Alkylmethylsiloxane immersion cooling medium
Patent Information
- Application Number
- JP2023524402
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-10-28
- Filing Date
- 2021-10-14
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-10-14
AI Technical Summary
Existing direct cooling fluids for data center equipment, such as fluorinated materials, mineral oils, PAO synthetic oils, and PDMS, face challenges including low boiling points, flammability, corrosion, swelling of rubber components, and compatibility issues, which limit their effectiveness and safety.
The use of alkylmethylsiloxanes as a cooling fluid with specific chemical structures and properties, including a flash point above 150°C, low viscosity, and compatibility with EPDM and silicone rubber, minimizing swelling and hydrogen gas production, addresses these challenges.
Alkylmethylsiloxanes provide efficient, safe, and reliable direct cooling by maintaining fluid integrity and preventing damage to electronic equipment, while ensuring environmental safety and compatibility with rubber components.
Smart Images

Figure 2022089214000001
Abstract
Description
Technical Field
[0001] The present invention relates to processes and systems using an immersion cooling fluid containing alkylmethylsiloxane.
[0002] Introduction As data center equipment becomes more powerful, the equipment generates more heat, which can thereby impede the life and performance of the data center equipment. To remove heat from the data center equipment, circulating air has been used. However, circulating air is not efficient enough to properly cool newer and more powerful equipment. More recently, heat transfer fluids that circulate within a closed path through the data center equipment have been used to remove heat from the equipment. This fluid does not come into direct contact with the equipment but rather flows through fluid conduits within the equipment. This is considered "indirect" fluid cooling of the equipment. The circulating enclosed fluid can be more efficient in heat removal than circulating air, but still is not as efficient as desired.
[0003] Very recently, "direct" fluid cooling of data center equipment has been introduced as a more efficient cooling means for data center equipment. Direct fluid cooling uses a fluid coolant that comes into direct contact with the data center equipment to cool the equipment. Typically, the equipment is often immersed in a fluid coolant that circulates around and through the equipment. This is an efficient means for cooling the equipment. However, there are challenges in directly contacting electronic equipment with a fluid. Direct fluid cooling is a special application that requires a rather special cooling fluid. Ideally, the cooling fluid is thermally conductive and also highly dielectric (i.e., a poor conductor). It is also important that the cooling fluid be compatible with the equipment it contacts, i.e., the cooling fluid should not degrade, change, or otherwise affect the equipment it contacts. Also, it is desirable that the fluid be environmentally safe, e.g., having low flammability and low toxicity.
[0004] Perhaps the most dominant fluids in the market for use as direct cooling fluids for data center equipment are fluorinated materials such as those sold under the names 3M(™) Fluorinert(™) Electronic Liquids and 3M(™) Novec(™) Engineered Fluids from 3M. "3M", "Fluorinert", and "Novec" are trademarks of 3M Company. These fluorinated materials tend to be efficient in heat removal. However, these fluorinated materials have relatively low boiling points (less than 200 degrees Celsius (°C), most less than 150 °C). The low boiling points of the fluorinated materials limit the application of the fluorinated materials to temperatures less than 175 °C according to the advertising literature of the fluorinated materials. The low boiling points also mean that the fluorinated materials evaporate relatively easily, which can result in the undesirable consequence of exposing workers and the environment to the fluorinated materials.
[0005] Mineral oil is another fluid that can be used as a direct cooling fluid for data center equipment. Mineral oil is desirable because it is inexpensive. However, mineral oil also has significant problems regarding direct cooling fluid applications. Mineral oil is only moderately efficient in heat removal and typically contains impurities such as sulfur, which can cause corrosion of data center equipment. Concerns regarding the flammability of mineral oil and the degradation of mineral oil over time have also been pointed out. Furthermore, mineral oil has a tendency to swell ethylene propylene diene monomer (EPDM) rubber, which can result in the failure of capacitors within a server and ultimately the server when used as a direct cooling fluid in contact with capacitors. Therefore, there is a risk of damaging electronic data center equipment exposed to mineral oil as a direct cooling fluid.
[0006] Polyalphaolefin (PAO) synthetic oils are yet another option for direct cooling fluids. While generally containing fewer impurities than mineral oils, PAO synthetic oils still present concerns regarding flammability and degradation over time. Like mineral oils, PAOs also tend to swell EPDM rubber, thus posing a risk of damage to electronic data center equipment exposed to PAO synthetic oils as a direct cooling fluid.
[0007] Polydimethylsiloxane (PDMS) is another option as a direct cooling fluid, offering a lower cost option, good compatibility with non-silicone components in data center equipment, relatively low flammability, and high stability against degradation compared to fluorinated fluids. However, PDMS tends to swell silicone rubber materials and weaken the peel adhesion strength of silicone rubber tacks, resulting in easier delamination of components bonded with silicone rubber. Silicone-based materials are often used in electronic devices as thermally conductive greases and gap fillers to thermally bond components. The swelling of these materials can lead to delamination of these materials from thermally bonded components, thereby reducing thermal bonding and heat transfer between thermally conductive components.
[0008] It is desirable to identify cooling fluids for special applications of direct cooling fluids for cooling electronic data center equipment. Cooling fluids should avoid the challenges associated with fluorinated fluids, mineral oils, PAO synthetic oils, and PDMS. In particular, it is desirable to identify direct cooling fluids having the following characteristics: It is a liquid at 25°C and a pressure of 101 kilopascals (760 millimercury pressure). • 100 square millimeters per second at 25°C (mm²) 2 Having a kinematic viscosity of less than / s, • Does not cause significant swelling of EPDM rubber or silicone rubber, nor does it penetrate them. • It has a flash point exceeding 150°C, • Does not need to contain halogens. [Overview of the project]
[0009] The present invention provides a direct contact (immersion) cooling process and system using a cooling fluid suitable for direct cooling applications, such as those involving electronic data center equipment. Remarkably, this fluid is (i) liquid at 25°C and a pressure of 101 kilopascals (kPa), and (ii) 100 mm at 25°C. 2 It has a kinematic viscosity of less than / s, (iii) does not significantly swell or penetrate EPDM rubber or silicone rubber, (iv) has a flash point above 150°C, and (v) does not necessarily have to contain halogens.
[0010] The cooling fluid of the present invention contains alkyl-modified PDMS ("alkylmethylsiloxane"). Concerns regarding alkylmethylsiloxane in direct cooling systems may include residual silyl hydride (SiH) and free hydrocarbon components. Residual SiH is undesirable because it tends to hydrolyze to silanol (SiOH) and release hydrogen gas. The generation of hydrogen gas in the presence of electronic components is an undesirable safety risk. The presence of silanol is a polar group that adversely affects the dielectric properties of siloxane, making siloxane inefficient as a direct cooling fluid. Free hydrocarbon components may cause phase clouding or even phase separation in the cooling fluid, potentially increasing swelling or imbibing of EPDM rubber. Remarkably, the alkylmethylsiloxane of the present invention not only achieves the fluid properties described in the previous paragraph, but also has an SiH concentration where the hydrogen of the SiH group is less than 10 parts per million by weight (ppm) based on the weight of the alkylmethylsiloxane, and a free hydrocarbon concentration of less than 20 percent by weight (wt%) based on the weight of the alkylmethylsiloxane.
[0011] In a first aspect, the present invention is a process comprising the step of immersing a device in a cooling fluid, the cooling fluid having the following average chemical structure (I): (CH3)3SiO-[(CH3)2)SiO] m -[R(CH3)SiO]n -Si(CH3)3(I) The formula comprises an alkyl-modified silicone oil having the following characteristics: in each occurrence, R is an alkyl or substituted alkyl group, the R group has 6 or more carbon atoms and 17 or fewer carbon atoms, the subscript m has a value of 1 or more and less than 22, the subscript n has a value of 1 or more, and the sum of m+n is greater than 5 and less than 50.
[0012] European Patent No. 0641849(B1) discloses the use of alkylmethylsiloxane fluids as heat transfer fluids. However, this reference does not mention any specific applications of direct cooling fluids, nor any benefits that direct cooling fluids offer in specific applications of direct cooling, with respect to PDMS or other direct cooling fluids. Furthermore, it has been found that not all alkylmethylsiloxane fluids, even those taught as heat transfer fluids in European Patent No. 0641849(B1), are suitable as direct cooling fluids. In particular, polydimethylsiloxanes having chemical structure (I) where R is a one-carbon alkyl group are unacceptable materials because they swell and penetrate silicone rubber. Short-chain alkyl groups of R are likely to function similarly to polydimethylsiloxanes. The examples herein show that when the R group has six or more carbon atoms, the examples are acceptable immersion cooling fluids.
[0013] In a second aspect, the present invention is an immersion cooling system comprising a device in a cooling fluid, wherein the cooling fluid has the following average chemical structure (I): (CH3)3SiO-[(CH3)2)SiO] m -[R(CH3)SiO] n -Si(CH3)3(I) The formula comprises an alkyl-modified silicone oil having the following characteristics: R is an alkyl or substituted alkyl having 6 or more carbon atoms and 17 or fewer carbon atoms in each occurrence, the subscript m has a value of 1 or more and less than 22, the subscript n has a value of 1 or more, and the sum of m+n is greater than 5 and less than 50. [Modes for carrying out the invention]
[0014] Unless a date is indicated along with the test method number, the test method refers to the test method most recent to the priority date of this document. References to test methods include both references to the testing association and the test method number. The following abbreviations and identifiers for test methods apply in this specification: ASTM refers to ASTM International methods, EN refers to European Norm, DIN refers to the German Institute for Standardization, ISO refers to the International Organization for Standardization, and UL refers to the Underwriters Laboratory.
[0015] Products identified by trade names refer to compositions available under those trade names as of the priority date of this document.
[0016] "Multiple" means two or more. "And / or" means "and, or alternatively." All ranges include the endpoint unless otherwise specified. Unless otherwise specified, all weight percentage (W%) values are relative to the weight of the composition, and all volume percentage (V%) values are relative to the volume of the composition.
[0017] The kinematic viscosity of individual polysiloxanes is measured according to ASTM D 445 using a glass capillary Cannon-Fenske viscometer at 25 degrees Celsius (°C), unless otherwise specified.
[0018] The flash point of the material is determined using a Cleveland Open Cup (COC). The COC measurement is performed on approximately 70 ml of the sample. The expected flash point is set to 100°C. The temperature is increased from 25°C to approximately 44°C at a rate of 14-17°C per minute, and then at a rate of 5-6°C per minute, until the flash point is determined.
[0019] Whether the fluid "significantly swells" or "significantly penetrates" the EPDM and silicone rubber is determined using the conformity test procedure described in the Examples section below.
[0020] The SiH concentration of the fluid is determined by combining 1.0 g of the sample material and 8.0 milligrams of pyrazine (as an internal standard) with 1.5 milliliters of deuterated chloroform to obtain a homogeneous solution. A portion of the solution is added to a 5 mm nuclear magnetic resonance (NMR) tube, and the 1H NMR spectrum is collected at 25°C using a Bruker AVANCE II 400 MHz NMR spectrometer with a zg pulse program, D1=15 seconds, and NS=32. The integrated intensity of the proton signal for SiH in the spectrum (a single peak from 4.65–4.78 ppm) provides the ratio of the number of hydrogen atoms on the Si atom to the pyrazine. The concentration of hydrogen on the silicon atoms can be calculated relative to the total weight of the sample material.
[0021] The free hydrocarbon concentration of the fluid is determined using gas-phase chromatography / mass spectrometry (GC / MS). Approximately 0.5 g of the fluid sample is diluted in approximately 4.5 g of toluene. The weight of the components is measured and recorded using a chemical balance. The diluted sample is analyzed by GC / MS using hydrocarbon standard chemicals, particularly those used as reactants in sample preparation, such as 1-hexene, 1-octene, 1-dodecene, and 1-tetradecene for calibration. An Agilent 7890A gas chromatography system equipped with a DB-5ms column (30 m x 0.25 mm inner diameter x 0.25 micrometer film), a constant helium carrier gas flow of 1.0 ml / min, oven parameters of 40°C, hold for 6 minutes, heating to 280°C at 15°C / min, hold for 10 minutes, for a total run time of 32.0 minutes, an autosampler system, and a 1 microliter sample were injected via a 10 microliter syringe with an inlet temperature of 280°C and a split ratio of 50:1. The detector was an MSD with an MS source temperature of 230°C, an MS quad temperature of 150°C, an Aux-2 temperature of 280°C, and an acquisition mode of scan mass 29-350.
[0022] "Alkyl" refers to a hydrocarbon group that can be derived from an alkane by removing a hydrogen atom. Alkyl groups can be linear or branched.
[0023] A "substituted alkyl" refers to a group similar to an alkyl group, except that one or more hydrogen atoms are replaced by non-hydrogen groups. For example, an alkyl group in which one or more hydrogen atoms are replaced by an aromatic group (such as phenyl or benzyl) or a halogen such as fluorine constitutes a substituted alkyl group.
[0024] In a first aspect, the present invention is a process comprising immersing a device in a cooling fluid. As used herein, “immersed” may mean partially submerging the device in the cooling fluid without completely submerging it, or preferably completely submerging the device in the cooling fluid. Similarly, “immerse,” “submerge,” and similar terms may mean less than complete submersion of the device, or complete submersion of the device.
[0025] In the broadest scope of the present invention, a device can be any article. Preferably, a device is a heat-generating article or a component fixed to a heat-generating article. For example, a device can be a heat sink fixed to (mounted on) a heat-generating article, a heat-generating article, or both a heat-generating article and a heat sink fixed to a heat-generating article. The present invention is particularly applicable to devices that are electronic devices. A device can be a computer or a part of a computer. In this specification, “computer” means an electronic device capable of storing, retrieving, and / or processing data. “Part of a computer” means any one of two or more components of a computer, or any combination thereof, and may include, for example, a power distribution component (such as an electronic transformer), a server having a circuit board on which multiple electronic components are mounted and which is located in a housing, the circuit board itself, an electronic random access memory component, a memory storage component, a central process unit (CPU), and a graphics processing unit, or any one of two or more components selected from these, or any combination thereof.
[0026] The cooling fluid may contain or consist of alkyl-modified silicone oil. Typically, the cooling fluid contains more than 50 weight percent (wt%) of alkyl-modified silicone oil, preferably 75 wt% or more, 90 wt% or more, 95 wt% or more, 98 wt% or more, and even 99 wt% or more, based on the weight of the cooling fluid. The cooling fluid may consist of alkyl-modified silicone oil.
[0027] Alkyl-modified silicone oil has the following average chemical structure (I): (CH3)3SiO-[(CH3)2)SiO] m -[R(CH3)SiO] n -Si(CH3)3(I) The formula has the following characteristics, where R is independently selected from alkyl groups and substituted alkyl groups in each occurrence, and the R group contains 6 or more, 7 or more, 8 or more, 9 or more, 10 or more, 11 or more, 12 or more, 13 or more, 14 or more, 15 or more, and even 16 or more, while simultaneously containing 17 or fewer, 16 or fewer, 15 or fewer, 14 or fewer, 13 or fewer, 12 or fewer, 11 or fewer, 10 or fewer, 9 or fewer, 8 or fewer, or even 7 or fewer carbon atoms, preferably R is selected from the group consisting of alkyl groups and substituted alkyl groups having the number of carbon atoms specified above, and the alkyl and substituents on the alkyl have a total number of carbon atoms within the range specified above. For example, the R group may be a phenyl-substituted alkyl, and the total number of carbon atoms is the sum of the number of alkyl carbon atoms and phenyl carbon atoms.
[0028] The subscript m has a value of 1 or more, can have a value of 2 or more, and can also have a value of 3 or more, and at the same time is typically less than 22, can be 20 or less, 15 or less, 10 or less, can be 9 or less, 8 or less, 7 or less, 6 or less, or even 5 or less.
[0029] The subscript n has a value of 1 or more, preferably 2 or more, 3 or more, 4 or more, and even 5 or more, while at the same time typically being less than 30, and may be 25 or less, 20 or less, 15 or less, 10 or less, 9 or less, 8 or less, 7 or less, or even 6 or less.
[0030] The sum of the subscripts m and n ("m+n") is a value of 5 or greater, and can be 6 or greater, 7 or greater, 8 or greater, 9 or greater, 10 or greater, 15 or greater, 20 or greater, and even 25 or greater, while at the same time having a value less than 50, and can be 40 or less, 30 or less, 25 or less, 20 or less, 15 or less, 10 or less, or even 9 or less.
[0031] by standard method1 H, 13 C, and 29 Using H, C, and Si nuclear magnetic resonance spectroscopy, determine the identity of the alkyl-modified silicone oil including the identity of the R group, as well as the values of m and n.
[0032] The alkyl-modified silicone oil has a kinematic viscosity of less than 100 millimeters squared per second (mm 2 / s, or centiStokes (cSt)), and can have a kinematic viscosity of 75 mm 2 / s or less, 50 mm 2 / s or less, preferably 30 mm 2 / s or less, more preferably 20 mm 2 / s or less, and can be 10 mm 2 / s or less, while at the same time, desirably, having a kinematic viscosity of more than 5 mm 2 / s. The selection of the R, m, and n values to achieve these ranges of kinematic viscosity is readily achievable.
[0033] It has been found that the R group in chemical structure (I) preferably has 6 or more carbon atoms. If R contains fewer than 6 carbon atoms, the alkyl-modified silicone oil is likely to have properties very similar to polydimethylsiloxane, which swells and penetrates silicone rubber. At the same time, it has been found that the R group in chemical structure (I) must have 17 or fewer carbon atoms, because if R has 18 or more carbon atoms, the material becomes a wax rather than a fluid at 25°C and a pressure of 101 kPa. The R group may be substituted or unsubstituted. For example, the R group may be halogenated (substituted with one or more halogens) or unhalogenated (halogen-free). Therefore, the alkyl-modified silicone oil may not contain halogens, and in fact, the cooling fluid as a whole may not contain halogens. The R group may be a phenyl-substituted alkyl group in which the alkyl component has fewer than 6 carbon atoms, but the total number of carbon atoms in the R group is 6, which is within the required range specified above. Alternatively, the R group may be an alkyl group having the required number of carbon atoms as specified above. The R group may be linear or branched. A branched structure may be desirable to lower the melting point of the alkyl-modified silicone oil.
[0034] Alkyl-modified silicone oil must have a subscript value of n that is 1 or 2 or more; otherwise, it is not an alkyl-modified silicone oil but rather polydimethylsiloxane.
[0035] The value of m+n is limited by the desire that the alkyl-modified silicone oil have a kinematic viscosity within the range described above.
[0036] Particularly preferred, the alkyl-modified silicone oil is selected from the group consisting of one or any combination of two or more alkyl-modified silicone oils having the chemical structure (I), wherein m is 3, n is 6, and R is a linear alkyl group having 6 to 16 carbon atoms; m is 5, n is 3, and R is a linear alkyl group having 10 carbon atoms; and m is 3, n is 4, and R is a 3-carbon alkyl group in which the central carbon is substituted with a phenyl group.
[0037] Alkyl-modified silicone oils can be synthesized by hydrosilylation reactions as described in the Examples section below.
[0038] The cooling fluid may include, or consist of, two or more alkyl-modified silicone oils, or even more specifically, two or more combinations of alkyl-modified silicone oils. Alternatively, the cooling fluid may include, or consist of, a mixture of alkyl-modified silicone oil and one or more additional fluids that satisfy the requirements of an immersion cooling fluid. For example, the cooling fluid may include alkyl-modified silicone oil and a fluorocarbon fluid, provided that the fluorocarbon fluid has a boiling point greater than 150°C.
[0039] Preferably, the cooling fluid contains less than 20 weight percent (wt%), preferably 10 wt% or less, 5 wt% or less, or 1 wt% or less of free hydrocarbons, and may not contain free hydrocarbons, where the wt% of hydrocarbons is relative to the weight of the alkyl-modified silicone oil. "Free hydrocarbons" refers to hydrocarbons that are not chemically bonded to non-hydrocarbon components (for example, alkyls on a siloxane molecule are not "free hydrocarbons," but hexane or 1-hexene would be "free hydrocarbons"). It is desirable to minimize free hydrocarbons because they may contribute to the swelling of organic materials such as EPDM rubber. Free hydrocarbons may also lower the flash point of the composition.
[0040] Preferably, the alkyl-modified silicone oil contains a minimal amount of SiH functional groups, if present. The degree of SiH functional groups is determined by measuring the weight percentage of H from the SiH functional groups relative to the weight of the alkyl-modified silicone oil. The weight percentage of H is preferably less than 10 parts per million (ppm), more preferably 9 ppm or less, 9 ppm or less, 7 ppm or less, 6 ppm or less, 6 ppm or less, 5 ppm or less, 4 ppm or less, 3 ppm or less, 2 ppm or less, or 1 ppm or less, where ppm is relative to the weight of the alkyl-modified silicone oil. The alkyl-modified silicone oil may not contain SiH functional groups at all.
[0041] The cooling fluid may contain any one or any combination of two or more optional components, such as antioxidants. Antioxidants, particularly alkyl group stabilizing antioxidants, may be desirable to increase the thermal stability of the cooling fluid. Suitable antioxidants are typically aromatic amines and / or hindered phenols. Examples of suitable antioxidants include those available under the trade names IRGANOX® 1076 and IRGANOX® 1010. IRGANOX is a trademark of BASF SE.
[0042] The process of the present invention comprises immersing a device in a cooling fluid containing or consisting of an alkyl-modified silicone oil, and may further comprise one or more additional steps. For example, the process may comprise cooling the cooling fluid (alkyl-modified silicone oil). For example, the cooling fluid may remain stationary in the container while the container cools the cooling fluid, with the device immersed in the cooling fluid. The cooling fluid may be circulated around the device immersed in the cooling fluid in the container (circulating bath), and the container cools the cooling fluid. The cooling fluid may be cooled in a separate cooling unit and circulated between the cooling unit and the container, where the device immersed in the cooling fluid is present such that the cooling fluid circulates around the device through the cooling unit during the cycle and then returns around the device.
[0043] In another embodiment, the present invention is an immersion cooling system. In this context, “system” means a set of components that are related to one another in a manner that achieves a particular purpose. In the present invention, the immersion cooling system comprises components that serve to achieve immersion cooling of a device that is immersed in a cooling fluid.
[0044] Various immersion cooling systems of different complexities are known in the industry, and the present invention encompasses any immersion cooling system, to the broadest extent.
[0045] The system of the present invention comprises a device in a cooling fluid, the cooling fluid comprising or consisting of an alkyl-modified silicone oil as described herein. The device is one of those described herein.
[0046] The system may further comprise a cooler that removes heat from the cooling fluid. The cooler may be a refrigerated container in which the cooling fluid exists to form a cooling bath in which the device is immersed. The system may further comprise a circulating component that causes the cooling fluid to flow around the device immersed in the cooling fluid. The circulating component may be an impeller submerged in the cooling fluid that causes a flow of fluid around the immersed device while the fluid and the device are in a single container, which may or may not be a cooler. Alternatively or additionally, the circulating component may be a circulating pump or other circulating component that flows the cooling fluid between the container containing the cooling fluid and the device immersed in the cooling fluid and another container or device that cools the cooling fluid during the cycle.
[0047] In particular, the cooling fluid preferably comes into direct contact with the device immersed in the cooling fluid in both the process and the system of the present invention. [Examples]
[0048] Table 1 lists the materials to be used in the following examples. DOWSIL, XIAMETER, and NORDEL are trademarks of The Dow Chemical Company. SpectraSyn is a trademark of Exxon Mobil Corporation. Ultra-S is a trademark of S-Oil Corporation.
[0049] [Table 1]
[0050] SiH siloxane and synthesis method SiH siloxane 1: (CH3)3SiO[H(CH3)SiO]1Si(CH3)3 It is prepared by equilibrating 70% by weight of hexamethyldisiloxane and 30% by weight of trimethylsiloxy-terminated methylhydrogen polysiloxane 2 with trifluoromethanesulfonic acid, as described in U.S. Patent Application Publication No. 2006 / 0264602(A1) and the documents cited therein.
[0051] SiH siloxane 2: (CH3)3SiO[(CH3)2Si)]3[H(CH3)SiO]5Si(CH3)3 It is prepared by equilibrating 14.9 wt% hexamethyldisiloxane, 62.9 wt% octamethylcyclotetrasiloxane, and 22.2 wt% trimethylsiloxy-terminated methylhydrogen polysiloxane 2 with a trifluoromethanesulfonic acid catalyst, as described in U.S. Patent Application Publication No. 2006 / 0264602(A1) and the documents cited therein.
[0052] SiH siloxane 3: (CH3)3SiO[H(CH3)SiO] 17 Si(CH3)3 It is prepared by equilibrating 10.11 wt% hexamethyldisiloxane and 89.89 wt% trimethylsiloxy-terminated methylhydrogen polysiloxane 2 with a trifluoromethanesulfonic acid catalyst, as described in U.S. Patent Application Publication No. 2006 / 0264602(A1) and the documents cited therein.
[0053] SiH siloxane 4: (CH3)3SiO[(CH3)2Si)]3[H(CH3)SiO]6Si(CH3)3 It is prepared by equilibrating 18.8 wt% hexamethyldisiloxane, 31.9 wt% octamethylcyclotetrasiloxane, and 49.3 wt% trimethylsiloxy-terminated methylhydrogen polysiloxane 2 with trifluoromethanesulfonic acid, as described in U.S. Patent Application Publication No. 2006 / 0264602(A1) and the documents cited therein.
[0054] SiH siloxane 5: (CH3)3SiO[(CH3)2Si)] 22 [H(CH3)SiO]2Si(CH3)3 It is prepared by equilibrating 8.26 wt% hexamethyldisiloxane, 84.91 wt% octamethylcyclotetrasiloxane, and 6.83 wt% trimethylsiloxy-terminated methylhydrogen polysiloxane 2 with trifluoromethanesulfonic acid, as described in U.S. Patent Application Publication No. 2006 / 0264602(A1) and the documents cited therein.
[0055] SiH siloxane 6: (CH3)3SiO[(CH3)2Si)] 16 [H(CH3)SiO] 38 Si(CH3)3 It is prepared by equilibrating 1.81 wt% hexamethyldisiloxane, 32.41 wt% octamethylcyclotetrasiloxane, and 65.78 wt% trimethylsiloxy-terminated methylhydrogen polysiloxane 2 with trifluoromethanesulfonic acid, as described in U.S. Patent Application Publication No. 2006 / 0264602(A1) and the documents cited therein.
[0056] SiH siloxane 7: (CH3)3SiO[(CH3)2Si)] 35 [H(CH3)SiO] 35 Si(CH3)3 It is prepared by equilibrating 7.11 wt% polydimethylsiloxane fluid (available from The Dow Chemical Company as DOWSIL® SH 200 fluid 10 cSt), 47.15 wt% octamethylcyclotetrasiloxane, and 45.74 wt% trimethylsiloxy-terminated methylhydrogen polysiloxane 1 with a trifluoromethanesulfonic acid catalyst, as described in U.S. Patent Application Publication No. 2006 / 0264602(A1) and the documents cited therein.
[0057] SiH siloxane 8: (CH3)3SiO[(CH3)2Si)] 25 [H(CH3)SiO] 55 Si(CH3)3 It is prepared by equilibration of 34.25 wt% of a dimethylsiloxane cyclic compound (available from The Dow Chemical Company as DOWSIL® 344 Fluid) and 64.75 wt% of trimethylsiloxy-terminated methylhydrogen polysiloxane 1 with a trifluoromethanesulfonic acid catalyst, as described in U.S. Patent Application Publication No. 2006 / 0264602(A1) and the documents cited therein.
[0058] SiH siloxane 9: (CH3)3SiO[(CH3)2Si)] 84 [H(CH3)SiO] 14 Si(CH3)3 It is prepared by equilibrating 1.76 wt% hexamethyldisiloxane, 85.8 wt% octamethylcyclotetrasiloxane, and 12.44 wt% trimethylsiloxy-terminated methylhydrogen polysiloxane 1 with trifluoromethanesulfonic acid, as described in U.S. Patent Application Publication No. 2006 / 0264602(A1) and the documents cited therein.
[0059] SiH siloxane 10: (CH3)3SiO[(CH3)2Si)]3[H(CH3)SiO]3Si(CH3)3 It is prepared by equilibrating 25.13 wt% hexamethyldisiloxane, 36.63 wt% octamethylcyclotetrasiloxane, and 38.24 wt% trimethylsiloxy-terminated methylhydrogen polysiloxane 1 with trifluoromethanesulfonic acid, as described in U.S. Patent Application Publication No. 2006 / 0264602(A1) and the documents cited therein.
[0060] Alkylmethylsiloxane sample Sample 1: (CH3)3SiO[(CH3)2Si)]3[(C6H 13 )(CH3)SiO]6Si(CH3)3 In a three-necked round-bottom flask, 246.2 grams (g) of 1-hexene and 78.5 milligrams (mg) of Pt-47D catalyst are added at 25°C under nitrogen purge. While stirring, 300.0 g of SiH siloxane 4 is added dropwise at 70°C, controlling the addition to maintain the temperature in the range of 70-80°C. After the addition is complete, stirring is continued for 4 hours. The resulting mixture is distilled to remove residual 1-hexene. The remaining material is Sample 1.
[0061] Sample 2: (CH3)3SiO[(CH3)2Si)]3[(C8H 17 )(CH3)SiO]6Si(CH3)3 In a three-necked round-bottom flask, 328.25 g of 1-octene and 78.5 mg of Pt-47D catalyst are added at 25°C under nitrogen purge. While stirring, 300.0 g of SiH siloxane 4 is added dropwise at 70°C, controlling the addition to maintain the temperature in the range of 70-80°C. After the addition is complete, stirring is continued for 4 hours. The resulting mixture is distilled to remove residual 1-octene. The remaining material is Sample 2.
[0062] Sample 3: (CH3)3SiO[(CH3)2Si)]3[(C 12 H 25 )(CH3)SiO]6Si(CH3)3 In a three-necked round-bottom flask, 492.7 g of 1-dodecene and 78.5 mg of Pt-47D catalyst are added at 25°C under nitrogen purge. While stirring, 300.0 g of SiH siloxane 4 is added dropwise at 70°C, controlling the addition to maintain the temperature in the range of 70-80°C. After the addition is complete, stirring is continued for 4 hours. The reaction product is washed three times with 100 ml (mL) of petroleum ether to remove residual 1-dodecene. Next, the resulting mixture is distilled to remove residual petroleum ether. The remaining material is Sample 3.
[0063] Sample 4: (CH3)3SiO[(CH3)2Si)]3[(C 14 H 29 )(CH3)SiO]6Si(CH3)3 In a three-necked round-bottom flask, 574.4 g of 1-tetradecene and 78.5 mg of Pt-47D catalyst are added at 25°C under nitrogen purge. While stirring, 300.0 g of SiH siloxane 4 is added dropwise at 70°C, controlling the addition to maintain the temperature in the range of 70-80°C. After the addition is complete, stirring is continued for 4 hours. The reaction product is washed three times with 100 mL of petroleum ether to remove residual 1-tetradecene. Next, the resulting mixture is distilled to remove residual petroleum ether. The remaining material is Sample 4.
[0064] Sample 5: (CH3)3SiO[(CH3)2Si)]3[(C 16 H 33 )(CH3)SiO]6Si(CH3)3 In a three-necked round-bottom flask, 657.0 g of 1-hexadecene and 78.5 mg of Pt-47D catalyst are added at 25°C under nitrogen purge. While stirring, 300.0 g of SiH siloxane 4 is added dropwise at 70°C, controlling the addition to maintain the temperature in the range of 70-80°C. After the addition is complete, stirring is continued for 4 hours. The resulting material is Sample 5.
[0065] Sample 5 has a boiling point above 250°C and a 45mm diameter at 25°C. 2 It has a kinematic viscosity of / s, a melting point of 15-20°C, a flash point above 200°C, a saturation water absorption rate of less than 300 parts by weight per 1 million parts by weight of the sample fluid, is colorless and transparent, has a low toxicity risk, a global warming potential of 0 (or approximately 0), and an ozone depletion potential of 0 (or approximately 0), showing only very slight signs of degradation during use.
[0066] Sample 6: (CH3)3SiO[(CH3)2Si)]3[(C 18 H 37 )(CH3)SiO]6Si(CH3)3 369.3 g of 1-octadecene and 65.0 mg of Pt-47D catalyst are added to a three-necked round-bottom flask at 25°C under nitrogen purge. 150.0 g of SiH siloxane 1 is added dropwise at 70°C while stirring, controlling the addition to maintain the temperature in the range of 70-80°C. After the addition is complete, stirring is continued for 4 hours. The resulting product is wax at 25°C and is therefore unsuitable as a cooling fluid. This demonstrates that the R group in chemical structure (I) must contain fewer than 18 carbon atoms.
[0067] Sample 7: (CH3)3SiO[(CH3)2Si)] 22 [(C8H 17 )(CH3)SiO]2Si(CH3)3 In a three-necked round-bottom flask, 44.3 g of 1-octene and 78.5 mg of Pt-47D catalyst are added at 25°C under nitrogen purge. While stirring, 300.0 g of SiH siloxane 5 is added dropwise at 70°C, controlling the addition to maintain the temperature in the range of 70-80°C. After the addition is complete, stirring is continued for 4 hours. The resulting product is distilled to reduce the residual 1-octene to less than 2% by weight of the product composition.
[0068] Sample 8: (CH3)3SiO[(CH3)2Si)]3[(C6H 13 )(CH3)SiO] 4.5 [(C 14 H 29 )(CH3)SiO] 1.5 Si(CH3)3 In a three-necked round-bottom flask, 114.9 g of 1-tetradecene and 78.5 mg of Pt-47D catalyst are added at 25°C under nitrogen purge. While stirring, 300.0 g of SiH siloxane 4 is added dropwise at 70°C, controlling the addition to maintain the temperature in the range of 70-80°C. After the addition is complete, stirring is continued for 2 hours. Next, 196.9 g of 1-hexene is added dropwise to the flask at 60°C under nitrogen purge, and after the addition is complete, the solution is maintained at 70°C for 2 hours. The resulting mixture is distilled to remove residual 1-hexene. The remaining material is Sample 8.
[0069] Sample 9: (CH3)3SiO[(CH3)2Si)]3[(C6H 13 )(CH3)SiO]3[(C 14 H 29 )(CH3)SiO]3Si(CH3)3 In a three-necked round-bottom flask, 229.8 g of 1-tetradecene and 78.5 mg of Pt-47D catalyst are added at 25°C under nitrogen gas purging. While stirring, 300.0 g of SiH siloxane 4 is added dropwise at 70°C, controlling the addition to maintain the temperature in the range of 70-80°C. After the addition is complete, stirring is continued for 2 hours. Next, 147.7 g of 1-hexene is added dropwise to the flask at 60°C under nitrogen purging, and after the addition is complete, the solution is maintained at 70°C for 2 hours. The resulting mixture is distilled to remove residual 1-hexene. The remaining material is sample 9.
[0070] Sample 10: (CH3)3SiO[(CH3)2Si)]3[(C6H 13 )(CH3)SiO] 1.5 [(C 14 H 29 )(CH3)SiO] 4.5 Si(CH3)3 In a three-necked round-bottom flask, 344.6 g of 1-tetradecene and 78.5 mg of Pt-47D catalyst are added at 25°C under nitrogen purge. While stirring, 300.0 g of SiH siloxane 4 is added dropwise at 70°C, controlling the addition to maintain the temperature in the range of 70-80°C. After the addition is complete, stirring is continued for 2 hours. Next, 98.5 g of 1-hexene is added dropwise to the flask at 60°C under nitrogen purge, and after the addition is complete, the solution is maintained at 70°C for 2 hours. The resulting mixture is distilled to remove residual 1-hexene. The remaining material is Sample 10.
[0071] Sample 11: (CH3)3SiO[(CH3)2Si)]3[(C8H 17 )(CH3)SiO]3[(C 14 H 29 )(CH3)SiO]3Si(CH3)3 In a three-necked round-bottom flask, 344.7 g of 1-tetradecene and 78.5 mg of Pt-47D catalyst are added at 25°C under nitrogen gas purge. While stirring, 300.0 g of SiH siloxane 4 is added dropwise at 70°C, controlling the addition to maintain the temperature in the range of 70-80°C. After the addition is complete, stirring is continued for 2 hours. Next, 131.3 g of 1-octene is added dropwise to the flask at 60°C under nitrogen purge, and after the addition is complete, the solution is maintained at 70°C for 2 hours. The resulting mixture is distilled to remove residual 1-octene. The remaining material is Sample 11.
[0072] Sample 12: (CH3)3SiO[(CH3)2Si)]3[(C 10 H 21 )(CH3)SiO]5Si(CH3)3 In a three-necked round-bottom flask, 410.6 g of 1-decene and 78.5 mg of Pt-47D catalyst are added at 25°C under nitrogen purge. While stirring, 300.0 g of SiH siloxane 10 is added dropwise at 70°C, controlling the addition to maintain the temperature in the range of 70-80°C. After the addition is complete, stirring is continued for 4 hours. The reaction product is washed three times with 100 ml (mL) of petroleum ether to remove residual 1-decene. Next, the resulting mixture is distilled to remove residual petroleum ether. The remaining material is Sample 12.
[0073] Sample 13: (CH3)3SiO[(CH3)2Si)] 16 [(C6H 13 )(CH3)SiO] 38 Si(CH3)3 In a three-necked round-bottom flask, 100.0 g of 1-hexene and 36.0 mg of Pt-47D catalyst are added at 25°C under nitrogen purge. While stirring, 100 g of SiH siloxane 6 is added dropwise at 70°C, controlling the addition to maintain the temperature in the range of 70-80°C. After the addition is complete, stirring is continued for 4 hours. The resulting mixture is distilled to remove residual 1-hexene. The remaining material is Sample 13.
[0074] Sample 14: (CH3)3SiO[(CH3)2Si)]35 [(C8H 17 )(CH3)SiO] 35 Si(CH3)3 In a three-necked round-bottom flask, 109.4 g of 1-octene and 36.0 mg of Pt-47D catalyst are added at 25°C under nitrogen purge. While stirring, 100 g of SiH siloxane 7 is added dropwise at 70°C, controlling the addition to maintain the temperature in the range of 70-80°C. After the addition is complete, stirring is continued for 4 hours. The resulting mixture is distilled to remove residual 1-octene. The remaining material is Sample 14.
[0075] Sample 15: (CH3)3SiO[(CH3)2Si)] 25 [(C8H 17 )(CH3)SiO] 55 Si(CH3)3 280.0 g of SiH siloxane 8 and 110 mg of Pt-47D catalyst are added to a 1000 ml three-necked round-bottom flask equipped with a reflux condenser, stirring rod, thermometer, and addition funnel. 486.0 g of 1-octene is added dropwise while stirring under nitrogen purging, maintaining the temperature in the range of 70-90°C. After the addition is complete, stirring is continued at 80°C for 4 hours. The reaction product is stripped under vacuum at 150°C for 3 hours to remove excess 1-octene, its isomers, and low-volatility cyclic siloxanes. The resulting product is filtered through a Zeta-Plus filter to obtain sample 15.
[0076] Sample 16: (CH3)3SiO[(CH3)2Si)] 84 [(C8H 17 )(CH3)SiO] 14 Si(CH3)3 546.0 g of SiH siloxane 9 and 110 mg of Pt-47D catalyst are added to a 1000 ml three-necked round-bottom flask equipped with a reflux condenser, stirring rod, thermometer, and addition funnel. 180.0 g of 1-octene is added dropwise while stirring under nitrogen purge and maintaining the temperature in the range of 70-90°C. After the addition is complete, stirring is continued at 80°C for 4 hours. The reaction product is stripped under vacuum at 150°C for 3 hours to remove excess 1-octene, its isomers, and low-volatility cyclic siloxanes. The resulting product is filtered through a Zeta-Plus filter to obtain sample 16.
[0077] Sample 17: (CH3)3SiO[(CH3)2Si)]3[(CH2C(CH)3-Ph)(CH3)SiO]3Si(CH3)3 351.0 g of SiH siloxane 10 and 110 mg of Pt-47D catalyst are added to a 1000 ml three-necked round-bottom flask equipped with a reflux condenser, stirring rod, thermometer, and addition funnel. 299.0 g of α-methylstyrene is added dropwise while stirring under nitrogen purge and maintaining the temperature in the range of 70-90°C. After the addition is complete, stirring is continued at 80°C for 4 hours. Another 135.0 g of α-methylstyrene and 330 mg of Pt-47D catalyst are added to the reaction mixture while maintaining the temperature at 80°C for 4 hours. Excess α-methylstyrene and low-volatility cyclic siloxane are removed by stripping at 150°C for 3 hours under vacuum. The mixture is filtered through a Zeta-Plus filter to obtain sample 17.
[0078] Sample 18: 80 / 20 weight blend of Sample 1 and Sample 13 160g of sample 1 was mixed with 40g of sample 13 using a magnetic stirring rod for 30 minutes to obtain a clear fluid, which is sample 18.
[0079] Sample 19: 80 / 20 weight blend of Sample 2 and Sample 14 160g of sample 2 was mixed with 40g of sample 14 using a magnetic stirring bar for 30 minutes to obtain a clear fluid, which is sample 19.
[0080] Sample 20: (CH3)3SiO[(C8H 17 )(CH3)SiO]8Si(CH3)3 Note: m=0 and n=8 In a three-necked round-bottom flask, 175.0 g of 1-octene and 36.0 mg of Pt-47D catalyst are added at 25°C under nitrogen purge. While stirring, 100.0 g of SiH siloxane 3 is added dropwise at 70°C, controlling the addition to maintain the temperature in the range of 70-80°C. After the addition is complete, stirring is continued for 4 hours. The resulting mixture is distilled to remove residual 1-octene. The remaining material is sample 20.
[0081] Sample 21: (CH3)3SiO[(C 14 H 29 )(CH3)SiO]8Si(CH3)3 Note: m=0 and n=8 In a three-necked round-bottom flask, 153.0 g of 1-tetradecene and 18.0 mg of Pt-47D catalyst are added at 25°C under nitrogen purge. While stirring, 50.0 g of SiH siloxane 3 is added dropwise at 70°C, controlling the addition to maintain the temperature in the range of 70-80°C. After the addition is complete, stirring is continued for 4 hours. The remaining material is sample 21.
[0082] Sample 22: (CH3)3SiO(C8H 17 )(CH3)SiOSi(CH3)3 Note: m=0 and n=1 This material is commercially available from Gelest as TM-081.
[0083] Characterization of the sample Using the procedure described above, each of the 19 samples is characterized for viscosity, flash point, SiH residue, and hydrocarbon residue. The compatibility of the samples with silicone rubber and EPDM rubber is further characterized while the samples are in a liquid state at 25°C, and using the following compatibility test procedure. The results of the sample characterization are shown in Table 3 below.
[0084] Conformity test. Cut test specimens of EPDM rubber and silicone rubber, each measuring 5 cm in length, 0.5 cm in width, and 2 mm in thickness. Record the initial length and initial weight of each sample material. Completely immerse the test specimen in one of the fluids in a container. Seal the container and heat to 50°C. Store the container at 50°C for 4 months, then remove the specimen and place absorbent paper on both sides of the specimen to absorb and dry. Record the length and weight of the specimen. Determine the change in length and weight relative to before immersion. An increase in length of more than 15% (final length more than 115% of the initial length) constitutes "significant swelling". An increase in weight of more than 50% (final weight more than 150% of the initial weight) constitutes "significant swelling". Significant swelling and / or significant swelling will result in failure of the conformity test.
[0085] For comparison, reference fluids polyalphaolefin, mineral oil, polydimethylsiloxane (PDMS), and fluorocarbon fluid 1 are also characterized in suitability tests with the following results in Table 2.
[0086] [Table 2]
[0087] Overall, both mineral oil and PAO oil failed due to significant swelling of EPDM, and PDMS failed due to both significant swelling and penetration of silicone rubber.
[0088] Table 3 provides the characterization results for samples 1 to 22. To receive an overall passing grade, each sample must meet all characterization requirements. • Fluid at 25℃ = Yes Viscosity at 25°C = 100 mm 2 / s less than ·Flash point over 150℃ • SiH residue less than 10 ppm • Hydrocarbon residue less than 20% by weight • Conformity testing = Passed for both silicone rubber and EPDM rubber.
[0089] The following samples will fail the overall assessment.
[0090] Sample 6: This sample is a wax at 25°C and demonstrates that the R group in chemical structure (I) must contain fewer than 18 carbon atoms.
[0091] Sample 7: This sample demonstrates that m should be less than 22.
[0092] Samples 13-16: These samples demonstrate that the viscosity becomes too high when the sum of the subscripts m and n (i.e., "m+n") exceeds 54.
[0093] Samples 20-22: These samples demonstrate that m must be greater than 0.
[0094] [Table 3] * NT = Not tested. If a sample fails one parameter before other parameters are tested, further testing is not necessary. The '#' symbol indicates a failing test characteristic.
Claims
1. A process comprising the step of immersing a device in a cooling fluid, the cooling fluid having the following average chemical structure (I): (CH 3 ) 3 SiO-[(CH 3 ) 2 ) SiO m -[R(CH 3 ) SiO n -Si(CH 3 ) 3 (I) wherein R, in each occurrence, is independently selected from the group consisting of alkyl groups and substituted alkyl groups, each R group having 6 or more and simultaneously 17 or less carbon atoms, subscript m has a value equal to or greater than 1 and simultaneously less than 22, subscript n has a value equal to or greater than 1, and the sum of m+n is greater than 5 and simultaneously less than 50.
2. The process of claim 1 , wherein the device is a heat generating device and / or a heat sink affixed to a heat generating device.
3. 3. The process of claim 1 or 2, wherein the R group in structure (I) is alkyl or phenyl substituted alkyl.
4. The process of any one of claims 1 to 3, wherein the quench fluid comprises less than 20 weight percent hydrocarbons, based on the quench fluid weight.
5. The process of any one of claims 1 to 4, wherein the process further comprises the step of cooling the cooling fluid.
6. 6. The process of claim 5, wherein the cooling fluid is circulated through a cooling unit, around the device, and then back around the device in cycles.
7. 1. An immersion cooling system comprising a device in a cooling fluid, the cooling fluid having the following average chemical structure (I): (CH 3 ) 3SiO-[(CH 3 ) 2 ) SiO m -[R(CH 3 ) SiO n -Si(CH 3 ) 3 (I) wherein R, in each occurrence, is independently selected from the group consisting of alkyl groups and substituted alkyl groups, each R group having 6 or more and simultaneously 17 or less carbon atoms, subscript m has a value greater than or equal to 1 and simultaneously less than 22, subscript n has a value greater than or equal to 1, and the sum of m+n is greater than 5 and simultaneously less than 50.
8. The immersion cooling system according to claim 7 , wherein the device is a heat-generating device and / or a heat sink fixed to the heat-generating device.
9. The immersion cooling system of any one of claims 7 to 8, wherein the system further comprises a chiller that removes heat from the cooling fluid.
10. 10. The immersion cooling system of claim 7, further comprising a circulation component for causing a flow of cooling fluid around the device immersed in the cooling fluid.