Manufacturing method for molten steel

By immersing electrodes and lances in molten slag and controlling oxygen supply within specific parameters, the method addresses the impracticality and cost of inert gas use, achieving efficient dephosphorization and denitrification in electric furnaces.

JP2024134727AActive Publication Date: 2024-10-04NIPPON STEEL CORPORATION

Patent Information

Application Number
JP2023045071
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04
Estimated Expiration
2043-03-22

AI Technical Summary

Technical Problem

Existing methods for producing low-nitrogen molten steel in electric furnaces are impractical due to high costs associated with the use of inert gases, and there is a need for a cost-effective method that can efficiently perform dephosphorization and denitrification.

Method used

A method involving submerged arc operation and controlled oxygen supply using lances, where the electrode and lance tips are immersed in molten slag to interrupt nitrogen gas contact, and oxygen is supplied within specific height and flow rate ranges to prevent nitrogen diffusion, as defined by equations (1) and (2).

Benefits of technology

This method effectively suppresses nitrogen absorption into molten iron, maintaining efficient dephosphorization and denitrification without increasing costs, while preventing lance damage and ensuring continuous slag formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134727000001_ABST
    Figure 2024134727000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method for molten steel that can efficiently perform dephosphorization and denitration in an electric furnace using a simple method that does not involve an increased cost.SOLUTION: In an electric furnace that has a lance for supplying oxygen to the inside of the furnace and a slag outlet on the side wall of a furnace body for discharging slag generated inside of the furnace, a manufacturing method for molten steel by discharging the slag while forming the slag, where the height measured vertically from a stationary molten steel surface of the electric furnace to the center of the nozzle at the tip of the lance is set to a range where the lance tip does not corrode and is not exposed during slag removal, and a condition is set for blowing oxygen gas onto the molten iron surface with a specified range of an oxygen gas flow rate, and the period in which the condition is met is set to 60% or more of the oxygen supply time.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing molten steel for producing low-nitrogen steel using an electric furnace. [Background technology]

[0002] In recent years, electric furnaces have been attracting attention as an environmentally friendly way to achieve decarbonization in steel production. When producing high-purity steel with low impurity content, typical impurities in steel materials include phosphorus and nitrogen. In the dephosphorization method in an electric furnace, phosphorus is oxidized with oxygen gas in the presence of slag, which is mainly composed of calcium oxide, and is absorbed into the slag as phosphoric acid. In addition, a method called "flowing slag operation" is commonly used in which the slag is expanded by foaming with carbon monoxide gas generated by the reaction of oxygen gas with carbon in the molten iron, and the slag is discharged outside the furnace through a slag outlet installed on the side wall of the furnace.

[0003] On the other hand, when producing molten steel using an electric furnace, the main nitrogen source in the steel is nitrogen gas in the atmosphere, and when the slag outlet is opened for the slag operation, the air inevitably flows into the furnace. In order to produce high-purity steel with low phosphorus and low nitrogen in the operation using an electric furnace, it is necessary to prevent the diffusion of the nitrogen gas that flows into the furnace by the slag operation onto the molten iron surface.

[0004] Therefore, as a technique for preventing diffusion of nitrogen gas onto the surface of molten iron in an electric furnace, Patent Document 1 discloses a method of supplying an inert gas such as argon into the furnace. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Special Publication No. 2022-500556 [Non-patent literature]

[0006] [Non-Patent Document 1] ISIJ Int., Vol. 51,(2011) No.9, p1439-1447. Summary of the Invention [Problem to be solved by the invention]

[0007] However, the method using an inert gas as described in Patent Document 1 has a problem in that it is not practical because it requires high costs due to the use of hollow electrodes and inert gas.

[0008] In view of the above problems, an object of the present invention is to provide a method for producing molten steel that is capable of efficiently carrying out dephosphorization and denitrification in an electric furnace by a simple method that does not increase costs. [Means for solving the problem]

[0009] The inventors of the present invention have studied methods for preventing the diffusion of nitrogen gas onto the molten iron surface, and first focused on the route by which nitrogen gas is supplied to the molten iron surface. It is believed that the diffusion of nitrogen gas onto the molten iron surface is promoted at a location where a flow from the top of the electric furnace toward the molten iron surface occurs. Such locations where a flow from above toward the molten iron surface occurs are assumed to be near the electrode where the arc jet is generated and near the lance that supplies oxygen into the electric furnace.

[0010] The inventors first noticed that the absorption of nitrogen gas near the electrode can be suppressed by submerged arc operation in which the electrode is immersed in the molten slag in the furnace. In submerged arc operation, the electrode is immersed in the molten slag, creating a state in which the arc jet is generated only below the slag surface, and the contact between the arc jet and the nitrogen gas in the furnace is physically blocked, thereby suppressing the supply of nitrogen gas to the molten iron surface.

[0011] The inventors also came up with the idea that, in the vicinity of the lance, as in the submerged arc operation, the tip of the lance can be immersed in the molten slag to block contact between the oxygen jet and the nitrogen gas in the furnace, thereby suppressing the supply of nitrogen gas to the molten iron surface. Depending on the flow rate of oxygen gas and the distance between the lance tip and the molten iron surface, the lance tip may melt or become exposed, causing nitrogen absorption to proceed. The inventors found that there are suitable conditions for these.

[0012] The present invention is as follows. [1] A method for producing molten steel in an electric furnace having a lance for supplying oxygen into the furnace and a slag discharge port for discharging slag generated in the furnace on a side wall of the furnace body, comprising the steps of: discharging the slag while foaming the slag, The height H (mm) measured vertically from the stationary molten iron surface of the electric furnace to the nozzle center position of the tip of the lance and the flow rate Q (Nm 3 / h) for 60% or more of the time during which oxygen is being supplied so as to satisfy the following formulas (1) and (2): {6540(Q / d) 2} 1 / 3 <H 49.5≦Q / A≦96.5 (2) In the formula, d is the inner diameter (mm) of the nozzle outlet of the lance, H1 is the height (mm) measured vertically from the stationary molten iron surface in the electric furnace to the bottom end of the slag outlet, w is the horizontal width (mm) of the slag outlet, and A is the maximum value of the horizontal cross-sectional area (m 2 ) Effect of the Invention

[0013] According to the present invention, it is possible to provide a method for producing molten steel that is capable of efficiently carrying out dephosphorization and denitrification in an electric furnace by a simple method that does not involve an increase in cost. [Brief description of the drawings] ​

[0014] [Figure 1] FIG. 2 is a diagram for explaining the internal structure of an electric furnace. [Diagram 2] FIG. 2 is a diagram for explaining a state in which oxygen gas collides with a molten iron surface. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. FIG. 1 is a diagram for explaining the internal structure of an electric furnace. As shown in FIG. 1, an alternating current is supplied to an electrode 3 from a power source (not shown), and an arc formed from the electrode 3 heats molten iron 2 in a furnace body 1 at an arc spot. A slag outlet 7 is provided on a side wall of the furnace body 1 and is used for discharging molten slag 6, etc. A movable lance 4a for supplying oxygen gas is inserted from the slag outlet 7, and the manipulator 5 can change the height of the tip of the movable lance 4a from the molten iron surface and the angle with respect to the molten iron surface within its movable range. In this embodiment, another movable lance 4b is inserted into the furnace body 1 and is used to supply a solid carbon source. Similarly, the manipulator 5 can change the height of the tip of the movable lance 4b from the molten iron surface and the angle with respect to the molten iron surface within its movable range.

[0016] 1, the slag discharge port 7 is always open, but when the movable lances 4a, 4b are not used, the movable lances 4a, 4b may be moved out of the furnace body 1 from the slag discharge port 7 and the slag discharge port 7 may be closed during that time. In other words, the slag discharge port 7 may be opened only when oxygen gas is fed or when a solid carbon source is supplied, and when slag is discharged.

[0017] Next, a specific method for producing molten steel will be described. First, in the furnace body 1, a part of the molten steel generated in the pre-charge is left as a seed molten metal. Scrap, a carbon source, and a lime source are charged into the seed molten metal. The electrode 3 is lowered to the vicinity of the molten iron surface, an arc is generated from the lower end of the electrode 3, and oxygen gas is blown from the movable lance 4a to melt the scrap. Next, while the arc is generated from the electrode 3, a solid carbon source is supplied from the movable lance 4b, and oxygen gas is continuously blown from the movable lance 4a to perform dephosphorization, decarburization, and denitrification treatment. By blowing oxygen gas in this way, oxygen reacts with carbon in the molten iron to generate CO gas, and the molten slag 6 forms, causing the slag surface of the molten slag 6 to rise. Then, for example, when the slag surface reaches a position slightly higher than the lower end of the slag discharge port 7, the molten slag 6 is discharged from the slag discharge port 7. Since the molten slag 6 is foaming even while it is being drained, the molten slag 6 is constantly being drained from the slag drain port 7 during the forming process. Then, when the concentrations of phosphorus and nitrogen have sufficiently decreased after blowing oxygen gas for a predetermined period of time, molten steel is tapped from the tapping hole.

[0018] On the other hand, since the slag outlet 7 is open and air flows into the furnace body 1, it is necessary to prevent the nitrogen gas from being absorbed into the molten iron. As mentioned above, it is considered that the diffusion of nitrogen gas to the molten iron surface is promoted at the point where the flow from the top of the electric furnace toward the molten iron surface occurs. Therefore, by immersing the electrode 3 in the molten slag 6, the arc jet is generated only below the slag surface, and the contact between the arc jet and the nitrogen gas in the furnace is physically blocked.

[0019] Furthermore, in this embodiment, the tip of the movable lance 4a is immersed in the molten slag 6 to block contact between the oxygen gas and the nitrogen gas in the furnace, thereby suppressing the supply of nitrogen gas to the molten iron surface. Here, when performing both slag flow operation and immersion of the lance tip, if the lance tip is brought close to the molten iron surface, immersion in the molten slag is guaranteed, but the blown oxygen gas may cause high-temperature molten iron to splash and the lance tip to melt. Since lance melting is undesirable from the viewpoint of equipment protection, it is necessary to avoid this. On the other hand, if the lance tip is moved too far from the molten iron surface, molten slag constantly flows out of the furnace during slag flow operation, making it difficult to immerse the lance tip in the molten slag.

[0020] From the above, in the slag flow operation, it is important to spray oxygen gas toward the molten iron surface at a lance height that can avoid melting of the tip of the lance while being immersed in the molten slag. In the example shown in FIG. 1, the movable lance 4b that supplies the solid carbon source is also immersed in the molten slag, but it is not necessary to immerse the movable lance 4b in the molten slag. However, from the viewpoint of the yield of the carbon source, it is preferable to immerse the movable lance 4b in the molten slag. The appropriate lance height will be explained below with reference to FIG. 2.

[0021] The scattering of molten iron when oxygen gas is blown is thought to occur because the kinetic energy of the oxygen gas, which reverses direction after colliding with the molten iron, is transferred to the molten iron. Assuming that the oxygen gas reverses direction after collision in a direction perpendicular to the lance axis, the flow velocity at the height of the stationary molten iron surface is v t (m / s), the maximum splash height of molten iron per unit volume is h max The potential energy of (mm) is expressed by the law of conservation of energy as shown in the following equation (3).

[0022]

number

[0023] In equation (3), η1 is the efficiency of energy transfer from oxygen gas to molten iron, ρ gis the density of oxygen gas (kg / m 3 ), ρ l is the density of molten iron (kg / m 3 ), θ is the angle between the lance axis direction and the vertical direction (deg), g is the gravitational acceleration (m / s 2 According to Non-Patent Document 1, the flow velocity v t is the oxygen gas flow rate v at the bottom of the cavity created by oxygen supply. j The relationship between the flow velocity v0 (m / s) of the oxygen gas at the nozzle outlet of the lance and the flow velocity v1 (m / s) is expressed by the following equations (4) and (5).

[0024]

number

[0025] In equations (4) and (5), η2 and η3 are the coefficients related to the attenuation of the oxygen gas jet, d is the inner diameter of the nozzle outlet (mm), H is the height from the stationary molten iron surface to the center of the lance nozzle (hereinafter referred to as the lance tip height) (mm), and d p represents the cavity depth (mm) from the stationary molten iron surface to the lowest part of the cavity. Furthermore, the cavity depth d p The following equation (6) holds between the kinetic energy of the oxygen gas and

[0026]

number

[0027] In order to avoid the splashing of molten iron onto the tip of the lance, the height H of the lance tip must be less than the maximum splash height h of the molten iron. max For simplicity, the flow rate of oxygen gas at the nozzle outlet of the lance, v0, is assumed to be the flow rate of oxygen gas supplied from the lance, Q (Nm 3 / h) divided by the cross-sectional area of ​​the lance nozzle outlet, and h max By rearranging equations (3) to (6) with =H, we obtain the relationship in equation (7) below.

[0028]

number

[0029] Here, η is a coefficient influenced by the lance angle, jet damping, and the rate of energy transfer from oxygen gas to molten iron. The inventors experimentally investigated the relationship between the lance tip height H and the oxygen gas flow rate Q and found that it can be approximated by η = 6540 within the normal operating range.

[0030] Next, to examine the thickness of the slag during slag flow operation, the increase and decrease in slag volume was modeled as follows. The forming slag volume V (m 3 Since the increase in slag volume per unit time is due to the continuous generation of CO gas produced by the decarburization reaction, it is considered that the increase in slag volume per unit time is proportional to the flow rate of oxygen gas Q. In addition, if the vertical height from the bottom of the slag discharge port to the stationary slag surface is h (mm) and the horizontal width of the slag discharge port is w (mm), the vertical cross-sectional area of ​​the slag flow at the slag discharge port is wh (mm 2 ) and the amount of slag flowing out per unit time is considered to be proportional to wh. Therefore, the change in the volume of slag in the tailings can be expressed as the following equation (8) using appropriate constants k1 and k2.

[0031]

number

[0032] According to formula (8), the slag volume V increases with oxygen flow, and when it reaches a height where dV / dt = 0, it becomes stationary and the volume stops changing. The condition where dV / dt = 0 is given by the following formula (9). h = k(Q / w) (9)

[0033] Here, k is a constant. Based on the above model, the present inventors experimentally determined k by measuring the height of the slag surface during operation in an electric furnace, and found that the actual slag height can be reproduced with k = 31.25 when the slag basicity is in a condition suitable for dephosphorization (C / S is about 1.2 to 3.5).

[0034] From the above, it is possible to immerse the tip of the lance in the molten slag without melting it by setting the height H (mm) of the tip of the lance, measured vertically from the stationary molten iron surface in the electric furnace to the center position of the nozzle at the tip of the lance, within the range of the following formula (1). {6540(Q / d) 2} 1 / 3 <H Here, H1 (mm) is the vertical height from the stationary molten iron surface to the bottom of the slag discharge port in an electric furnace.

[0035] In addition, in order to prevent the adsorption of nitrogen from the atmosphere, it is desirable to keep the tip of the lance immersed in the slag for a long time. Therefore, it is essential to foam the molten slag quickly and maintain the slag state after the start of oxygen supply. Here, if the oxygen gas flow rate Q is small and the amount of CO gas generated is small, the expansion speed of the molten slag is low, and it takes a long time for the lance tip to be immersed. In addition, if the oxygen gas flow rate Q is small, the amount of foaming is small, so the amount of slag discharged per unit time in the slag operation is also small, and the operation time is long, which increases the operation cost. On the other hand, if the oxygen gas flow rate Q becomes excessive, the large amount of CO gas generated will blow over the slag surface without foaming the slag, leading to the exposure of the lance tip.

[0036] The state of forming is determined by the amount of CO gas generated per unit area of ​​the stationary molten iron surface in the electric furnace. From this viewpoint, the flow rate Q of oxygen gas suitable for the present invention is set to a range that satisfies the following formula (2). 49.5≦Q / A≦96.5 (2) In formula (2), A is the maximum horizontal cross-sectional area in the electric furnace (m 2 ​).

[0037] The conditions shown in formulas (1) and (2) need to be maintained for as long as possible while oxygen is being supplied from the lance. As a result of experiments conducted by the present inventors, it was found that when the conditions shown in formulas (1) and (2) are maintained for at least 60% of the time during which oxygen is being supplied, nitrogen absorption into the molten iron is suppressed and damage to the lance due to the splashing of molten iron can be prevented.

[0038] In addition, in the present invention, it is desirable to eliminate factors that inhibit the expansion of the slag due to foaming as much as possible in order to maintain the flowing slag state. If the temperature of the molten slag becomes too high, the viscosity of the molten slag decreases, and the bubbles contained in the molten slag become more likely to break, which leads to the inhibition of foaming. Therefore, in a preferred embodiment of the present invention, oxygen gas is used solely for the oxidation of the molten iron components, and is supplied into the furnace so as to avoid heat generation due to the combustion of the generated CO gas.

[0039] In addition, in this embodiment, an example in which the molten slag is discharged without tilting the electric furnace has been described, but the present invention can also be applied to the case in which the molten slag is discharged by tilting the furnace body. However, the stationary molten iron surface and the slag surface change depending on whether the furnace body is tilted or not. Since the electrode 3 is located almost in the center of the furnace, the immersion depth of the electrode 3 relative to the slag surface does not change significantly, but since the lance is located close to the slag discharge port, the height of the lance tip from the stationary molten iron surface changes significantly unless the height of the lance tip is adjusted by the manipulator. For this reason, it is necessary to adjust the height H of the lance tip so that it satisfies formula (1) even when the furnace body is tilted. In addition, the height of the electrode 3 may be adjusted when the furnace body is tilted as necessary.

[0040] As described above, when the furnace body is tilted to discharge molten slag from the slag discharge port, it is necessary that formulas (1) and (2) are satisfied for at least 60% of the time that oxygen is supplied, both when the furnace body is tilted and when it is not (when the tilt angle is 0°). Here, the tilt angle is defined as 0° when the molten iron surface in the furnace is perpendicular to the direction of the longitudinal central axis of the electrode (vertical direction). In addition, the flow rate Q of oxygen gas is also assumed to satisfy formula (2) both when the furnace body is tilted and when it is not (when the tilt angle is 0°), and A is the maximum value (m 2 )

[0041] In addition, when the removal of the molten slag is completed and the furnace body is returned to the tilt angle of 0°, the supply of oxygen gas is temporarily stopped. After the furnace body is returned to its original position, the height H of the lance tip is adjusted again and the supply of oxygen gas is resumed.

[0042] The height of the stationary molten iron surface in an electric furnace can be calculated, for example, from the weight of molten iron melted in the electric furnace and the shape and tilt angle of the electric furnace, but it can also be measured using other means such as an optical method. In addition, although an AC electric furnace has been described in this embodiment, the present invention can also be applied to a DC electric furnace. EXAMPLES

[0043] Next, an embodiment of the present invention will be described, but the conditions are merely examples of conditions for confirming the feasibility and effects of the present invention, and the present invention is not limited to the description of the embodiment. The present invention can be implemented in various ways to achieve the object of the present invention without departing from the gist of the present invention.

[0044] As shown in Figure 1, when the furnace shell inner diameter is 6.8 m and the tilt angle is 0°, the maximum horizontal cross-sectional area A of the electric furnace is 36.3 m. 2The experiment was carried out using an AC electric furnace having a slag outlet 7 on the side wall with a horizontal width w of 1000 mm and a height of 995 mm, and the electric furnace was tiltable up to 15° toward the tap hole side and 10° toward the slag outlet side. The movable lances 4a and 4b were both 4.1 m long and had a nozzle outlet inner diameter d of 36 mm, and the vertical height H from the stationary molten iron surface to the nozzle center position at the tip of the lance was adjustable within a range of 0 to 890 mm.

[0045] In the experiments, the nominal tapping rate was 110 t, and 65 t of seed molten metal was left behind during tapping. The total weight of the nominal tapping rate and seed molten metal of the electric furnace was 175 t, and molten iron of the same weight was melted in the electric furnace in both the inventive example and the comparative example. In the inventive example and the comparative example, the height H1 measured vertically from the stationary molten iron surface to the bottom end of the slag outlet 7 of the electric furnace was in the range of 370 to 450 mm depending on the tilting angle.

[0046] The specific procedure for the experiment was as follows: first, scrap, anthracite, and quicklime as a slag-forming material for dephosphorization were charged into a 65-ton seed bath. The amount of quicklime charged was 30 kg / t, based on the amount of molten iron in the electric furnace when all the scrap was melted. The anthracite was supplied using the movable lance 4b of the manipulator 5. Then, the electrode 3 was lowered to the vicinity of the molten iron surface, and the scrap was melted by arcing through the electrode 3 and supplying oxygen gas from the movable lance 4a of the manipulator 5. After that, the arcing was stopped and the molten iron was sampled.

[0047] Next, the application of the arc was restarted, and anthracite was supplied as a solid carbon source into the molten iron at a rate of 150 kg / min using the movable lance 4b of the manipulator 5, while oxygen gas was supplied from the movable lance 4a at the same time. The oxygen gas flow rate Q and the height H of the lance tip from the stationary molten iron surface in the present invention and comparative examples were set to the values ​​shown in Table 1 below. The oxygen gas flow rate Q shown in Table 1 was the same as that when scrap was melted.

[0048] In the example where the furnace body was tilted to remove the molten slag, the angle of the movable lance 4a was adjusted in accordance with the tilting of the furnace body, so the height H of the lance tip from the stationary molten iron surface showed maximum and minimum values. The maximum value of the lance tip height H was mainly the height when the furnace body was not tilted, and the minimum value was mainly the height when the furnace body was tilted. However, the height of the molten iron surface fluctuated due to tilting, and the height H of the lance tip was adjusted to correspond to the fluctuation, so the maximum and minimum values ​​did not always match the height when not tilted and the height when tilted to the maximum, respectively. The height of the stationary molten iron surface was calculated by predicting the amount of molten iron in the furnace from the amount of seed molten iron and scrap charged into the furnace and the energy charged by the arc current and oxygen gas supply, and converted into the height of the stationary molten iron surface. The height H of the lance tip was calculated by subtracting the calculated height of the stationary molten iron surface from the height of the movable lance 4a controlled by the manipulator 5. It was also confirmed that during the supply of anthracite and oxygen gas, in the invention examples and comparative examples 1 to 12, slag flowed out of the electric furnace from the slag discharge port, resulting in flowing slag operation.

[0049] And oxygen gas is 875Nm 3 At this point, the supply of anthracite and oxygen gas was stopped, and the molten iron in the furnace was sampled. After confirming by chemical analysis that the carbon content of all samples was less than 0.05% by mass and the phosphorus content was less than 0.01% by mass, the molten iron in the electric furnace was tapped into a ladle.

[0050] In the present invention and this comparative example, evaluation was performed from two points of view: the effect of suppressing nitrogen absorption and the soundness of the equipment. Regarding the suppression of nitrogen absorption, the nitrogen concentration of the sample after oxygen supply was measured, and taking into account the processing capacity of the downstream equipment, those that were less than 40 ppm were marked with an O in the table, and those that were 40 ppm or more were marked with an X. Regarding the soundness of the equipment, the tip of the movable lance 4a of the manipulator used to supply oxygen gas after tapping was checked, and those that showed corrosion due to the scattering of molten iron were marked with an X in the table, and those that did not show corrosion were marked with an O. The experimental results are shown in Table 1 below.

[0051] [Table 1]

[0052] The underlines in Table 1 indicate that the conditions of the present invention are not met. In the example where the lance tip height H is greater than the upper limit of formula (1), the lance tip is not sufficiently immersed in the molten slag, so the flow of nitrogen gas from above toward the molten iron surface cannot be sufficiently blocked, and the effect of suppressing nitrogen absorption is insufficient. In the example where the lance tip height H is less than the lower limit of formula (1), although the flow of nitrogen gas could be blocked, the lance tip was too close to the molten iron surface, and thus the lance tip was melted.

[0053] Furthermore, in the example where oxygen gas was sprayed under conditions lower than the lower limit of formula (2), it took a long time for the lance tip to be immersed, and therefore nitrogen absorption could not be suppressed during that time. In addition, in the example where oxygen gas was sprayed under conditions exceeding the upper limit of formula (2), the lance tip was exposed, and therefore the flow of nitrogen gas could not be sufficiently blocked, and the nitrogen absorption suppression effect was insufficient. In contrast, all of Examples 1 to 8 of the present invention were excellent in terms of the nitrogen absorption suppression effect and the equipment soundness.

[0054] In addition, when comparing examples in which both formula (1) and formula (2) were satisfied and not satisfied, in Comparative Examples 11 and 12, both formula (1) and formula (2) were satisfied for only 55% of the time that oxygen was supplied, resulting in insufficient results in terms of nitrogen absorption suppression or equipment soundness. On the other hand, in Inventive Examples 7 and 8, both formula (1) and formula (2) were satisfied for 60% of the time that oxygen was supplied, resulting in good results in both cases. [Explanation of symbols]

[0055] 1 Furnace body 2. Molten Iron 3 electrodes 4a, 4b Movable lance 5. Manipulator 6 Molten slag 7. Slag outlet

Claims

[Claim 1] A method for producing molten steel in an electric furnace having a lance for supplying oxygen into the furnace and a slag discharge port for discharging slag generated in the furnace on a side wall of the furnace body, comprising the steps of: discharging the slag while foaming the slag, The height H (mm) measured vertically from the stationary molten iron surface of the electric furnace to the nozzle center position of the tip of the lance and the flow rate Q (Nm 3 / h) for 60% or more of a time during which oxygen is being supplied so as to satisfy the following formulas (1) and (2): {6540(Q / d) 2 } 1 / 3 <H<H 1 +31.25(Q / w) ・・・(1) 49.5≦Q / A≦96.5 ... (2) In the formula, d is the inner diameter (mm) of the nozzle outlet of the lance, H 1 is the height (mm) measured vertically from the stationary molten iron surface to the bottom end of the slag outlet in the electric furnace, w is the horizontal width (mm) of the slag outlet, and A is the maximum horizontal cross-sectional area (m 2 )

Citation Information

Patent Citations

  • Method and device for controlling depth of lance

    JP1984056513A

  • Arc furnace steel making

    JP1996176639A

  • Production of low nitrogen molten steel with arc electric furnace

    JP1998046226A

  • Electric power control method of steam supply power generating gas turbine combined plant

    JP1998266812A

  • Refining method for low-nitrogen steel using an electric furnace

    JP2022500556A

Cited By