Manufacturing method of silicic acid-based fertilizer
Patent Information
- Application Number
- JP2023043666
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-18
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-03-18
AI Technical Summary
【0028】 本発明の効果として、けい酸質肥料において、炭酸化したALC粉粒状物とALCを混合することで、また、結晶形態を選定した炭酸化したALCを混合することで、カルシウムの溶出速度とpHを調整し、多様な作物に対応でき、様々な土壌環境に適したけい酸質肥料を製造し、使用することができる。
Smart Images

Figure 2024132750000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a siliceous fertilizer. [Background technology]
[0002] Generally, lightweight aerated concrete (hereinafter referred to as ALC) is made by adding water to a mixture of siliceous raw materials such as natural silica stone and silica sand, and calcareous raw materials such as quicklime made from limestone, cement, and gypsum, and then adding metallic aluminum to the mixture to foam it. The green cake obtained in the first curing step is then cut to the required size with a piano wire, and then the second curing step is performed using steam curing at high temperature and pressure in an autoclave.
[0003] The resulting ALC can be cut to the required dimensions to produce a variety of molded products, and used as building materials such as ALC panels for a wide range of applications including various exterior walls, partitions, roofs, and floors.
[0004] Traditionally, powder or granular ALC has been used as fertilizer, and is classified as a siliceous fertilizer under the Fertilizer Control Law. The main component, soluble silicic acid, is a useful element that improves resistance to pests and helps crop growth by forming silicified cells. The calcium component is a secondary element that improves soil acidity, forms cell walls, and provides nutrients to crops.
[0005] The elution of calcium increases the pH, but depending on the pH value, some crops may not be suitable for this. For example, soluble silica is necessary for the growth of rice seedlings, but if the pH is high, the growth of the seedlings is inhibited, so siliceous fertilizer made from ALC powder and granular material is not suitable. Also, if calcium is eluted quickly and the pH is high, an antagonistic effect is created, inhibiting the absorption of other nutrients, such as potassium, one of the three major fertilizer elements.
[0006] Patent Document 1, JP 2004-244549 A, "Gardening soil and soil improvement material using waste ALC and manufacturing method thereof," describes ALC with a carbonation degree of 40% or more, and Patent Document 2, JP 06-141671 A, "Inorganic porous body," describes ALC with a carbonation degree of 82.6% (Example 3), which is used as a siliceous fertilizer with a controlled pH. Patent Document 3 describes an acidic fertilizer that uses ALC with a low carbonation degree and contains a relatively large amount of amorphous silica. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent Publication No. 2004-244549 [Patent Document 2] Patent Publication No. 06-141671 [Patent Document 3] Patent No. 5912887 Summary of the Invention [Problem to be solved by the invention]
[0008] However, the methods of use in Patent Documents 1 and 2 use only ALC with a fixed degree of carbonation, making it difficult to accommodate various soil types and growing organisms. The method in Patent Document 3 has the advantage that it is applied under weakly acidic to neutral flooded conditions, contains a large amount of non-crystalline, water-soluble silicic acid, and is absorbed by crops (e.g., limited to Gramineae plants), but it is still difficult to accommodate various soil types and growing organisms.
[0009] Therefore, the present invention provides a method for producing a siliceous fertilizer, which is a neutral to weakly alkaline ALC carbonated fertilizer that is versatile and can be used not only for gramineous plants but also for various crops such as vegetables, and is effective for gramineous plants. [Means for solving the problem]
[0010] As a result of extensive research, the inventors have come up with the following invention. [1] Provided is a method for producing a siliceous fertilizer in which a pH value is adjusted to 8 or more and 10.5 or less by using carbonated ALC powdery granules obtained by carbonating lightweight aerated concrete (hereinafter, ALC), or by mixing the carbonated ALC powdery granules with ALC powdery granules. [2] The present invention provides a method for producing a siliceous fertilizer according to [1], characterized in that the crystal form of calcium carbonate in the carbonated ALC powdery granules is mainly one of vaterite, aragonite, or calcite, and does not exhibit a main X-ray diffraction peak of tobermorite.
[0011] [3] A method for using a silicate fertilizer comprises using carbonated ALC powdery granules obtained by carbonating lightweight aerated concrete, or mixing the carbonated ALC powdery granules with ALC powdery granules, and applying the mixture to adjust the pH of seed sowing soil, main field soil, or culture soil to a range of 6 to 7.3. [4] Provided is a method for using a siliceous fertilizer according to [3], characterized in that the crystal form of calcium carbonate in the carbonated ALC is mainly one of vaterite, aragonite, or calcite, and does not exhibit a main X-ray diffraction peak of tobermorite.
[0012] The silicate fertilizer of the present invention is obtained by using carbonated ALC powdery granular material obtained by carbonating ALC, or by mixing this with ALC powdery granular material obtained by crushing ALC.
[0013] By contacting the ALC with carbon dioxide gas, the calcium silicate hydrate in the ALC is carbonated to produce calcium carbonate. The calcium silicate hydrate is tobermorite. The autoclave-cured lightweight cellular concrete is a lightweight cellular concrete mainly composed of porous calcium silicate hydrate obtained by adding a foaming agent to the main raw materials of siliceous raw materials and calcareous raw materials, pre-curing the materials, and then hydrothermally synthesizing the materials in an autoclave. The concrete is mass-produced as a building material or heat insulating material, and may utilize defective products generated during the manufacturing process of the autoclave-cured lightweight cellular concrete or scraps generated at construction sites.
[0014] From the viewpoint of improving the reactivity with carbon dioxide, it is preferable to use the ALC which has been coarsely crushed in advance using a crusher such as a crusher, a pin mill, or a ball mill to obtain a powdered form. The particle size range is approximately 1.2 mm to 4.0 mm, and the particle size is preferably fine, with the sieve opening being less than 0.85 mm, 0.85 mm to less than 2.0 mm, and 2.0 mm or more fractions being 70% or more, less than 30%, and 0%, respectively, or a granular material having a particle size distribution of less than 0.85 mm, 0.85 mm to less than 2.0 mm, 2.0 mm to less than 4.0 mm, and 4.0 mm or more fractions being less than 30%, less than 60%, 10% or more, and 0%, respectively. If the powder is too fine, it will scatter when used in fields, etc.
[0015] The carbon dioxide gas can be derived from limestone in cement factories, and can contribute greatly to carbon-free, carbon recycling, and carbon fixation. At this time, the carbon dioxide gas concentration in the carbon dioxide gas atmosphere is preferably 4 to 40% by volume, more preferably 5 to 30% by volume, from the viewpoints of shortening the treatment time and easiness of forming the carbon dioxide gas atmosphere. If the concentration is less than 4% by volume, the carbonation treatment takes a long time, which becomes a problem. Regarding the temperature during the treatment, from the viewpoint of shortening the treatment time, the reaction temperature is up to 20 to 80°C, preferably 30 to 60°C. This is also related to the conditions for obtaining a single phase of crystal form. If the temperature is less than 20°C, it takes a long time to generate calcium carbonate, which is not preferable. If the temperature exceeds 80°C, the cost of thermal energy increases, which is not preferable. Furthermore, carbonation can be performed using solid carbon dioxide (dry ice) as a source. In this case, a carbon dioxide gas atmosphere close to 100% by volume can be obtained, but the temperature inside the reaction vessel is set to 20 to 80°C, preferably 30 to 60°C.
[0016] In addition, the relative humidity during the carbonation treatment is preferably 2 to 100%, more preferably 40 to 95%, and particularly preferably 50 to 80%, from the viewpoints of shortening the treatment time and facilitating the adjustment of the target relative humidity. If the humidity is less than 2%, it is not preferable because it takes a long time to generate calcium carbonate. The treatment time varies depending on the treatment conditions, but if it is extremely short, the content of calcium carbonate in the ALC may be reduced. Note that the carbonation treatment can be performed in a shorter time by increasing the treatment pressure.
[0017] Calcium carbonate produced by carbonation of ALC is calcite, aragonite, or vaterite. The speed at which calcium dissolves varies depending on the crystal form. For example, in the case of calcite type, the crystal form is stable, so the effect of neutralizing acidic soil due to calcium dissolution is small, but it can adjust the pH for a long time. For example, calcium carbonate of aragonite type has a needle-shaped crystal structure, so it is effective at neutralizing acidic soil due to calcium dissolution and is fast.
[0018] In addition, because vaterite calcium carbonate has a plate-like crystal structure, it is less effective at neutralizing acidic soil than aragonite calcium carbonate, but it can adjust the pH for a relatively long period of time. Vaterite calcium carbonate is known to be unstable and to rearrange into other crystal structures, but when ALC powder and granular material is carbonated, it is possible to obtain a relatively stable crystal structure by adjusting the carbon dioxide concentration, atmospheric temperature, humidity, pH, etc. In addition, vaterite calcium carbonate is known to adsorb and fix harmful components such as heavy metals in soil.
[0019] Before and after carbonation of coarse ALC, the change in pore shape is small, and the change in volume is small, so the bulk density hardly changes at all. Figure 1 shows an enlarged view of ALC granules before carbonation, and Figure 2 shows an enlarged view of ALC granules after carbonation. The scale is as shown in the figure.
[0020] ALC powder and granules In order to facilitate mixing with carbonated ALC, it is preferable to use non-carbonated ALC that has been coarsely pulverized into granular form using a pulverizer such as a crusher, pin mill, or ball mill. The upper limit of the average particle size of the coarsely pulverized ALC is preferably 4 mm or less, more preferably 2 mm or less.
[0021] Mixing Treatment Method Non-carbonated ALC and carbonated ALC can be mixed uniformly easily using a ribbon mixer, pot blender, rotary mixer, etc. Non-carbonated ALC and carbonated ALC have similar bulk specific gravity, so they do not separate when mixed, and there is little change in shape due to carbonation, making them easy to mix uniformly. When two different types of fertilizers are mixed, they separate due to the difference in bulk specific gravity, making it difficult to mix uniformly.
[0022] How to Measure pH The pH of the mixed fertilizer was measured by adding 1 part fertilizer to 2.5 parts distilled or purified water, stirring for 30 minutes, and then measuring the supernatant liquid with a commercially available pH meter. The same results were also obtained when the fertilizer was moistened with distilled or purified water and left to stand for 30 minutes and then directly measured. The pH of the soil was also measured using the same procedure. However, when measuring directly, the measured values vary more than when measuring the supernatant liquid, so the average value of five measurements was used.
[0023] In the case of using only carbonated ALC powdery granules, it is preferable to sufficiently carbonate the ALC powdery granules until the pH reaches 8 or more and 9 or less. At this time, it is preferable that the degree of carbonation is 80% or more, and the main powder X-ray diffraction peak of tobermorite cannot be confirmed. The pH of the sufficiently carbonated ALC powdery granules and the siliceous fertilizer itself in which the ALC powdery granules are mixed is preferably adjusted to 8 or more and 10.5 or less.
[0024] Fertilizers in this pH range can be used to support a variety of soil types and growing conditions. Below a pH of 8, they are not very effective as alkaline fertilizers, even for plants that tolerate acidity, and above a pH of 10.5, there are few plants that prefer alkaline soil in this range.
[0025] In addition, the crystal form of calcium carbonate in the carbonated ALC powder is mainly one of vaterite type, aragonite type, or calcite type, and in order to perform carbonation sufficiently, it is preferable that the main X-ray diffraction peak of tobermorite is below the lower limit of detection. In this way, a carbonated ALC powder having a pH of 9 or less can be obtained.
[0026] Furthermore, it is preferable to use carbonated ALC powdery granules obtained by carbonating lightweight cellular concrete, or to mix the carbonated ALC powdery granules with ALC powdery granules, and apply them as fertilizer to adjust the pH of the seed sowing soil, main field, or culture soil to a range of 6 to 7.3.
[0027] Soil in this pH range can be obtained by using carbonated ALC granular fertilizer alone, or by changing the mixing ratio of carbonated ALC granular fertilizer with ALC granular fertilizer to lower the pH by mixing more carbonated ALC granular fertilizer. The standard is about 50g of fertilizer per 1 liter of soil. Effect of the Invention
[0028] The effect of the present invention is that by mixing carbonated ALC powder and granular material with ALC, or by mixing carbonated ALC with a selected crystal form, the calcium dissolution rate and pH can be adjusted to accommodate a variety of crops, and a siliceous fertilizer suitable for various soil environments can be produced and used.
[0029] For example, if the soil has an initial pH of less than 5.5, ALC powder and granular material alone is effective, but if the soil has a pH of 8.5 or higher, it is preferable to use carbonated ALC powder and granular material alone. If the soil has a pH of 5.5 to 8.5, the mixture ratio of the two can be adjusted appropriately to fertilize the plant at the optimal ratio. [Brief description of the drawings]
[0030] [Figure 1] FIG. 2 is a close-up of ALC granules before carbonation. [Diagram 2] FIG. 2 is a close-up of the ALC granules after full carbonation. [Diagram 3] FIG. 1 shows powder X-ray diffraction patterns of fully carbonated ALC granules and ALC granules before carbonation. [Figure 4] This figure shows the results of comparing the growth conditions of tomatoes planted in a seedbed and grown by thoroughly irrigating them with ion-exchanged water from above. [Diagram 5] This figure shows the results of comparing the growth conditions of tomatoes planted in a seedbed from the side, after which the seedlings were grown by thoroughly irrigating them with ion-exchanged water. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0031] The present invention will now be described with reference to examples. Ingredients used: The following ingredients were used: (1) ALC: Clion lightweight aerated concrete scraps (2) Culture soil: Honens Culture Soil No. 3 (rice), Naebijin N200 (cabbage), Nippi Engei Culture Soil No. 1 (tomato), pH values are 5.8, 6.0, and 6.3, respectively. (3) Paddy rice: Koshihikari, cabbage: Asashio, tomato: Rinka, (4) Water: Tap water
[0032] The chemical composition of the raw materials used was analyzed using an energy dispersive X-ray fluorescence analyzer (Shimadzu Corporation, "EDX-8000"). The analysis results, expressed as oxides, are shown in Table 1.
[0033] [Table 1]
[0034] [Example 1] The ALC scraps were crushed using a crusher until the grain size was 4 mm or less. The resulting granular ALC was placed in a carbonation vessel, and solid carbon dioxide (dry ice) was added so that the tobermorite in the ALC would turn into calcium carbonate (CaCO3). The vessel was then left to stand for two days to obtain carbonated ALC. The obtained carbonated ALC was subjected to qualitative analysis using a powder X-ray diffractometer (Rigaku Corporation, "MultiFlex 2kW"). The amount of calcium carbonate was measured using a TG-DTA (Rigaku Corporation's "Thermo plus EVO2"). The degree of carbonation is the value shown by the following formula 1.
[0035] Formula 1: Carbonation degree (%) = C / Cmax × 100 Here, C is the weight loss of calcium carbonate produced by carbonation of ALC due to decomposition of carbon dioxide gas at 600 to 800°C in thermal analysis, converted into CaO, and Cmax is the CaO equivalent of the total calcium contained in the carbonated ALC. The carbonation degree is preferably 80% or more, and the main diffraction peak of tobermorite at 2θ=7.8 degrees completely disappears. This is to ensure sufficient carbonation and a pH of 8 to 9.
[0036] 1. Mineral Composition FIG. 3 shows the powder X-ray diffraction patterns of the carbonated ALC granules and the ALC granules before carbonation. (1) Carbonated ALC granules: Carbonated ALC granules manufactured by Clion Co., Ltd. Carbonation rate: 80.6% Bulk density: 0.75kg / L Main components: calcite, quartz It contains calcite that is carbonated to the extent that the main diffraction peak of tobermorite (2θ=7.8 degrees) cannot be detected. (2) ALC granules: ALC granules manufactured by Clion Co., Ltd. Bulk density: 0.75kg / L Main components: Tobermorite, quartz
[0037] Tomato seedling results after potting: Fill seedling trays (plastic) with seedling culture soil (pH: 6.3) and sow the seeds. After sowing, cover with carbonated ALC powder or ALC powder. After covering with soil, flood the trays. The comparison of growth conditions is shown in Table 2.
[0038] [Table 2]
[0039] 150g of each fertilizer was applied and covered with 3L of culture soil for tomato seedlings (Nihon Hiryo Co., Ltd., Nippi Engei Baido No. 1, pH 6.3) to prepare a seedbed. Tomatoes were sown in the seedbed, and the seedlings were thoroughly watered with ion-exchanged water to conduct a seedling test. The results of the comparison of growth conditions are shown in Figures 4 and 5.
[0040] As shown in Figures 4 and 5, the growth of tomatoes is increased in the culture soil on the left that has been fertilized with only carbonated ALC powder granules and siliceous fertilizer, compared to the culture soil on the right that has been fertilized with ALC powder granules.
[0041] Comparative growth experiment of rice, cabbage, and tomatoes Table 3 shows the pH and evaluation of fertilizers using 3L of culture soil with a pH of 5.8 to 6.3, with a total of 150g of ALC powder and carbonated ALC powder in different ratios. Each evaluation was made by comprehensively evaluating the number of leaves, leaf length, root spread, and leaf color. The evaluation criteria were (good) ◎>○>○△>△ (average).
[0042] [Table 3]
[0043] As shown in Table 3, the growth rate differs depending on the plant being grown. For example, rice seedlings and tomatoes grow well in a relatively low pH range with a 0% ALC powder ratio. Conversely, cabbage grows well in a high pH range with a 80% ALC powder ratio. When the ALC powder ratio is 100%, if the soil pH is high, some plants may not grow well. However, even if the soil pH is low, the pH can be adjusted by using a large amount of ALC powder to create an environment suitable for plant growth. Table 4 shows the pH value of cabbage soil fertilized with fertilizers with different ratios of ALC powder and carbonated ALC powder.
[0044] [Table 4]
Claims
1. A method for producing a siliceous fertilizer, the pH of which is adjusted to 8 or more and 10.5 or less, by using carbonated ALC powdery granules obtained by carbonating lightweight aerated concrete (hereinafter referred to as ALC) or by mixing the carbonated ALC powdery granules with ALC powdery granules.
2. 2. The method for producing a siliceous fertilizer according to claim 1, characterized in that the crystal form of calcium carbonate in the carbonated ALC powdery granules is mainly one of vaterite type, aragonite type, or calcite type, and does not show a main X-ray diffraction peak of tobermorite.
3. A method for using a siliceous fertilizer comprising the steps of: using a carbonated ALC powdery granule obtained by carbonating lightweight aerated concrete (hereinafter referred to as ALC); or mixing the carbonated ALC powdery granule with an ALC powdery granule; and applying the mixture to adjust the pH of any of the soil for sowing seeds, the main field, and the culture soil to 6 or more and 7.3 or less.
4. 4. The method for using a siliceous fertilizer according to claim 3, characterized in that the crystal form of calcium carbonate in the carbonated ALC is mainly one of vaterite type, aragonite type, or calcite type, and does not show a main X-ray diffraction peak of tobermorite.
Citation Information
Patent Citations
recorder
JP1984012887A
Inorganic porous material
JP1994141671A
Horticultural soil using ALC waste material, soil-improving material and method for producing the same
JP2004244549A