Dry mortar composition, particularly adhesive mortar

The use of high-content air-entraining agents in a dry mortar composition improves CO2 diffusion and yield, addressing environmental and logistical issues in adhesive mortars by enhancing recarbonation and reducing packaging volume.

FR3148792A1Active Publication Date: 2024-11-22VICAT PROD IND VPI

Patent Information

Application Number
FR2023004814
Authority / Receiving Office
FR · FR
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-15
Publication Date
2024-11-22
Estimated Expiration
2043-05-15

AI Technical Summary

Technical Problem

Conventional adhesive mortars have low porosity, limiting CO2 diffusion and recarbonation, and lightweight mortars with lower paste densities struggle with slow CO2 diffusion and increased packaging volume, impacting environmental footprint and industrial efficiency.

Method used

A dry mortar composition with a higher content of air-entraining agents, between 0.1% and 2%, to reduce paste density without fillers, enhancing CO2 diffusion and yield, while maintaining a manageable volume.

Benefits of technology

The solution facilitates a 40% improvement in recarbonation depth and a 100% increase in bonding surface area per mass, reducing carbon footprint and logistical challenges.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Dry mortar composition, in particular adhesive mortar. The invention relates to a dry mortar composition, preferably adhesive mortar, having an uncompacted density between 900 g / L and 1400 g / L and comprising at least one air-entraining agent at a mass content between 0.1% and 2%. The invention also relates to a wet mortar obtained from mixing this dry mortar composition, as well as a method for fixing tiles to a substrate using this dry mortar composition.
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Dry mortar composition, in particular adhesive mortar

[0001] The present invention relates to a dry mortar composition, in particular adhesive mortar.

[0002] A dry mortar composition is a composition ready to be mixed with water. It is a powdery mixture which contains one or more hydraulic binders, aggregates and possible additives. After mixing with water (i.e. mixing), a paste is obtained, in other words "a wet mortar", which can be applied to a support (for example a floor or a wall) or between assembly elements. After drying, the mortar is hardened and thus fixes the materials together. It can also adhere to a support and form a surface layer on a wall or a floor.

[0003] This is why mortar is used in many construction, renovation, or landscaping projects as a bonding element, a sealant, or as a coating. Depending on the nature of the construction work, its function is: - to assemble and bind together different construction materials (for example bricks, masonry blocks, concrete blocks, agglomerates); - to make lightweight screeds, coat, glue, joint, repair and seal various construction elements such as copings, tiles or natural or reconstituted stones.

[0004] Among the mortars is the adhesive mortar which is an adhesive for tiles. The wet adhesive mortar is placed on a substrate (for example a concrete slab) in order to ensure the fixing of the tiles on it.

[0005] For the purposes of the disclosure of the present invention, the terms detailed below are defined as follows: - a “dry mortar composition” corresponds to mortar in powder form (or in other words in powder form); - the “unpacked density” corresponds to the “apparent density” of the dry mortar composition. It is also called “bulk density”. The unpacked density can be measured according to the certification standard: Technical document 11-04 “Mortars and related products: Thin-joint mounting mortars for small masonry elements” of March 14, 2022, revision no. 2, from the Scientific and Technical Center for Construction (hereinafter abbreviated as “CSTB”); - a “wet mortar” corresponds to the product obtained after mixing a dry mortar composition with water. It comes in the form of a paste; - the “paste density” corresponds to the density of a wet mortar obtained by mixing a dry mortar composition. The paste density can be measured according to standard NF EN 1015-6.

[0006] The present invention is explained below with particular reference to adhesive mortars without this limiting its scope.

[0007] Improving the environmental performance of buildings is a crucial issue in achieving carbon neutrality objectives. From the construction phase to the destruction or deconstruction of the building, the objective is to choose materials that reduce the environmental impact of buildings.

[0008] As explained above, the mortar, in particular the adhesive mortar, comprises one or more hydraulic binders which may include Portland cement.

[0009] However, the manufacture of Portland cement results in greenhouse gas emissions, mainly CO2, according to the following two mechanisms: - Portland cement is composed of a mixture of limestone and clay. Clinkering requires heating to a temperature of 1450°C: the limestone then transforms into quicklime and CO2. The decarbonation of limestone thus produces CO2 emissions; - the use of fuels to achieve these high clinkerization temperatures also generates CO2 emissions. In this regard, cement manufacturers are seeking to limit fossil fuels and are developing the use of waste or biomass.

[0010] Cement-based mortars, in particular adhesive mortars, are then mixed with water and hardening is linked to dissolution-crystallization phenomena with the formation of different mineral phases such as hydrated calcium silicates, ettringite or portlandite.

[0011] These different phases have a recarbonation capacity. This means that when they come into contact with CO2 in the air, these phases change and capture this CO2 in a sustainable manner. This natural recarbonation phenomenon occurs throughout the material's lifetime and therefore constitutes a first means of reducing the carbon footprint linked to the manufacturing process and use of cement-based materials.

[0012] However, the natural recarbonation of an adhesive mortar is strongly limited by a low gas permeability of said adhesive mortar due to its low porosity which hinders the diffusion of gases. However, the adhesive mortars currently on the market, hereinafter referred to as "conventional adhesive mortars", are not optimized in terms of paste density, as well as porosity to facilitate the diffusion of CO2 through the adhesive mortar for better propagation of recarbonation under the tiles.

[0013] To facilitate the diffusion of CO2 through the adhesive mortar, one solution could therefore consist of lowering the paste density of conventional adhesive mortars, which is currently between 1,500 g / L and 1,700 g / L. Such adhesive mortars, hereinafter referred to as "lightweight adhesive mortars", already exist because they have lower paste densities, generally between 1,100 g / L and 1,300 g / L. However, this solution is not satisfactory because the lowering of the paste density is achieved by adding light fillers or otherwise referred to as "low-density fillers". In the context of the present invention, "low-density fillers" means fillers whose apparent density is at most 600 kg / m3. For example, these can be closed and hollow particles such as expanded glass particles. However, it turns out that these light fillers slow down the diffusion of CO2 through these lightweight adhesive mortars.

[0014] Furthermore, in addition to increasing the recarbonation of the adhesive mortar, another area of ​​improvement to reduce its carbon footprint and its environmental impact could be based on increasing its yield.

[0015] For the purposes of the disclosure of the present invention, the term "mortar yield" means the mass of dry mortar composition that is necessary for said mortar to be applied satisfactorily to 1 m2 of support. Thus, in the case of adhesive mortar, the yield of the adhesive mortar is the mass of dry mortar composition that is necessary to satisfactorily fix 1 m2 of tiles to a support.

[0016] Improving the yield of the adhesive mortar thus involves less packaging, transport, use of critical raw materials such as silica sand per m2 of adhesive mortar applied.

[0017] Now, to return to the lightweight adhesive mortars presented above, the latter, thanks to their low paste densities, certainly have a better yield than conventional adhesive mortars for the same mass of dry composition. But due to the presence of light fillers in their dry composition, their volume (namely their volume of powders) for the same mass is much greater than that of a conventional adhesive mortar. The bags of lightweight adhesive mortars should therefore be almost twice as large as those of conventional adhesive mortars; which is not possible for reasons of ergonomics and handling for the operator or for transport. This is why lightweight adhesive mortars are mainly sold in 15 kg bags with a yield per bag ultimately close to that of a conventional adhesive mortar sold in 25 kg bags.

[0018] The inventors of the present invention have sought to overcome all these drawbacks detailed above with regard to so-called “conventional” and “lightweight” adhesive mortars, by developing a new dry mortar composition, in particular dry mortar glue, for which the carbon footprint of said mortar and its impact on the environment are reduced thanks to the following two areas of improvement: - the diffusion of CO2 through the mortar is facilitated for better propagation of recarbonation (and therefore in particular the diffusion of CO2 through the adhesive mortar under the tiles); - the yield of the mortar is increased without increasing the volume of powder required (in other words the volume of the dry mortar composition); which allows for better industrial and logistical efficiency.

[0019] The invention thus has as its first subject a dry mortar composition, preferably adhesive mortar, the unpacked density of which is between 900 g / L and 1,400 g / L, preferably between 1,000 g / L and 1,300 g / L and which is characterized in that it comprises at least one air-entraining agent at a mass content expressed relative to the total mass of said dry mortar composition of between 0.1% and 2%, preferably between 0.2% and 0.9%.

[0020] In the context of the disclosure of the present invention, the term "air-entraining agent" means an agent which is designed to reduce the surface tension of the water during the preparation of the wet mortar (i.e. during mixing). More precisely, during mixing, the air-entraining agent will position itself at the water-air interface. This thus improves the dispersion of the dry mortar composition in the water, as well as the stability of the wet mortar paste obtained at the end of mixing. During mixing, fine air bubbles are entrained. The air-entraining agent improves the workability of the mortar by lightening the wet mortar paste and making it perfectly stable. Indeed, thanks to the air-entraining agent, the air injected into the wet mortar during mixing remains "trapped" in said wet mortar and makes it possible to develop a network of porosity during the hardening of the material (i.e. the mortar).

[0021] In the field of construction, it is already known to use air-entraining agents in implementation products, such as facade coatings where they make it possible to control the homogeneity of the porosity of the mortar, which improves their resistance to frost cycles. In addition, particularly for repair mortars, air-entraining agents soften the mortar and facilitate its mixing and application to the support. However, for these different applications for facade or repair coating mortars, the mass content of air-entraining agent must be limited so as not to degrade the mechanical strength of the mortar. In this respect, it is generally recommended that this mass content should not exceed 0.05% (this mass content being expressed relative to the total mass of the dry mortar composition). In addition, it is known that an excess of air-entraining agent generally causes instability of the entrained air.

[0022] As regards adhesive mortars, their dry compositions do not contain generally not such air-entraining agents, as they instead include thickening agents and redispersible polymers which also entrain a certain amount of air during the mixing of the adhesive mortar and which are sufficient to improve the workability of the adhesive mortar.

[0023] The originality of the present invention therefore lies in the presence of at least one air-entraining agent in the dry mortar composition at a much higher mass content (namely 10 to 20 times higher) than that generally used in dry mortar compositions known from the state of the art.

[0024] The presence of the air-entraining agent in a very large quantity in the dry mortar composition according to the invention makes it possible to significantly lower the density of the paste compared with that of the conventional adhesive mortars mentioned above. This gives the mortar according to the invention the following advantages: - the incorporation of a much greater quantity of air into the wet mortar paste and the improvement of the distribution of air bubbles in said paste during mixing; - the increase in the porosity of the hardened mortar which facilitates the diffusion of CO2 through the mortar under the tiles and, consequently, improves the quantity of CO2 captured during the life of the mortar; which contributes to the reduction of its carbon footprint; - because the unpacked density of the dry mortar composition is close to that of a conventional adhesive mortar, this allows for the same volume of powders (in other words the same volume of dry mortar composition) and the same mass of bag as that of a conventional adhesive mortar (namely 25 kg) to treat a larger bonding surface. The yield of the mortar according to the invention is therefore improved and makes it possible to reduce the industrial impacts, linked to transport and those of materials linked to packaging in its environmental balance.

[0025] It is important to emphasize that the dry mortar composition according to the invention has been developed to entrain a significant amount of air during mixing in order to lower the paste density without having to add lightweight fillers. This air entrainment is completely controlled in order to: - to obtain a homogeneous distribution of air bubbles in the wet mortar paste during mixing and that the wet mortar remains stable (i.e. that the air entrained during mixing does not escape, or at least to a lesser extent, from the wet mortar paste); - to avoid any instability of the entrained air which, as explained above, can occur in the event of excess air-entraining agent.

[0026] During experiments on a dry adhesive mortar composition according to the invention, the inventors were able to observe the following remarkable advantages: - an improvement in the recarbonation depth of 40% over the lifetime of said mortar; which helps to increase recarbonation per m2 by 100% compared to a conventional adhesive mortar of the same classification; - an increase of at least 75% of the m2 bonded with the adhesive mortar according to the invention, for the same mass and the same size of bag compared to a conventional adhesive mortar; which implies a reduction in the difficulty on site for the same applied surface of adhesive mortar (namely fewer bags, therefore less load-bearing, a very light consistency of the adhesive mortar therefore ease of application and mixing).

[0027] The various constituents of the dry mortar composition according to the invention are now described in more detail.

[0028] The dry mortar composition according to the invention comprises at least one air-entraining agent. As explained above, these air-entraining agents are known to those skilled in the art in the field of construction. The air-entraining agent is an agent designed to reduce the surface tension of water during the preparation of the wet mortar by positioning itself at the water-air interface. This is why the air-entraining agent can be chosen from anionic, cationic, non-ionic or amphoteric surfactants.

[0029] The air-entraining agent may be chosen from: - anionic surfactants, for example alkyl sulfates, alkyl ether sulfates, alkaryl sulfonates, alkylsuccinates, alkylsulpho succinates, alkoyl sarcosinates, alkyl phosphates, alkylether phosphates, alkylether carboxylates and alpha-olefin sulfonates; - non-ionic surfactants, for example ethoxylated fatty alcohols, mono- or di-alkyl alkanolamides, alkyl polyglucosides; - amphoteric surfactants, for example alkyl amine oxides, alkyl betaines, alkyl amido propyl betaines, alkyl sulfo betaines, alkyl glycinates, alkyl amphopropionates and alkyl amidopropyl hydroxysultaines.

[0030] Preferably, the air-entraining agent is chosen from: - sodium alkyl sulfates (for example, the agents marketed by Ashland under the trade names Silipon® RN6031 and RN 6068), - sodium alpha olefin sulfonates (for example, agents marketed by Ashland under the trade name Silipon® RN 7002 or by Clariant under the trade name Hostapur OSB), - ethoxylated fatty alcohols (for example the agent marketed by the Ashland company under the trade name Silipon® RN 8018).

[0031] As explained above, the mass content of air-entraining agent expressed relative to the total mass of the dry mortar composition is between 0.1% and 2%, preferably between 0.2% and 0.9%.

[0032] The dry mortar composition according to the invention comprises at least one hydraulic binder.

[0033] The hydraulic binder can be chosen from: - cements, preferably Portland cements (more preferably those conforming to European standard EN 197-1), aluminous and / or sulfo-aluminous cements, - calcium sulfates (natural or synthetic gypsum, calcium sulfate hemihydrate, anhydrite), - silico-aluminous binders, fly ash, metakaolins, ground granulated blast furnace slag, calcined clays.

[0034] As an example of Portland cement, this may be Portland cement marketed under the trade name PERFORMAT® CEM I 52.5 R CE CP2 NF by the company Vicat or Portland cement CEM II / A-LL 52.5 R CE CP2 NF marketed by the company Holcim or Portland cement CEM I 52.5 R CE CP2 NF marketed by the company Calcia.

[0035] As an example of aluminous and / or sulfoaluminous cement, this may be the cement marketed under the trade name ALPENAT CK by the company Vicat or the cement marketed under the trade name FONDU® by the company Imerys.

[0036] As an example of calcium sulfate, it may be natural semi-hydrated gypsum marketed under the trade name Molda 3 N by the company Formula Saint Gobain or synthetic calcium sulfate marketed under the name CAB 30 by the company Lanxess.

[0037] As an example of ground granulated blast furnace slag, it may be ground granulated blast furnace slag marketed by the company Ecocem. Ground granulated blast furnace slag contributes to improving the mechanical strength of the mortar.

[0038] The mass content of at least one hydraulic binder, expressed relative to the total mass of the dry mortar composition, may be between 10% and 99%, preferably between 40% and 80%.

[0039] The dry mortar composition according to the invention may further comprise at least one sand, for example siliceous, calcareous, silico-calcareous or magnesium sands.

[0040] For example, this may be silica sand marketed under the trade name BE32 by the company Sibelco or silica sand marketed under the trade name PE2LS by the company Fulchiron.

[0041] The mass content of at least one sand, expressed relative to the total mass of the dry mortar composition may be between 0.1% and 85%, preferably between 5% and 40%.

[0042] The dry mortar composition according to the invention may further comprise at least one setting accelerator additive.

[0043] The setting accelerator additive can be chosen from: - alkali and alkaline-earth salts of hydroxides, halides, nitrates, nitrites, carbonates, thiocyanates, sulfates, thiosulfates, perchlorates, silica, aluminium, preferably from chlorides and their sodium or calcium salts, carbonates and their sodium or lithium salts, sulfates and their sodium or potassium salts, calcium hydroxides and formates, - carboxylic and hydrocarboxylic acids and their salts, - alkanolamines, - insoluble silicate compounds such as silica fumes, fly ash or natural pozzolans, quaternary ammonium silicates, - finely divided mineral compounds such as silica gels or finely divided calcium and / or magnesium carbonates, - hydrated calcium silicate germs, - amorphous calcium aluminates.

[0044] The mass content of at least one setting accelerator additive, expressed relative to the total mass of the dry mortar composition, may be between 0.01% and 8%, preferably between 0.5% and 5%.

[0045] The dry mortar composition according to the invention may further comprise at least one setting-retarding additive.

[0046] The setting retardant additive may be chosen from carboxylic acids and their salts, polysaccharides and their derivatives, borates and their salts, citric acid and its salts, sodium gluconates, tartaric acid and its salts.

[0047] The mass content of at least one setting-retarding additive, expressed relative to the total mass of the dry mortar composition, may be between 0.001% and 2%, preferably between 0.01% and 0.3%.

[0048] The dry mortar composition according to the invention may further comprise at least one thickener.

[0049] The thickener may be chosen from polysaccharides such as cellulose or starch ethers, preferably methylcelluloses, hydroxyethylcelluloses, methylhydroxypropylcelluloses, modified or unmodified methylhydroxyethylcelluloses, guar ethers, mineral thickeners and polyacrylamides.

[0050] As an example of thickeners, mention may be made of the thickener marketed under the trade name Culminai® UP 1540 by the company Ashland or the thickener marketed under the trade name WALOCEL® MKX. 40000 PF 01 by Dow Chemical Company.

[0051] The mass content of at least one thickener, expressed relative to the total mass of the dry mortar composition, may be between 0.05% and 4%, preferably between 0.3% and 2%.

[0052] The dry mortar composition according to the invention may further comprise at least one redispersible polymer.

[0053] The redispersible polymer may be chosen from homo- or copolymers of ethylene-vinyl acetate, acrylics, styrene butadiene, styrene acrylic, vinyl acetate and polyvinyl alcohol.

[0054] As an example of redispersible polymers, mention may be made of the polymer based on copolymers of vinyl acetate and ethylene marketed by the company Celanese under the trade name MP2100.

[0055] The mass content of at least one redispersible polymer, expressed relative to the total mass of the dry mortar composition, may be between 0.1% and 20%, preferably between 1% and 10%.

[0056] The dry mortar composition according to the invention may further comprise at least one light filler as defined above. It may for example be expanded perlite, expanded glass, silica aerogels, expanded polystyrene, cenospheres, hollow alumina beads, expanded clays, pumice, hollow glass beads, silicate foam grains or even rhyolite.

[0057] If the dry mortar composition according to the invention comprises at least one light filler, the mass content of the light filler expressed relative to the mass of the dry mortar composition may not exceed 10%, preferably 5%, more preferably 2%, even more preferably 1%, preferably 0.5% and most preferably 0.1%. This mass content of light fillers is much lower than that of the lightweight adhesive mortars mentioned above for which a high content of these light fillers hinders the diffusion of CO2 within the adhesive mortar under the tiles.

[0058] However, in a most preferred manner, the dry mortar composition is free of light filler. By "free of light filler" is meant in the context of the present invention that the mass content of light filler, expressed relative to the total mass of the dry mortar composition, does not exceed 0.01%.

[0059] The dry mortar composition according to the invention may comprise other additives called “additional additives” than those detailed above. For example, these may be additional additives chosen from fibers, water repellents, colorants, gas generating agents, foaming agents and fluidizing agents.

[0060] The colorants can be chosen from organic and / or mineral pigments (preferably oxides of iron, titanium, chromium, tin, nickel, cobalt, zinc, antimony), sodium aluminosilicate polysulfides, carbon, cobalt, manganese, zinc sulfides, as well as pigments with high transparency or high infrared reflectance.

[0061] The mass content of these additional additives, expressed relative to the total mass of the dry mortar composition, may be between 0.001% and 5%, preferably between 0.01% and 1%.

[0062] In one embodiment of the invention, the dry mortar composition may comprise, in mass percentages expressed relative to the total mass of said dry mortar composition: - between 0.1% and 2%, preferably between 0.2% and 0.9%, of at least one air-entraining agent, - between 10% and 99%, preferably between 40% and 80%, of cement, - between 0.05% and 4%, preferably between 0.3% and 2% of thickener, - optionally ground granulated blast furnace slag and, if present in said composition at a mass percentage not exceeding 90%, preferably between 5% and 60%, - optionally sand and, if present in said composition at a mass percentage not exceeding 85%, preferably between 5% and 30%, - optionally a setting accelerator additive and, if present in said composition at a mass percentage not exceeding 11%, preferably between 1.5% and 7%.

[0063] The different technical characteristics of the constituents of the dry mortar composition according to the invention which have been described above can of course be combined with each other in any possible combination.

[0064] The dry mortar composition according to the invention is preferably a dry adhesive mortar composition (namely a tile adhesive).

[0065] The dry mortar composition according to the invention may also be a dry assembly mortar composition (i.e. for the assembly and mounting of masonry materials), exterior and interior coating, or adhesive for exterior insulation systems.

[0066] The dry mortar composition according to the invention is preferably stored in bags with a capacity of 25 kg of said dry mortar composition.

[0067] The dry mortar composition according to the invention makes it possible to produce, after mixing, a wet mortar that is particularly pleasant and easy for the operator to lay, without too much effort. The wet mortar thus obtained after mixing has a smooth, creamy and slightly foamy texture.

[0068] This is why the invention also relates to a wet mortar which is characterized in that it has been obtained after mixing a dry mortar composition according to the invention as described above with water. The wet mortar has a paste density which is preferably between 700 g / L and 1,400 g / L, more preferably between 1,000 g / L and 1,200 g / L.

[0069] The volumetric air content expressed relative to the total volume of said wet mortar according to the invention is advantageously between 30% and 70%, preferably between 40% and 55%.

[0070] The loss of paste density at 30 minutes of the wet mortar according to the invention is less than 100 g / L which is a threshold value established in the certification reference: Technical document 11-03 “Mortars and related products: Single-layer rendering mortars” of March 14, 2022, revision no. 2, of the CSTB for facade rendering mortars in order to define the stability of the wet mortar. The wet mortar according to the invention therefore perfectly meets this stability criterion.

[0071] The consistency of the wet mortar according to the invention is advantageously between 20 mm and 45 mm. The consistency of a wet mortar is determined with a penetrometer. This involves measuring the penetration of a penetrometer spindle into a sample of the wet mortar over a given time. The higher the penetration value measured (and expressed in mm), the more fluid the consistency of the wet mortar. Conversely, the lower this penetration value, the heavier and thicker the wet mortar.

[0072] The invention also relates to a process for preparing a wet mortar according to the invention which is characterized in that a dry mortar composition according to the invention as described above is mixed with water.

[0073] Preferably, the mixing is mechanical and can advantageously be carried out with an electric mixer.

[0074] The rotation speed of the electric mixer must be sufficient to ensure the mixing of the dry mortar composition with the water in an efficient manner in order to avoid the appearance of lumps and to allow the incorporation of air into the wet mortar paste. The adjustment of the electric mixer to obtain an appropriate mixture of the dry mortar composition with the water is perfectly within the reach of a person skilled in the art.

[0075] The rotation speed of the electric mixer is advantageously between 400 rpm and 1100 rpm, preferably between 600 rpm and 900 rpm. A speed greater than 600 rpm improves the quantity of air introduced into the wet mortar paste and thus maximizes the yield obtained with the mortar according to the invention.

[0076] The mixing time must be sufficient to allow homogenization of the wet mortar paste and incorporation of air. The mixing time with the electric mixer can be between 1 minute and 5 minutes, preferably between 2 minutes and 3 minutes. Most preferably, the mixing time is 3 minutes. This makes it possible to obtain a mortar according to the invention having optimal characteristics, in particular those described above (for example with regard to consistency).

[0077] Thus, in an advantageous embodiment of the invention, the method for preparing a wet mortar according to the invention is characterized in that a dry mortar composition according to the invention is mixed with water using an electric mixer whose rotation speed is between 400 rpm and 1,100 rpm, preferably between 600 rpm and 900 rpm, for a period of between 1 minute and 5 minutes, preferably between 2 minutes and 3 minutes.

[0078] In the context of the present invention, the term "mixing rate" means the weight ratio between the water and the dry mortar composition used during mixing.

[0079] The mixing rate is determined by the operator according to the consistency of the wet mortar that he wishes to obtain. The selection of the mixing rate is perfectly within the reach of a person skilled in the art. Thus, advantageously, the operator chooses a mixing rate such that he obtains a wet mortar having a consistency of between 20 mm and 45 mm.

[0080] For example, the mixing rate can be between 0.45 and 0.55.

[0081] As regards the characteristics of the electric mixer, the latter may have different whisk geometries which may be single or double. It may therefore be a 4-blade USG whisk, helical, right-hand helical hexagonal, left-hand helical hexagonal, helix, high shear force or even a 5 QT wire mixing whisk. Among these whisk models, some of them have blades which promote the incorporation of air and which are particularly suitable for obtaining optimal performance. These are the helical whisk, right-hand helical hexagonal, left-hand helical hexagonal, as well as the 5QT wire mixing whisk which are preferably used in the context of the invention.

[0082] It should be noted that the search for air entrainment with a mixing tool, for example with a mixing tool chosen from those described above, is counter-intuitive for those skilled in the art who would usually seek to limit the incorporation of air during mixing so as not to denature the mortar.

[0083] Advantageously, a flat-bottomed container is used to mix the dry mortar composition and the water. This may be a bucket or a trough. Buckets with a diameter and height of 357 mm x 370 mm provide the best results for mixing the wet mortar paste (i.e., a reduction in lumps and optimal yield). These buckets are well known to the person skilled in the art.

[0084] As explained above, the dry mortar composition is preferably a dry adhesive mortar composition. Mixing the dry adhesive mortar composition makes it possible to obtain a wet adhesive mortar according to the invention, preferably having the technical characteristics described above.

[0085] Therefore, another object of the invention is a method of fixing a tile to a support which is characterized in that it comprises at least the following steps: - a dry adhesive mortar composition according to the invention as described above is mixed with water to obtain a wet adhesive mortar according to the invention as described above, preferably as described above for the preparation of a wet mortar according to the invention; - the said wet adhesive mortar is applied to the support and / or to the tiles; - the tiles are applied to the said support.

[0086] As explained above, it is possible to mix with an electric mixer whose rotation speed is between 400 rpm and 1100 rpm, preferably between 600 rpm and 900 rpm, for a duration of between 1 minute and 5 minutes, preferably between 2 minutes and 3 minutes.

[0087] The support may be a wall, a partition or a floor (for example a screed). The tiling may be in the form of tiles or tile slabs. The material of the tiling may be chosen, for example, from ceramic, sandstone, cement, stone or marble materials. The wet mortar may, for example, be applied to the support and / or the tiling using an adhesive comb, a float, a trowel or a notched spatula.

[0088] The application of the wet adhesive mortar to the support and / or to the tiles, as well as the application of the tiles to the support are steps perfectly within the reach of those skilled in the art.

[0089] The invention will be better understood with the aid of the detailed description of experiments carried out with a dry adhesive mortar composition according to the invention and two comparative dry adhesive mortar compositions.

[0090] EXPERIMENTAL PART:

[0091] Experiments were carried out with: - a dry mortar adhesive composition according to the invention and hereinafter referred to as “mortar invention”; - a dry composition of classic adhesive mortar and hereinafter referred to as “comparative mortar 1”; - a dry composition of lightweight adhesive mortar and hereinafter referred to as “comparative mortar 2”.

[0092] The dry mortar composition according to the invention comprised in mass percentages expressed relative to the total mass of said dry composition: - 40% CEM II 52.5R cement (1st hydraulic binder); - 35% crushed granulated blast furnace slag (2nd hydraulic binder); - 4% vinyl acetate and ethylene copolymer (redispersible polymer); - 19.85% BE32 sand (silica sand 0.2-0.5mm); - 0.35% sodium alpha olefin sulfonate (air entraining agent); - 0.8% hydroxymethylcellulose 50000-60000 mPa (thickener);

[0093] This dry mortar adhesive composition according to the invention has been classified “C2E” according to standard NF EN 12004-1:2017.

[0094] The classic dry adhesive mortar composition was a dry adhesive mortar composition marketed by the company Vicat Produits Industriels under the trade name V350 Collimix fluid. This dry adhesive mortar composition comparative 1 was classified “C2E” according to standard NF EN 12004-1:2017.

[0095] The dry composition of lightweight adhesive mortar was a dry composition of adhesive mortar marketed by the company Vicat Produits Industriels under the trade name V430 / V431 Colliflex confort. This dry composition of comparative adhesive mortar 2 was classified “C2S1E” according to standard NF EN 12004-1:2017.

[0096] The dry mortar compositions according to the invention, comparative 1 and comparative 2 were mixed according to a mixing rate specified in table 1 below with an electric mixer comprising a right-hand helical hexagonal geometry blade for a period of 3 minutes and at a mixing speed of 810 rpm so as to obtain wet mortars according to the invention, comparative 1 and comparative 2.

[0097] Table 1 below details for the invention mortar and comparative mortars 1 and 2: - the unpacked density which was determined according to the aforementioned certification standard, namely Technical Document 11-04 “Mortars and related products: Thin-joint mounting mortars for small masonry elements” of March 14, 2022, revision no. 2, from the CSTB; - the mixing rate used to obtain the wet mortar; - the apparent density of the paste which was determined according to standard NF EN 1015-6; - the stability of the paste at 30 minutes which was determined according to the aforementioned certification standard, namely Technical Document 11-03 “Mortars and related products: Single-layer rendering mortars” of March 14, 2022, revision no. 2, from the CSTB; - the yield in m2 for a double-bonding application on tiles and a concrete slab with a U9 comb for a 25 kg bag; - the yield in m2 for a double-glue application on tiles and a concrete slab with a U9 comb for a 15 kg bag; - the consistency expressed in mm and as defined above.

[0098] [Tables 1] Comparative mortar 1 Invention mortar Comparative mortar 2 Bulk volume (g / L) 1,300 1,150 800 Mixing rate (%) 26 52 44 Paste density (g / L) 1,650 1,100 1,300 Paste stability after 30 minutes (g / L) 1,660 (+10 g / L) 1,112 (+12 g / L) 1,30S: (+8 g / L) Consistency (mm) 37 33 36 Yield per 25 kg bag (m2) 5.2 9.2 Yield per 15 kg bag (m2) 3J2 5.52 4.2

[0099] In view of the results detailed in Table 1, we note that: - The mortar according to the invention has a bulk density relatively close to that of comparative mortar 1 (i.e. the conventional adhesive mortar) and a much lower paste density (1,100 g / L versus 1,650 g / L). Its paste density is even lower than that of comparative mortar 2 (i.e. the lightweight adhesive mortar). This shows that the presence of a significant amount of air-entraining agent (0.35%) makes it possible to lower the paste density, even without the addition of fillers (in particular light fillers). - The wet mortar according to the invention remains perfectly stable after 30 minutes in comparison with comparative mortars 1 and 2. - The invention mortar has better yields for 25 kg and 15 kg bags than comparative mortars 1 and 2.

[0100] Two types of models were prepared with the invention mortar and the comparative mortar 1 to use them in recarbonation experiments.

[0101] The first model was a tile model and was obtained in the following manner:

[0102] The adhesive mortar tested (namely invention or comparison 1) was applied using a 20 half-moon comb in simple gluing on a square-shaped fiber cement board (51cm x 51 cm).

[0103] A square-shaped porcelain stoneware tile (50 cm x 50 cm) with a thickness of 1 cm was positioned and glued onto the tested adhesive mortar.

[0104] After 16 hours of drying, the model was jointed around its periphery using a commercial cement-based joint. The joint width was 5 mm.

[0105] After 7 days of drying, the model was gas-sealed using a two-layer epoxy resin with the aim of having only the upper face of the model in contact with the CO2.

[0106] The 2nd model was a prism model and was obtained in the following manner:

[0107] The tested adhesive mortar (namely invention or comparison 1) was applied in a mold having the shape of a prism with dimensions 4 cm x 4 cm x 16 cm.

[0108] The prisms were demolded after 24 hours of drying. Then after 7 days of drying at 23°C, the faces were gas-sealed using an epoxy resin in two layers, with the aim of having only one 4 cm x 4 cm face of the prism in contact with the CO2.

[0109] The 1st and 2nd models were placed in accelerated aging conditions in an oven with the following parameters: - CO2 volume content: 3%; - temperature of 20°C; - humidity of 65%.

[0110] Several samples were taken from the 1st and 2nd models at several times.

[0111] The CO2 capture measurement was carried out by thermogravimetric analysis.

[0112] To do this, the mass loss of the sample was measured at different temperatures. Free water or water present in certain hydrates, as well as the organic parts, are released between 80 and 600°C. Between 600 and 900°C, only the fixed CO2 is released.

[0113] However, sands or calcareous fillers also release their CO2 over this same temperature range. This is why it was necessary to produce a so-called "control" sample with the same batches of the mortars tested, which were left to harden in a pillbox protected from CO2 in the air (therefore without the possibility for the adhesive mortars tested to capture CO2 from the air) in order to be able to measure for this control sample the quantity of CO2 released by the sands and calcareous fillers when they are subjected to temperatures between 600°C and 900°C.

[0114] Then, after subtracting this quantity of CO2 released by the sands and limestone loads at these high temperatures, it was possible to deduce the quantity of CO2 actually captured by recarbonation by the adhesive mortars tested.

[0115] The recarbonation depth of the tested adhesive mortars was also determined with these samples.

[0116] A pH indicator (phenolphthalein) was applied to detect the recarbonation front.

[0117] The recarbonation results obtained with the 1st and 2nd models are detailed below.

[0118] Recarbonation results with the I^-model (prism):

[0119] The prisms were removed from the recarbonation oven at different times. They were then cut along their length, and then the aforementioned pH indicator was applied to reveal the recarbonation front and thus be able to measure the recarbonation depth.

[0120] Table 2 below details for the invention mortar and comparative mortar 1 the recarbonation depth (expressed in mm) as a function of the number of days in the accelerated aging conditions detailed above.

[0121] The 2nd column of Table 2 shows the correspondence between these numbers of days under accelerated aging conditions and their equivalent numbers of days under natural conditions. This correspondence can be easily determined by taking into consideration that the volume content of CO2 in the oven was 3% and that in the air is approximately 357 ppm. 7 days under accelerated aging conditions correspond to 588 days (84 weeks) under natural conditions. 31 days under accelerated aging conditions correspond to 2604 days (372 weeks, a little over 7 years) under natural conditions. 97 days under accelerated aging conditions correspond to 8148 days (1164 weeks, a little over 22 years) under natural conditions.

[0122] [Tables2] Number of days under accelerated conditions Equivalent number of days under natural conditions Recarbonation depth of comparative mortar 1 (in mm) Recarbonation depth of invention mortar [in mm] y 5S8 15: 22 31 2604 37 55 97 8148 ^4 75

[0123] In view of the results detailed in Table 2, it is noted that the invention mortar has a greater recarbonation depth than that of comparative mortar 1.

[0124] The service life of adhesive mortars is approximately 50 years. This value is used as a reference on the environmental and safety data sheets for these construction products.

[0125] Therefore, from linear regressions established from the results detailed in Table 2 above, it was determined that after 50 years under natural conditions, the depth of recarbonation of: - mortar invention is 117 mm, - comparative mortar 1 is 83 mm.

[0126] The inventive mortar has a better recarbonation depth after 50 years in natural conditions than comparative mortar 1.

[0127] Thus, the diffusion of CO2 in the invention mortar is 40% faster and deeper than that of comparative mortar 1.

[0128] Recarbonation results with the 2™Mnaquette (tiles):

[0129] The samples were taken after 3 months under accelerated aging conditions, i.e. approximately 21 years in equivalent natural conditions.

[0130] The samples were taken on the diagonal of the porcelain stoneware tile (50 cm on each side) at the following distances measured from the corner of the tile: 5 cm, 20 cm and 35 cm.

[0131] Table 3 below details the quantity of CO2 captured by the adhesive mortar tested at the location of the sample taken (i.e. on the diagonal of the tile at 5 cm, 20 cm and 35 cm). This quantity is expressed in kg of CO2 captured relative to one tonne of dry composition of the adhesive mortar tested (i.e. “kg CO2 / t. equivalent”).

[0132] [Tables3] Quantity of CO2 captured (kg CCh / t. equivalent) on the diagonal of the tile at: Mortar invention Comparative mortar 1 5 cm 102 33.1 20 cm 14.9 13.3 35 cm 4.8 2.6

[0133] These results were processed using mathematical methods in order to model the recarbonation under the entire porcelain stoneware tile and to deduce an average value of the quantity of CO2 captured after these 3 months under accelerated aging conditions (or 21 years under natural conditions) for: - the mortar invention: 58 kg CO2 / t. equivalent; - comparative mortar 1: 17 kg CO2 / t. equivalent.

[0134] In view of the yields in m2 detailed in table 1 above for the invention mortar and comparative mortar 1 and in view of these average values ​​of quantity of CO2 captured, we deduce that for 1 m2 of adhesive mortar applied using a comb U9: - 0.08 kg of CO2 are recarbonated with comparative mortar 1, - 0.157 kg of CO2 are recarbonated with the invention mortar,

[0135] after 3 months under accelerated aging conditions (or 21 years under natural conditions). The quantity of CO2 captured after 3 months under accelerated aging conditions (or 21 years under natural conditions) is therefore twice as high with the invention mortar as with comparative mortar 1.

Claims

Claims

1. Dry mortar composition, preferably adhesive mortar, the unpacked density of which is between 900 g / L and 1,400 g / L, preferably between 1,000 g / L and 1,300 g / L, characterized in that it comprises at least one air-entraining agent at a mass content expressed relative to the total mass of said dry mortar composition of between 0.1% and 2%, preferably between 0.2% and 0.9%.

2. Dry mortar composition according to claim 1, characterized in that the at least one air-entraining agent is chosen from alkyl sulfates, alkyl ether sulfates, alkaryl sulfonates, alkylsuccinates, al-kylsulpho succinates, alkoyl sarcosinates, alkyl phosphates, alkylether phosphates, alkylether carboxylates, alpha-olefin sulfonates, ethoxylated fatty alcohols, mono- or di-alkyl alkanolamides, alkyl polyglucosides, alkyl amine oxides, alkyl betaines, alkyl amido propyl betaines, alkyl sulfo betaines, alkyl glycinates, alkyl amphopropionates and alkyl amidopropyl hydroxysultaines.

3. Dry mortar composition according to claim 2, characterized in that the at least one air-entraining agent is chosen from sodium alkyl sulfates, sodium alpha olefin sulfonates and ethoxylated fatty alcohols.

4. Dry mortar composition according to any one of claims 1 to 3, characterized in that it comprises at least one hydraulic binder chosen from cements, calcium sulfates, silico-aluminous binders, fly ash, metakaolins, ground granulated blast furnace slags and calcined clays.

5. Dry mortar composition according to claim 4, characterized in that the mass content of the at least one hydraulic binder, expressed relative to the total mass of the dry mortar composition, is between 10% and 99%, preferably between 40% and 80%.

6. Dry mortar composition according to any one of claims 1 to 5, characterized in that it further comprises at least one thickener chosen from cellulose or starch ethers, preferably methylcelluloses, hydroxyethylcelluloses, methylhydroxypropylcelluloses, modified or unmodified methylhydroxyethylcelluloses, guar ethers, mineral thickeners and polyacrylamides.

7. Dry mortar composition according to claim 6, characterized in that the mass content of at least one thickener, expressed relative to the total mass of said dry mortar composition, is between 0.05% and 4%, preferably between 0.3% and 2%.

8. Dry mortar composition according to any one of claims 1 to 7, characterized in that it further comprises at least one redispersible polymer chosen from homo- or copolymers of ethylene-vinyl acetate, acrylics, styrene butadiene, styrene acrylic, vinyl acetate and polyvinyl alcohol.

9. Dry mortar composition according to claim 8, characterized in that the mass content of the at least one redispersible polymer, expressed relative to the total mass of the dry mortar composition, is between 0.1% and 20%, preferably between 1% and 10%.

10. Dry mortar composition according to claim 1, characterized in that it comprises, in mass percentages expressed relative to the total mass of said dry mortar composition: - between 0.1% and 2%, preferably between 0.2% and 0.9%, of at least one air-entraining agent, - between 10% and 99%, preferably between 40% and 80%, of cement, - between 0.05% and 4%, preferably between 0.3% and 2%, of thickener, - optionally ground granulated blast furnace slag and, if present in said composition at a mass percentage not exceeding 90%, preferably between 5% and 60%, - optionally sand and, if present in said composition at a mass percentage not exceeding 85%, preferably between 5% and 30%, - optionally a setting accelerator additive and, if present in said composition at a mass percentage not exceeding 11%, preferably between 1.5% and 7%.

11. Dry mortar composition according to any one of claims 1 to 10, characterized in that it is free from light filler.

12. Wet mortar, characterized in that it is obtained after mixing a dry mortar composition according to any one of claims 1 to 11 with water and in that it has: - a paste density of between 700 g / L and 1,400 g / L, preferably between 1,000 g / L and 1,200 g / L, - an air volume content, expressed relative to the total volume of said wet mortar, between 30% and 70%, preferably between 40% and 55%.

13. Process for preparing a wet mortar according to claim 12, characterized in that a dry mortar composition according to any one of claims 1 to 11 is mixed with water using an electric mixer whose rotation speed is between 400 rpm and 1100 rpm, preferably between 600 rpm and 900 rpm, for a period of between 1 minute and 5 minutes, preferably between 2 minutes and 3 minutes.

14. Method for fixing a tile to a support, characterized in that it comprises at least the following steps: - mixing a dry adhesive mortar composition according to any one of claims 1 to 11 with water to obtain a wet adhesive mortar according to claim 12; - applying said wet adhesive mortar to the support and / or to the tile; - applying the tile to said support.

15. Method for fixing a tile to a support according to claim 14, characterized in that it is mixed with an electric mixer whose rotation speed is between 400 rpm and 1100 rpm, preferably between 600 rpm and 900 rpm, for a duration of between 1 minute and 5 minutes, preferably between 2 minutes and 3 minutes.

Citation Information

Patent Citations

  • USE OF BLOOD IN THE CEMENT, MORTARS AND CONCRETE INDUSTRY TO OBTAIN A LIGHTWEIGHT MATERIAL

    BE861443A

  • Ultra-lightweight concrete and use thereof

    EP2364962A2

  • Adhesive composition, useful for attaching inorganic and organic materials e.g. tiles and PVC coating on substrate, comprises cement base including adhesive mortar, and aqueous dispersion including methacrylic polymer

    FR3002772A1

  • ACOUSTIC ABSORPTION COATING.

    FR3075195A1

  • Dry mortar composition, particularly tile adhesive mortar

    FR3096365A1

Cited By

  • Green low-carbon C30 self-compacting concrete using dry-mixed mortar tail powder and preparation method of green low-carbon C30 self-compacting concrete