Catalyst bed containing a particulate photocatalytic catalyst

JP2023546080A5Active Publication Date: 2024-10-15IFP ENERGIES NOUVELLES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023522773
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-10-15
Filing Date
2021-10-06
Publication Date
2024-10-15
Estimated Expiration
2041-10-06

AI Technical Summary

Technical Problem

Existing photocatalytic materials face inefficiencies in photocatalytic performance due to the limited penetration depth of irradiation, particularly in the UV-A, UV-B, and visible ranges, leading to suboptimal activation of semiconductor materials.

Method used

The use of structured, spherical mineral particles with calibrated diameters for Mie scattering enhances the penetration and distribution of radiation, combined with semiconductor materials, improving photocatalytic performance by up to ten times.

Benefits of technology

The calibrated structured particles significantly increase the photocatalytic activity of semiconductor materials, allowing deeper irradiation penetration and improved reaction efficiency in liquid and gaseous media, including CO2 reduction, water splitting, and VOC conversion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The present invention relates to a catalyst bed containing a specific photocatalytic catalyst, which comprises structured particles b made of inorganic material in combination with at least one semiconductor material a having photocatalytic properties, the combination being produced by: mixing the structured particles b made of inorganic material with the semiconductor material a in particulate form and / or by chemical or physicochemical deposition of the semiconductor material a on the structured particles b made of inorganic material, the structured particles b being substantially spherical in shape and having an average diameter between 22 nm and 8.0 μm.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to the field of photocatalysis, and is intended to treat liquid or gas phases by contacting them with photocatalytic materials, which are then irradiated with a light source emitting light in a suitable wavelength range. The present invention more particularly relates to a new type of photocatalytic material, its preparation method and its use. [Background technology]

[0002] Photocatalysis is based on the principle of activating a semiconductor, acting as a photocatalyst, using energy provided by light irradiation. A semiconductor is characterized by its band gap, i.e., the energy difference between its conduction band and its valence band, which is specific to the semiconductor. Photocatalysis can be defined as the absorption of a photon, the energy of which is greater than the band gap width between the valence band and the conduction band, which, in the case of a semiconductor, induces the formation of an electron-hole pair. There is excitation of an electron into the conduction band and the formation of a hole in the valence band. This electron-hole pair allows the formation of free radicals, which react with compounds present in the medium, initiating oxidation / reduction reactions, or recombine according to various mechanisms. Any photon with an energy greater than the band gap can be absorbed by the semiconductor. Photons with an energy lower than the band gap cannot be absorbed by the semiconductor.

[0003] The fields of application are enormous: photocatalysis can therefore be used to carry out the decontamination of gaseous media, in particular to convert compounds of the VOC (Volatile Organic Compounds) type by oxidation, or to treat liquid media (e.g., containing toluene, benzene, ethanol, or acetone). Photocatalysis can also be used to convert CO2 in gaseous media by reduction, converting it into upgradeable compounds, in particular those with one or more carbons, such as CO, methane, methanol, carboxylic acids, ketones, or other alcohols: CO2 is therefore actively converted, rather than captured and stored to reduce its content in the atmosphere. It is also possible to carry out photolysis of water in liquid or gaseous media to produce upgradeable hydrogen H2, in particular as a low-carbon energy source.

[0004] A photocatalytic material in the form of a porous monolith is known from Patent Document 1. This photocatalytic material contains 20% to 70% by weight of TiO2, relative to the total weight of the monolith, and 30% to 80% by weight of a refractory oxide chosen from silica, alumina or silica-alumina, relative to the total weight of the monolith, has a bulk density of less than 0.19 g / mL, and has a specific porosity, in particular with regard to macroporosity and mesoporosity. This therefore relates to a material that combines a semiconductor (titanium oxide), which is the source of its photocatalytic properties, with one or two refractory oxides, and also has a specific porosity that results in photocatalytic performance qualities superior to those that would be obtained with a material composed entirely of titanium oxide.

[0005] The subject of the present invention is therefore the development of improved photocatalytic materials, in particular with further improved photocatalytic performance qualities and also with improved implementation and / or manufacturing. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2018 / 197432 Summary of the Invention [Means for solving the problem]

[0007] (Summary of the Invention) The present invention relates first of all to a catalyst bed containing a granular photocatalytic catalyst, said bed comprising structured particles b made of mineral material, said structured particles being combined with at least one semiconductor material a having photocatalytic properties, said combination being characterized by: - mixing structured particles b made from mineral material with semiconductor material a in particle form, and / or - Chemical or physicochemical deposition of a semiconductor material a on structured particles b made from mineral materials caused by The structured particles b are essentially spherical and have an average diameter of 22 nm to 8.0 μm, preferably 30 nm to 7.5 μm.

[0008] The mineral materials of interest to the present invention are essentially inert to photocatalysis, since they are of the electrical insulator type: they are materials with a band gap greater than 6 eV.

[0009] Preferably, the catalyst bed is intended to be a fixed bed (especially as opposed to a fluidized bed).

[0010] The present invention therefore chooses to disperse a semiconductor material in a non-semiconductor mineral material by calibrating the size of the particles of this mineral material according to the range of wavelengths of irradiation of the semiconductor material that allows the generation of electron-hole pairs and therefore the desired photocatalytic reaction, since traditionally in the field of photocatalysis, irradiation sources are chosen in the UV-A, UV-B and / or visible ranges, which define the range of wavelengths that can activate traditional semiconductor materials, such as titanium oxide.

[0011] In fact, the present invention utilizes what is known under the term Mie scattering by selecting particles (herein referred to as structured particles) made of mineral materials that are spherical and have a specific average diameter, thereby causing optimal scattering of radiation preferentially in the direction of the incident radiation: Mie scattering is directly related to the wavelength of the incident radiation and describes preferential scattering of radiation in its incident axis for spherical particles whose radius is 0.1 to 10 times the wavelength in question. The structured particles of the present invention, with their appropriately adjusted diameter, therefore amplify the effectiveness of irradiation in the range from UV-A rays to the visible range: they scatter radiation from the surface of the catalyst bed primarily in the direction of incidence, significantly increasing the probability of irradiation of the semiconductor material and thus improving its photocatalytic activity. This is because the penetration depth of the incident radiation within the catalyst bed is deeper, allowing radiation to reach areas of the semiconductor material that are difficult for radiation to reach.

[0012] It has been discovered that the photocatalytic performance qualities of a material can be improved by a factor of two, in fact three or four, and even in the most preferred configurations by a factor of ten or more, compared to materials similarly configured but having particles outside this size range and / or particles that are non-spherical, providing great flexibility in the practice of the invention. Thus, depending on the priority given to catalytic performance quality versus cost, it is possible to choose to amplify the performance qualities of the material as much as possible with the same amount of semiconductor, or to amplify it to a lesser extent, or to keep it at a minimum the same by reducing the amount of semiconductor in the material.

[0013] The present invention provides two alternative or cumulative variations for constructing the material, both of which have their advantages; The variant with two types of particles, structured particles and semiconducting particles, is advantageous because it is simple to manufacture, since it does not require the integration of the two types of material, and because the preparation is based solely on the mixing of the two powders, without chemical reactions, heat treatments, etc. This variant also allows for a very easy adaptation of the catalyst bed to any shape and any dimension. It makes it possible to form the bed in situ, directly in the reactor in which the bed must be placed, without any prior pre-adjustment, in particular by easily adapting the ratio between the two types of particles case by case, except for providing a suitable device to ensure as homogeneous a mixture as possible between the two types of particles. It is also possible to prepare the mixture in advance so that only one product is deposited to form the bed.

[0014] Another variant, consisting of chemically / physicochemically depositing a semiconductor on structured particles, also presents advantages: it ensures a controlled distribution of the semiconductor, an integration between the two materials that favors their interaction, especially in this case with respect to the radiation scattered by the particles. In this way, it provides a "ready-to-use" product for forming a catalyst bed in a reactor. It should be noted that the structured particles can be completely or only partially covered with the semiconductor. It should also be noted that, according to this variant, provision can be made for a certain proportion of the structured particles to remain free of semiconductor material deposition.

[0015] Advantageously, the structured particles are (essentially) spherical and solid: their solidity gives them better mechanical properties, better mechanical strength, wear resistance, abrasion resistance, etc.

[0016] Preferably, all of the particles in the bed are randomly arranged, as this has surprisingly been found to be beneficial for the photocatalytic performance qualities of the material. The term "randomized" is understood to refer to the fact that the particles of the material are not arranged in an orderly manner and do not form layers of three-dimensionally aligned particles. The material according to the present invention thus exhibits interparticle spaces of non-uniform size and position that are randomly arranged within the material. Furthermore, these spaces differ depending on whether a mixture of particles (of different sizes and shapes) or a variation with only one type of particle (structured particles at least partially covered by semiconductor) is involved.

[0017] Preferably, when the bed contains the semiconductor material a in the form of particles, said particles exhibit an average size of at most 100 nm, in particular at most 50 nm, and at least 5 nm, preferably 10 to 30 nm, where it should be noted that these particles are not, or even necessarily, spherical, and their average size is not conditioned by the wavelength of the irradiating radiation.

[0018] Preferably, the catalyst bed according to the invention exhibits a porosity, which is equal to the ratio of the void volume in the photocatalytic bed to the total volume of the bed consisting of voids and particles, of at least 40% and preferably at most 80%, in particular 40% to 70%. This porosity is indirectly an indicator of the disordered arrangement of the aforementioned materials, since the porosity is minimal for perfectly organized spheres, and the porosity according to the invention is greater than this minimum ratio.

[0019] Preferably, the catalyst bed according to the invention exhibits a "dilution factor" equal to the ratio of the volume occupied by the structured particles b made of mineral material to the volume occupied by the sum of the semiconductor material(s) a, a' and the structured particles b made of mineral material: up to 80%, in particular 5% to 70%, preferably 10% to 50%. This dilution factor of up to 80% is chosen in particular for chemical or physicochemical deposition of the semiconductor material a onto the structured particles b made of mineral material, but is of course applicable to both variants of the invention.

[0020] The term "dilution ratio" is used to reflect the ratio of active material (semiconductor) to structured particles, which are a priori not active or barely active. The higher the dilution ratio, the greater the amount of structured particles. From the examples below, it will be seen that this dilution ratio can be increased without overall decreasing, and in fact improving, the photocatalytic performance qualities of the material. Insofar as the density of materials, especially semiconductors, can vary greatly from one semiconductor to another, it is more sensible to reason in terms of dilution ratios by volume rather than by mass.

[0021] In one embodiment of the present invention, the catalyst bed can comprise (at least) two different semiconductor materials, a first material a and a second material a', which can be produced by: - mixing structured particles b made from a mineral material with semiconductor material(s) in the form of particles of a first material a and particles of a second material a', respectively, and / or - chemical or physicochemical deposition of semiconductor materials a, a' on the carrier particles b; by deposition of both a first semiconductor material a and a second semiconductor material a' on the structured particles b, or by deposition of a first semiconductor material a on a first portion of the structured particles b and deposition of a second semiconductor material a' on a second portion of the structured particles b.

[0022] Therefore, there are three powders to be mixed of three different materials a, a' and b, i.e. either two powders b+a and b+a' (structured particles covered with either the first semiconductor or the second semiconductor), or a single powder b+a+a' (structured particles covered with both the first and second semiconductor).

[0023] Of course, based on the same principle, it is possible to use more than two different semiconductor materials, and in variants where semiconductors are deposited on their surfaces, there remains the option of the bed also containing certain portions of the structured particles that are not covered by the semiconductor material.

[0024] Advantageously, the structured particles b made from mineral material may be made from metal oxide(s), in particular from oxides of metals of groups IIIa and IVa of the periodic table, preferably chosen from aluminum oxide, silicon oxide, and mixtures of aluminum oxide and silicon oxide.

[0025] Advantageously, the semiconductor materials a, a' and / or the semiconductor materials a, a' may be chosen from inorganic semiconductors, which may be chosen from one or more elements of group IVa, such as silicon, germanium, silicon carbide or silicon-germanium. They may also be used in combination with elements of groups IIIa and Va, such as GaP, GaN, InP and InGaAs, or elements of groups IIb and VIa, such as CdS, ZnO and ZnS, or elements of groups Ib and VIIa, such as CuCl and AgBr, or elements of groups IVa and VIa, such as PbS, PbO, SnS and PbSnTe, or elements of groups Va and VIa, such as Bi2Te3 and Bi2O3, or elements of groups IIb and Va, such as Cd3P2, Zn3P2 and Zn3As2, or elements of groups Ib and VIa, such as CuO, Cu2O and Ag2S, or or elements of groups VIIIb and VIa, such as CoO, PdO, Fe2O3 and NiO, or elements of groups VIb and VIa, such as MoS2 and WO3, or elements of groups Vb and VIa, such as V2O5 and Nbr2O5, or elements of groups IVb and VIa, such as TiO2 and HfS2, or elements of groups IIIa and VIa, such as In2O3 and In2S3, or elements of groups VIa and the lanthanides, such as Ce2O3, Pr2O3, Sm2S3, Tb2S3 and La2S3, or elements of groups VIa and the actinides, such as UO2 and UO3.

[0026] Preferably, they comprise at least one of the following metal oxides: titanium oxide, tungsten oxide, cerium oxide, bismuth oxide, zinc oxide, copper oxide, vanadium oxide, iron oxide, cadmium oxide, preferably selected from TiO2, Bi2O3, CdO, Ce2O3, CeO2, CeAlO3, CuO, Fe2O3, FeTiO3, ZnFe2O3, V2O5, ZnO, WO3 and ZnFe2O4, alone or as a mixture.

[0027] The semiconductor materials a, a' or at least one of the semiconductor materials a, a' may be doped with one or more ions chosen from metal ions, in particular ions of V, Ni, Cr, Mo, Fe, Sn, Mn, Co, Re, Nb, Sb, La, Ce, Ta, Ti, or from non-metal ions, in particular C, N, S, F, P, or by a mixture of metal and non-metal ions.

[0028] The semiconductor materials a, a' or at least one of the semiconductor materials a, a' may also contain one or more elements in the metallic state selected from the elements of groups IVb, Vb, VIb, VIIb, VIIIb, Ib, IIb, IIIa, IVa and Va of the Periodic Table of the Elements, preferably in direct contact with said semiconductor material, which are preferentially metals from the group consisting of platinum, palladium, gold, nickel, cobalt, ruthenium, silver, copper, rhenium or rhodium.

[0029] It should be noted that throughout this specification, groups of chemical elements are given according to the CAS IUPAC classification (CRC Handbook of Chemistry and Physics, published by CRC Press, 81st edition, 2000-2001), rather than according to the new classification. For example, group VIII according to the CAS classification corresponds to metals in groups 8, 9 and 10 according to the new IUPAC classification.

[0030] The catalyst bed according to the invention can have a thickness of up to 1 cm, in particular up to 5 mm, and in particular at least 10 μm. Preferably, its thickness is at least 100 or 200 microns. This thickness depends in particular on the penetration depth of the radiation from the irradiation source into the bed.

[0031] Another subject of the invention is a method for obtaining a catalyst bed as defined above, by mixing, on the one hand, structured particles of mineral material b and, on the other hand, particles of semiconducting material a, to produce a homogeneous distribution of the two types of particles in the bed. On both laboratory and industrial scale, devices of the screw mixer / mill type exist to ensure homogeneous mixing.

[0032] Another subject of the invention is a method for obtaining a catalyst bed as defined above, in which the deposition of semiconductor materials a, a' or at least one of the mineral materials of semiconductor materials a, a' on structured particles b is carried out by impregnating said structured particles with a solution of at least one precursor of the semiconductor material, or by ion exchange, or by an electrochemical route, in particular of the molten salt type, followed by drying and optional calcination. It is also possible to choose chemical vapor deposition (CVD), spray drying or atomic layer deposition (ALD), or any other technique known to experts in this type of deposition.

[0033] Another subject of the present invention is any reactor for the photocatalytic treatment of feedstocks in gaseous and / or liquid form, comprising at least one photocatalytic bed as defined above, mounted in fixed manner within said reactor, since the advantages of Mie scattering on structured particles can be best exploited when the bed is fixed (as opposed to a moving bed reactor).

[0034] Another subject of the invention is a method for the photocatalytic treatment of a feedstock in gaseous or liquid form, comprising: - placing at least one photocatalytic bed as defined above in a fixed manner in the reactor, - contacting the feedstock with a catalyst bed in a reactor; and The photocatalytic bed is irradiated during the contacting operation by at least one radiation source emitting in the UVA-A range and / or the UV-B range and / or the visible range, in particular in the wavelength range from 220 to 800 nm, preferably in the wavelength range from 300 to 750 nm.

[0035] Another subject of the invention is a method in which the photocatalytic treatment is: - Photo-oxidation of components present in liquid or gaseous feedstocks, specifically for the purpose of decontaminating / decontaminating said feedstocks; or - Photocatalytic reduction of CO2 from liquid or gaseous feedstocks, or - Photolysis of feedstock water in liquid or gaseous form to produce H2.

[0036] (List of drawings) FIG. 1 shows a schematic re-emission pattern of an incident beam on a particle due to Rayleigh-type and Mie-type scattering.

[0037] FIG. 2 shows a transmission electron microscopy (TEM) image of semiconductor particles made from titanium oxide used according to an embodiment of the photocatalytic material of the present invention.

[0038] FIG. 3 shows a scanning electron microscopy (SEM) image of structured particles made from silicon oxide used according to an embodiment of the photocatalytic material of the present invention.

[0039] FIG. 4 represents a simplified diagram of an installation aimed at measuring the performance qualities of the photocatalytic material according to the invention.

[0040] FIG. 5 represents a graph quantifying the photocatalytic performance qualities of two examples of materials according to the invention, with the fraction by volume of semiconductor made of titanium oxide of the material according to the invention on the horizontal axis, which material comprises these semiconductor particles and structured particles made of silicon oxide, and the mass fraction by volume of semiconductor made of titanium oxide of the material according to the invention on the vertical axis, μmol / m 2 The total consumption of electrons over 20 hours per square meter is expressed as: DETAILED DESCRIPTION OF THE INVENTION

[0041] (Description of the embodiment) The present invention relates to the composition of a photocatalytic bed with mineral structured particles, in this case solid, calibrated according to the wavelength of the radiation emitted by the light source to activate the semiconductor material so that the radiation is largely and preferentially scattered in the direction of the radiation incident on the surface of these spheres by taking advantage of Mie scattering.

[0042] Therefore, FIG. 1 provides a simplified schematic representation of the aforementioned Mie scattering phenomenon: on the left, a light source S is symbolically represented, emitting radiation of a given wavelength λ. The diameter of spherical particle P1 is not calibrated according to the present invention and is less than 0.1λ. Spherical particle P1 re-emits the incident radiation fairly uniformly in all directions; this is Rayleigh scattering. On the other hand, particle P2 has a diameter calibrated to be between 0.1λ and 10λ, so that particle P2 re-emits radiation favorably along the direction of the incident radiation; this is Mie scattering. This is what the present invention uses, and as a result, the calibrated particle "guides" more radiation deep into the catalyst bed, facilitating its propagation and therefore better utilizing the semiconductor material.

[0043] The semiconductor material combined with these particles then experiences a surprising increase in its photocatalytic activity. This activity can be utilized in all known areas of photocatalysis of liquid and / or gaseous fluids. It can be the reduction of CO2, the photocatalytic production of H2 by photoconversion of water (also referred to as "water splitting"), or even the photocatalytic decontamination of air (conversion of VOCs) or water.

[0044] The invention will be illustrated below by non-limiting examples using different photocatalytic materials and different structured particles.

[0045] (Photocatalytic materials) Photocatalytic material a1. Photocatalytic material a1 is titanium oxide: it is TiO2 available from Aldrich under the trade name Aeroxide® P25, with a purity of 99.5%. The titanium oxide is in the form of fine particles. Its particle size, measured by transmission electron microscopy (TEM), is 21 nm. Its specific surface area, measured by the BET method, is 52 m 2 / g. BET is an abbreviation: it is the Brunauer-Emmett-Teller method as defined in S. Brunauer, PH Emmett and E. Teller, J. Am. Chem. Soc., 1938, 60(2), pp 309-319.

[0046] Crystallographically, this titanium oxide is in the form of a mixture of rutile and anatase.

[0047] FIG. 2 is an image obtained by TEM of these titanium oxide particles: it can be seen that they are of irregular shape and that they tend to agglomerate.

[0048] Photocatalytic material A2. Photocatalytic material A2 is titanium oxide doped with platinum metal particles, prepared by photo-evaporation in the following manner: 0.0712 g of HPtCl 6 6H O (37.5 wt. % metal) was introduced into 500 mL of distilled water. 50 mL of this solution was removed and placed in a jacketed glass reactor. 3 mL of methanol was then added, followed by 250 mg of a1-type TiO (Aeroxide® P25, Aldrich®, purity >99.5%), with stirring to form a suspension.

[0049] The mixture is then left under UV irradiation for 2 hours while stirring. The lamp used to provide UV radiation is a 125W HPK® mercury vapor lamp. The mixture is then centrifuged at 3000 rpm for 10 minutes to recover the solid. This is followed by two washing operations with water, each followed by centrifugation. Finally, the recovered powder is placed in an oven at 70°C for 24 hours.

[0050] This results in a photocatalytic material a2, whose Pt element content is measured to be 0.99 wt % by inductively coupled plasma-atomic emission spectroscopy (ICP-AES).

[0051] Photocatalytic material a3. Photocatalytic material a3 is a commercially available semiconductor based on WO3 (available from Sigma-Aldrich, exhibiting a particle size of less than 100 nm). The specific surface area is measured by the BET method and is 20 m 2 / g. The particle size of the photocatalytic material is 50±5nm as measured by X-ray diffraction (Debye-Scherrer method).

[0052] Photocatalytic material a4. Photocatalytic material a4 is a mixture of titanium oxide and copper oxide with platinum particles (Cu2O / Pt / TiO2). It is prepared by the following method: A solution of Cu(NO3)2 is prepared by dissolving 0.125 g of Cu(NO3)2·3H2O (Sigma-Aldrich®, 98%) in 50 mL of a 50 / 50 isopropanol / H2O mixture, resulting in a Cu2+ concentration of 10.4 mmol / L.

[0053] The following was introduced into the reactor: 0.20 g of photocatalytic material a2, 25 mL of distilled water, and finally 25 mL of isopropanol. The system was purged in the dark under a flow of argon (100 mL / min) for 2 hours. The reactor was thermostatically controlled at 25° C. throughout the synthesis.

[0054] The flow of argon is then reduced to 30 mL / min, and irradiation of the reaction mixture begins. The lamp used to provide UV radiation is a 125W HPK® mercury vapor lamp. 50 mL of copper nitrate solution is then added to the mixture. The mixture is left under irradiation with stirring for 10 hours. The mixture is then centrifuged at 3000 rpm for 10 minutes to recover the solid. Two washing operations with water are then performed, with centrifugation after each washing operation. Finally, the recovered powder is placed in an oven at 70°C for 24 hours.

[0055] Photocatalytic material a4, Cu2O / Pt / TiO2, is obtained here. The Cu element content is measured to be 2.2 wt% by ICP-AES. By XPS (X-ray Photoelectron Spectrometry), the copper oxide phase is 67% Cu2O and 33% CuO.

[0056] (Structured particles) Structured particles b1. The structured particles b1 selected in some of the following examples are spherical particles made of commercially available SiO2-based silicon oxide, which can be obtained from Alfa Aesar (CAS: 7631-86-9): they are beads with a purity of more than 99.9% and have an average diameter of 0.4 μm, as measured by laser particle size analysis.

[0057] FIG. 3 is an image obtained by SEM of these beads, which indeed shows that they are very uniform in their size and their shape.

[0058] Structured particles b2. The structured particles b2 chosen in other examples are particles made from commercially available SiO2-based silicon oxide, which can be obtained from Sigma-Aldrich under the commercial reference Davisil Grade 710, 10-14 μm: these are beads with a purity of more than 99%, the average size of which, measured by laser particle size analysis, is 12.7 μm (volume distribution).

[0059] The semiconductor particles a1 to a4 and the structuring particles b1 (SiO2 powder) or b2 (SiO2 powder with a particle size larger than that of b1) are mechanically mixed at a dilution rate varying between 0% and 75% by volume to obtain a homogeneous distribution of the two types of particles in the material. In the sense of the present invention, it is recalled that the "dilution rate" is equal to the ratio of the volume occupied by the structuring particles made from mineral material to the volume occupied by the sum of the semiconductor material(s) and the structuring particles.

[0060] Next, as shown in Figure 4, each sample (3) of the photocatalytic material of each example was tested for photocatalytic reduction of CO in the gas phase in the following manner: a continuously operated reactor (1) was used, in the cavity of which a fixed bed (2) was placed horizontally, containing a sintered material (4), on which the sample (3) was placed. The reactor (1) had a quartz optical window (5) on its upper wall, facing the sample (3). A UV-visible radiation source (6) was placed above the reactor, facing the window (5).

[0061] In operation, reactor (1) is fed via an inlet at the top with a stream (7) of gaseous CO, which has previously been bubbled through a vessel / saturator filled with water (8). Stream (7) passes through sample (3) and then exits via an outlet at the bottom in the form of stream (9), which is analyzed in-line by a gas analyzer of the micro gas chromatograph type (10).

[0062] The UV-visible radiation source (6) is a xenon lamp available from Asahi under the trade name MAX303.

[0063] The tests are carried out on samples (3) of an amount between 45 and 70 mg, the weight of which varies depending on the chosen dilution rate, while the thickness of the catalyst bed (2) and therefore of the sample (3) remains fixed and is equal to 0.3 mm.

[0064] The operating conditions are as follows: - Ambient temperature - Atmospheric pressure - CO2 flow rate (7) through the water saturator (8): 18 mL / h - Duration of test for each sample: 20h - Xenon lamp (6) irradiation output: 80W / m 2 The temperature is kept constant and measurements are taken in the wavelength range of 315 to 400 nm.

[0065] The target conversion of CO2 corresponds to the following reaction:

[0066] [ka]

[0067] Measurement of the photocatalytic performance quality of the samples is performed by microchromatography with a device (10), and the production of H, CH, and CO resulting from the reduction of CO and H2O is monitored by analysis every 6 minutes. Products of the reduction of CO2, such as CO, methane, and even ethane, are identified. The average photocatalytic activity is expressed in μmol of photogenerated electrons consumed by the reaction per square meter of illuminated catalyst surface area over the duration of the test.

[0068] (Example) All of the examples performed and their results are shown in Table 1 below.

[0069] [Table 1]

[0070] From this table it can be seen that the photocatalytic activity of the "mixed" material combining the semiconductor material according to the invention with structured particles is significantly higher than the photocatalytic activity of a material consisting only of the semiconductor material that is responsible for the photocatalytic activity of the material.

[0071] Comparing the results of Example 1 (comparative) and Example 2, it can be seen that with 25% less semiconductor material (Example 2), the photocatalytic activity jumps to 4.5 times. Starting with different semiconductors (materials a2, a3, a4), the "starting" photocatalytic activity is higher for materials made of 100% semiconductor, and the present invention can increase it by at least 4 times by combining it with structured particles: Example 9 therefore achieves an excellent level of photocatalytic activity.

[0072] Figure 5 shows the results of Examples 2 and 3 in graph form. The volume fraction of particles made from TiO2 is shown on the horizontal axis, and the total consumption of electrons per square meter over 20 hours is shown on the vertical axis. From this figure, it can be seen that Example 3 (diamonds in the graph), in which the size of structured particles b2 is too large, shows much worse results than Example 2 (circles in the graph), in which structured particles b1 are size-calibrated to favor Mie scattering.

[0073] This calibration of structured particles is simple to select and obtain, and is significantly easier than having to refine other parameters where the control of the macro- or microporosity of the material type is more complex.

[0074] It will be appreciated that the present invention is very flexible in its implementation: depending on the desired level of performance, on the item of equipment and on the reactor chosen, it will be possible to adapt the composition of the material according to the invention by varying the choice of materials, the dilution ratio and the way in which the mixing between the two materials will be carried out (mechanical mixing, chemical or physico-chemical combination, etc.). [Brief explanation of the drawings]

[0075] [Figure 1] 1 shows a schematic re-emission pattern of an incident beam on a particle due to Rayleigh-type and Mie-type scattering. [Figure 2] 1 shows a transmission electron microscopy (TEM) image of semiconductor particles made from titanium oxide used according to an embodiment of the photocatalytic material of the present invention. [Figure 3] 1 shows a scanning electron microscopy (SEM) image of structured particles made from silicon oxide used according to an embodiment of the photocatalytic material of the present invention. [Figure 4] 1 represents a simplified diagram of an installation aimed at measuring the performance qualities of photocatalytic materials according to the invention. [Figure 5] 1 shows a graph quantifying the photocatalytic performance qualities of two examples of materials according to the invention, with the fraction by volume of semiconductor made from titanium oxide of the material according to the invention on the horizontal axis and the total consumption of electrons over 20 hours per square meter, expressed in μmol / m2, on the vertical axis.

Claims

1. A catalyst bed comprising a particulate photocatalytic catalyst, said bed comprising structured particles b made of a mineral material, said structured particles being combined with at least one semiconductor material a having photocatalytic properties, said combination being characterized by: - mixing structured particles b made from mineral material with semiconductor material a in particle form, and / or - chemical or physicochemical deposition of a semiconductor material a on structured particles b made of mineral materials caused by, A catalyst bed, characterized in that the structured particles b are essentially spherical in shape and have a mean diameter of between 22 nm and 8.0 μm, preferably between 30 nm and 7.5 μm.

2. 2. The catalyst bed of claim 1 wherein all of the particles in the bed are randomly arranged.

3. 3. A catalyst bed according to claim 1 or 2, characterized in that, when the bed contains the semiconductor material a in the form of particles, said particles a exhibit an average size of at most 100 nm, in particular at most 50 nm and at least 5 nm, preferably between 10 and 30 nm.

4. Catalyst bed according to any one of claims 1 to 3, characterized in that it exhibits a porosity, which is equal to the ratio of the void volume in the photocatalytic bed to the total volume of the photocatalytic bed consisting of voids and particles: at least 40% and preferably at most 80%, in particular between 40% and 70%.

5. 5. A catalyst bed according to any one of claims 1 to 4, characterized in that it exhibits a "dilution factor", which is equal to the ratio of the volume occupied by the structured particles b made of mineral material to the volume occupied by the sum of the one or more semiconductor materials a, a' and the structured particles b made of mineral material, in particular in the case of chemical or physicochemical deposition of semiconductor materials a on the structured particles b made of mineral material: at most 80%, in particular between 5% and 70%, preferably between 10% and 50%.

6. 6. A catalyst bed according to any one of claims 1 to 5, comprising at least two different semiconducting materials, a first material a and a second material a', produced by: - mixing of structured particles b made of mineral material with one or more semiconductor materials in the form of particles of a first material a and particles of a second material a', respectively, and / or - chemical or physicochemical deposition of semiconductor materials a, a' on the carrier particle b; either deposition of both a first semiconductor material a and a second semiconductor material a' on the structured particle b, or deposition of a first semiconductor material a on a first portion of the structured particle b and deposition of a second semiconductor material a' on a second portion of the structured particle b.

7. 7. A catalytic bed according to claim 1, characterized in that the structured particles b made from mineral material are made from one or more metal oxides, in particular from oxides of metals of groups IIIa and IVa of the periodic table, preferably selected from aluminium oxide, silicon oxide, mixtures of aluminium and silicon oxides.

8. At least one of the semiconductor materials a and a' or the semiconductor materials a and a' contains at least one of the following metal oxides: titanium oxide, tungsten oxide, cerium oxide, bismuth oxide, zinc oxide, copper oxide, vanadium oxide, iron oxide, and cadmium oxide, and preferably TiO 2 , Bi 2 O 3 , CdO, Ce 2 O 3 , CeO 2 , CeAlO 3 ,CuO,Fe 2 O 3 , FeTiO 3 , ZnFe 2 O 3 , V 2 O 5 , ZnO, WO 3 and ZnFe 2 O 4 8. A catalyst bed according to claim 1, characterized in that it is selected, alone or as a mixture, from

9. 9. Catalytic bed according to any one of the preceding claims, characterized in that the semiconductor material a, a' or at least one of the semiconductor materials a, a' is doped with one or more ions chosen from metal ions, in particular the ions of V, Ni, Cr, Mo, Fe, Sn, Mn, Co, Re, Nb, Sb, La, Ce, Ta, Ti, or from non-metallic ions, in particular C, N, S, F, P, or from a mixture of metallic and non-metallic ions.

10. 10. A catalytic bed according to any one of the preceding claims, characterized in that the semiconductor material a, a' or at least one of the semiconductor materials a, a' also comprises one or more elements in the metallic state selected from the elements of groups IVb, Vb, VIb, VIIb, VIIIb, Ib, IIb, IIIa, IVa and Va of the Periodic Table of the Elements, in direct contact with said semiconductor material, preferably selected from platinum, palladium, gold, nickel, cobalt, ruthenium, silver, copper, rhenium or rhodium.

11. A method for obtaining a catalytic bed according to any one of claims 1 to 10, characterized in that the structured particles of said mineral material b, on the one hand, and the particles of said semiconductor material a, on the other hand, are mixed to produce a homogeneous distribution of the two types of particles in the bed.

12. A method for obtaining a catalytic bed according to any one of claims 1 to 10, characterized in that the deposition of the semiconductor material a, a' or at least one mineral material of the semiconductor material a, a' on the structured particles b is carried out by impregnating said structured particles with a solution of at least one precursor of the semiconductor material, by ion exchange or by an electrochemical route, in particular of the type using molten salts, followed by drying and optional calcination, by chemical vapour deposition, by spray drying or by atomic layer deposition.

13. A reactor (1) for the photocatalytic treatment of a feedstock in gaseous or liquid form, comprising at least one photocatalytic bed (2) according to any one of claims 1 to 10, mounted in said reactor in a fixed manner.

14. A method for the photocatalytic treatment of a feedstock (7) in gaseous and / or liquid form, characterized in that: - at least one photocatalytic bed (2) according to any one of claims 1 to 10 is arranged in a fixed manner in the reactor (1), - said feedstock (7) is contacted in a reactor with a catalyst bed (2), and The photocatalytic bed (2) is irradiated during the contacting operation by at least one radiation source (6) emitting in the UVA-A range and / or the UV-B range and / or the visible range, in particular in the wavelength range from 220 to 800 nm, preferably in the wavelength range from 300 to 750 nm.

15. 15. The method according to claim 14, wherein the photocatalytic treatment is as follows: - photo-oxidation of components present in liquid or gaseous feedstocks, specifically aimed at decontaminating / decontaminating said feedstocks, or - CO from the feedstock in liquid or gaseous form 2 photocatalytic reduction of -H 2 Photolysis of liquid or gaseous feed water to produce