Urea adsorbent

A urea adsorbent with a specific silica-to-alumina ratio and 8-membered oxygen ring structure in zeolite significantly improves urea adsorption capacity, addressing the inefficiencies of previous adsorbents in treating dialysis wastewater.

JP2024134834APending Publication Date: 2024-10-04TOSOH CORP +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023045235
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing urea adsorbents using zeolite have insufficient urea adsorption capacity for effective treatment and regeneration of dialysis wastewater.

Method used

A urea adsorbent comprising zeolite with a specific composition, featuring a molar ratio of silica to alumina (SiO2/Al2O3) between 22 and 45, a sodium content of 1.0% by mass or less, and a skeletal structure with an 8-membered oxygen ring, preferably of CHA, AEI, or AFX type, enhances urea adsorption capacity.

Benefits of technology

The described urea adsorbent achieves a high urea adsorption amount per unit mass of zeolite, making it effective for treating and regenerating dialysis wastewater.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134834000001
    Figure 2024134834000001
Patent Text Reader

Abstract

To provide at least one of a urea adsorbent containing zeolite with a high urea adsorption rate per unit mass of zeolite, and a urea adsorbing method using the same.SOLUTION: A urea adsorbent comprises zeolite that has a skeleton structure with the largest pore composed of an oxygen 8-membered ring, where the molar ratio of silica to alumina (SiO2 / Al2O3 ratio) is more than 22 to 45 or less, and the sodium content in terms of oxide is 1.0 mass% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a urea adsorbent containing zeolite and a method for adsorbing urea. [Background technology]

[0002] Dialysis is a process that artificially removes waste products from blood using dialysis fluid. The waste products, mainly urea, are removed from the blood by contacting the blood with the dialysis fluid through a semipermeable membrane. A large amount of dialysis fluid is used per dialysis session, and dialysis is performed frequently. As a result, a large amount of dialysis fluid is discharged and treated as waste fluid (dialysis effluent) after dialysis. In recent years, attention has been focused on home dialysis, where dialysis patients undergo dialysis at home, from the perspective of improving quality of life, but the handling of dialysis effluent is an obstacle to its widespread use.

[0003] Therefore, urea adsorbents using zeolite have been studied for the purpose of treating and regenerating dialysis effluent. For example, Patent Document 1 reports a urea adsorption fiber containing a water-insoluble polymer and ZSM-5 with a molar ratio of silica to alumina (SiO2 / Al2O3 ratio) of 40. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2018 / 139047 Summary of the Invention [Problem to be solved by the invention]

[0005] In Patent Document 1, the amount of urea adsorbed per unit mass of zeolite was not sufficient for the purpose of treating and regenerating dialysis effluent. [Means for solving the problem]

[0006] In this disclosure, we have investigated urea adsorbents using zeolites, and as a result, we have found that, among zeolites having a framework structure in which the largest pore is an 8-membered oxygen ring, zeolites having a specific composition are suitable as urea adsorbents with a high urea adsorption capacity per unit mass of zeolite.

[0007] That is, the present invention is as described in the claims, and the gist of the present disclosure is as follows. [1] A urea adsorbent comprising: a zeolite having a framework structure in which the largest pore is an eight-membered oxygen ring, a molar ratio of silica to alumina (SiO2 / Al2O3 ratio) of more than 22 and not more than 45, and a sodium content, calculated as an oxide, of 1.0 mass% or less. [2] The urea adsorbent according to [1], wherein the zeolite has a potassium content, calculated as an oxide, of 1.0 mass% or less. [3] The urea adsorbent according to [1] or [2], wherein the skeletal structure in which the largest pore is an 8-membered oxygen ring is a CHA type, an AEI type, an AFX type or a LEV type. [4] The urea adsorbent according to any one of [1] to [3], wherein the zeolite is a crystalline aluminosilicate. [5] A method for adsorbing urea, comprising contacting urea with the zeolite contained in the urea adsorbent according to any one of [1] to [4] above. [6] A zeolite for use in urea adsorption, having a framework structure in which the largest pore is an 8-membered oxygen ring, a molar ratio of silica to alumina (SiO2 / Al2O3) greater than 22 but not greater than 45, and a sodium content, calculated as oxide, not greater than 1.0 mass%. [7] A urea adsorbent for use in urea adsorption, comprising a zeolite having a framework structure in which the largest pore is an 8-membered oxygen ring, a molar ratio of silica to alumina (SiO2 / Al2O3 ratio) greater than 22 and less than or equal to 45, and a sodium content, calculated as oxide, of 1.0 mass% or less. Effect of the Invention

[0008] The present disclosure can provide at least one of a urea adsorbent containing a zeolite having a high urea adsorption amount per unit mass of the zeolite and a urea adsorption method using the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] First, the meaning of each term in this specification will be explained.

[0010] In this specification, "zeolite" refers to a compound having a regular structure in which skeleton atoms (hereinafter also referred to as "T atoms") are arranged via oxygen (O), and the T atoms are composed of at least one of metal atoms and metalloid atoms. Examples of metal atoms include at least one selected from the group consisting of aluminum (Al), titanium (Ti), iron (Fe), zinc (Zn), gallium (Ga) and tin (Sn), with aluminum being preferred. Examples of metalloid atoms include at least one selected from the group consisting of boron (B), silicon (Si), germanium (Ge), arsenic (As), antimony (Sb) and tellurium (Te), with silicon being preferred.

[0011] A "zeolite-like substance" is a compound having a regular structure in which T atoms are oxygen-mediated, and the T atoms contain at least an atom other than a metal or a metalloid. Examples of zeolite-like substances include complex phosphorus compounds containing phosphorus (P) as the T atom, such as aluminophosphate (AlPO) and silicoaluminophosphate (SAPO). "Zeolite-like substances" are distinguished from "zeolites" in which the T atoms are composed of at least one of metal atoms and metalloid atoms.

[0012] Zeolites in which the T atoms are composed of aluminum (Al) and silicon (Si) are classified as crystalline aluminosilicates. Crystalline aluminosilicates include non-substituted crystalline aluminosilicates in which the T atoms are composed only of aluminum and silicon, and substituted crystalline aluminosilicates in which some of the aluminum and silicon that make up the T atoms are replaced with other metal atoms and metalloid atoms.

[0013] In this specification, the term "crystalline aluminosilicate" refers to a zeolite in which the T atoms are aluminum (Al) and silicon (Si). The "crystalline aluminosilicate" exhibits a crystalline XRD peak in its powder X-ray diffraction (hereinafter also referred to as "XRD") pattern, and is distinguished from the "amorphous aluminosilicate" which does not exhibit a crystalline XRD peak.

[0014] In this specification, the "ordered structure" of a zeolite is a skeletal structure specified by a structure code (hereinafter, also simply referred to as "structure code") defined by the Structure Commission of the International Zeolite Association. For example, "CHA-type zeolite" is a zeolite having a skeletal structure specified by the structure code "CHA". The skeletal structure (structure code) of each zeolite can be identified, for example, by comparison with the XRD pattern (hereinafter, also referred to as "reference pattern") described in Collection of simulated XRD powder patterns for zeolites, Fifth revised edition (2007).

[0015] In this specification, the XRD patterns include those obtained by XRD measurement under the following conditions. Acceleration current / voltage: 40mA / 40kV Radiation source: CuKα radiation (λ=1.5405Å) Measurement mode: Continuous scan Scan condition: 40° / min Measurement range: 2θ=3° to 43° Divergence vertical limit slit: 10mm Divergence / entrance slit: 1° Receiving slit: open Detector: D / teX Ultra Ni filter used

[0016] The crystalline XRD peak is a peak that is detected by identifying the 2θ of the peak top in the analysis of the XRD pattern using a general analysis software (e.g., IGOR Pro 8, manufactured by WaveMetrics, or SmartLab StudioII, manufactured by Rigaku). Although not particularly limited, the half-width (full width at half maximum) of the XRD peak can be, for example, 2θ=0.50° or less.

[0017] Hereinafter, one embodiment of the present disclosure will be described.

[0018] The urea adsorbent of the present embodiment contains zeolite having a framework structure in which the largest pore is an 8-membered oxygen ring, a molar ratio of silica to alumina (SiO2 / Al2O3 ratio) of more than 22 and not more than 45, and a sodium content calculated as oxide of 1.0 mass% or less.

[0019] The zeolite contained in the urea adsorbent of the present embodiment is not particularly limited as long as it satisfies the above-mentioned conditions, but from the viewpoint of adsorbing more urea, it is preferably a crystalline aluminosilicate.

[0020] The zeolite contained in the urea adsorbent of this embodiment has a skeletal structure in which the largest pore is an 8-membered oxygen ring. A skeletal structure in which the largest pore is an 8-membered oxygen ring refers to a skeletal structure in which the pore with the largest number of oxygen atoms among the pores formed in the skeletal structure (i.e., pores formed by oxygen and T atoms) is an 8-membered oxygen ring. The skeletal structure in which the largest pore is an 8-membered oxygen ring may be a skeletal structure consisting only of pores with 8-membered oxygen rings, or may be a skeletal structure consisting of pores with 8-membered oxygen rings and pores with less than 8 oxygen atoms (for example, at least one of 6-membered oxygen rings and 4-membered oxygen rings).

[0021] The number of oxygen atoms in the pores depends on the zeolite framework structure, and can be determined from the zeolite framework structure. The number of oxygen atoms in the pores in each framework structure is described in, for example, ATLAS OF ZEOLITE FRAMEWORK TYPES (6th Edition, Elsevier, Structure Commission of the International Zeolite Association, 2007).

[0022] In the urea adsorbent of this embodiment, the skeletal structure in which the largest pore is an 8-membered oxygen ring is preferably a CHA type, an AEI type, an AFX type, or a LEV type, from the viewpoint of better adsorbing urea, and is more preferably a CHA type.

[0023] The zeolite contained in the urea adsorbent of the present embodiment has a molar ratio of silica to alumina (SiO2 / Al2O3 ratio) of more than 22 and not more than 45. From the viewpoint of better adsorbing urea, the molar ratio of silica to alumina (SiO2 / Al2O3 ratio) is more preferably more than 22 and not more than 35, even more preferably 23 or more and 32 or less, and particularly preferably 23 or more and 29 or less.

[0024] The zeolite contained in the urea adsorbent of this embodiment has a sodium content of 1.0 mass% or less calculated as oxide. From the viewpoint of better adsorbing urea, the sodium content of oxide is preferably 0.8 mass% or less, more preferably less than 0.5 mass%, even more preferably 0.1 mass% or less, and even more preferably less than 0.1 mass%. The state of sodium contained in the zeolite is not particularly limited, but examples thereof include a state in which sodium ions, sodium compounds (e.g., Na2O), or both are contained.

[0025] The oxide-equivalent sodium content (mass%) is the content relative to 100 mass% of zeolite, and can be calculated as the percentage of the mass of the zeolite, calculated as sodium oxide (Na2O) for the sodium (Na) contained in the zeolite. In this specification, the content of a certain component being equal to or less than a predetermined content (or less than a predetermined content) may mean that the component is contained at or less than the predetermined content (or less than the predetermined content), or that the component is not contained (i.e., 0 mass%).

[0026] The zeolite contained in the urea adsorbent of this embodiment has a framework structure in which the largest pore is an 8-membered oxygen ring, the molar ratio of silica to alumina (SiO2 / Al2O3 ratio) is more than 22 and not more than 45, and the sodium content calculated as oxide is not more than 1.0 mass%, so long as this structure is not particularly limited.

[0027] From the viewpoint of applying the urea adsorbent of this embodiment to the treatment and regeneration of dialysis effluent, the zeolite contained in the urea adsorbent of this embodiment preferably has a potassium content of 1.0 mass% or less, more preferably 0.1 mass% or less, and particularly preferably less than 0.01 mass% in terms of oxide. The potassium content (mass%) in terms of oxide is the content relative to 100 mass% of zeolite, and can be calculated as the percentage of the mass of potassium (K) contained in the zeolite converted into potassium oxide (KO) relative to the mass of the zeolite.

[0028] In the zeolite contained in the urea adsorbent of the present embodiment, from the viewpoint of better adsorbing urea, the total content of sodium in terms of oxide and potassium in terms of oxide is preferably 1.0 mass% or less, more preferably 0.8 mass% or less, even more preferably 0.5 mass% or less, even more preferably 0.1 mass% or less, and particularly preferably less than 0.02 mass%.

[0029] The zeolite contained in the urea adsorbent of this embodiment may be of any cationic type, and may be, for example, an ammonium type (NH + type), sodium type (Na + type), potassium type (K + type) or proton type (H + From the viewpoint of applying the urea adsorbent of the present embodiment to the treatment and regeneration of dialysis effluent, the zeolite contained in the urea adsorbent of the present embodiment is a proton type (H + type) or sodium type (Na + The proton type (H + It is more preferable that the .alpha.-type is used.

[0030] The content of zeolite in the urea adsorbent of the present embodiment can be, for example, 20 mass % or more and 100 mass % or less with respect to 100 mass % of the urea adsorbent.

[0031] The urea adsorbent of the present embodiment may be composed only of the above-mentioned zeolite, but may also contain other substances other than zeolite, such as one or more selected from the group consisting of a binder, a molding aid, and water.

[0032] The binder may be an organic binder, an inorganic binder, or both of these binders. Examples of the organic binder include at least one selected from the group consisting of polyethylene oxide, hydroxyethyl methylcellulose, starch, corn starch, molasses, lactose, gelatin, dextrin, gum arabic, alginic acid, polyethylene glycol, and polyvinylpyrrolidone. Examples of the inorganic binder include at least one selected from the group consisting of clay, silica, alumina, and zirconia. From the viewpoint of applying the urea adsorbent of this embodiment to the treatment and regeneration of dialysis effluent, the binder is preferably an inorganic binder, and among inorganic binders, at least one of silica and zirconia is more preferable, and silica is particularly preferable.

[0033] The content of the binder in the urea adsorbent of this embodiment can be, for example, 5% by mass or more and 70% by mass or less relative to 100% by mass of the urea adsorbent.

[0034] Examples of the molding aid include water-soluble or water-insoluble celluloses such as carboxylmethylcellulose (hereinafter also referred to as "CMC"), hydroxycellulose, hydroxypropylmethylcellulose, hydroxypropylcellulose, ethylcellulose, and cellulose nanofiber; guar gum derivatives such as at least one of guar gum and hydroxypropylguar gum; polysaccharides such as at least one selected from the group of xanthan gum, welan gum, and gellan gum belonging to biogums; polyethyleneimine derivatives; polyvinylvinylidone (hereinafter also referred to as "PVP"); alcohols such as at least one selected from the group of glycerin, polyvinyl alcohol, and ethylene glycol derivatives; cationic, anionic, or nonionic surfactants; aqueous urethane; polyacrylic acid derivatives, and the like, and these may be contained not only alone but also in combination of two or more. The CMC may be sodium carboxymethylcellulose (hereinafter also referred to as "Na-CMC"). A preferred molding aid is at least one of Na-CMC and hydroxypropylcellulose.

[0035] The content of the molding aid in the urea adsorbent of this embodiment can be, for example, 0.1% by mass or more and 10% by mass or less relative to 100% by mass of the urea adsorbent.

[0036] The water content in the urea adsorbent of this embodiment can be, for example, 0.1 mass % or more and 40 mass % or less relative to 100 mass % of the urea adsorbent.

[0037] The urea adsorbent of this embodiment contains a binder in addition to the zeolite described above, which makes it easier to mold the urea adsorbent of this embodiment into a predetermined shape. The urea adsorbent of this embodiment contains a molding aid and water in addition to the zeolite and binder described above, which improves moldability. The urea adsorbent in the form of a molded body can be produced, for example, by molding a mixture of the zeolite and binder (and molding aid and water as necessary) into a predetermined shape and firing it. The shape of the molded body is not particularly limited, but at least one selected from the group consisting of spherical, approximately spherical, elliptical, cylindrical, polyhedral, and amorphous can be exemplified.

[0038] From the viewpoint of improving the adsorption efficiency of urea and reducing the pressure loss when a fluid containing urea is passed through, the size of the molded body is preferably 0.1 mm or more and 4.0 mm or less in median diameter, and more preferably 0.3 mm or more and 2.0 mm or less in median diameter. The median diameter is the particle size (d 50 )

[0039] Next, a method for producing the zeolite contained in the urea adsorbent of this embodiment will be described.

[0040] The method for producing the zeolite contained in the urea adsorbent of the present embodiment is not particularly limited, but one example can be a method including a crystallization step of crystallizing a composition containing an aluminum source, a silicon source, a structure directing agent, an alkali source, and water (hereinafter also referred to as the "raw material composition").

[0041] The aluminum source contained in the raw material composition is a compound containing aluminum (Al), and examples thereof include one or more selected from the group consisting of aluminum isopropoxide, aluminum sulfate, aluminum chloride, aluminum hydroxide, pseudoboehmite, alumina sol, and amorphous aluminosilicate. Note that substances containing aluminum (Al) and silicon (Si), such as amorphous aluminosilicate, can be used not only as an alumina source, but also as a silica source, which will be described later.

[0042] The silica source contained in the raw material composition is a compound containing silicon (Si), and examples thereof include one or more selected from the group consisting of silica sol, fumed silica, colloidal silica, precipitated silica, sodium silicate, amorphous silicic acid, and amorphous aluminosilicate.

[0043] The source of the structure directing agent (hereinafter also referred to as "SDA") may be any substance that directs a zeolite having a framework structure in which the largest pore is an 8-membered oxygen ring, and a known SDA capable of directing a zeolite having a framework structure (structure code) to be produced can be used. For example, an SDA directing a CHA-type zeolite may include at least one of the group consisting of (1-adamantyl)trimethylammonium (hereinafter also referred to as "ATMA") cation, cyclohexylethylammonium (hereinafter also referred to as "CDMEA") cation, N-methyl-3-quinuclidinol cation, trimethylbenzylammonium cation, tetraethylammonium cation, and N,N,N-trimethylexoaminonorbornene cation. The SDA may be in the form of a salt, and examples of the salt include one or more salt forms selected from chloride, bromide, iodide, and hydroxide. When a salt of ATMA is used as the SDA, the salt of ATMA is preferably a hydroxide of ATMA.

[0044] The alkali source contained in the raw material composition is a compound containing an alkali metal element, and can be exemplified by a compound containing one or more alkali metal elements selected from the group consisting of sodium, potassium, cesium, and rubidium. The alkali source may be in the form of one or more salts selected from the group consisting of hydroxides, carbonates, chlorides, bromides, iodides, and sulfates containing an alkali metal element. Preferred alkali sources include at least one of the group consisting of sodium hydroxide, sodium carbonate, sodium chloride, sodium bromide, sodium iodide, and sodium sulfate. The alkali source is not limited to the form of a salt, and may be in a form other than a salt, such as sodium silicate.

[0045] The water contained in the raw material composition may be, for example, distilled water, deionized water, pure water, or two or more of these. When the raw materials other than water contained in the raw material composition contain water, such as hydrates, structural water, or solvents, the water contained in the raw materials other than water can be considered as the water contained in the raw material composition.

[0046] The raw material composition may be composed only of an aluminum source, a silicon source, a structure directing agent source, an alkali source, and water, but may also contain other raw materials in addition to these raw materials. Examples of other raw materials include seed crystals.

[0047] The composition of the raw material composition can be appropriately selected depending on the framework structure of the zeolite to be produced, and the following molar composition can be given as an example of a preferred composition: In the following composition, each ratio is a molar (mol) ratio, SiO2 is silica (mol), Al2O3 is alumina (mol), H2O is water (mol), M is an alkali metal element (mol), SDA is an organic structure directing agent (mol), OH is 1, 1, 1, 1, 1, 1, 1, 1, 1, 1, 1, 1, 1, 1, 1, 1, 1, - is the total amount (mol) of hydroxide ions in the raw material composition. SiO2 / Al2O3 ratio=more than 22, preferably 24 or more, and 60 or less, preferably 45 or less, more preferably 35 or less SDA / SiO2 ratio = 0.01 or more, preferably 0.05 or more, and 0.30 or less, preferably 0.20 or less M / SiO2 ratio = 0.01 or more, preferably 0.05 or more, and 0.30 or less, preferably 0.20 or less H2O / SiO2 ratio = 2 or more, preferably 5 or more, and 100 or less, preferably 50 or less OH - / SiO2 ratio = 0.1 or more, preferably 0.15 or more, and 0.35 or less, preferably 0.28 or less

[0048] The crystallization treatment of the raw material composition may be performed by crystallizing the raw material composition so as to obtain a zeolite having a skeleton structure (structure code) in which the largest pore is an 8-membered oxygen ring, and the treatment method and conditions may be appropriately selected depending on the zeolite having a skeleton structure (structure code) to be produced. A preferred treatment method is to subject the raw material composition to hydrothermal treatment. The hydrothermal treatment may be performed by placing the raw material composition in a sealed pressure-resistant container and heating it. Examples of hydrothermal treatment conditions include the following. Treatment temperature: 110°C or higher, 130°C or higher, or 150°C or higher, and 210℃ or less, 200℃ or less, or 190℃ or less Processing time: 8 hours or more, 10 hours or more, or 15 hours or more, and 500 hours or less or 300 hours or less Processing pressure: Natural pressure

[0049] The method for producing the zeolite contained in the urea adsorbent of the present embodiment may include, in addition to the above-mentioned crystallization step, one or more steps selected from the group consisting of a washing step, a drying step, an SDA removal step, an ammonium treatment step, and a calcination treatment step.

[0050] The washing step is a step of washing the zeolite obtained by crystallization. For example, in the washing step, the zeolite obtained by crystallization may be washed with pure water.

[0051] The drying step is a step of removing moisture from the crystallized zeolite or from the washed zeolite. The conditions of the drying step are not particularly limited as long as moisture can be removed from the zeolite. For example, the drying temperature can be 100°C or higher and 150°C or lower. For example, the drying time can be 2 hours or higher and 20 hours or lower. For example, the drying atmosphere can be air.

[0052] The SDA removal step is a step for removing SDA contained in the crystallized zeolite, the washed zeolite, or the dried zeolite. Usually, the zeolite crystallized using SDA contains SDA in its pores. By including the SDA removal step, the SDA contained in the zeolite can be removed.

[0053] The SDA removal treatment can be carried out under any conditions as long as SDA is removed. Examples of the method for removing SDA include at least one selected from the group consisting of a liquid phase treatment using an acidic aqueous solution, an exchange treatment using a resin or the like, and a heat treatment (thermal decomposition). From the viewpoint of manufacturing efficiency, the SDA removal treatment is preferably a heat treatment (thermal decomposition). The conditions of the heat treatment (thermal decomposition) are not particularly limited as long as SDA is removed. For example, the heat treatment temperature can be 400° C. or higher and 800° C. or lower. Also, for example, the heat treatment time can be 1 hour or higher and 5 hours or lower. Also, for example, the atmosphere during the heat treatment can be air.

[0054] The ammonium treatment step is a step for removing alkali metals contained in the crystallized zeolite, the washed zeolite, the dried zeolite, or the SDA-removed zeolite. The ammonium treatment can be performed by a known method, for example, by contacting the zeolite with an aqueous solution containing ammonium ions. The longer the time for which the aqueous solution containing ammonium ions is contacted with the zeolite, the greater the amount of alkali metals removed from the zeolite, and the higher the ammonium ion concentration in the aqueous solution contacted with the zeolite, the greater the amount of alkali metals removed from the zeolite. The conditions for the ammonium treatment may be appropriately adjusted in consideration of such characteristics so that the sodium content of the zeolite obtained by the treatment is 1.0 mass% or less in terms of oxide.

[0055] The calcination treatment is a treatment for calcining (heating) zeolite, and can be performed on zeolite obtained by crystallization, washed zeolite, dried zeolite, SDA-removed zeolite, or ammonium-treated zeolite. The conditions for the calcination treatment are not particularly limited, but for example, the calcination temperature can be 400°C or higher and 700°C or lower. For example, the calcination time can be 1 hour or higher and 5 hours or lower. For example, the atmosphere during the calcination treatment can be air. If the zeolite to be calcined is an ammonium-treated zeolite (i.e., a cation type of ammonium (NH4 + In the case of zeolite with a cation type of proton (H type), the cation type is converted to proton type (H type) by calcination at 400 to 700 degrees Celsius. + It becomes a zeolite of type .

[0056] The zeolite contained in the urea adsorbent of the present embodiment can be produced by the production method including the above-mentioned steps. The produced zeolite can be used as the urea adsorbent of the present embodiment. The produced zeolite may be mixed with the other components (binder, molding aid, and water) described above as necessary, and the resulting mixture may be molded and fired to produce a urea adsorbent in the form of a molded body.

[0057] The urea adsorbent of this embodiment can be used for adsorption of urea. Adsorption of urea using the urea adsorbent of this embodiment can be performed by contacting urea with the zeolite contained in the urea adsorbent of this embodiment. Urea can be contacted with the zeolite in a state where it is contained in a fluid such as a gas or liquid, and it is preferable to contact it with the zeolite in a state where it is contained in a liquid. Specific methods for contacting zeolite with urea include, for example, a method in which the urea adsorbent of this embodiment is filled in a fixed bed flow-type reaction tube and a fluid containing urea is passed through it, and a method in which the urea adsorbent of this embodiment is dispersed in a fluid containing urea and left or shaken.

[0058] The adsorption of urea using the urea adsorbent of this embodiment proceeds by contacting urea with the zeolite contained in the urea adsorbent of this embodiment, so the contact conditions between the zeolite and urea are not particularly limited. As an example, the contact temperature between the zeolite and urea can be 10 to 45°C. The contact time between the zeolite and urea can be appropriately set depending on the amount of urea to be adsorbed.

[0059] As shown in the examples described below, the urea adsorbent of the present embodiment described above has a high urea adsorption amount per unit mass of zeolite. As an example, the urea adsorbent of the present embodiment exhibits a urea adsorption amount of 1 mass% or more (urea adsorption amount represented by formula (1) described below). Therefore, the urea adsorbent of the present embodiment is useful for treating and regenerating dialysis effluent.

[0060] Although the reason why the urea adsorbent of this embodiment shows a high urea adsorption amount is not clear, it is presumed that the zeolite contained in the urea adsorbent of this embodiment captures urea through pores of 8-membered oxygen rings, and that since aluminum is contained in the zeolite at a predetermined density that exerts electrostatic interaction with urea, the urea captured by the pores of 8-membered oxygen rings is less likely to leave the zeolite, resulting in a high urea adsorption amount. It is presumed that in zeolites with a molar ratio of silica to alumina outside the range of more than 22 and not more than 45, or in zeolites with a sodium content of more than 1.0 mass% calculated as oxide, electrostatic interaction with urea is less likely to occur, resulting in a low urea adsorption amount.

[0061] Of the urea adsorbents of the present embodiment described above, a preferred embodiment is, for example, a urea adsorbent containing zeolite having a skeletal structure in which the largest pore is an 8-membered oxygen ring, a molar ratio of silica to alumina (SiO2 / Al2O3 ratio) of 23 or more and 30 or less, and a sodium content calculated as oxide of 1.0 mass% or less.

[0062] Furthermore, as another preferred embodiment, for example, there can be mentioned a urea adsorbent containing a zeolite having a framework structure in which the largest pore is an 8-membered oxygen ring, a molar ratio of silica to alumina (SiO2 / Al2O3 ratio) of more than 22 and not more than 45, and further having a total content of sodium calculated as oxide and potassium calculated as oxide of 1.0 mass% or less.

[0063] In addition, as another preferred embodiment, for example, a silica-to-alumina silicate having a skeleton structure in which the largest pore is an 8-membered oxygen ring, a molar ratio of silica to alumina (SiO2 / Al2O3 ratio) of more than 22 to 45 or less, a sodium content calculated as an oxide of 1.0 mass% or less, and a proton type (H + urea adsorbents containing zeolites of the urea type. EXAMPLES

[0064] The present disclosure will be described in more detail below with reference to examples, but the present disclosure is not limited to these examples.

[0065] (Identification of crystalline phase) The samples were subjected to XRD measurement using a general powder X-ray diffractometer (name: Ultima IV Protectus, manufactured by Rigaku Corporation) under the following measurement conditions: Acceleration current / voltage: 40mA / 40kV Radiation source: CuKα radiation (λ=1.5405Å) Measurement mode: Continuous scan Scan condition: 40° / min Measurement range: 2θ=3° to 43° Divergence vertical limit slit: 10mm Divergence / entrance slit: 1° Receiving slit: open Detector: D / teX Ultra Ni filter used

[0066] The obtained XRD pattern was subjected to baseline correction, and detection and intensity analysis of each XRD peak after correction, using an analysis program (trade name: IGOR Pro 8, manufactured by WaveMetrics) attached to the measuring device. The skeletal structure (crystal structure) of the sample was identified by comparing the corrected XRD pattern with the XRD pattern (reference pattern) described in Collection of simulated XRD powder patterns for zeolites, Fifth revised edition (2007). In addition, the number of oxygen atoms in the largest pore (pore with the highest number of oxygen atoms) in the identified skeletal structure was identified using ATLAS OF ZEOLITE FRAMEWORK TYPES (6th Edition, Elsevier, Structure Commission of the International Zeolite Association, 2007).

[0067] (composition analysis) A sample solution was prepared by dissolving 2 mg of the measurement sample in 10 mL of an acid solution (HF: 0.96 mass%, HNO3: 1.2 mass%) obtained by mixing hydrofluoric acid (HF concentration: 48 mass%), nitric acid (HNO3 concentration: 60 mass%), and pure water. The sample solution was measured by inductively coupled plasma atomic emission spectrometry (ICP-AES) using a general ICP device (device name: OPTIMA5300DV, manufactured by PerkinElmer). From the obtained measured values ​​of Si, Al, Na, and K, the converted values ​​were calculated by converting them into oxides (SiO2, Al2O3, Na2O, and K2O), and the SAR (SiO2 / Al2O3), Na2O content (mass%), and K2O content (mass%) of the sample were calculated from the calculated converted values.

[0068] (Urea adsorption evaluation) Urea (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was dissolved in a phosphate buffer (Dulbecco's phosphate buffered saline, manufactured by Nacalai Tesque, Inc.) to prepare a 230 mg / dL urea solution (urea solution before evaluation). Next, 3 mL of the urea solution and 10 mg of zeolite powder were placed in a 5 mL microtube, and then ultrasonicated for 5 seconds to disperse the zeolite powder in the urea solution. The microtube was shaken at 37°C for 2 hours. After shaking, the zeolite powder and the supernatant (urea solution) were centrifuged, and 200 μL of the collected supernatant was used as the urea solution after evaluation.

[0069] The urea solutions before and after the evaluation were each diluted 5-fold with phosphate buffer to prepare reaction solutions. 5 μL of each reaction solution was dispensed into a microplate (96-well plate), and a urea measurement kit (Urea Assay Kit, BioChain Institute Inc.; 100 μL of ortho-phthalaldehyde solution (concentration 0.4% by mass or less, sulfuric acid: 10% by mass), and 100 μL of boric acid solution (concentration 0.8% by mass or less, sulfuric acid: 22% by mass) were dropped into the reaction solution. After the dropping, the reaction solution was colored orange by reaction with urea, and used as the measurement solution.

[0070] A common microplate reader (instrument name: Infinite M Nano+, manufactured by TECAN) was used to measure the absorbance of the measurement solution at 520 nm by absorption spectrometry, and the urea concentration of the urea solution before and after the evaluation was calculated using a calibration curve. The urea adsorption amount (mass%) per unit weight of zeolite was calculated using the following formula (1). Urea adsorption amount = (ab)×c÷d×100 (mass%)...(1) a: Urea concentration in the urea solution before evaluation [mg / dL] b: Urea concentration in the urea solution after evaluation [mg / dL] c: Volume of urea solution [dL] d: Mass of zeolite powder [mg] The calibration curve was prepared using a standard sample (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) with a known urea concentration.

[0071] Example 1 An aqueous solution of (1-adamantyl)trimethylammonium (hereinafter also referred to as "ATMA") hydroxide, pure water, an aqueous solution of sodium hydroxide, and amorphous aluminosilicate (SAR: 25.3) were added and thoroughly mixed to obtain a raw material composition having the following molar composition. SiO2 / Al2O3= 25.3 ATMA / Si = 0.081 Na / Si = 0.084 K / Si = 0.084 H2O / Si = 18 OH - / Si = 0.249

[0072] The raw material composition was sealed in a stainless steel autoclave with an internal volume of 80 ml, and heated at 150 ° C. for 48 hours while rotating at 55 rpm. The product after heating was separated into solid and liquid, and the obtained solid was washed with 5 times the mass of pure water. The washed solid was dried in the air at 110 ° C. for 20 hours, and then calcined in the air at 600 ° C. for 2 hours to obtain a primary calcined powder. Next, the obtained primary calcined powder was mixed with 5 times the mass of a 20% by mass ammonium chloride aqueous solution to perform ion exchange, and then washed with 10 times the mass of pure water of the solid, dried in the air at 110 ° C. for 20 hours, and then calcined in the air at 600 ° C. for 1 hour to obtain zeolite, which was used as the adsorbent of this example.

[0073] The zeolite obtained has a cationic type of H + The zeolite was a CHA-type zeolite (largest pore: 8-membered oxygen ring, zeolite: crystalline aluminosilicate (unsubstituted)) with an SAR of 24.7, a Na2O content of less than 0.01 mass% (below the detection limit), and a K2O content of less than 0.01 mass% (below the detection limit).

[0074] Example 2 In order to adjust the sodium content, the CHA-type zeolite obtained in the example was washed with a 0.03% by mass aqueous solution of sodium chloride, which was 15 times the mass of the CHA-type zeolite, and then washed with 10 times the mass of pure water and dried in the air at 110°C for 20 hours to obtain a zeolite, which was used as the adsorbent of this example.

[0075] The zeolite obtained has a cationic type of H + and Na + The zeolite was a CHA-type zeolite (largest pore: oxygen 8-membered ring, zeolite: crystalline aluminosilicate (unsubstituted)) with an SAR of 24.7, a Na2O content of 0.36 mass%, and a K2O content of less than 0.01 mass% (below the detection limit).

[0076] Example 3 An aqueous solution of ATMA hydroxide, pure water, an aqueous solution of sodium hydroxide and an amorphous aluminosilicate (SAR: 29.5) were added and thoroughly mixed to obtain a raw material composition having the following molar composition. SiO2 / Al2O3= 29.5 ATMA / Si = 0.081 Na / Si = 0.094 K / Si = 0 H2O / Si = 12 OH - / Si = 0.175

[0077] The obtained raw material composition was sealed in a stainless steel autoclave having an internal volume of 80 ml and heated at 170°C for 70 hours while rotating at 55 rpm in the same manner as in Example 1 to obtain a zeolite, which was used as the adsorbent of this example.

[0078] The zeolite obtained has a cationic type of H + The zeolite was a CHA-type zeolite (largest pore: 8-membered oxygen ring, zeolite: crystalline aluminosilicate (unsubstituted)) with an SAR of 29.2, a Na2O content of less than 0.01 mass% (below the detection limit), and a K2O content of less than 0.01 mass% (below the detection limit).

[0079] Comparative Example 1 The zeolite obtained in Example 1 was washed with a 20% by mass aqueous sodium chloride solution in an amount 15 times the mass of the solid content, and then washed with pure water in an amount 10 times the mass of the solid content, and dried in the air at 110°C for 20 hours to obtain a zeolite, which was used as the adsorbent of this comparative example.

[0080] The zeolite obtained has a cationic type of H + and Na + The zeolite was a CHA-type zeolite (largest pore: oxygen 8-membered ring, zeolite: crystalline aluminosilicate (unsubstituted)) with an SAR of 24.7, a Na2O content of 1.27 mass%, and a K2O content of less than 0.01 mass% (below the detection limit).

[0081] Comparative Example 2 A zeolite was obtained in the same manner as in Example 1, except that an ATMA hydroxide aqueous solution, pure water, a sodium hydroxide aqueous solution, a potassium hydroxide aqueous solution, and an amorphous aluminosilicate (SAR: 23.3) were mixed to obtain a raw material composition having the following molar composition, and this zeolite was used as the adsorbent of this comparative example. SiO2 / Al2O3= 23.3 ATMA / Si = 0.081 Na / Si = 0.140 K / Si = 0.029 H2O / Si = 18 OH - / Si = 0.250

[0082] The zeolite obtained has a cationic type of H + The zeolite was a CHA-type zeolite (largest pore: 8-membered oxygen ring, zeolite: crystalline aluminosilicate (unsubstituted)) with an SAR of 22.0, a Na2O content of less than 0.01 mass% (below the detection limit), and a K2O content of less than 0.01 mass% (below the detection limit).

[0083] Comparative Example 3 A zeolite was obtained in the same manner as in Example 1, except that an ATMA hydroxide aqueous solution, pure water, a sodium hydroxide aqueous solution, a potassium hydroxide aqueous solution, and an amorphous aluminosilicate (SAR: 62.7) were mixed to obtain a raw material composition having the following molar composition, and this zeolite was used as the adsorbent of this comparative example. SiO2 / Al2O3= 62.7 ATMA / Si = 0.081 Na / Si = 0.068 K / Si = 0.101 H2O / Si = 18 OH - / Si = 0.250

[0084] The zeolite obtained has a cationic type of H +The zeolite was a CHA-type zeolite (largest pore: 8-membered oxygen ring, zeolite: crystalline aluminosilicate (unsubstituted)) with an SAR of 52.1, a Na2O content of less than 0.01 mass% (below the detection limit), and a K2O content of less than 0.01 mass% (below the detection limit).

[0085] Comparative Example 4 An ATMA hydroxide solution, pure water, a sodium hydroxide solution, amorphous silica (product name: Nipsil LP, manufactured by Tosoh Silica Corporation), aluminum hydroxide, and FAU-type zeolite (product name: 320NAA, manufactured by Tosoh Corporation; SAR: 18.0, Na2O: 7.3% by mass, K2O: less than 0.01% by mass (detection limit)) were mixed to obtain a raw material composition having the following composition. SiO2 / Al2O3= 34.0 ATMA / Si = 0.190 Na / Si = 0.240 K / Si = 0 H2O / Si = 12 OH - / Si = 0.430

[0086] The raw material composition was sealed in a stainless steel autoclave with an internal volume of 80 ml, and heated at 150°C for 64 hours while rotating at 55 rpm. The product after heating was separated into solid and liquid, and the obtained solid was washed with 5 times the mass of pure water. The washed solid was dried in air at 110°C for 20 hours, and then calcined in air at 600°C for 2 hours to obtain zeolite, which was used as the adsorbent of this comparative example.

[0087] The zeolite obtained has a cationic type of H + And Na + The zeolite was a CHA-type zeolite (largest pore: oxygen 8-membered ring, zeolite: crystalline aluminosilicate (unsubstituted)) with an SAR of 22.3, a Na2O content of 2.20 mass%, and a K2O content of less than 0.01 mass% (below the detection limit).

[0088] Comparative Example 5 The same MOR-type zeolite (product name: 640HOA, manufactured by Tosoh Corporation; SAR: 18.0, Na2O: 0.05% by mass, K2O: less than 0.01% by mass (below detection limit), largest pore: 12-membered oxygen ring, zeolite: crystalline aluminosilicate (unsubstituted type)) as the MOR-type zeolite used in Reference Example 2 of WO 2018 / 139047 was used as the adsorbent in this comparative example.

[0089] Comparative Example 6 MFI type zeolite (product name: 822HOA, manufactured by Tosoh Corporation; SAR: 23.9, Na2O: 0.05% by mass, K2O: less than 0.01% by mass (below detection limit), largest pore: 10-membered oxygen ring, zeolite: crystalline aluminosilicate (unsubstituted type)) was used as the adsorbent in this comparative example.

[0090] Comparative Example 7 The same MFI zeolite (product name: 840HOA, manufactured by Tosoh Corporation; SAR: 38.7, Na2O: 0.02% by mass, K2O: less than 0.01% by mass (below detection limit), largest pore: 10-membered oxygen ring, zeolite: crystalline aluminosilicate (unsubstituted type)) as the MFI zeolite used in Reference Example 3 of WO 2018 / 139047 was used as the adsorbent in this comparative example.

[0091] Comparative Example 8 Beta zeolite (product name: 940HOA, manufactured by Tosoh Corporation; SAR: 40.7, Na2O: 0.04% by mass, K2O: less than 0.01% by mass (below detection limit), largest pore: 12-membered oxygen ring, zeolite: crystalline aluminosilicate (unsubstituted type)) was used as the adsorbent in this comparative example.

[0092] Comparative Example 9 LTL type zeolite (product name: 500KOA, manufactured by Tosoh Corporation; SAR: 6.2, Na2O: 0.22 mass%, K2O: 16.6 mass%, largest pore: 12-membered oxygen ring, zeolite: crystalline aluminosilicate (unsubstituted type)) was used as the adsorbent in this comparative example.

[0093] The results of evaluating the urea adsorption of the adsorbents of the Examples and Comparative Examples are shown in the table below. [Table 1]

[0094] It can be seen from Table 1 that the adsorbents of the Examples have a higher urea adsorption amount than the adsorbents of the Comparative Examples. In other words, it was found that the adsorbents of the Examples have a higher urea adsorption amount per unit mass of zeolite than the adsorbents of the Comparative Examples.

Claims

1. It has a framework structure in which the largest pore is an 8-membered oxygen ring, and the molar ratio of silica to alumina (SiO 2 / Al 2 O 3 The urea adsorbent comprises a zeolite having a urea content ratio (ratio) of more than 22 to 45 or less and a sodium content, calculated as an oxide, of 1.0 mass% or less.

2. 2. The urea adsorbent according to claim 1, wherein the zeolite has a potassium content, calculated as an oxide, of 1.0 mass % or less.

3. 2. The urea adsorbent according to claim 1, wherein the skeletal structure in which the largest pore is an 8-membered oxygen ring is a CHA type, an AEI type, an AFX type or an LEV type.

4. 2. The urea adsorbent according to claim 1, wherein the zeolite is a crystalline aluminosilicate.

5. A method for adsorbing urea, comprising contacting urea with the zeolite contained in the urea adsorbent according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Urea-adsorbing fibers, method of manufacturing same, blood purification filter using same, and blood purification apparatus using same