Positive electrode plate and nonaqueous electrolyte secondary battery

The positive electrode plate with a specific composition and structure addresses the issue of decreased fusing properties and increased resistance in high nickel content batteries by optimizing the active material and resistance, ensuring effective performance in charged states.

JP2024134740AInactive Publication Date: 2024-10-04PRIME PLANET ENERGY & SOLUTIONS INC
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2023045087
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The use of a positive electrode active material with a high nickel content in non-aqueous electrolyte secondary batteries leads to decreased fusing properties and increased resistance when stored in a charged state.

Method used

A positive electrode plate design with a specific composition and structure, including a positive electrode active material represented by Li (1+x) Ni y Me (1-y) O 2, where 0≦x≦0.1 and 0.8≦y<1, and Me includes Mn, Co, and Al, along with a controlled ratio of first and second particles, acetylene black content, and adjusted plate resistance, enhances fusing properties and suppresses resistance increase.

Benefits of technology

The electrode plate maintains excellent fusing properties and prevents resistance increase in charged non-aqueous electrolyte secondary batteries, even with high nickel content active materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134740000001
    Figure 2024134740000001
Patent Text Reader

Abstract

To provide a positive electrode plate which is excellent in fusing properties and capable of suppressing an increase in resistance of a nonaqueous electrolyte secondary battery when being stored in a charged state.SOLUTION: A positive electrode plate includes an active material layer including a positive electrode active material. The positive electrode active material includes an active material represented by formula (I). An electrode plate resistance when a test cell using a lithium metal plate as a counter electrode of the positive electrode plate is charged to 4.3 V, is 0.5 Ω cm2 or more and 1.0 Ω cm2 or less. Li(1+x)NiyMe(1-y)O2 (I) [In the formula, 0≤x≤0.1 and 0.8≤y<1, and Me includes two or more selected from the group consisting of Mn, Co, Al, and Ti.]SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode plate and a non-aqueous electrolyte secondary battery. [Background technology]

[0002] It is known that in non-aqueous electrolyte secondary batteries such as lithium ion secondary batteries, a lithium transition metal composite oxide, which is a composite oxide of lithium and a transition metal, is used as the positive electrode active material contained in the active material layer of the positive electrode plate. Patent Document 1 discloses that by optimizing the distribution state of the conductive material in the active material layer containing the lithium transition metal composite oxide, it is possible to suppress an increase in resistance and increase the capacity of the battery. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2012 / 086186 Summary of the Invention [Problem to be solved by the invention]

[0004] By using a positive electrode active material with a high content of nickel (Ni) as the lithium transition metal composite oxide, it is possible to increase the capacity of the battery. However, the active material layer containing such a positive electrode active material has a low resistance, and the fusing property of the positive electrode plate is easily reduced.

[0005] The present disclosure aims to provide a positive electrode plate that has excellent fusing properties and can suppress an increase in the resistance of a nonaqueous electrolyte secondary battery when stored in a charged state, even when a positive electrode active material with a high nickel content is used. [Means for solving the problem]

[0006] [1] A positive electrode plate having an active material layer containing a positive electrode active material, The positive electrode active material has the following formula (I): Li (1+x) Niy Me (1-y) O2(I) [In the formula, 0≦x≦0.1 and 0.8≦y<1, and Me includes two or more elements selected from the group consisting of Mn, Co, Al, and Ti.] The active material is represented by When a test cell using a lithium metal plate as the counter electrode of the positive electrode was charged to 4.3 V, the plate resistance was 0.5 Ω cm 2 1.0Ω cm or more 2 Below is the positive plate. [2] When the test cell is charged within a potential range of 4.25 V or more and 4.35 V or less, the plate resistance is less than 0.5 Ω cm 2 1.0Ω cm or more 2 The positive electrode plate according to [1], which is as follows: [3] The positive electrode plate according to [1] or [2], wherein the active material includes first particles having an average particle diameter (D50) of 10 μm or more and second particles having an average particle diameter (D50) of less than 10 μm. [4] The positive electrode plate according to [3], wherein the first particles are secondary particles formed by agglomeration of primary particles. [5] The positive electrode plate according to [3] or [4], wherein a content ratio of the first particles to the second particles is 5 / 5 or more and 8 / 2 or less in mass ratio (first particles / second particles). [6] The positive electrode plate according to any one of [1] to [5], wherein the active material layer contains 0.7 mass % or more and 1.2 mass % or less of acetylene black with respect to the total amount of the positive electrode active material. [7] The positive electrode plate according to [6], wherein the average particle diameter (D50) of the acetylene black is 10 nm or more and 50 nm or less. [8] The specific surface area of ​​the acetylene black is 50 m 2 / g or more 200m 2 / g or less. [9] The active material layer has a basis weight of 350 g / m 2 The positive electrode plate according to any one of [1] to [8], having a surface roughness of 500 g / m or more and 500 g / m or less.

[10] The density of the active material layer is 3.3 g / cm 3 More than 3.7g / cm 3The positive electrode plate according to any one of [1] to [9], which is:

[11] The positive electrode plate according to any one of [1] to

[10] , wherein the content of the active material relative to the total amount of the positive electrode active material is 95 mass % or more and 100 mass % or less.

[12] An electrode assembly having a positive electrode plate, a negative electrode plate, and a separator interposed between the positive electrode plate and the negative electrode plate according to any one of [1] to

[11] ; and an electrolyte. Effect of the Invention

[0007] According to the present disclosure, it is possible to provide a positive electrode plate that has excellent fusing properties and can suppress an increase in the resistance of a nonaqueous electrolyte secondary battery when stored in a charged state, even when a positive electrode active material with a large nickel content is used. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] (Positive plate) The positive electrode plate can be used in a non-aqueous electrolyte secondary battery (hereinafter also referred to as a "battery"). The positive electrode plate has an active material layer that contains a positive electrode active material.

[0009] The positive electrode active material includes an active material represented by the following formula (I) (hereinafter also referred to as "active material (I)"). Li (1+x) Ni y Me (1-y) O2(I) [In the formula, 0≦x≦0.1 and 0.8≦y<1, and Me includes two or more elements selected from the group consisting of Mn, Co, Al, and Ti.]

[0010] The plate resistance (hereinafter referred to as "plate resistance (R1)") when a test cell using a lithium metal plate as the counter electrode to the positive plate was charged to 4.3 V was 0.5 Ω cm 2 1.0Ω cm or more 2The test cell is a battery cell composed of a positive electrode plate and a lithium metal plate. The plate resistance (R1) is the resistance of the positive electrode plate when the test cell is charged to 4.3 V, and can be measured using an electrode resistance measurement system. The plate resistance (R1) is preferably 0.6 Ω cm 2 More than 0.9Ω cm 2 More preferably, it is 0.6 Ω cm or less. 2 More than 0.8Ω cm 2 The following is the result.

[0011] By having the positive plate have an active material layer containing the active material (I), it is possible to increase the capacity of the battery. On the other hand, the inclusion of the active material (I) may decrease the plate resistance, which may decrease the fusing property of the positive plate. As described above, the positive plate has a plate resistance (R1) of 0.5 Ω cm during charging of the test cell. 2 This improves the fusing ability of the positive plate. The plate resistance (R1) of the test cell during charging was 1.0 Ω cm 2 By setting the value to be equal to or less than this, it is possible to suppress an increase in resistance when the battery is stored in a charged state.

[0012] The plate resistance when the test cell is charged within a potential range of 4.25 V to 4.35 V (hereinafter referred to as "plate resistance (R2)") is preferably 0.5 Ω cm 2 1.0Ω cm or more 2 The plate resistance (R2) is preferably 0.6 Ω cm 2 More than 0.9Ω cm 2 More preferably, it is 0.6 Ω cm or less. 2 More than 0.8Ω cm 2 The range of the plate resistance (R2) is preferably the same as the range of the plate resistance (R1). The plate resistance (R2) is the resistance of the positive plate when the test cell is charged to 4.25 V or more and 4.35 V or less, and can be measured using an electrode resistance measurement system.

[0013] The plate resistance (R2) of the test cell during charging is 0.5 Ω cm 2By setting the plate resistance (R2) of the test cell at 1.0 Ω cm or more, the fusing property of the positive plate can be improved. 2 By setting the value to be equal to or less than 1, it is possible to suppress an increase in the capacitance when the battery is stored in a charged state.

[0014] The plate resistance (R1) and the plate resistance (R2) can be adjusted by the type and content of the components contained in the active material layer, the basis weight and density of the active material layer, the manufacturing conditions when forming the active material layer, etc. For example, the plate resistance (R1) and the plate resistance (R2) can be adjusted by the type, particle size, specific surface area, and content of the conductive material described below, the basis weight and density of the active material layer, etc. When the active material layer is formed by applying a slurry to a current collector and drying it as described below, the plate resistance (R1) and the plate resistance (R2) can also be adjusted by adjusting the drying conditions such as the drying speed at which the applied slurry is dried. For example, when the slurry contains a conductive material, if the drying speed is increased, the plate resistance (R1) and the plate resistance (R2) can be relatively increased due to the influence of migration of the conductive material.

[0015] The active material (I) may be a compound represented by the above formula (I). In formula (I), x may be 0.01≦x≦0.09, 0.03≦x≦0.08, or 0.05≦x≦0.07. In formula (I), y may be 0.81≦y≦0.98, 0.82≦y≦0.95, or 0.83≦y≦0.90. In formula (I), Me is preferably two or more selected from the group consisting of Mn, Co, and Al, and more preferably contains three of Mn, Co, and Al, or two of Mn and Co. The composition of the active material (I) can be determined by high-frequency inductively coupled plasma (ICP) emission spectrometry.

[0016] The active material (I) is, for example, Li (1+0.07) Ni 0.81 Co 0.05 Mn 0.12 Al 0.02 O2 and Li (1+0.01) Ni 0.83 Co 0.12 Mn0.05 At least one of O2.

[0017] The positive electrode active material may contain one or more active materials (I), or may contain an active material other than the active material (I). The content of the active material (I) relative to the total amount of the positive electrode active material is preferably 95% by mass or more and 100% by mass or less, more preferably 95% by mass or more and 99% by mass or less, and may be 96% by mass or more and 98% by mass or less. When two or more active materials (I) are contained, the content of the active material (I) refers to the total amount.

[0018] The active material (I) preferably includes first particles having an average particle diameter (D50) of 10 μm or more and second particles having an average particle diameter (D50) of less than 10 μm. The average particle diameter (D50) of the first particles may be 12 μm or more, or 15 μm or more, and is usually 25 μm or less. The average particle diameter (D50) of the second particles may be 9 μm or less, or 8 μm or less, and is usually 3 μm or more. The average particle diameter (D50) in this specification is the particle diameter at which the cumulative frequency from the smaller particle diameter in the volume-based particle size distribution is 50%. The volume-based particle size distribution can be measured by a laser diffraction particle size distribution measuring device.

[0019] The first particles and the second particles may have the same composition or different compositions as long as they are the active material represented by formula (I).

[0020] The first particles are preferably secondary particles formed by agglomeration of primary particles. When the first particles are secondary particles, the average primary particle diameter of the first particles is preferably less than 1 μm, and usually 0.01 μm or more. The second particles may be primary particles (single particles), or may be particles formed by agglomeration of 2 to 3 primary particles. The average primary particle diameter of the second particles is preferably 1 μm or more, and usually less than 10 μm. The average primary particle diameter in this specification can be determined by analyzing a cross-sectional SEM image observed by a scanning electron microscope (SEM). For example, a cross-section of the active material layer or a cross-section of a resin in which the first particles and the second particles are embedded is photographed by SEM, and 30 primary particles are randomly selected from the obtained cross-sectional SEM image. The grain boundaries of the selected 30 primary particles are observed to identify the outer shape of the primary particles, and the major axis (longest axis) of each of the 30 primary particles is determined, and the average value is taken as the average primary particle diameter.

[0021] The content ratio of the first particles to the second particles in the active material (I) is preferably 5 / 5 to 8 / 2, and may be 6 / 4 to 7 / 3, in terms of mass ratio (first particles / second particles). When the content ratio of the first particles to the second particles is within the above range, the plate resistance (R1) and the plate resistance (R2) can be easily adjusted to the above range.

[0022] The active material layer may contain, in addition to a positive electrode active material such as the active material (I), a conductive material, a binder, and the like.

[0023] The conductive material may be, for example, a carbon material. The carbon material may be, for example, one or more selected from the group consisting of fibrous carbon, carbon black (acetylene black, ketjen black, etc.), coke, and activated carbon. The fibrous carbon may be, for example, carbon nanotubes (CNT). The CNT may be a single-walled carbon nanotube (SWCNT) or a multi-walled carbon nanotube such as a double-walled carbon tube (DWCNT).

[0024] The active material layer preferably contains acetylene black as a conductive material. The content of acetylene black in the active material layer is preferably 0.7% by mass or more and 1.2% by mass or less, and may be 0.8% by mass or more and 1.2% by mass or less, or may be 0.9% by mass or more and 1.1% by mass or less, based on the total amount of the positive electrode active material. When the content of acetylene black is within the above range, it becomes easy to adjust the plate resistance (R1) and the plate resistance (R2) to the above range.

[0025] The average particle diameter (D50) of acetylene black is preferably 10 nm or more and 50 nm or less, and may be 15 nm or more and 45 nm or less, or may be 20 nm or more and 40 nm or less. The average particle diameter (D50) of acetylene black can be measured by the above-mentioned method. When the average particle diameter (D50) of acetylene black is within the above-mentioned range, it becomes easy to adjust the plate resistance (R1) and the plate resistance (R2) to the above-mentioned range.

[0026] The specific surface area (BET) of acetylene black is preferably 50 m 2 / g or more 200m 2 / g or less, 60m 2 / g or more 180m 2 / g or less, and 2 / g or more 150m 2 / g or less. The specific surface area of ​​acetylene black can be measured by a nitrogen adsorption method. When the specific surface area of ​​acetylene black is within the above range, the plate resistance (R1) and the plate resistance (R2) can be easily adjusted to the above range.

[0027] The binder may be, for example, one or more selected from the group consisting of styrene butadiene rubber (SBR), polyvinylidene fluoride (PVdF), and polytetrafluoroethylene (PTFE).

[0028] The weight of the active material layer is preferably 350 g / m 2 More than 500g / m 2 More preferably, it is 370 g / m or less. 2More than 470g / m 2 Less than or equal to 380 g / m 2 More than 450g / m 2 If the basis weight of the active material layer is within the above range, the plate resistance (R1) and the plate resistance (R2) can be easily adjusted to the above range.

[0029] The density of the active material layer is preferably 3.3 g / cm 3 More than 3.7g / cm 3 Less than or equal to 3.4 g / cm 3 More than 3.6g / cm 3 If the density of the active material layer is within the above range, the plate resistance (R1) and the plate resistance (R2) can be easily adjusted to the above range.

[0030] The positive electrode plate may have a current collector, and the active material layer may be formed on the current collector. The current collector is, for example, a metal foil made of an aluminum material such as aluminum or an aluminum alloy.

[0031] (Manufacturing method of positive electrode plate) The positive electrode plate can be manufactured by forming an active material layer on a current collector. The active material layer can be formed by applying a slurry onto the current collector, drying it, and compressing it as necessary.

[0032] The method for producing a positive electrode plate includes, for example, a method for producing a positive electrode plate having a current collector and an active material layer formed on the current collector, A step of preparing a slurry containing a positive electrode active material including an active material (I), N-methyl-2-pyrrolidone (hereinafter also referred to as "NMP"), and a conductive material; A step of applying the slurry onto a current collector and drying it to form an active material layer; When a test cell using a lithium metal plate as the counter electrode of the positive electrode was charged to 4.3 V, the plate resistance was 0.5 Ω cm 2 1.0Ω cm or more 2 and selecting the type and amount of conductive material to be contained in the slurry, as follows:

[0033] In the step of preparing the slurry, a slurry containing a binder may be prepared in addition to the positive electrode active material, NMP, and conductive material. The active material (I), the positive electrode active material, and the conductive material may be those described above. The conductive material is preferably acetylene black.

[0034] The step of forming the active material layer may involve applying a slurry, drying the slurry, and compressing the resulting layer to form the active material layer.

[0035] The plate resistance of the test cell can be measured by the method described above. The plate resistance may be in the range of the plate resistance (R1) described above. The plate resistance of the test cell may be the plate resistance (R2) described above. In this case, the type and amount of conductive material may be selected so that the plate resistance (R2) falls within the above range. The conductive material is preferably selected in consideration of the composition as well as physical properties such as the average particle size (D50) and the specific surface area.

[0036] By selecting the type and amount of conductive material so that the plate resistance of the test cell falls within the above range, it is possible to manufacture a positive plate that has excellent melting resistance and can suppress an increase in the resistance of the nonaqueous electrolyte secondary battery when stored in a charged state.

[0037] (Method of selecting the type and amount of conductive material) The method for selecting the type and amount of the conductive material contained in the active material layer of the positive electrode plate is as follows: A step of preparing a positive electrode plate having a positive electrode active material containing an active material (I) and an active material layer containing a conductive material; A step of preparing a test cell using a positive electrode plate and a lithium metal plate as a counter electrode of the positive electrode plate; The plate resistance when the test cell was charged to 4.3 V was 0.5 Ω cm 2 1.0Ω cm or more 2 and selecting the type and amount of conductive material to be contained in the active material layer of the positive electrode plate as follows.

[0038] The step of preparing the positive electrode plate may include, for example, the step of preparing the above-mentioned slurry and the step of forming the active material. The active material (I), the positive electrode active material, and the conductive material may be those described above. The conductive material is preferably acetylene black.

[0039] The plate resistance of the test cell can be measured by the method described above. The plate resistance may be in the range of the plate resistance (R1) described above. The plate resistance of the test cell may be the plate resistance (R2) described above. In this case, the type and amount of conductive material may be selected so that the plate resistance (R2) falls within the above range. The conductive material is preferably selected in consideration of the composition as well as physical properties such as the average particle size (D50) and the specific surface area.

[0040] By selecting the type and amount of conductive material contained in the active material layer by the above-mentioned selection method and manufacturing a positive electrode plate based on this selection result, it is possible to obtain a positive electrode plate that is excellent in melting resistance and can suppress an increase in the resistance of the nonaqueous electrolyte secondary battery when stored in a charged state. The manufacturing method of the positive electrode plate may be to manufacture the positive electrode plate by forming an active material layer so that the type and amount of conductive material are selected by the above-mentioned selection method.

[0041] (Nonaqueous electrolyte secondary battery) The battery may include the positive electrode plate described above. The battery usually includes an electrode body and an electrolyte. The battery may further include a case that contains the electrode body and the electrolyte. A resin sheet serving as an electrode holder may be disposed between the electrode body and the case.

[0042] The electrode assembly may have the above-mentioned positive electrode plate, negative electrode plate, and a separator interposed between the positive electrode plate and the negative electrode plate. The electrode assembly may be of a wound type or a laminated type.

[0043] The negative electrode may have a negative electrode current collector and a negative electrode active material layer formed on the negative electrode current collector. The negative electrode current collector is, for example, a metal foil made of a copper material such as copper or a copper alloy. The negative electrode active material layer includes a negative electrode active material and may further include one or both of a binder and a conductive assistant.

[0044] Examples of the negative electrode active material include carbon-based active materials containing carbon (C) atoms such as graphite; and metal-based active materials containing metal elements such as metal simple substances or metal oxides containing elements selected from the group consisting of silicon (Si), tin (Sn), antimony (Sb), bismuth (Bi), titanium (Ti), and germanium (Ge). Examples of the binder include cellulose-based binders such as carboxymethyl cellulose (CMC), styrene butadiene rubber (SBR), and the like. Examples of the conductive assistant include carbon materials such as fibrous carbon, carbon black (e.g., acetylene black, ketjen black), coke, and activated carbon. Examples of the fibrous carbon include those described above.

[0045] The separator may be a porous sheet (film, nonwoven fabric, etc.) made of a resin such as polyethylene, polypropylene, polyester, cellulose, or polyamide. The porous sheet may have a single-layer structure or a multi-layer structure of two or more layers. The separator may have a functional layer on the surface of the porous sheet. The functional layer may be at least one of a heat-resistant layer and an adhesive layer for bonding to a positive electrode plate and a negative electrode plate.

[0046] The electrolyte may be a non-aqueous electrolyte, for example, a non-aqueous solvent such as an organic solvent containing a supporting salt. Examples of the non-aqueous solvent include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC). Examples of the supporting salt include lithium perchlorate (LiClO4) and lithium hexafluorophosphate (LiPF6).

[0047] The case is a housing that houses the electrode assembly. The case is preferably made of metal, and can be formed using, for example, aluminum, an aluminum alloy, iron, an iron alloy, or the like. EXAMPLES

[0048] The present disclosure will be described more specifically below with reference to examples and comparative examples. [Comparative Examples 1 to 5, Examples 1 to 2] (Cathode active material) As the positive electrode active material, the following first particles and second particles were used in a mass ratio (first particles / second particles) of 7 / 3. ·First particle: Li (1+0.07) Ni 0.81 Co 0.05 Mn 0.12 Al 0.02 O2 (average particle diameter (D50): 17μm) ·Second particle: Li (1+0.01) Ni 0.83 Co 0.12 Mn 0.05 O2 (average particle diameter (D50): 6μm)

[0049] (Conductive material) The conductive material used was acetylene black as described below. Acetylene Black (1) (AB(1)): Average particle diameter (D50): 35nm, specific surface area (BET): 68m 2 / g Acetylene Black (2) (AB(2)): Average particle diameter (D50): 26nm, specific surface area (BET): 131m 2 / g

[0050] (Preparation of positive electrode plate) The positive electrode active material, conductive material, and NMP were mixed to prepare a slurry. The conductive material was acetylene black (AB(1) or AB(2)) as shown in Table 1, and the blending amount (amount relative to the total amount of the positive electrode active material) was shown in Table 1. The slurry was applied to both sides of a current collector, dried, and compressed to obtain a positive electrode plate in which an active material layer was formed on the current collector. The basis weight and density per side of the active material layer were each 200 g / m 2 and 3.5 g / cm 3 It was.

[0051] (Preparation of negative electrode plate) A negative electrode active material layer containing natural graphite as a negative electrode active material was formed on a negative electrode current collector to obtain a negative electrode plate. The weight and density of the negative electrode active material layer per side were 125 g / m 2 and 1.5 g / cm 3 It was.

[0052] (Battery cell manufacturing) An electrode assembly was fabricated using the positive and negative electrode plates and a separator fabricated above, and a battery cell was fabricated using the electrode assembly and an electrolyte.

[0053] [Composition of positive electrode active material] The compositions of the first and second particles were determined by high-frequency inductively coupled plasma (ICP) emission spectrometry.

[0054] [Measurement of average particle size (D50)] The average particle diameters (D50) of the first particles, the second particles, and the acetylene black were measured using a laser diffraction particle size distribution analyzer as the particle diameter at which the cumulative particle volume from the small particle size side in the volume-based particle size distribution becomes 50% of the total particle volume.

[0055] [Measurement of plate resistance] Test cells were prepared using the positive electrode plates prepared in the examples and comparative examples and a lithium metal plate as a counter electrode for the positive electrode plates. The test cells were charged to a potential of 4.27 to 4.3 V, and the plate resistance at a potential of 4.3 V was measured using an electrode resistance measuring system "RM2610" (manufactured by Hioki E.E. Corporation). The results are shown in Table 1.

[0056] In the test cells prepared using the positive plates obtained in Examples 1 and 2, when the battery was charged to a potential range of 4.25 V or more and 4.35 V or less, the plate resistance was 0.5 Ω cm at any potential. 2 1.0Ω cm or more 2 It was within the following range:

[0057] [Measurement of specific surface area (BET)] The specific surface area (BET) of acetylene black was measured by the nitrogen adsorption method in which liquid nitrogen was adsorbed onto the surface of acetylene black.

[0058] [Evaluation of fusing ability] An evaluation cell was prepared to evaluate the fusing property using the positive electrode plates prepared in the examples and comparative examples. The evaluation cell was connected in parallel to a constant voltage power source with a maximum current of 200A so that a current simulating a large cell was passed, and a nail was inserted into the evaluation cell. The heat generation rate after the positive electrode plate was fusing (after the nail was removed) was measured, and the heat generation rate of the examples and comparative examples was calculated as a relative value when the heat generation rate of Comparative Example 3 was set as 100 (reference), and evaluated according to the following criteria. The results are shown in Table 1. A: The heat release rate is less than 17. B: The heat release rate is 50 or more.

[0059] [Measurement of battery cell resistance retention rate] The battery cells prepared in the examples and comparative examples were adjusted to a SOC (charging rate) of 50% in an environment of 25°C. Thereafter, constant current discharge was performed for 10 seconds at current values ​​of 1C, 2C, 3C, 4C, and 5C, and the voltage after 10 seconds was measured, and the initial resistance of the battery cell was calculated by IV plot. Next, the battery cell was charged to 4.2V and kept at 60°C for 60 days, and then the resistance of the battery cell was calculated in the same manner as above in an environment of 25°C, and this was taken as the resistance of the battery cell after storage in a charged state. The resistance retention rate [%] was calculated according to the following formula. The results are shown in Table 1. Resistance retention rate [%] = (resistance after storage in charged state / initial resistance) x 100

[0060] [Table 1]

[0061] From Table 1, it can be seen that the battery cells obtained in Examples 1 and 2 have excellent melting properties and can suppress an increase in resistance when stored in a charged state. In contrast, it can be seen that the battery cells obtained in Comparative Examples 1, 2, and 4 have excellent melting properties, but their resistance increases when stored in a charged state. It can be seen that the battery cells obtained in Comparative Examples 3 and 5 can suppress an increase in resistance when stored in a charged state, but their melting properties are reduced.

Claims

1. A positive electrode plate having an active material layer containing a positive electrode active material, The positive electrode active material has the following formula (I): Li (1+x) Ni y Me (1-y) O 2 (I) [In the formula, 0≦x≦0.1 and 0.8≦y<1, and Me includes two or more elements selected from the group consisting of Mn, Co, Al, and Ti.] The active material is represented by When a test cell using a lithium metal plate as a counter electrode to the positive electrode plate was charged to 4.3 V, the plate resistance was 0.5 Ω cm 2 1.0Ω・cm or more 2 Below is the positive plate.

2. When the test cell was charged within a potential range of 4.25 V to 4.35 V, the plate resistance was less than 0.5 Ω cm 2 1.0Ω・cm or more 2 2. The positive electrode plate of claim 1 , wherein:

3. The positive electrode plate according to claim 1 , wherein the active material includes first particles having an average particle diameter (D50) of 10 μm or more and second particles having an average particle diameter (D50) of less than 10 μm.

4. The positive electrode plate according to claim 3 , wherein the first particles are secondary particles formed by agglomeration of primary particles.

5. The positive electrode plate according to claim 3 , wherein a content ratio of the first particles to the second particles is 5 / 5 or more and 8 / 2 or less in mass ratio (first particles / second particles).

6. The positive electrode plate according to claim 1 , wherein the active material layer contains 0.7% by mass or more and 1.2% by mass or less of acetylene black with respect to the total amount of the positive electrode active material.

7. The positive electrode plate according to claim 6, wherein the average particle diameter (D50) of the acetylene black is 10 nm or more and 50 nm or less.

8. The specific surface area of ​​the acetylene black is 50 m 2 / g or more 200m 2 The positive electrode plate according to claim 6, wherein the surface area of ​​the positive electrode is 0.1 μm or less.

9. The active material layer has a basis weight of 350 g / m 2 The positive electrode plate according to claim 1 , having a surface area of ​​500 g / m or less.

10. The density of the active material layer is 3.3 g / cm 3 3.7g / cm or more 3 2. The positive electrode plate of claim 1 , wherein:

11. The positive electrode plate according to claim 1 , wherein a content of the active material relative to a total amount of the positive electrode active material is 95 mass % or more and 100 mass % or less.

12. An electrode assembly having a positive electrode plate, a negative electrode plate, and a separator interposed between the positive electrode plate and the negative electrode plate according to any one of claims 1 to 11; and an electrolyte.

Citation Information

Patent Citations

  • Lithium secondary battery

    JP1999265719A

  • Non-aqueous electrolyte battery, battery pack, and automobile

    JP2007328952A

  • Lithium-transition metal compound oxide

    JP2008214186A

  • Nonaqueous electrolyte secondary battery

    JP2008269928A

  • Lithium ion secondary battery

    JP2013065467A