Composite particle, conductive paste, and electronic component
Composite particles with controlled large and small particle sizes address the issue of cracks and discontinuities in ceramic electronic components by enhancing thermal contraction start temperature and coverage, improving the performance of electrode layers.
Patent Information
- Application Number
- JP2023043143
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-17
- Publication Date
- 2024-10-01
AI Technical Summary
The challenge in ceramic electronic components is the occurrence of cracks and discontinuities in thinner internal electrode layers due to differences in sintering start temperatures between ceramic layers and internal electrode layers, and the use of conventional composite particles fails to ensure sufficient coverage and heat shrinkage properties.
The development of composite particles with large particles having a specific size range and small particles attached to their surfaces, where the small particles create steric hindrance to increase the thermal contraction start temperature, and the use of a conductive paste containing these particles to form electrode layers.
This solution enhances the coverage and heat shrinkage properties of electrode layers, reducing cracks and discontinuities, and improves the overall performance of ceramic electronic components by maintaining a higher thermal contraction start temperature.
Smart Images

Figure 2024132401000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an electronic component having an electrode layer, and to composite particles and a conductive paste used in forming the electrode layer of the electronic component. [Background technology]
[0002] In ceramic electronic components such as multilayer ceramic capacitors, the ceramic layers and internal electrode layers are becoming thinner in response to the demand for smaller size and larger capacity. However, when the internal electrode layers are made thinner, cracks and discontinuities may occur in the internal electrode layers after sintering due to the difference in sintering start temperature between the ceramic layers and the internal electrode layers, and the coverage rate of the internal electrode layers with respect to the ceramic layers may decrease.
[0003] As a measure to reduce the difference in sintering start temperature, a method of forming an internal electrode layer using a conductive paste to which ceramic common material powder has been added has been proposed (for example, Patent Document 1). By adding ceramic common material powder to the conductive paste, it is expected that the effect of delaying the sintering of the internal electrode layer (sintering delay effect) can be achieved. However, in such conductive paste, the ceramic common material powder is prone to agglomeration, and the metal components become spherical during the process of sintering the internal electrode layer, so that a sufficient sintering delay effect may not be obtained. In addition, the ceramic common material powder may diffuse into the ceramic layer and affect the composition of the ceramic layer.
[0004] In addition to the above measures, a method has been proposed in which composite particles, in which minute ceramic particles are fixed to the surface of metal particles, are used as the raw powder of the conductive paste (for example, Patent Document 2). The thermal shrinkage onset temperature of such composite particles is higher than that of uncomposite metal particles. Furthermore, the ceramic particles fixed to the surface are less likely to aggregate than the ceramic co-material powder added individually to the conductive paste. Therefore, by using such composite particles as the raw powder of the conductive paste, an improvement in the coverage rate of the internal electrode layer can be expected.
[0005] However, in recent years, the demand for thinner layers in ceramic electronic components has been increasing, and there is a demand for further improvement in the thermal shrinkage properties of the composite particles used as raw material powder. For example, in Patent Document 2, Ni particles having an average particle size (converted to Feret's diameter) of 0.2 μm or 0.5 μm are used to evaluate the thermal shrinkage properties of the composite particles, but in order to meet the recent demand for thinner layers, it is necessary to use metal particles with a smaller particle size than those in Patent Document 2. However, if the metal particles are made smaller in diameter, the thermal shrinkage start temperature will be lowered, and there is a possibility that the coverage rate of the internal electrode layer cannot be sufficiently ensured. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2013-55314 A [Patent Document 2] JP 2000-282102 A Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the exemplary embodiments of the present invention is to provide a composite particle having a high heat shrinkage initiation temperature, and a conductive paste using the composite particle. [Means for solving the problem]
[0008] In order to achieve the above object, the composite particles according to the present invention are The present invention has large particles and small particles attached to the surfaces of the large particles and having a smaller particle size than the large particles, The large particles have an average crystallite size of 20 nm or more and 80 nm or less.
[0009] When the composite particles have the above-mentioned properties, the heat shrinkage initiation temperature can be made higher than before.
[0010] Preferably, the composite particle has a sulfur content of 3000 ppm by mass or less.
[0011] Preferably, the average coverage of the small particles with respect to the large particles is 18% or more.
[0012] Preferably, the large particles have an average particle size of 20 nm or more and 200 nm or less.
[0013] Preferably, the ratio of the average particle size of the small particles to the average particle size of the large particles is 0.01 or more and 0.30 or less.
[0014] Preferably, the large particles comprise nickel or a nickel alloy containing Sn.
[0015] Preferably, the small particles contain at least one selected from barium titanate, silicon oxide, titanium oxide, aluminum oxide, and zirconium oxide.
[0016] A conductive paste according to the present invention includes the above composite particles, a binder, and a solvent. Also, an electronic component according to the present invention has an electrode layer formed using the conductive paste. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a cross-sectional view showing a multilayer ceramic electronic component according to one embodiment. [Diagram 2] FIG. 2 is a schematic diagram showing a cross section of a composite particle according to one embodiment. [Diagram 3] FIG. 3 is a schematic diagram for explaining a method for measuring the average coverage rate in a composite particle. [Figure 4] FIG. 4 is a schematic diagram for explaining a method for measuring the average coverage rate in a composite particle. [Diagram 5] FIG. 5 is a schematic diagram for explaining a method for measuring the average coverage rate in a composite particle. [Figure 6]FIG. 6 is a schematic diagram for explaining a method for measuring the heat shrinkage starting temperature by the tangent line method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.
[0019] First embodiment: Composite particles As shown in FIG. 2, each composite particle 12 according to this embodiment has one large particle 14 and a plurality of small particles 16 attached to the surface of the large particle 14.
[0020] The large particles 14 are conductive metal particles and may contain, as a main component, Ni, Cu, Ag, Pd, or an alloy containing at least one selected from these metal elements. The large particles 14 are preferably Ni particles or Ni alloy particles containing Sn (hereinafter referred to as NiSn-based alloy particles).
[0021] When the large particles 14 are Ni particles, the purity of Ni is preferably, for example, 98 wt% or more, and in addition to Ni, trace elements such as Fe, Co, Cr, Mn, Cu, Pd, Mg, Si, Ca, Na, K, Cl, O, C, and N may be contained. Even when the large particles 14 are NiSn-based alloy particles, the above trace elements may be contained. The ratio of Ni to Sn in the large particles 14 of the NiSn-based alloy is not particularly limited, and the content of Sn may be, for example, 1 wt% or more and 50 wt% or less.
[0022] In the composite particle 12, each large particle 14 may have the same material, or the large particle 14 may include two or more types of particle groups made of different materials (i.e., two or more types of large particles 14 made of different materials may be mixed together). In this embodiment, "different materials" refers to cases where the elements constituting the particles are different, or cases where the elements constituting the particles are the same but have different composition ratios.
[0023] The average particle size (R) of the large particles 14 may be 200 nm or more, but is not necessarily limited thereto. However, from the viewpoint of reducing the thickness of the electrode layer formed using the composite particles 12, it is preferably 20 nm or more and 200 nm or less, more preferably 20 nm or more and 150 nm or less, and even more preferably 30 nm or more and 100 nm or less. In addition, the coefficient of variation (standard deviation / average particle size) in the particle size distribution of the large particles 14 is not particularly limited, but may be, for example, 30% or less. When the large particles 14 include two or more types of particle groups made of different materials, each particle group may have a different particle size distribution, but it is preferable that the average particle size of each particle group is within the above range.
[0024] In this embodiment, the term "average particle size" refers to the arithmetic mean value of the equivalent circle diameter, and the term "particle size distribution" refers to the distribution of the equivalent circle diameter.
[0025] In the composite particle 12 of this embodiment, the average crystallite diameter (D C ) is 20 nm or more and 80 nm or less, preferably more than 20 nm and 80 nm or less, more preferably more than 20 nm and 50 nm or less, and even more preferably 30 nm or more and 50 nm or less. Here, the crystallite size means the size of the crystals present inside each large particle 14.
[0026] Average crystallite size of large particle 14 (D C ) may be measured by X-ray diffraction (XRD). Specifically, an X-ray diffraction chart of the composite particles 12 is obtained by 2θ / θ measurement, and a diffraction peak originating from the large particles 14 is identified in the X-ray diffraction chart. Then, from the identified diffraction peak, the average crystallite diameter (D C ) can be calculated.
number
[0027] The small particles 16 are oxide particles having a smaller particle size than the large particles 14. The material of the small particles 16 is not particularly limited, and for example, the small particles 16 preferably contain at least one selected from barium titanate, silicon oxide, titanium oxide, aluminum oxide, and zirconium oxide, more preferably contain barium titanate or silicon oxide, and further preferably contain barium titanate. In the composite particle 12, each small particle 16 may have the same material, or the small particles 16 may contain two or more types of particle groups having different materials (i.e., two or more types of small particles 16 having different materials may be mixed).
[0028] The average particle size (r) of the small particles 16 is not necessarily limited, but is preferably 3 nm or more and 30 nm or less, and more preferably 3 nm or more and 20 nm or less. When the small particles 16 include two or more particle groups made of different materials, each particle group may have a different particle size distribution, but it is preferable that the average particle size of each particle group is within the above range. In addition, the ratio (r / R) of the average particle size of the small particles 16 to the average particle size of the large particles 14 is preferably 0.01 to 0.30, more preferably 0.01 to 0.20, and even more preferably 0.03 to 0.17. By setting r / R within the above range, the steric hindrance described below can be more effectively exerted.
[0029] In this embodiment, each large particle 14 is a core particle in the composite particle 12. On the other hand, each small particle 16 has a smaller particle size than the large particles 14 and acts to create steric hindrance in the composite particle 12. Steric hindrance means a function of suppressing direct contact between the surfaces of adjacent large particles 14. In the composite particle 12, the small particles 16 attached to the surface of each large particle 14 are interposed between the adjacent large particles 14, thereby creating steric hindrance. Due to such steric hindrance, the thermal shrinkage onset temperature of the composite particle 12 can be made higher than the thermal shrinkage onset temperature of a powder consisting of only the large particles 14.
[0030] In addition, in the particle structure in which the above-mentioned steric hindrance occurs, the average crystallite diameter (D C ) in the range of 20 nm or more and 80 nm or less, the thermal shrinkage starting temperature can be shifted to a higher temperature side than that of conventional composite particles. In particular, in the composite particle 12 of this embodiment, the thermal shrinkage starting temperature can be made sufficiently high not only when the average particle size (R) of the large particles 14 is 200 nm or more, but also when the average particle size (R) of the large particles 14 is reduced to less than 200 nm.
[0031] The reason why the heat shrinkage starting temperature increases as a result of controlling the crystallite size is not necessarily clear, but the following reasons are considered, for example.
[0032] In conventional composite particles, even if steric hindrance is exerted, it is believed that the shape of the core metal particle is easily deformed at high temperatures of 400°C or more. When the shape of the metal particle is deformed, it is believed that adjacent metal particles are bonded to each other in the gaps between the microparticles made of inorganic compounds, etc. In particular, when the average particle size of the metal particles is small, less than 200 nm, the particle shape is easily deformed at high temperatures, and the bonding between the metal particles between the microparticles becomes significant, and it is believed that the effect of improving the thermal shrinkage properties is not sufficiently obtained.
[0033] In contrast, in the composite particle 12 of the present embodiment, the large particle 14 has a diameter of 20 nm or less. C By satisfying the requirement of ≦80 nm, the ratio of the average particle diameter to the average crystallite diameter of large particles 14 (R / D C ) is lower than that of conventional composite particles. In other words, the volume ratio of each crystallite in each large particle 14 is higher than that of conventional composite particles. In this way, by increasing the volume ratio of each crystallite inside the large particle 14, it is believed that the shape of the large particle 14 is less likely to collapse even in high temperature ranges. As a result, it is believed that it is possible to suppress the large particles 14 from joining together in the gaps between the small particles 16, and to increase the thermal shrinkage starting temperature.
[0034] When the average particle size (R) of the large particles 14 is in the range of 20 nm or more and 100 nm or less, R / D Cis 5.0 or less, and preferably 3.0 or less. When the average particle size (R) of the large particles 14 is in the range of more than 100 nm and 200 nm or less, R / D C is 10.0 or less, preferably 8.0 or less, and more preferably 4.0 or less. C The lower limit of R / D is 1.0. C By controlling the amount of the resin within the above range, the heat shrinkage property can be further improved.
[0035] The sulfur content in the composite particles 12 is preferably 3000 ppm by mass or less, and more preferably 10 ppm by mass or less. When the sulfur content is less than 10 ppm by mass, the composite particles 12 may be considered to be substantially free of sulfur. The sulfur contained in the composite particles 12 is considered to be mainly derived from the large particles 14. The sulfur component may be mixed as an impurity when the large particles 14 are produced, or may be intentionally added as an additive. By controlling the sulfur content in the composite particles 12 to 3000 ppm by mass or less (preferably 10 ppm or less), it is possible to suppress a decrease in the melting point due to sulfurization of the large particles 14. The sulfur content may be measured by inductively coupled plasma emission spectroscopy (ICP), a carbon / sulfur analyzer, or the like.
[0036] In the composite particle 12, the average coverage of the small particles 16 to the large particles 14 may be 10% or more, preferably 18% or more, more preferably 18% or more and 50% or less, and even more preferably 18% or more and 30% or less. By setting the average coverage of the small particles 16 to the large particles 14 to 18% or more, the steric hindrance caused by the small particles 16 can be more effectively exerted. In addition, the standard deviation of the coverage of the small particles 16 to the large particles 14 is preferably 0% or more and 20% or less, and more preferably 0% or more and 5% or less. By reducing the variation in the coverage, the steric hindrance can be more effectively exerted. The above-mentioned standard deviation of the coverage (particularly 5% or less) can be realized, for example, by manufacturing the composite particle 12 by an electrostatic adsorption method.
[0037] The method for measuring the particle sizes of the large particles 14 and the small particles 16 and the coverage of the small particles 16 with respect to the large particles 14 is not necessarily limited, but it is preferable to employ, for example, an image analysis method as described below.
[0038] First, a liquid containing the composite particles 12 is dropped onto a sample stage and air-dried. Next, the composite particles 12 on the sample stage are observed using a scanning electron microscope (SEM) (a scanning transmission electron microscope (STEM) may also be used) to obtain an SEM image of the composite particles 12. The observation magnification when obtaining the SEM image is not particularly limited and may be appropriately determined according to the average particle size (R) of the large particles 14. For example, the observation magnification may be set so that the area per field of view is approximately (R×8)×(R×6). FIG. 3 shows a schematic diagram of an SEM image.
[0039] Next, from among the large particles 14 included in the SEM image, "large particles 14 with a visible outline" are selected. In FIG. 4, "large particles 14 with a visible outline" are selected from among the large particles 14 included in FIG. 3, and the outline of the selected large particle 14 is shown in bold. In addition, in FIG. 4, the outline of "small particles 16 with a visible outline" attached to the "large particle 14 with a visible outline" is also shown in bold. Note that "large particles 14 with a visible outline" refers to large particles 14 whose entire outline is included in the SEM image and which are present in the foreground in the SEM image. Therefore, if even a part of the outline is missing, the large particle 14 does not become "large particles 14 with a visible outline". Also, if even a part of the large particle 14 exists behind (behind) another large particle 14, the large particle 14 does not become "large particles 14 with a visible outline".
[0040] The circle-equivalent diameter of the "large particle 14 with a visible outline" identified by the above method is measured, and the particle size distribution and average particle size (R) of the large particle 14 are calculated. The circle-equivalent diameter of the "small particle 16 with a visible outline" attached to the "large particle 14 with a visible outline" is measured, and the particle size distribution and average particle size (r) of the small particle 16 are calculated. The circle-equivalent diameter may be measured using image analysis software, and the average particle sizes (R and r) are preferably calculated by measuring the circle-equivalent diameters of at least 1,000 particles.
[0041] When measuring the coverage, first, a particle to be measured is selected from among the "large particles 14 whose outlines can be confirmed." Then, the particle size Ra of the particle to be measured is measured, and the center of gravity G of the particle to be measured is identified. Next, as shown in FIG. 5, a circle with a radius of 0.25 times Ra is drawn from the center of gravity G, and the circle is designated as a virtual circle 18. Next, the area A0 of the virtual circle 18 and the total area A1 of the small particles 16 contained in the virtual circle 18 are measured, and the coverage of the small particles 16 in the particle to be measured is calculated as the ratio of A1 to A0 (A1 / A0). The coverage of at least 100 large particles 14 is calculated using the above method, and the average value is designated as the average coverage.
[0042] The standard deviation of the coverage may be calculated based on the following formula 2.
number
[0043] In the image analysis described above, the composite particle 12 may contain particles with a coverage of 0%, but the number ratio (number density) of particles with a coverage of 0% in the composite particle 12 is preferably 10% or less.
[0044] In the image analysis as described above, the number of agglomerates of small particles 16 in an area of (R×80)×(R×60) is preferably 3 or less, more preferably 1 or less, and even more preferably 0.
[0045] An example of a method for producing the composite particle 12 according to this embodiment will be described below.
[0046] First, the large particles 14 and the small particles 16 are prepared. The method for producing the large particles 14 may be a liquid phase synthesis method or a gas phase synthesis method, and the method for producing the large particles 14 is not necessarily limited. The average crystallite diameter (D C ) can be controlled based on various conditions, such as the type of precursor, temperature, and cooling rate, during synthesis of the large particles 14. The sulfur content in the composite particles 12 can be controlled by, for example, carrying out a desulfurization treatment during the production of the large particles 14.
[0047] From the viewpoint of producing metal particles with a small particle size, the liquid phase method is more suitable than the gas phase method, and the liquid phase method is generally used to produce metal particles with a size of 200 nm or less. However, in the current liquid phase method, the crystallite size tends to be small, and it is difficult to achieve an average crystallite size of 20 nm or more. Therefore, when producing large particles 14 by the liquid phase method, a process for increasing the crystallite size is required after the synthesis of large particles 14. As an example of such a process, a method of heat treating large particles 14 at a low temperature at which the shape of large particles 14 is not distorted can be mentioned.
[0048] From the viewpoint of producing metal particles with a small ratio of particle size to crystallite size, gas phase methods such as PVD and CVD are more suitable than liquid phase methods, and it is preferable to adopt a gas phase method in the production of composite particles 12. However, the current gas phase method is not suitable for producing metal particles with a small particle size, and it is difficult to achieve an average particle size of 200 nm or less. Therefore, when producing large particles 14 by the gas phase method, first, a mother powder is produced under conditions that obtain a wide particle size distribution with a predetermined crystallite size. Then, the mother powder is classified until the desired average particle size (for example, preferably 200 nm or less, more preferably 100 nm or less) is obtained, thereby obtaining large particles 14.
[0049] In addition, R≦200 nm and 20 nm≦D CAs a method for achieving both ≦80 nm, if a more optimal manufacturing method than the above can be found through future research and development, the manufacturing method of the large particles 14 is not limited to the above method.
[0050] The method for producing the small particles 16 is not particularly limited, and they may be produced by, for example, a liquid phase synthesis method or a solid phase synthesis method.
[0051] Next, the composite particle 12 is produced by attaching the small particles 16 to the surface of the large particles 14. The method for attaching the small particles 16 is not necessarily limited, but it is preferable to adopt an electrostatic adsorption method. The electrostatic adsorption method is a method in which the large particles 14 and the small particles 16 are charged with opposite charges and then mixed together to composite the large particles 14 and the small particles 16 by electrical attraction.
[0052] The nanometer-order oxide particles used as the small particles 16 have hydroxyl groups on their outermost surface, and therefore are basically highly hydrophilic and disperse well in water or highly polar solvents, such as alcohols and glycols. Although it depends on the manufacturing method and dispersion method, oxide particles often have a negative surface charge. A dispersion containing the small particles 16 is obtained by dispersing such small particles 16 with a positive surface charge in an organic solvent such as alcohols, glycols, or ketones. To stabilize the dispersion of the small particles 16, a small amount of additive may be added to the dispersion.
[0053] On the other hand, the metal particles used as the large particles 14 have a very weak positive or negative charge. It is preferable to change the surface potential of the large particles 14 to a strong positive potential using a polymer electrolyte such as polydiallyldimethylammonium chloride (PDDA) or polyethyleneimine (PEI). Then, the large particles 14 having a positive surface potential are dispersed in an organic solvent such as alcohols, glycols, or ketones, in the same manner as the small particles 16, to obtain a dispersion containing the large particles 14. To stabilize the dispersion of the large particles 14, a small amount of additive may be added to the dispersion.
[0054] Next, the dispersion liquid containing the small particles 16 and the dispersion liquid containing the large particles 14 are mixed in a desired ratio, and the small particles 16 are electrostatically adsorbed onto the surfaces of the large particles 14. Thereafter, the organic solvent is removed to obtain the composite particles 12.
[0055] Fig. 7A is an example of an SEM image of large particles 14 (Ni particles) before attachment of small particles 16. Fig. 7B is an example of an SEM image after electrostatic adsorption, in which it can be seen that small particles 16 (barium titanate particles) are attached to the surfaces of large particles 14 shown in Fig. 7A.
[0056] 7B, in the electrostatic adsorption method, the small particles 16 can be attached to the surfaces of the large particles 14 in a nearly monodisperse state, and aggregation of the small particles 16 can be suppressed. In addition, in the electrostatic adsorption method, the amount of the small particles 16 attached to the large particles 14 can be easily controlled, and the coverage rate of the small particles 16 with respect to the large particles 14 can be controlled to an optimal range for effectively exerting steric hindrance.
[0057] The composite particles 12 according to this embodiment can be used as a raw material powder for forming an electrode layer in various electronic components, and is preferably used as a raw material powder for forming an internal electrode layer of a multilayer ceramic electronic component. The electrode layer (internal electrode layer) as described above is formed by sintering a conductive paste containing the composite particles 12. The conductive paste may be produced by mixing the composite particles 12 with a known binder and a known solvent.
[0058] Second embodiment: Multilayer ceramic electronic component In the second embodiment, a multilayer ceramic capacitor 2 shown in FIG. 1 will be described as an example of a multilayer ceramic electronic component using the composite particles 12 of the first embodiment.
[0059] The multilayer ceramic capacitor 2 has an element body 4 and a pair of external electrodes 6 formed on the outer surface of the element body 4. The element body 4 has ceramic layers 20 and internal electrode layers 20 that are substantially parallel to a plane including the X-axis and Y-axis, and inside the element body 4, the ceramic layers 20 and internal electrode layers 10 are alternately laminated along the Z-axis direction. Here, "substantially parallel" means that most parts are parallel, but may have some parts that are not parallel, and the ceramic layers 20 and internal electrode layers 10 may have some unevenness or be inclined.
[0060] The ceramic layer 20 includes a dielectric composition. The composition of the dielectric composition is not particularly limited. For example, the ceramic layer 20 may include any of BaTiO3, CaTiO3, SrTiO3, CaZrO3, (K 1-x Na x )Sr2Nb5O 15 , Ba3TiNb4O 15 , and (Ba 1-x Ca x )(Ti 1-y Zr y )O3, etc. as a main component. In addition to the above-mentioned main components, the ceramic layer 20 may also contain one or more accessory components. Examples of the accessory components of the ceramic layer 20 include Mn compounds, Mg compounds, Cr compounds, Co compounds, Ni compounds, compounds containing rare earth elements, Si compounds, and Li compounds.
[0061] The average thickness of each ceramic layer 20 is not particularly limited, and is preferably 2 μm or less, more preferably 1.5 μm or less, and even more preferably 0.8 μm or less. The lower limit of the average thickness of the ceramic layer 20 is not particularly limited, and may be, for example, about 0.3 μm. The number of layers of the ceramic layer 20 may be appropriately determined according to the desired characteristics, and is not particularly limited. For example, the number of layers of the ceramic layer 20 is preferably 20 layers or more, and more preferably 50 layers or more.
[0062] The internal electrode layer 10 is formed by sintering the composite particle 12 of the first embodiment, and the large particles 14 in the composite particle 12 become the conductive component of the internal electrode layer 10 after sintering. The internal electrode layer 10 is preferably formed of composite particles 12 containing large particles 14 made of Ni or NiSn-based alloy. In other words, the conductive component of the internal electrode layer 10 is preferably Ni or NiSn-based alloy.
[0063] On the other hand, the small particles 16 of the composite particle 12 may remain as an insulating material inside the internal electrode layer 10 after sintering. When the total of the conductor component and the insulating material in the internal electrode layer 10 is 100 mass%, the content of the insulating material in the internal electrode layer 10 may be, for example, 0.4 mass% or more and 20 mass% or less, and preferably 3 mass% or more and 15 mass% or less. A part of the small particles 16 may be diffused into the ceramic layer 20 after sintering. By using barium titanate particles as the small particles 16, even if the small particles 16 diffuse into the ceramic layer 20, the compositional variation in the ceramic layer 20 can be suppressed.
[0064] The internal electrode layers 10 are laminated between the ceramic layers 20, and the number of layers is determined according to the number of layers of the ceramic layers 20. The average thickness of each of the internal electrode layers 10 is not necessarily limited, and is preferably 2.0 μm or less, more preferably 1.5 μm or less, and even more preferably 0.8 μm or less. By using the composite particles 12 of the first embodiment as a raw material powder, the internal electrode layers 10 can be made thin (for example, 0.8 μm or less) while suppressing the occurrence of cracks and discontinuities. The lower limit of the average thickness of the internal electrode layers 10 is not particularly limited, and may be, for example, about 0.3 μm. The average thickness t E In order to form the internal electrode layer 10, E It is preferable to use large particles 14 having an average particle size (R) of 0.2 times or less.
[0065] The internal electrode layers 10 are laminated such that one end is alternately exposed to two end faces of the element body 4. A pair of external electrodes 6 are formed on both end faces of the element body 4 and are electrically connected to the exposed ends of the alternately arranged internal electrode layers 10. By connecting the internal electrode layers 10 and the external electrodes 6 in the manner shown in Fig. 1, a capacitor circuit is formed by the external electrodes 6 and the internal electrode layers 10. That is, the ceramic layers 20 present in the capacitance region are sandwiched between the internal electrode layers 10 of different polarities, and a voltage can be applied to the ceramic layers 20.
[0066] The pair of external electrodes 6 may include a baked electrode layer, a resin electrode layer, a plated electrode layer, etc., and may be composed of a single electrode layer or may be composed of a laminate of multiple electrode layers. For example, the external electrode 6 may have a three-layer structure of a baked electrode layer containing Cu-a Ni plating layer-a Sn plating layer (laminate in the order listed). When the external electrode 6 is formed with this three-layer structure, the Sn plating layer is located on the outermost surface of the external electrode 6, and therefore the solder wettability of the external electrode 6 is good.
[0067] Next, an example of a method for manufacturing the multilayer ceramic capacitor 2 shown in FIG. 1 will be described.
[0068] First, a conductive paste used to form the internal electrode layers 10 and a ceramic layer paste used to form the ceramic layers 20 are prepared.
[0069] The conductive paste is produced by kneading the composite particles 12 of the first embodiment, a binder, and a solvent. In addition to the above, additives such as a dispersant, an antioxidant, a ceramic powder, and an organometallic solution may be added to the conductive paste. The conductive paste may be an organic paint or a water-based paint, and the binder and the solvent used in the conductive paste are not particularly limited.
[0070] For example, when the conductive paste is an organic paint, polyvinyl butyral, acrylic, ethyl cellulose, etc. may be used as the binder, and methyl ethyl ketone, methanol, ethanol, acetone, toluene, terpineol, butyl carbitol, acetate, etc. may be used as the solvent. When the conductive paste is a water-based paint, water may be used as the solvent, and polyvinyl alcohol, water-soluble acrylic resin, water-soluble polyvinyl butyral resin, etc. may be used as the binder.
[0071] The ceramic layer paste may be produced by kneading the main component powder of the dielectric composition, the binder, and the solvent. In addition to the above, additives such as subcomponent powder, dispersant, and antioxidant may be added to the ceramic layer paste. The ceramic layer paste may be an organic paint or a water-based paint, and the binder and solvent used in the conductive paste are not particularly limited. The ceramic layer paste may also use the same binder and solvent as the conductive paste.
[0072] Next, the dielectric paste is formed into a sheet by a doctor blade method or the like to obtain a ceramic green sheet. Then, the conductive paste is applied in a predetermined pattern onto the ceramic green sheet by various printing methods such as screen printing or a transfer method. As a method for applying the conductive paste, it is preferable to adopt screen printing or gravure printing from the viewpoint of easily maintaining the structure of the composite particles 12.
[0073] A mother laminate is obtained by laminating multiple layers of green sheets on which internal electrode patterns are formed, and then pressing them in the lamination direction. At this time, one or more layers of green sheets on which no internal electrode patterns are formed are laminated on the top and bottom surfaces of the mother laminate in the lamination direction.
[0074] The mother laminate obtained by the above steps is cut into a predetermined size by dicing or pressing to obtain a plurality of green chips. If necessary, the green chips may be solidified and dried to remove plasticizers, and may be barrel-polished using a horizontal centrifugal barrel machine after solidification and drying.
[0075] Next, the green chip obtained above is subjected to a binder removal process and a firing process to obtain the element body 4.
[0076] The conditions of the binder removal process are not particularly limited and may be appropriately determined depending on the type of binder added to the dielectric paste and the conductive paste. For example, the temperature rise rate may be preferably 5 to 300°C / hour, the holding temperature may be preferably 180 to 800°C, and the temperature holding time may be preferably 0.5 to 24 hours. The atmosphere of the binder removal process may be an air atmosphere (i.e., in air) or a reducing atmosphere.
[0077] The firing conditions are not particularly limited as long as they are set to conditions under which the internal electrode layers 10 and the ceramic layers 20 are sintered. For example, in the firing process, the heating rate may be 50°C / hour to 500°C / hour, and is preferably 200°C / hour to 300°C / hour. The holding temperature in the firing process is preferably 1200°C to 1350°C, and more preferably 1220°C to 1300°C. The temperature holding time is preferably 0.5 hours to 8 hours, and more preferably 2 hours to 3 hours. The atmosphere in the firing process is preferably a reducing atmosphere, and the atmospheric gas is preferably, for example, a humidified mixed gas of N2 and H2.
[0078] The oxygen partial pressure in the firing atmosphere may be appropriately determined depending on the type of conductive component in the conductive paste. When the conductive component is a base metal such as Ni or a Ni alloy, the oxygen partial pressure in the firing atmosphere is 1.0×10 -14 MPa~1.0×10 -10 The temperature drop rate in the firing treatment is preferably 50° C. / hour to 500° C. / hour.
[0079] After firing in a reducing atmosphere, the element body 4 may be subjected to an annealing treatment. The conditions for the annealing treatment are not particularly limited. For example, the oxygen partial pressure in the atmosphere is 1.0×10 -9 MPa~1.0×10 -5 The annealing pressure may be set to MPa, the annealing temperature may be set to 950° C. to 1150° C., and the temperature holding time may be set to 0 hours to 20 hours. As the annealing atmospheric gas, for example, humidified N2 gas or the like may be used.
[0080] In the above-mentioned binder removal treatment, firing treatment, and annealing treatment, in order to moisten the N2 gas or mixed gas, for example, a wetter or the like may be used, and in this case, the water temperature is preferably about 5 to 75° C. Furthermore, the binder removal treatment, firing treatment, and annealing treatment may be performed consecutively or independently.
[0081] Next, a pair of external electrodes 6 are formed on the outer surface of the element body 4 obtained above. The method of forming the external electrodes 6 is not particularly limited. For example, when forming a baked electrode as the external electrode 6, a conductive paste containing glass frit may be applied to the end surface of the element body 4 by a dipping method, and then the element body 4 may be heated at a predetermined temperature. When forming a resin electrode as the external electrode 6, a conductive paste containing a thermosetting resin may be applied to the end surface of the element body 4, and then the element body 4 may be heated at a temperature at which the thermosetting resin hardens. Furthermore, after forming the baked electrode or resin electrode by the above method, sputtering, vapor deposition, electrolytic plating, or electroless plating may be performed to form the external electrode 6 having a multilayer structure.
[0082] Through the above steps, a multilayer ceramic capacitor 2 having a cross section as shown in FIG. 1 can be manufactured.
[0083] In the multilayer ceramic capacitor 2, the composite particles 12 having a high thermal shrinkage start temperature are used to form the internal electrode layers 10, so that the difference between the sintering start temperature of the internal electrode layers 10 and the sintering start temperature of the ceramic layers 20 can be reduced. Therefore, the occurrence of cracks or discontinuities in the internal electrode layers 10 can be suppressed, and the coverage of the internal electrode layers 10 with respect to the ceramic layers 20 can be improved more than before. Specifically, in the multilayer ceramic capacitor 2 to which the composite particles 12 are applied, even when the layers are thinned, the coverage of the internal electrode layers 10 with respect to the ceramic layers 20 can be set to 80% or more (preferably 90% or more). By improving the coverage of the internal electrode layers 10, various characteristics of the multilayer ceramic capacitor 2, such as capacitance, can be improved.
[0084] Furthermore, when the internal electrode layer 10 is formed using the composite particles 12, it is possible to suppress the diffusion of the small particles 16, which are oxide particles, into the ceramic layer 20. As a result, it is possible to suppress the composition of the ceramic layer 20 from deviating from the target composition.
[0085] Although an embodiment of the present invention has been described above, the present invention is not limited to the above-described embodiment, and various modifications can be made without departing from the spirit of the present invention.
[0086] The electronic components to which the composite particles 12 are applied are not limited to multilayer ceramic capacitors, and the composite particles 12 can be applied to other electronic components. The other electronic components include all electronic components in which ceramic layers are laminated via internal electrode layers, such as bandpass filters, inductors, multilayer three-terminal filters, piezoelectric elements, PTC thermistors, NTC thermistors, and varistors.
[0087] The internal electrode layer 10 may be formed using a conductive paste containing the composite particles 12 and conductive particles other than the composite particles 12. The conductive particles other than the composite particles 12 are not particularly limited, and may be, for example, Ni particles, Ni-based alloy particles, Cu particles, or Cu-based alloy particles that are not composited with the small particles 16. In this case, the conductive paste used contains the composite particles 12 in an amount of preferably 20% by mass to 60% by mass, more preferably 25% by mass to 45% by mass, based on a total content of the composite particles 12 and the conductive particles being 100% by mass.
[0088] The internal electrode layer 10 may also contain a common material that is not derived from the small particles 16. The common material that is not derived from the small particles 16 is added to the conductive paste as a single common material, not as a part of the composite particle 12. The average particle size of the common material that is not derived from the small particles 16 is not particularly limited, and may be larger than the average particle size of the small particles 16, and may be 0.003 μm or more and 0.100 μm or less. The material of the common material that is not derived from the small particles 16 is not particularly limited, but it is preferable to use an oxide contained in the ceramic layer 20 in order to reduce the influence on the composition of the ceramic layer 20.
[0089] Furthermore, the composite particles 12 may be used to form the external electrodes 6. For example, the external electrodes 6 may be formed using a conductive paste containing the composite particles 12 and a thermosetting resin. EXAMPLES
[0090] The present disclosure will be described below based on more detailed examples, but the present disclosure is not limited to these examples.
[0091] (Experiment 1) In experiment 1, the average particle size (R) and the average crystallite size (D C Five types of Ni particles with different properties were prepared, and the composite particles shown in Table 1 were manufactured.
[0092] The Ni particles of sample 1 and sample 5 were each produced by hydrothermal synthesis (liquid phase method), and the Ni particles of sample 5 were subjected to heat treatment after synthesis to increase the crystallite size. For samples 2 to 4 and sample 6, mother powder was produced by CVD (vapor phase method), and the mother powder was classified to obtain Ni particles with an adjusted average particle size. For the Ni particles of sample 4, the mother powder was subjected to desulfurization treatment when produced by CVD.
[0093] In each sample of Experiment 1, small particles made of barium titanate (hereinafter referred to as BT particles) were attached to the surface of the Ni particles by electrostatic adsorption. Specifically, the Ni particles were mixed with an aqueous solution containing PDDA, and the surfaces of the Ni particles were positively charged. Next, the BT particles, which originally had a negative surface potential, were put into an aqueous solution containing positively charged Ni particles, and the Ni particles and the BT particles were composited by electrostatic adsorption. The obtained powder was then collected from the aqueous solution and dried to obtain composite particles for each sample.
[0094] In sample 4a, composite particles were produced by mixing sulfur powder with the composite particles of sample 4 in order to investigate the effect of sulfur on the composite particles. In sample 6a, composite particles were produced using the Ni particles of sample 6 and by changing the blending ratio of BT particles during electrostatic adsorption. In addition, in samples 6b and 6c, composite particles were produced using the Ni particles of sample 6 and by changing the particle size of the BT particles to be attached to the Ni particles.
[0095] The composite particles of each sample were evaluated as follows.
[0096] Image analysis First, the composite particles were added to ethanol at a ratio of 0.5% by mass, and mixed by a vortex mixer for 1 minute. The ethanol solution to which the composite particles were added was left to stand for 1 to 2 hours to allow the composite particles to settle. Then, the supernatant of the ethanol solution was removed by decantation, and the remaining liquid was added again to ethanol and mixed. The obtained composite particle-containing liquid was dropped onto an SEM stage and air-dried. Then, the composite particles remaining on the SEM stage were observed using an SEM, and SEM images of the composite particles were obtained.
[0097] The SEM images were analyzed using image analysis software to measure the average particle size (R) of Ni particles, the coefficient of variation (CV) in the particle size distribution of Ni particles, the average particle size (r) of BT particles attached to Ni particles, and the average coverage of BT particles on Ni particles. In this case, the particle size distribution of Ni particles and BT particles was calculated by measuring the circle equivalent diameter of 1000 or more particles, and the average coverage of BT particles on Ni particles was calculated by analyzing 100 or more Ni particles.
[0098] Measurement of average crystallite size by XRD An X-ray diffraction chart of the composite particles was obtained using XRD, and the Ni diffraction peaks in the X-ray diffraction chart were identified. From the identified diffraction peaks, the average crystallite diameter (D C ) was calculated.
[0099] Sulfur content measurement The sulfur content in the composite particles was measured by ICP. In the ICP used in this experiment, the detection limit of sulfur was 10 mass ppm, and "<10" in Table 1 means that sulfur was not detected and the sulfur content was less than 10 mass ppm. In addition, "≒1000" in Table 1 means that the sulfur content was in the range of 800 mass ppm to 1300 mass ppm, and "≒2000" means that the sulfur content was in the range of 1800 mass ppm to 2300 mass ppm.
[0100] Measurement of heat shrinkage start temperature For each sample, the thermal shrinkage start temperature of the Ni particles before composite and the thermal shrinkage start temperature of the composite particles were measured by thermomechanical analysis (TMA). In the measurement, a Rigaku Thermo plus EVO2 was used as a TMA measuring device, and the thermal shrinkage start temperature was determined by the tangent method.
[0101] In the tangent method, the intersection point of the tangent at the inflection point and the baseline is identified, and the temperature (T0) at the intersection point is identified as the thermal shrinkage start temperature, as shown in Fig. 6. The inflection point may be identified, for example, by referring to a DTMA curve obtained by differentiating a TMA curve as shown in Fig. 6, and the maximum value of the DTMA curve may be taken as the inflection point.
[0102] When measuring the thermal shrinkage start temperature or sintering start temperature by TMA, the temperature at which a certain shrinkage rate is reached may be specified as the thermal shrinkage start temperature or sintering start temperature, such as temperature T1 at a shrinkage rate of 10% shown in Figure 6. However, the shrinkage rate is affected by organic residues and voids in the evaluation sample, and the temperature at the set shrinkage rate (for example, T1 in Figure 6) tends to be higher than the temperature at the intersection specified by the tangent method (for example, T0 in Figure 6). In this experiment, we decided to adopt the tangent method in order to reduce the effects of organic residues and voids and measure the thermal shrinkage start temperature more accurately.
[0103] The thermal shrinkage start temperature of the raw material powder used to form the ceramic layers of the multilayer ceramic capacitor varies depending on the composition of the dielectric composition, but is, for example, 1000°C to 1200°C, which is higher than the thermal shrinkage temperature of metal particles. Therefore, in the evaluation of the composite particles in this experiment, it is determined that a composite particle having a higher thermal shrinkage start temperature is preferable as an electrode material. Specifically, the thermal shrinkage start temperature of the composite particles is preferably 600°C or higher, and more preferably 900°C or higher.
[0104] The evaluation results of each sample in Experiment 1 are shown in Table 1. [Table 1]
[0105] As shown in Table 1, the Ni particles of Sample 1 produced by a conventional hydrothermal synthesis method had an average crystallite diameter of less than 20 nm. Although the thermal shrinkage onset temperature of the composite particles of Sample 1 was higher than that of Ni particles alone, the characteristics were insufficient from the viewpoint of application as an electrode material to multilayer ceramic electronic components.
[0106] On the other hand, in the examples of Samples 2 to 4, 4a, 5 to 6, and 6a to 6c, the average crystallite size of the Ni particles was in the range of 20 nm to 80 nm, and by using the Ni particles, the thermal shrinkage starting temperature of the composite particles could be shifted to a higher temperature of 600° C. or more. This result shows that by increasing the average crystallite size of the large particles within a predetermined range, the thermal shrinkage properties of the composite particles can be further improved.
[0107] Although the same Ni particles were used in sample 6 and sample 6a, sample 6a, which has a higher average coverage of BT particles on the Ni particles, was able to achieve a higher heat shrinkage start temperature. Furthermore, comparing sample 2 and sample 3, sample 2, which has a relatively higher average coverage of BT particles, had a higher heat shrinkage start temperature than sample 3. Although sample 2 has a smaller average particle size of Ni particles than sample 3, it achieved a higher heat shrinkage start temperature, which shows that the average coverage of BT particles contributes to the heat shrinkage properties of the composite particles. These results show that the heat shrinkage start temperature can be increased by setting the average coverage of small particles to 18% or more.
[0108] Comparing sample 3 and sample 4, sample 4, which contains substantially no sulfur, had a higher heat shrinkage start temperature than sample 3, which contains sulfur. Note that sulfur was intentionally added later to sample 4a, and the addition of sulfur caused the heat shrinkage start temperature of sample 4a to be lower than that of sample 4. These results show that the heat shrinkage start temperature can be increased by reducing the sulfur content.
[0109] In Sample 6b and Sample 6c, BT particles having a larger particle size than Sample 6 and Sample 6a were used as the small particles, and the heat shrinkage onset temperature was higher than that of Sample 6 and Sample 6a. This result shows that the heat shrinkage onset temperature can be further improved by controlling r / R within a specified range.
[0110] (Experiment 2) In Experiment 2, the composite particles according to Sample 3 produced in Experiment 1 were used to produce a multilayer ceramic capacitor according to Example I in the following procedure.
[0111] First, a conductive paste for forming the internal electrode layers was prepared. The conductive paste was produced by kneading the composite particles of sample 3, ethyl cellulose (binder), and terpineol (solvent). The compounding ratio of the composite particles in the conductive paste was set to 45 mass%, the compounding ratio of the binder to 3 mass%, and the compounding ratio of the solvent to 52 mass%.
[0112] Next, a green sheet for the ceramic layer containing BaTiO3 as a main component was prepared, and a conductive paste was applied onto the green sheet to form an internal electrode pattern. The green sheets on which the internal electrode pattern was formed were then stacked in multiple layers and pressed in the stacking direction to obtain a mother laminate. At this time, protective green sheets on which no internal electrode pattern was formed were stacked on the upper and lower surfaces of the mother laminate. The mother laminate was cut into a predetermined size by dicing to obtain multiple green chips.
[0113] Next, the green chip was subjected to binder removal, firing, and annealing to obtain an element body (fired body). Next, a pair of external electrodes was formed by applying and firing an external electrode paste to two end faces of the element body, thereby obtaining a multilayer ceramic capacitor (hereinafter referred to as a capacitor sample) having a structure as shown in FIG. 1. The dimensions of the element body in the capacitor sample were width 12 mm x depth 20 mm x height 12 mm. In addition, the average thickness of each ceramic layer in the capacitor sample was 0.80 μm, the average thickness of each internal electrode layer was 0.50 μm, and the number of ceramic layers sandwiched between the internal electrode layers was 4.
[0114] Comparative example I In Experiment 2, a multilayer ceramic capacitor according to Comparative Example I was manufactured under the same manufacturing conditions as in Example I, using the composite particles of Sample 1 (Comparative Example) manufactured in Experiment 1. The dimensions of the element body in the capacitor sample of Comparative Example I were width 12 mm × depth 20 mm × height 12 mm. In Comparative Example I, the average thickness per ceramic layer in the capacitor sample was 0.80 μm, the average thickness per internal electrode layer was 0.51 μm, and the number of ceramic layers sandwiched between the internal electrode layers was 4.
[0115] Cross-sectional analysis The cross section of the capacitor sample manufactured above was mirror-polished and observed by SEM. Through the SEM observation, the average thickness of the ceramic layer and the average thickness of the internal electrode layer were measured, and the average coverage of the internal electrode layer with respect to the ceramic layer was calculated.
[0116] The average coverage of the internal electrode layer in Comparative Example I was 74%. On the other hand, in Example I, the cracks and discontinuities of the internal electrode layer were reduced compared to Comparative Example I, and the average coverage of the internal electrode layer was 94%. From this result, it was found that the coverage of the internal electrode layer in the multilayer ceramic capacitor can be improved by forming the internal electrode layer using composite particles having a high thermal shrinkage starting temperature. [Explanation of symbols]
[0117] 12 … Composite particles 14 ... Large particles 16 … small particles 18 … Imaginary circle 2. Multilayer ceramic capacitors 4 … Element body 10 … Internal electrode layer 20 … ceramic layer 6 … External electrode
Claims
1. The present invention has large particles and small particles attached to the surfaces of the large particles and having a smaller particle size than the large particles, The average crystallite size of the large particles is 20 nm or more and 80 nm or less.
2. 2. The composite particle according to claim 1, having a sulfur content of 3000 ppm by mass or less.
3. 3. The composite particle according to claim 1, wherein an average coverage rate of the small particles with respect to the large particles is 18% or more.
4. 3. The composite particle according to claim 1, wherein the large particles have an average particle size of 20 nm or more and 200 nm or less.
5. 3. The composite particle according to claim 1, wherein the ratio of the average particle size of the small particles to the average particle size of the large particles is 0.01 or more and 0.30 or less.
6. 3. The composite particle of claim 1 or 2, wherein the large particle comprises nickel or a nickel alloy containing Sn.
7. 3. The composite particle according to claim 1, wherein the small particles contain at least one selected from the group consisting of barium titanate, silicon oxide, titanium oxide, aluminum oxide, and zirconium oxide.
8. A conductive paste comprising the composite particles according to claim 1 , a binder, and a solvent.
9. An electronic component having an electrode layer formed using the conductive paste according to claim 8.
Citation Information
Patent Citations
Composite nickel fine powder and its production
JP2000282102A
Ceramic electronic component and method of manufacturing the same
JP2013055314A