Deposition method and deposition device
The film forming method using adsorption-inhibiting, silicon-containing, and nitriding gases with plasma treatment addresses the challenge of forming silicon nitride films with enhanced wet etching resistance and embeddability, ensuring a uniform V-shaped cross-sectional shape.
Patent Information
- Application Number
- JP2023044492
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods struggle to form silicon nitride films with excellent wet etching resistance and embeddability in recesses on substrate surfaces, particularly in maintaining a V-shaped cross-sectional shape to prevent voids and seams.
A film forming method involving the sequential use of adsorption-inhibiting, silicon-containing, nitriding, and adsorption-promoting gases, with plasma treatment, to control the adsorption density and promote uniform film deposition in recesses.
The method achieves silicon nitride films with improved wet etching resistance and embeddability, maintaining a V-shaped cross-sectional shape and reducing voids and seams.
Smart Images

Figure 2024134274000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a film forming method and a film forming apparatus. [Background technology]
[0002] Patent documents 1 and 2 disclose a technique for filling a recess in a substrate surface with a silicon nitride film. 3 NH 2 forming an adsorption site consisting of a Cl group in the entire recess; 2 It is described that a step of forming non-adsorption sites in the upper part of the recessed portion and leaving adsorption sites in the lower part of the recessed portion by supplying a gas to the substrate surface and a step of supplying a silicon-containing gas to the substrate surface are carried out in this order. Patent Document 2 describes the use of not only halogen gas but also non-halogen gas as the adsorption inhibitor gas.
[0003] Patent Document 3 discloses a technique for forming a silicon nitride film on a substrate surface. As a specific example, Patent Document 3 discloses a method for forming a silicon nitride film on a substrate surface using dichlorosilane (DCS: SiH 2 Cl 2 ) gas onto the substrate surface; 2 Gas and N 2 a step of converting a modifying gas made of a gas into plasma and supplying the plasma to a substrate surface; 3 and supplying a nitriding gas composed of a gas to the surface of the substrate without converting it into plasma. The steps are repeated in this order. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2018-10950 A [Patent Document 2] JP 2022-111765 A [Patent Document 3] JP 2020-113743 A Summary of the Invention [Problem to be solved by the invention]
[0005] One aspect of the present disclosure provides a technique for forming a silicon nitride film having excellent wet etching resistance and embeddability in a recessed portion on a substrate surface. [Means for solving the problem]
[0006] A film forming method according to an embodiment of the present disclosure includes a step of forming a silicon nitride film in a recess on a substrate surface. The step of forming the silicon nitride film includes a step of generating plasma of an adsorption inhibitor gas that inhibits adsorption of a silicon-containing gas and supplying the plasma to the substrate surface, a step of supplying the silicon-containing gas to the substrate surface, and a step of generating plasma of a nitriding gas that nitrides adsorbates of the silicon-containing gas and supplying the plasma to the substrate surface. The nitriding gas is N 2 The step of forming the silicon nitride film includes a step of supplying an adsorption promoting gas that promotes adsorption of the silicon-containing gas to the substrate surface, and repeats a process including supplying the adsorption inhibiting gas, the silicon-containing gas, and the nitriding gas one or more times, and supplying the adsorption promoting gas one or more times, multiple times. Effect of the Invention
[0007] According to one aspect of the present disclosure, a silicon nitride film having excellent wet etching resistance and embeddability can be formed in a recessed portion on a substrate surface. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a cross-sectional view illustrating a film forming method according to an embodiment. [Diagram 2] FIG. 2 is a flow chart showing an example of a film forming process. [Diagram 3] FIG. 3 is a diagram showing the film formation conditions in Examples 1 to 4. [Figure 4] FIG. 4 is a diagram showing the film formation conditions in Examples 5 to 9. [Diagram 5]FIG. 5 is a SEM photograph of the substrate obtained under the film formation conditions of Example 8. [Figure 6] FIG. 6 is a graph showing the relationship between the WER and the depth of the silicon nitride films obtained under the film formation conditions of Examples 1 and 2. In FIG. [Figure 7] FIG. 7 is a diagram showing the relationship between GPC and depth for silicon nitride films obtained under the film formation conditions of Examples 1 to 4. As shown in FIG. [Figure 8] FIG. 8 is a diagram showing the relationship between GPC and depth for the silicon nitride films obtained under the film formation conditions of Examples 5 to 7. In FIG. [Figure 9] FIG. 9 is a graph showing the relationship between GPC and depth for the silicon nitride films obtained under the film formation conditions of Examples 6, 8, and 9. [Figure 10] FIG. 10 is a graph showing the relationship between GPC and depth for the silicon nitride films obtained under the film formation conditions of Examples 1, 2 and 8. [Figure 11] FIG. 11 is a diagram showing the relationship between GPCX-250 and depth of the silicon nitride films obtained under the film formation conditions of Examples 1, 2 and 8. [Figure 12] FIG. 12 is a graph showing the relationship between WER0 and GPC0-250 of the silicon nitride films obtained under the film formation conditions of Examples 1, 2 and 8. [Figure 13] FIG. 13 is a cross-sectional view showing a film forming apparatus according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. In the drawings, the same or corresponding components are denoted by the same reference numerals, and the description thereof may be omitted.
[0010] A film forming method according to one embodiment will be described with reference to Fig. 1. The film forming method includes a step of forming a silicon nitride film Wc in a recess Wb on a substrate surface Wa as shown in Fig. 1. This step is also referred to as a film forming step hereinafter. The substrate W is a silicon wafer in this embodiment, but may be a compound semiconductor wafer. The substrate W has a recess Wb on the substrate surface Wa. The recess Wb is a trench in this embodiment, but may be a via hole.
[0011] The film forming process fills the inside of the recess Wb with the silicon nitride film Wc while maintaining the V-shaped cross-sectional shape in order to suppress the generation of voids and seams. The film forming process, which will be described in detail later, includes a process of supplying an adsorption inhibitor gas to the substrate surface Wa in order to maintain the V-shaped cross-sectional shape. The adsorption inhibitor gas inhibits the adsorption of the silicon-containing gas.
[0012] The adsorption inhibitor gas is adsorbed to the substrate surface Wa. The adsorbates Wd of the adsorption inhibitor gas form non-adsorption sites that inhibit the adsorption of the silicon-containing gas. The density of the non-adsorption sites decreases the deeper from the substrate surface Wa. As a result, the deeper from the substrate surface Wa, the easier it is for the silicon-containing gas to be adsorbed. Thus, the silicon nitride film Wc can be filled into the recess Wb while maintaining the V-shaped cross-sectional shape. The density distribution of the non-adsorption sites is controlled by the supply time of the adsorption inhibitor gas, etc.
[0013] An example of a film forming process will be described with reference to FIG. 2. The film forming process includes, for example, steps S101 to S108 as shown in FIG. 2. In FIG. 2, k and m are integers of 1 or more, and n is an integer of 2 or more. The order of steps S101 to S108 is not limited to the order shown in FIG. 2. It is not necessary to perform all of steps S101 to S108. For example, step S103 may be omitted. Also, steps not shown may be included. Steps not shown include, for example, supplying a purge gas and adjusting the flow rate of the gas. The purge gas replaces gas remaining inside the processing vessel.
[0014] The technology of the present disclosure will be described in detail later, but in the supply of nitriding gas (step S104), N 2 This uses NH as the nitriding gas. 3 Compared to the case where a nitriding gas is used, the film quality of the silicon nitride film Wc can be improved and the wet etching resistance can be improved. 2If gas is used, the embeddability is reduced. Therefore, before the supply of the adsorption inhibitor gas (step S101) is carried out again, the supply of the adsorption promoter gas (step S106) is carried out. This makes it possible to maintain the V-shaped cross-sectional shape and improve the embeddability.
[0015] Step S101 includes plasmatizing an adsorption inhibitor gas and supplying it to the substrate surface Wa. The adsorption inhibitor gas is adsorbed to the substrate surface Wa. The adsorption inhibitor gas adsorbates Wd to form non-adsorption sites that inhibit the adsorption of the silicon-containing gas. The density of the non-adsorption sites decreases as the depth from the substrate surface Wa increases. The density distribution of the non-adsorption sites is controlled by the supply time of the adsorption inhibitor gas, etc.
[0016] The adsorption inhibitor gas includes, for example, at least one of a halogen gas, a non-halogen gas, or a mixture of a halogen gas and a non-halogen gas. The halogen gas is, for example, F 2 Gas, Cl 2 gas or HF gas, preferably Cl 2 Non-halogen gases are, for example, N 2 Chlorine (Cl) or nitrogen (N) is likely to be adsorbed to the adsorption sites of the silicon-containing gas and is likely to inhibit the adsorption of the silicon-containing gas.
[0017] The processing conditions of step S101 may be changed according to the number of times step S101 is performed, for example, the supply time of the adsorption inhibitory gas may be changed. In the early stage of the film formation process, the aspect ratio (depth / opening width) of the recess Wb is large, and it is necessary to make the density difference of the non-adsorption sites in the depth direction of the recess Wb large. Therefore, in the early stage of the film formation process, Cl, which has a high adsorption inhibitory effect, is used as the adsorption inhibitory gas. 2 The gas is supplied for a first set time, which helps maintain the V-shaped cross-sectional shape.
[0018] On the other hand, in the later stage of the film formation process, the aspect ratio (depth / opening width) of the recess Wb becomes smaller, so that the V-shaped cross-sectional shape is easily maintained even if the density difference of the non-adsorption sites in the depth direction of the recess Wb becomes smaller. Therefore, in the later stage of the film formation process, the adsorption inhibitor gas is supplied for a second set time. The second set time is the same as or shorter than the first set time. This makes it possible to improve throughput while maintaining the V-shaped cross-sectional shape.
[0019] Although not shown, step S101 may include a first process of plasmatizing a mixed gas of a halogen gas and a non-halogen gas and supplying the plasma to the substrate surface Wa, and a second process of plasmatizing only one of the halogen gas and the non-halogen gas and supplying the plasma to the substrate surface Wa. In this case, step S101 may alternately repeat the first process and the second process multiple times.
[0020] In the early stage of the film formation process, the Cl 2 The partial pressure of the gas is N 2 By increasing the partial pressure of the gas, Cl 2 The adsorption inhibition effect of gas is N 2 In the latter stage of the film formation process, the N in the mixed gas may be relatively higher than the adsorption inhibition effect of the gas. 2 The partial pressure of the gas is Cl 2 By increasing the partial pressure of the gas, 2 The adsorption inhibition effect of gas is Cl 2 Alternatively, the partial pressure may be adjusted to be higher than the adsorption inhibition effect of the gas.Instead of or in addition to the partial pressure, the supply time may be adjusted.
[0021] The conditions in step S101 are, for example, as follows: Time: 0.05 seconds to 6 seconds, RF power: 10W~500W, Pressure: 0.1 Torr (13.3 Pa) to 50 Torr (6.7 kPa), Temperature: 350℃~600℃.
[0022] Step S102 includes supplying a silicon-containing gas to the substrate surface Wa. The deeper the substrate surface Wa, the lower the density of the adsorption inhibitor gas adsorbent Wd, and the higher the density of the silicon-containing layer, which is the adsorption material of the silicon-containing gas. Therefore, the silicon nitride film Wc can be filled into the recess Wb while maintaining the V-shaped cross-sectional shape, and the occurrence of voids and seams can be suppressed.
[0023] The silicon-containing gas may contain silicon (Si), but preferably contains a halogen. The halogen is, for example, chlorine (Cl), bromine (Br) or iodine (I). The silicon-containing gas is, for example, dichlorosilane (DCS: SiH 2 Cl 2 The silicon-containing gas is monochlorosilane (MCS: SiH 3 Cl) gas, trichlorosilane (TCS: SiHCl 3 ) gas, silicon tetrachloride (STC: SiCl 4 ) gas, or hexachlorodisilane (HCDS:Si 2 Cl 6 ) Gas may also be used.
[0024] The conditions in step S102 are, for example, as follows: Time: 1 second to 10 seconds, Pressure: 0.1 Torr (13.3 Pa) to 50 Torr (6.7 kPa), Temperature: 350℃~600℃.
[0025] Step S103 includes plasmatizing the modifying gas and supplying it to the substrate surface Wa. The modifying gas modifies the silicon-containing layer. The silicon-containing layer contains halogen in addition to silicon (Si), and the modifying gas removes the halogen contained in the silicon-containing layer. This allows dangling bonds of Si to be formed. As a result, the Si-containing layer can be activated, and nitridation of the Si-containing layer can be promoted. The modifying gas is H 2 The reformed gas includes H 2 In addition to the gas, an inert gas may be included. The inert gas may be a rare gas such as Ar gas or N2 The supply of the modifying gas (step S103) is preferably performed after the supply of the silicon-containing gas (step S102) and before the supply of the nitriding gas (step S104).
[0026] The conditions in step S103 are, for example, as follows: Time: 1 second to 10 seconds, RF power: 100W~3kW, Pressure: 0.1 Torr (13.3 Pa) to 50 Torr (6.7 kPa), Temperature: 350℃~600℃.
[0027] Step S104 includes generating a nitriding gas plasma and supplying the plasma to the substrate surface Wa. The nitriding gas nitrides the silicon-containing layer. The nitriding gas is N 2 The nitriding gas contains N 2 In addition to the gas, an inert gas may be included. The inert gas is a rare gas such as Ar gas. As will be described later in detail, NH 3 Gas, not N 2 By using the gas, the film quality of the silicon nitride film Wc can be improved, and the wet etching resistance can be increased.
[0028] The conditions in step S104 are, for example, as follows: Time: 1 second to 10 seconds, RF power: 100W~3kW, Pressure: 0.1 Torr (13.3 Pa) to 50 Torr (6.7 kPa), Temperature: 350℃~600℃.
[0029] In step S105, it is checked whether steps S101 to S104 have been performed a set number of times (k times). In this embodiment, k is 1, but it may be an integer equal to or greater than 2. If the number of times has not reached k, steps S101 to S104 are performed again. On the other hand, if the number of times has reached k, step S106 is performed.
[0030] Step S106 includes supplying an adsorption promoting gas to the substrate surface Wa. The adsorption promoting gas promotes adsorption of the silicon-containing gas. The adsorption promoting gas may or may not be plasmatized. By supplying the adsorption promoting gas (step S106) before supplying the adsorption inhibiting gas again (step S101), the V-shaped cross-sectional shape can be maintained and the embeddability can be improved.
[0031] The adsorption promoting gas is NH 2 It preferably contains the group NH 2 The groups function as adsorption sites for the silicon-containing gas. 3 N instead of gas 2 By using gas, NH 2 In step S106, NH 2 The groups can be adsorbed over the entire substrate surface Wa and over the entire depth of the recesses Wb. Therefore, by performing step S101 thereafter, it is easy to create a difference in density of adsorption sites in the depth direction of the recesses Wb, and the embedding property can be improved.
[0032] The adsorption promoting gas is, for example, NH 3 Gas, N 2 H 4 Gas, N 2 H 2 Gas, CH 3 NHNH 2 Gas, CH 3 NH 2 The adsorption promoting gas includes at least one selected from NH 2 In addition to the gas containing the group, the gas may contain a rare gas such as Ar gas. 2 In addition to the radical-containing gas, a gas containing a hydrocarbon radical may also be included.
[0033] The conditions in step S106 are, for example, as follows: Time: 1 second to 10 seconds, RF power: 0W~500W Pressure: 0.1 Torr (13.3 Pa) to 50 Torr (6.7 kPa), Temperature: 350℃~600℃.
[0034] In step S107, it is checked whether step S106 has been performed a set number of times (m times). In this embodiment, m is 1, but may be an integer equal to or greater than 2. If the number of times has not reached m, step S106 is performed again. On the other hand, if the number of times has reached m, step S108 is performed.
[0035] In step S108, it is checked whether steps S101 to S104 have been performed a set number of times (k times) and step S106 has been performed a set number of times (m times). n may be an integer equal to or greater than 2. If the number of times has not reached n, the processing from step S101 onwards is performed again. On the other hand, if the number of times has reached n, the current processing is terminated.
[0036] Experimental data will be described with reference to FIG. 3 to FIG. 12. FIG. 3 to FIG. 4 show the film formation conditions of Example 1 to Example 9. In Example 1 to Example 9, the steps shown in FIG. 3 or FIG. 4 were performed n times in order from left to right. In Example 1 to Example 9, k was 1, m was 1, and n was 300. In FIG. 3 and FIG. 4, the steps just before S101, just before S103, just before S104, and just before S106 are steps for adjusting the flow rate of gas. In FIG. 3 and FIG. 4, "plasma" being "ON" means that the gas was made into plasma, and "plasma" being "OFF" means that the gas was not made into plasma. Examples 1 to 7 are reference examples, and Examples 8 to 9 are working examples. FIG. 5 shows an SEM photograph of a substrate W obtained under the film formation conditions of Example 8 as a representative example. As shown in FIG. 5, according to Example 8, when filling the inside of the recess Wb with the silicon nitride film Wc, the generation of voids and seams could be suppressed.
[0037] First, the relationship between the WER and the depth of the silicon nitride film obtained under the film forming conditions of Examples 1 and 2 will be described with reference to FIG. 6. The WER is the etching speed of the silicon nitride film by dilute hydrofluoric acid (HF concentration: 0.5% by volume). The smaller the WER, the better the film quality. In Example 1, N was used as the nitriding gas. 2 In Example 2, NH was used as the nitriding gas. 3 As shown in Fig. 6, NH 3 N instead of gas 2 It can be seen that the use of gas can reduce the WER and improve the film quality.
[0038] Next, referring to FIG. 7, the relationship between the GPC and the depth of the silicon nitride film obtained under the film forming conditions of Examples 1 to 4 will be described. GPC is the film forming speed of the silicon nitride film per cycle. If the GPC is larger as the depth increases, the cross-sectional shape becomes V-shaped. In Example 3, the film forming process was performed under substantially the same conditions as Example 1, except that step S101 was omitted. In Example 4, the film forming process was performed under substantially the same conditions as Example 2, except that step S101 was omitted.
[0039] In FIG. 7, by comparing Example 2 and Example 4, NH 3 When using a nitriding gas, it is found that if an adsorption inhibitor gas is supplied (step S101), a V-shaped cross-sectional shape can be obtained even without supplying an adsorption promoter gas (step S106). 2 When gas is used, it is found that a V-shaped cross-sectional shape cannot be obtained even if the supply of the adsorption inhibitor gas (step S101) is performed.
[0040] From the results in Fig. 6 and Fig. 7, N 2 When gas is used, NH is used as the nitriding gas. 3 It can be seen that the film quality of the silicon nitride film Wc can be improved and the wet etching resistance can be improved compared to the case where a nitriding gas is used, but the embedding ability is deteriorated. 2By combining the use of the gas with the supply of the adsorption promoting gas, both wet etching resistance and embeddability are achieved.
[0041] Next, the relationship between GPC and depth of the silicon nitride film obtained under the film forming conditions of Examples 5 to 7 will be described with reference to FIG. 8. In Example 5, the supply of the adsorption promoting gas (step S106) was not performed, whereas in Examples 6 and 7, the supply of the adsorption promoting gas (step S106) was performed. It can be seen from FIG. 8 that the GPC increases by performing the supply of the adsorption promoting gas (step S106). Note that in all of Examples 5 to 7, the nitriding gas was N 2 In addition, in all of Examples 5 to 7, the supply of the adsorption inhibitor gas (step S101) was not performed.
[0042] In Fig. 8, by comparing Example 6 and Example 7, it can be seen that if the adsorption promoting gas is made into plasma, the GPC can be increased and the throughput (number of wafers processed per unit time) can be improved. On the other hand, if the adsorption promoting gas is not made into plasma, it can be seen that the GPC can be increased at a constant rate regardless of the depth direction. If the GPC can be increased at a constant rate, it is advantageous in obtaining a V-shaped cross-sectional shape by supplying an adsorption inhibiting gas (step S101).
[0043] Next, the relationship between the GPC and the depth of the silicon nitride films obtained under the film formation conditions of Examples 6, 8, and 9 will be described with reference to Fig. 9. In Examples 6, 8, and 9, the film formation process was performed under the same conditions except for the supply time of the adsorption inhibitor gas (time of S101) as shown in Fig. 4. It can be seen from Fig. 9 that the GPC can be reduced by extending the supply time of the adsorption inhibitor gas.
[0044] Next, the relationship between the GPC and the depth of the silicon nitride films obtained under the film forming conditions of Examples 1, 2, and 8 will be described with reference to FIGS. 10 and 11. X-250 This refers to the ratio of GPC at a depth of X nm when the GPC at a depth of 250 nm is taken as 1. From Figs. 10 and 11, especially Fig. 11, it can be seen that N 2It can be seen that when gas is used, a V-shaped cross-sectional shape can be obtained by supplying an adsorption inhibiting gas (step S101) and an adsorption promoting gas (step S106).
[0045] Next, referring to FIG. 12, the WER0 and GPC of the silicon nitride films obtained under the film forming conditions of Examples 1, 2, and 8 were compared. 0-250 In FIG. 12, the relationship between WER 0 is the WER at a depth of 0 nm. 0-250 This refers to the ratio of GPC at a depth of 0 nm when the GPC at a depth of 250 nm is taken as 1. It can be seen from Fig. 12 that according to Example 8, a silicon nitride film having physical properties intermediate between those of Examples 1 and 2 can be obtained.
[0046] A film forming apparatus according to one embodiment will be described with reference to Fig. 13. The film forming apparatus includes a processing vessel 1, a holder 2, a shower head 3, an exhaust unit 4, a gas supply unit 5, a plasma generating unit 8, a control unit 9, and the like.
[0047] The processing vessel 1 is made of a metal such as aluminum and has a substantially cylindrical shape. The processing vessel 1 accommodates a substrate W. A loading / unloading port 11 is formed in a side wall of the processing vessel 1 for loading or unloading the substrate W. The loading / unloading port 11 is opened and closed by a gate valve 12. An annular exhaust duct 13 having a rectangular cross section is provided on the main body of the processing vessel 1. A slit 13a is formed along the inner peripheral surface of the exhaust duct 13. An exhaust port 13b is formed in the outer wall of the exhaust duct 13. A top wall 14 is provided on the upper surface of the exhaust duct 13 so as to close the upper opening of the processing vessel 1 via an insulating member 16. A seal ring 15 is used to hermetically seal the space between the exhaust duct 13 and the insulating member 16. The partition member 17 partitions the inside of the processing vessel 1 into upper and lower sections when the holder 2 and the cover member 22 are raised to a processing position described later.
[0048] The holder 2 holds the substrate W horizontally inside the processing vessel 1. The holder 2 is formed in a disk shape having a size corresponding to the substrate W, and is supported by a support member 23. The holder 2 is made of a ceramic material such as AlN or a metal material such as an aluminum or nickel alloy, and has a heater 21 embedded therein for heating the substrate W. The heater 21 generates heat when power is supplied from a heater power source (not shown). The output of the heater 21 is controlled by a temperature signal from a thermocouple (not shown) provided near the upper surface of the holder 2, thereby controlling the substrate W to a predetermined temperature. The holder 2 is provided with a cover member 22 made of ceramics such as alumina so as to cover the outer peripheral region of the upper surface and the side surfaces.
[0049] A support member 23 for supporting the holding part 2 is provided on the bottom surface of the holding part 2. The support member 23 extends from the center of the bottom surface of the holding part 2 through a hole formed in the bottom wall of the processing vessel 1 to the bottom of the processing vessel 1, and its lower end is connected to a lifting mechanism 24. The lifting mechanism 24 raises and lowers the holding part 2 via the support member 23 between a processing position shown in FIG. 13 and a transfer position shown by a two-dot chain line below the processing position where the substrate W can be transferred. A flange 25 is attached to the bottom of the processing vessel 1 of the support member 23. A bellows 26 is provided between the bottom surface of the processing vessel 1 and the flange 25. The bellows 26 separates the atmosphere inside the processing vessel 1 from the outside air, and expands and contracts with the lifting and lowering operation of the holding part 2.
[0050] Three support pins 27 (only two shown) are provided near the bottom surface of the processing vessel 1 so as to protrude upward from a lifting plate 27a. The support pins 27 are raised and lowered via the lifting plate 27a by a lifting mechanism 28 provided below the processing vessel 1. The support pins 27 are inserted into through holes 2a provided in the holder 2 at the transfer position and can be protruded and retracted from the upper surface of the holder 2. The substrate W is transferred between the transfer mechanism (not shown) and the holder 2 by raising and lowering the support pins 27.
[0051] The shower head 3 supplies gas into the processing vessel 1 in a shower-like manner. The shower head 3 is made of metal, is provided to face the holder 2, and has approximately the same diameter as the holder 2. The shower head 3 has a main body 31 and a shower plate 32. The main body 31 is fixed to the ceiling wall 14 of the processing vessel 1. The shower plate 32 is connected below the main body 31. A gas diffusion space 33 is formed between the main body 31 and the shower plate 32. A gas introduction hole 36 is provided in the gas diffusion space 33 so as to penetrate the center of the ceiling wall 14 and the main body 31 of the processing vessel 1. An annular protrusion 34 protruding downward is formed on the periphery of the shower plate 32. A gas discharge hole 35 is formed on the inner flat portion of the annular protrusion 34. When the holder 2 is in the processing position, a processing space 38 is formed between the holder 2 and the shower plate 32, and the upper surface of the cover member 22 and the annular protrusion 34 are close to each other to form an annular gap 39.
[0052] The exhaust unit 4 exhausts the inside of the processing vessel 1. The exhaust unit 4 has an exhaust pipe 41 connected to the exhaust port 13b, and an exhaust mechanism 42 having a vacuum pump, a pressure control valve, etc. connected to the exhaust pipe 41. During processing, gas inside the processing vessel 1 reaches the exhaust duct 13 through the slit 13a, and is exhausted by the exhaust mechanism 42 from the exhaust duct 13 through the exhaust pipe 41.
[0053] The gas supply unit 5 supplies various gases into the processing vessel 1 via, for example, the shower head 3. The gas supply unit 5 includes a gas source 51 and a gas line 52. The gas source 51 includes, for example, a mass flow controller and a valve (none of which are shown). The gases supplied include an adsorption inhibitor gas, a silicon-containing gas, a nitriding gas, a modifying gas, and an adsorption promoter gas, as shown in FIG. 2. The gases supplied may include a purge gas. The various gases are introduced from the gas source 51 into the gas diffusion space 33 via the gas line 52 and the gas introduction hole 36.
[0054] The plasma generating unit 8 converts the gas supplied by the gas supply unit 5 into plasma. The film forming apparatus is, for example, a capacitively coupled plasma apparatus, in which the holding unit 2 functions as a lower electrode and the shower head 3 functions as an upper electrode. The holding unit 2 is grounded via a capacitor (not shown). However, the holding unit 2 may be grounded, for example, without a capacitor, or may be grounded via a circuit combining a capacitor and a coil. The shower head 3 is connected to the plasma generating unit 8.
[0055] The plasma generating unit 8 supplies high frequency power (hereinafter also referred to as "RF power") to the showerhead 3. The plasma generating unit 8 has an RF power source 81, a matching box 82, and a power feed line 83. The RF power source 81 is a power source that generates RF power. The RF power has a frequency suitable for generating plasma. The frequency of the RF power is, for example, within a range from 450 KHz in the low frequency band to 2.45 GHz in the microwave band. The RF power source 81 is connected to the main body 31 of the showerhead 3 via the matching box 82 and the power feed line 83. The matching box 82 has a circuit for matching the load impedance to the internal impedance of the RF power source 81.
[0056] Although the plasma generating unit 8 has been described as supplying RF power to the shower head 3 serving as the upper electrode, the present invention is not limited to this. It may be configured to supply RF power to the holder 2 serving as the lower electrode. The plasma generating unit 8 is not limited to capacitively coupled plasma, and may generate other types of plasma, such as inductively coupled plasma or remote plasma.
[0057] The control unit 9 is, for example, a computer, and includes a CPU (Central Processing Unit), a RAM (Random Access Memory), a ROM (Read Only Memory), an auxiliary storage device, etc. The CPU operates based on a program stored in the ROM or the auxiliary storage device, and controls the operation of the film forming apparatus. The control unit 9 controls the exhaust unit 4, the gas supply unit 5, and the plasma generation unit 8, and performs control to implement the film forming method shown in FIG. 2.
[0058] Although the embodiments of the film forming method and the film forming apparatus according to the present disclosure have been described above, the present disclosure is not limited to the above-mentioned embodiments. Various changes, modifications, substitutions, additions, deletions, and combinations are possible within the scope of the claims. Naturally, these also fall within the technical scope of the present disclosure. [Explanation of symbols]
[0059] W substrate Wa substrate surface Wb Concave Wc silicon nitride film
Claims
1. 1. A method for forming a film, comprising the steps of: forming a silicon nitride film in a recess on a surface of a substrate, the step of forming the silicon nitride film includes a step of plasmatizing an adsorption inhibitor gas that inhibits adsorption of a silicon-containing gas and supplying the plasmatized gas to the substrate surface, a step of supplying the silicon-containing gas to the substrate surface, and a step of plasmatizing a nitriding gas that nitrides adsorbates of the silicon-containing gas and supplying the plasmatized gas to the substrate surface, The nitriding gas is N 2 Including gas, The process of forming the silicon nitride film includes a step of supplying an adsorption-promoting gas that promotes adsorption of the silicon-containing gas to the substrate surface, and the process of performing a process including supplying the adsorption-inhibiting gas, supplying the silicon-containing gas, and supplying the nitriding gas one or more times, and supplying the adsorption-promoting gas one or more times is repeated multiple times in the film formation method.
2. The adsorption promoting gas is NH 2 The film forming method according to claim 1 , further comprising a group.
3. The adsorption promoting gas is NH 3 Gas, N 2 H 4 Gas, N 2 H 2 Gas, CH 3 N.H.N.H. 2 Gas, CH 3 N.H. 2 The method of claim 2 , further comprising at least one selected from the group consisting of a gas.
4. The step of forming the silicon nitride film includes a step of generating plasma of a modifying gas that modifies an adsorbed substance of the silicon-containing gas and supplying the plasma to the surface of the substrate; The reformed gas is H 2 The film forming method according to any one of claims 1 to 3, further comprising a gas.
5. 5. The film forming method according to claim 4, wherein the supply of the modifying gas is performed after the supply of the silicon-containing gas and before the supply of the nitriding gas.
6. The film forming method according to claim 4 , wherein the modifying gas further includes an inert gas.
7. 4. The film forming method according to claim 1, wherein the step of forming the silicon nitride film comprises the step of converting the adsorption promoting gas into plasma and supplying the plasma to the surface of the substrate.
8. 4. The film forming method according to claim 1, wherein the step of forming the silicon nitride film comprises the steps of: supplying the adsorption promoting gas to the substrate surface without converting the adsorption promoting gas into plasma; and converting the adsorption promoting gas into plasma and supplying the adsorption promoting gas to the substrate surface.
9. 9. The film forming method according to claim 8, wherein the step of forming the silicon nitride film comprises a step of supplying the adsorption promoting gas to the substrate surface without converting the adsorption promoting gas into plasma, and a step of converting the adsorption promoting gas into plasma and supplying the adsorption promoting gas to the substrate surface, the steps being repeated multiple times.
10. 4. The film forming method according to claim 1, wherein the adsorption inhibiting gas includes at least one of a halogen gas, a non-halogen gas, or a mixed gas of the halogen gas and the non-halogen gas.
11. 11. The film forming method according to claim 10, wherein the step of forming the silicon nitride film comprises the steps of: converting a mixed gas of the halogen gas and the non-halogen gas into plasma and supplying the plasma to the substrate surface; and converting only one of the halogen gas and the non-halogen gas into plasma and supplying the plasma to the substrate surface.
12. 12. The film formation method according to claim 11, wherein the step of forming the silicon nitride film includes a step of converting a mixed gas of the halogen gas and the non-halogen gas into plasma and supplying the plasma to the substrate surface, and a step of converting only one of the halogen gas and the non-halogen gas into plasma and supplying the plasma to the substrate surface, the steps being alternately repeated multiple times.
13. The halogen gas is Cl 2 gas, the non-halogen gas being N 2 The film forming method according to claim 10 , wherein the gas is a gas.
14. 4. The film forming method according to claim 1, wherein the silicon-containing gas contains silicon and a halogen.
15. a processing vessel for accommodating a substrate; a holder for holding the substrate inside the processing vessel; a gas supply unit that supplies a gas into the processing chamber; a plasma generating unit that converts the gas supplied by the gas supply unit into plasma; A control unit that controls the gas supply unit and the plasma generation unit; Equipped with The control unit performs control for implementing the film forming method according to any one of claims 1 to 3.
Citation Information
Patent Citations
Deposition method of silicon nitride film
JP2018010950A
Method for deposition of nitride film and apparatus for deposition of nitride film
JP2020113743A
Silicon nitride film forming method and film forming apparatus
JP2022111765A
Cited By
Substrate processing method and substrate processing apparatus
WO2026160002A1