection structure, strengthening the fixation, electrical and thermal conductivity,and making uniform deformation and automatic return to the initial position possible; The magnetically oriented modified multi-walled carbon nanotubes in the functional coating should have a dumbbell-shaped structure, with an inner diameter of at least 5 nm, an outer diameter of not more than 20 nm, and a length of not more than 1200 nm, after oxidation and chemical modification, they present a fiber structure with wider ends and a narrower center, once aligned, the wider lower ends connect respectively to the surface of the metal foil while the upper ends connect to each other, now binding the other conductive nanoparticles of different sizes and the modified nanofibers to the narrower center of the fiber, which forms a three-dimensional island-bridge structure anchored at both ends and aligned,where the elastic three-dimensional network limits the deformation and displacement of the modified multi-walled carbon nanotubes and conductive nanoparticles during battery operation; this structure automatically adapts and compensates for internal volume variations, as well as deformations and displacements of the conductive nanoparticles during the charge and discharge cycles of the,
2. lithium battery, providing the connection between the functional coating, the surface of the metal foil and the active material. The high-performance lithium battery current collector cited in claim 1 is characterized by the steps of preparing the modified multi-walled carbon nanotube: (1) Oxidation of carbon nanotubes: An appropriate amount of multi-walled carbon nanotubes is placed in a mixture of concentrated sulfuric acid and concentrated nitric acid at a volume ratio of 1:3, and then ultrasonicated for 2 hours to evenly disperse the multi-walled carbon nanotubes in the acid solution, thereby obtaining a dispersed solution; This dispersed solution is then placed in a thermostatic magnetic stirrer and stirred at 55°C for 6 hours to oxidize the carbon nanotubes and cut them into short tubes of 150-400 nm; Then, it is diluted with deionized water, vacuum filtered using a 0.22 pm filter membrane and a membrane filter, and then washed repeatedly with deionized water until the pH of the filtrate is close to 7;the black solid on the filter membrane is then dried in a vacuum drying box at 60°C for 24 hours, then crushed and sieved through a 100-mesh sieve, to finally obtain oxidized, cut and purified multi-walled carbon nanotubes; (2) Amination of carbon nanotubes: the oxidized multi-walled carbon nanotubes and an excess of diamine compound are placed in an inert solvent, to be ultrasonicated for 1 hour, then mixed with a dicyclohexylcarbodiimide (DCC) condensation reagent, the whole is then heated under reflux at 70°C for 32 hours; The excess amine, DCC and reaction by-products are washed ultrasonically with anhydrous ethanol, the whole is then vacuum filtered with a 0.22 μm filter membrane and a membrane filter, and then washed repeatedly with anhydrous ethanol; The black substance on the filter membrane is dried in a vacuum drying box at 65°C for 24 hours, then crushed and sieved through a 200-mesh sieve, to finally obtain amine-modified magnetic multi-walled carbon nanotubes; (3) Dumbbell-shaped structuring: Magnetic multi-walled carbon nanotubes modified with amine groups and particles of conductive nanomaterial are added into an inert solvent, dispersed by ultrasound for 1 hour, and then heated under reflux at 70°C for 24 hours with the condensation reagent; The excess condensation reagent and reaction by-products are then washed by ultrasound with anhydrous ethanol, the whole is then vacuum filtered with a 0.45 μm filter membrane and a membrane filter, and then washed repeatedly with anhydrous ethanol, The black substance on the filter membrane is dried in a vacuum drying box at 65°C for 24 hours, crushed and sieved through a 200-mesh sieve, to finally obtain modified multi-walled carbon nanotubes with a dumbbell structure, with thick ends and a thin center.
3. The high-performance lithium battery current collector recited in claim 2 is characterized by the step of oxidizing carbon nanotubes (1) or the oxidizing action of the acid mixture to break the unstable pentagonal and heptagonal carbon rings located at the helical twist points of the carbon nanotubes due to their large length-to-diameter ratio, and cut them to form short carbon nanotubes with open ends, thereby making the treated carbon nanotubes shorter with open ends; This causes the carbon atoms at the ends to be oxidized, thereby forming carboxyl groups, which provides many contact sites for grafting reactions at the ends;At the same time, the shortened carbon nanotubes have vacant points created by the local opening of the CC bonds, the presence of these vacancies induces magnetic moments nearby, thus giving the carbon nanotubes a weak magnetism.;
4. The high-performance lithium battery current collector recited in claim 2 is characterized by the dumbbell-shaped structuring step (3) or the nanoparticles of the conductor are carbon black with a diameter of 20 to 250 nm, covered with a large amount of carboxyl groups on their surface reacting with carbon nanotubes modified with amine groups to form amide bonds, stably connecting, thereby forming thicker anchoring parts at both ends of the modified multi-walled carbon nanotubes.
5. The high-performance lithium battery current collector recited in claim 2 is characterized in that 1,6-hexanediamine, 1,4-butylenediamine, or p-phenylenediamine is used as the diamine compound in step (2), reacting by the amine groups they contain with the carboxyl groups at the ends of the carbon nanotubes to form amide bonds, with the other exposed amine group, thereby completing the amine modification of the carbon nanotubes; The grafted diamine pushes adjacent carbon nanotubes apart, thereby increasing the spacing between the nanotubes, while the presence of the steric hindrance of the diamine weakens the hydrogen bonds formed between the multi-walled carbon nanotubes during the oxidation process, improving the dispersibility of the aminated carbon nanotubes, which promotes the subsequent grafting of the conductive nanoparticles containing a large amount of carboxyl groups;Dicyclohexylcarbodiimide (DCC) is used as a condensing agent in step (2), and acts as a dehydrating agent to accelerate the reaction between amine and carboxyl groups forming amide bonds as well as to stabilize the bond; Acetone or xylene is used as an inert solvent in step (3);
6. A conductive paste for the high-performance lithium battery current collector according to any one of claims 1 to 5 characterized in that it is an aqueous dispersion prepared from modified multi-walled carbon nanotubes, conductive nanoparticles, modified nanofibers, a dispersant, a binder and a solvent, with a solid content of 0.1 to 10%, a viscosity of 200 to 1000 mPa-s, and a pH of 8 to 11; The weight proportions of the components of this conductive paste are respectively as follows: modified multi-walled carbon nanotubes: conductive nanoparticles: modified nanofibers: dispersant: binder: solvent = (0.01-1.8): (0.01-0.2): (0.02-2): (0.02-20): (0.05-20): (56-99.89).
7. The conductive paste for the high-performance lithium battery current collector recited in claim 6 is characterized in that the modified nanofibers are cellulose or chitin nanofibers (ChNF) modified by carboxylation, sulfonation, phosphating or quaternization, dispersed in a
8. deionized aqueous medium, with a solids content of 0.1 to 3.0 wt%; These modified nanofibers are suitable for aqueous media, providing a three-dimensional porous network structure, and the negatively charged groups induce electrostatic repulsion between the fibers, forming a stable colloid, thus allowing the modified conductive agents to remain confined in their developed pores; in the functional coating, they intertwine with the modified conductive agents to form a three-dimensional network structure, improving the overall performance of the current collector; Polyvinylpyrrolidone (PVP), polyvinyl alcohol (PVA), or poly-N-vinylacetamide (PNVA) are used as dispersant in an amount of 20 to 1000 times the weight of the modified conductor in dry powder form, this dispersant, suitable for aqueous media, allows uniform dispersion of the modified conductive agents in the conductive paste; Resin resistant to lithium-ion battery electrolytes and high voltages (such as polyacrylate (PAA) or its salt with a wide molecular weight distribution, a modified acrylic resin, a modified polyacrylonitrile (PAN) resin, or a mixture of these resins) is used as a binder; dispersed in a deionized aqueous medium with a solid content of 5 to 30% by weight, this binder is suitable for aqueous media, allowing the conductive paste to adhere between the current collector and the positive / negative electrode material, improving their attachment capacity; Deionized water is used as a solvent. The method for preparing the conductive paste for high-performance lithium battery current collector cited in claims 6 or 7 is characterized by the following steps: E1: Preparation of materials: The modified multi-walled carbon nanotubes, conductive nanoparticles, modified nanofibers, dispersant, binder, and solvent are prepared in the indicated proportions; E2: Preparation of high concentration modified conductor suspension: The modified nanofibers and dispersant are weighed according to the proportions, then added to 1 / 3 of the solvent and dissolved completely by mechanical stirring, the required modified conductor is then weighed and then added to the mixed solution to be ultrasonicated for 30 minutes to obtain a modified conductor suspension (specifically a high-concentration modified multi-walled carbon nanotube suspension); E3: Magnetic loading: The modified conductor suspension is placed in a strong external magnetic field to activate magnetic loading to further stimulate the magnetic anisotropy of the modified multi-walled carbon nanotubes, thereby obtaining a high-concentration magnetic modified multi-walled carbon nanotube suspension; E4: Initial dispersion: The binder is added in the corresponding proportion to the high-concentration magnetic modified multi-walled carbon nanotube suspension, and then the solvent is added back to the required amount; preliminary dispersion is carried out by first using a high-speed vacuum disperser and then a ball mill;The shear speed of the vacuum disperser should be 10-25 m / s, with a vacuum pressure of at least 0.085 MPa, and a dispersion time of 1-5 hours while in the ball mill, the diameter of the balls should be 0.2-2 mm, with a proportion of 30-90%, a rotation speed of 600-10000 rpm, and a grinding time of 0.1-5 hoursm; E5: Secondary dispersion: Secondary dispersion is carried out by using ultrasonic processing equipment for ultrasonic resonance; an alternating magnetic field on both sides is applied to make the modified multi-walled carbon nanotubes and conductive nanoparticles disperse uniformly and align in the same direction under the induction of the magnetic field, thus obtaining a conductive paste with magnetic orientation.;
9. The method of claim 8 has the following characteristics: In steps E2 and E5, the ultrasonic treatment equipment is an ultrasonic generator immersed in the liquid with an ultrasonic frequency of each power unit of 20 kHz to 40 kHz and a power of 1 kW to 3 kW; In steps E3 and E5, the intensity of the alternating magnetic field is 0.1 to 5 T, with a frequency of 40 to 60 Hz.
10. The method for manufacturing the high-performance current collector for lithium battery recited in claims 1 to 5 is characterized by the following steps: (A1) A current collector metal foil, a dispersed conductive paste are prepared and coating equipment, ultrasonic equipment, constant magnetic field generating equipment, and drying equipment are set up; (A2) The already dispersed conductive paste is applied to the surface of the metal foil to form on this surface a liquid colloidal layer with a viscosity of 200-1000 mPa-s at 25°C and a thickness of 500-1200 nm; (A3) A constant magnetic field is applied perpendicular to the surface of the metal foil on the liquid colloidal layer, so that the oriented modified conductive agent aligns orderly under the induction of the applied magnetic field, and gradually unfolds, forming a parallel network, intertwined with the matrix; (A4) By continuing to apply the magnetic field, the layer dries, the solvent and volatile components evaporate, the modified conductive agent maintains its alignment and posture while the viscosity of the layer increases and quickly fixes, aligning parallel in the thickness direction with an inclination of 15-45° until the solidified components of the conductive paste fix on the surface of the metal foil, forming a dense functional coating with a thickness of not more than 800 nm, thereby creating on the surface of the metal foil a three-dimensional network structure with enhanced fixation, electrical and thermal conductivity and being able to shrink easily.
11. The method recited in claim 10 also comprises the following step (A3): (A3-1) The temperature of the conductive paste or the layer after coating is raised to 45-65°C for pre-drying, which allows to prolong the coagulation time and thus reduce the viscosity of this liquid colloidal layer, increasing the kinetic energy allowing the modified conductive agent to unfold,
12. straighten and align in an oriented manner; ultrasound can also be applied to this liquid colloidal layer, to further increase the kinetic energy for the modified conductive agent to unwind, straighten and align in an oriented manner, thereby accelerating the parallel network arrangement of the modified conductive agent and increasing the density of the three-dimensional connection structure formed between the modified conductive agent and the matrix, thereby forming on the surface of the metal foil a three-dimensional network structure with enhanced attachment, electrical and thermal conductivity, limited deformation and capable of self-shrinkage. A high-performance current collector for a lithium battery, comprising a metal foil and a functional coating formed by applying a conductive paste to one or both surfaces of the metal foil, forming after drying a functional layered covering structure with a thickness of not more than 800 nm;the functional coating comprises several strip-shaped modified conductive agents which are multi-walled carbon nanotubes modified by magnetic orientation, after curing, these modified conductive agents are parallel to each other in the coating and form an angle of 15-45° with the surface of the metal foil, orienting obliquely, they are interwoven with modified nanofibers, a binder and other modified conductive agents to form an oriented three-dimensional network connection structure, strengthening the fixation, electrical and thermal conductivity, and making uniform deformation and automatic return to the initial position possible;The magnetically oriented modified multi-walled carbon nanotubes in the functional coating should have a dumbbell-shaped structure, with an inner diameter of at least 5 nm, an outer diameter of not more than 20 nm, and a length of not more than 1200 nm, after oxidation and chemical modification, they present a fiber structure with wider ends and a narrower center, once aligned, the wider lower ends connect respectively to the surface of the metal foil while the upper ends connect to each other, now binding the other oxidized graphites of different sizes and the modified nanofibers to the narrower center; of the fiber, which forms a three-dimensional island-bridge structure anchored at both ends and aligned, where the elastic three-dimensional network limits the deformation and displacement of the modified multi-walled carbon nanotubes and conductive nanoparticles during battery operation; this structure automatically adapts and compensates for internal volume variations, as well as deformations and displacements of the conductive nanoparticles during the charge and discharge cycles of the lithium battery, ensuring the connection between the functional coating, the surface of the metal foil and the active material.