Nitride semiconductor structure, light-emitting element, light source device, and method for manufacturing nitride semiconductor structure

The nitride semiconductor structure addresses unstable characteristics in surface-emitting lasers by using a current confinement layer with varying In composition and hydrogen concentrations to enhance current and optical confinement, improving device performance.

JP2024134882APending Publication Date: 2024-10-04RICOH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023045313
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

The existing nitride semiconductor structures, particularly in surface-emitting lasers, face issues with insufficient current confinement leading to increased threshold values and unstable characteristics due to the in-plane distribution of In composition and band gaps, which affects current and light confinement.

Method used

A nitride semiconductor structure is designed with a current confinement layer having regions with varying In composition and hydrogen atom concentrations, where the second region has a lower In composition and twice the hydrogen atom concentration of the first region, creating a high electrical resistance to confine current effectively and enhance optical confinement.

Benefits of technology

This design stabilizes the current confinement structure, reduces threshold values, and enhances optical confinement, resulting in improved performance of nitride semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134882000001_ABST
    Figure 2024134882000001_ABST
Patent Text Reader

Abstract

To provide a nitride semiconductor structure, a light-emitting element, a light source device, and a method for manufacturing a nitride semiconductor structure, capable of obtaining stable characteristics.SOLUTION: According to one aspect of the disclosed technology, a nitride semiconductor structure includes a nitride semiconductor layer containing Mg as impurities. The nitride semiconductor layer has a first region and a second region surrounding the first region in a plane parallel to the nitride semiconductor layer. An In composition in the second region is less than an In composition in the first region, and a hydrogen atom concentration in the second region is at least two times higher than a hydrogen atom concentration in the first region.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a nitride semiconductor structure, a light emitting device, a light source device, and a method for manufacturing a nitride semiconductor structure. [Background technology]

[0002] In edge-emitting lasers and surface-emitting lasers, in order to efficiently amplify light, the current is confined to a narrow region, causing a population inversion, and the light is confined there and amplified. For example, a current confinement structure is created by embedding an n-type semiconductor layer in the current-free region of the p-type semiconductor layer on the wafer surface side.

[0003] Patent Document 1 discloses a nitride semiconductor structure in which a nitride semiconductor layer containing In, such as AlInN, is heat-treated in an atmosphere containing hydrogen to partially evaporate In from the nitride semiconductor layer, thereby fabricating a current confinement structure. Summary of the Invention [Problem to be solved by the invention]

[0004] In the method described in Patent Document 1, an in-plane distribution of the In composition of a nitride semiconductor layer is formed, and regions with different bandgaps are provided in the plane. The nitride semiconductor structure disclosed in Patent Document 1 has a current confinement structure that makes it difficult for current to flow in regions with a large bandgap. However, simply distributing regions with different bandgaps may result in insufficient current confinement. Therefore, if a nitride semiconductor layer including this current confinement structure is used in a surface-emitting laser, there is a concern that characteristics may deteriorate, such as an increase in threshold value.

[0005] An object of the present invention is to provide a nitride semiconductor structure, a light emitting device, a light source device, and a method for manufacturing the nitride semiconductor structure that are capable of obtaining stable characteristics. [Means for solving the problem]

[0006] According to one aspect of the disclosed technique, a nitride semiconductor structure has a nitride semiconductor layer containing Mg as an impurity, the nitride semiconductor layer having a first region and a second region surrounding the first region in a plane parallel to the nitride semiconductor layer, the In composition of the second region being smaller than the In composition of the first region, and the hydrogen atom concentration of the second region being at least two times higher than the hydrogen atom concentration of the first region. Effect of the Invention

[0007] According to the disclosed technology, stable characteristics can be obtained. [Brief description of the drawings]

[0008] [Figure 1] 1 is a cross-sectional view showing a nitride semiconductor structure according to a first embodiment. [Figure 2A] 1A to 1C are cross-sectional views (part 1) illustrating a method for manufacturing a nitride semiconductor structure according to a first embodiment. [Figure 2B] 5A to 5C are cross-sectional views (part 2) illustrating the method for manufacturing the nitride semiconductor structure according to the first embodiment. [Figure 2C] 5A to 5C are cross-sectional views (part 3) illustrating the method for manufacturing the nitride semiconductor structure according to the first embodiment. [Figure 2D] 4 is a cross-sectional view (part 4) showing the method for manufacturing the nitride semiconductor structure according to the first embodiment. FIG. [Diagram 3] FIG. 4 is a cross-sectional view showing a nitride semiconductor structure according to a second embodiment. [Figure 4A] 5A to 5C are cross-sectional views (part 1) illustrating a method for manufacturing a nitride semiconductor structure according to a second embodiment. [Figure 4B] 5A to 5C are cross-sectional views (part 2) illustrating a method for manufacturing a nitride semiconductor structure according to a second embodiment. [Figure 4C] 6A to 6C are cross-sectional views (part 3) illustrating a method for manufacturing a nitride semiconductor structure according to a second embodiment. [Figure 5A] 4 is a cross-sectional view (part 1) showing a manufacturing method for separately producing a hydrogen atom concentration distribution and an In composition distribution in a current confinement layer in a manufacturing method of a nitride semiconductor structure according to the first embodiment. FIG. [Figure 5B] 4 is a cross-sectional view (part 2) showing the manufacturing method for the nitride semiconductor structure according to the first embodiment, in which the hydrogen atom concentration distribution and the In composition distribution are separately produced in the current confinement layer. FIG. [Figure 5C] 4 is a cross-sectional view (part 3) showing the manufacturing method for the nitride semiconductor structure according to the first embodiment, in which the hydrogen atom concentration distribution and the In composition distribution are separately produced in the current confinement layer. FIG. [Figure 5D] FIG. 4 is a cross-sectional view (part 4) showing the manufacturing method for the nitride semiconductor structure according to the first embodiment, in which the hydrogen atom concentration distribution and the In composition distribution are separately produced in the current confinement layer. [Figure 6] FIG. 11 is a cross-sectional view showing a light-emitting diode according to a third embodiment. [Figure 7A] 11A to 11C are cross-sectional views (part 1) illustrating a method for manufacturing a light-emitting diode according to a third embodiment. [Figure 7B] 13A to 13C are cross-sectional views (part 2) illustrating the method for manufacturing the light-emitting diode according to the third embodiment. [Figure 7C] 13A to 13C are cross-sectional views (part 3) illustrating the method for manufacturing the light-emitting diode according to the third embodiment. [Figure 7D] 13A to 13C are cross-sectional views (part 4) illustrating the method for manufacturing the light-emitting diode according to the third embodiment. [Figure 8] FIG. 11 is a cross-sectional view showing a surface-emitting laser according to a fourth embodiment. [Figure 9A] 10A to 10C are cross-sectional views (part 1) illustrating a method for manufacturing a surface-emitting laser according to a fourth embodiment. [Figure 9B] 13A to 13C are cross-sectional views (part 2) illustrating the method for manufacturing the surface-emitting laser according to the fourth embodiment. [Figure 9C] 13A to 13C are cross-sectional views (part 3) illustrating the method for manufacturing the surface-emitting laser according to the fourth embodiment. [Figure 9D] 13A to 13C are cross-sectional views (part 4) illustrating the method for manufacturing the surface-emitting laser according to the fourth embodiment. [Figure 10] FIG. 11 is a cross-sectional view showing a surface-emitting laser according to a fifth embodiment. [Figure 11A]11A to 11C are cross-sectional views (part 1) illustrating a method for manufacturing a surface-emitting laser according to a fifth embodiment. [Figure 11B] 13A to 13C are cross-sectional views (part 2) illustrating the method for manufacturing the surface-emitting laser according to the fifth embodiment. [Figure 11C] 13A to 13C are cross-sectional views (part 3) illustrating the method for manufacturing the surface-emitting laser according to the fifth embodiment. [Figure 11D] 13A to 13C are cross-sectional views (part 4) illustrating the method for manufacturing the surface-emitting laser according to the fifth embodiment. [Figure 12] FIG. 13 is a diagram showing a layout of a projection device according to a sixth embodiment. [Figure 13] FIG. 13 is a diagram showing a layout of a floodlight device according to a seventh embodiment. [Figure 14] FIG. 13 is a diagram showing a layout of a projection device according to an eighth embodiment. [Figure 15] FIG. 13 is a perspective view of a configuration example of a head mounted display according to a ninth embodiment. [Figure 16] FIG. 13 is a cross-sectional view of an example of the configuration of a head mounted display according to a ninth embodiment. [Figure 17] FIG. 23 is a diagram illustrating an example of the configuration of a biometric authentication device according to a tenth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, embodiments of the present disclosure will be described with reference to the accompanying drawings. In this specification and the drawings, components having substantially the same functional configuration may be denoted by the same reference numerals to avoid repetitive description. In the following description, the side on which the nitride semiconductor layer is located as viewed from the substrate is defined as the upper side. However, the nitride semiconductor structure etc. may be used upside down and may be arranged at any angle.

[0010] (First embodiment) First, a first embodiment will be described. The first embodiment relates to a nitride semiconductor structure. Fig. 1 is a cross-sectional view showing the nitride semiconductor structure according to the first embodiment.

[0011] 1, the nitride semiconductor structure 100 according to the first embodiment has an n-type semiconductor layer 104, an active layer 102 on the n-type semiconductor layer 104, and a p-type semiconductor layer 105 on the active layer 102. Examples of materials constituting the p-type semiconductor layer 105 include nitride semiconductors such as AlInN, InGaN, and AlGaInN.

[0012] The p-type semiconductor layer 105 has a lower semiconductor layer 105a on the active layer 102, a current confinement layer 101 on the lower semiconductor layer 105a, and an upper semiconductor layer 105b on the current confinement layer 101. The lower semiconductor layer 105a, the current confinement layer 101, and the upper semiconductor layer 105b all contain Mg (magnesium) as an impurity.

[0013] The current confinement layer 101 is a layer containing In (indium) and has a first region 101a and a second region 101b surrounding the first region 101a in a plane parallel to the current confinement layer 101. The In composition of the second region 101b is smaller than that of the first region 101a. Furthermore, the hydrogen atom concentration of the second region 101b is higher than that of the first region 101a.

[0014] The nitride semiconductor structure 100 is formed on, for example, a substrate 103. For example, a substrate on which a nitride semiconductor layer can be laminated is used as the substrate 103. For example, a nitride semiconductor substrate such as a GaN substrate or an AlN substrate can be used as the substrate 103. For example, a GaN template in which a nitride semiconductor layer is formed on a heterogeneous substrate can also be used as the substrate 103. For example, a sapphire substrate, a Si substrate, a GaAs substrate, a SiC substrate, etc. can be used as the heterogeneous substrate.

[0015] In the nitride semiconductor structure 100, as described above, the In composition of the second region 101b is smaller than the In composition of the first region 101a. Therefore, the band gap of the second region 101b is larger than the band gap of the first region 101a. Furthermore, the hydrogen atom concentration contained in the second region 101b is higher than the hydrogen atom concentration contained in the first region 101a. The Mg contained in the current confinement layer 101 is inactivated by bonding with hydrogen atoms. Since the hydrogen atom concentration of the second region 101b is higher than that of the first region 101a, the concentration of inactivated Mg is high. Therefore, the electrical resistance of the second region 101b is higher than that of the first region 101a. Therefore, inside the current confinement layer 101, the current is blocked by the second region 101b, which has a large band gap and high electrical resistance, and the current selectively flows through the first region 101a. The hydrogen atom concentration in the second region 101b is preferably at least two times higher than the hydrogen atom concentration in the first region 101a.

[0016] The hydrogen atom concentration in each of the first region 101a and the second region 101b divided by the Mg concentration is defined as the Mg deactivation rate. When the Mg deactivation rate of the first region 101a is less than 0.5, more preferably less than 0.3, the first region 101a contains a large amount of activated Mg, and the electrical resistance decreases. When the deactivation rate of the second region 101b is 0.5 or more, more preferably 0.9 or more, the second region 101b contains less activated Mg, and the electrical resistance increases. Therefore, the current is blocked more effectively in the second region 101b and flows more effectively in the first region 101a.

[0017] By making the In composition different between the first region 101a and the second region 101b, not only current confinement due to the difference in band gap occurs, but also a light confinement effect due to the difference in refractive index occurs within the plane of the current confinement layer 101. In general, the higher the In composition, the higher the refractive index of the nitride semiconductor. Therefore, by making the In composition of the first region 101a higher than that of the second region 101b, the refractive index of the first region 101a becomes higher than that of the second region 101b. Therefore, the light emitted by the active layer 102 is easily confined within a plane parallel to the current confinement layer 101, that is, within a plane parallel to the substrate 103. From the viewpoint of the light confinement effect, it is preferable that the current confinement layer 101 contains Al. This is because it is easy to increase the difference in refractive index between the first region 101a and the second region 101b. And the excellent light confinement effect is extremely suitable for edge-emitting lasers and surface-emitting lasers.

[0018] The n-type semiconductor layer 104 is a nitride semiconductor layer doped with impurities such as Si, Ge, etc. As the n-type semiconductor layer 104, for example, an n-GaN layer or an n-AlGaN layer can be used. The p-type semiconductor layer 105 is a nitride semiconductor layer doped with Mg as an impurity. As the p-type semiconductor layer 105, for example, a p-GaN layer or a p-AlGaN layer can be used.

[0019] The active layer 102 emits light by confining carriers injected from, for example, the n-type semiconductor layer 104 or the p-type semiconductor layer 105. For example, in order to obtain high light emission efficiency, it is preferable to use, as the active layer 102, a multiple quantum well layer in which an InGaN layer and a GaN layer are alternately stacked, or a multiple quantum well layer in which two types of InGaN layers having different compositions are alternately stacked.

[0020] The thickness of the current confinement layer 101 is not limited, but is preferably 10 nm or more. This is to suppress hole tunneling in the second region 101b. If the current confinement layer 101 is too thick, crystal defects are likely to occur due to the difference in lattice constant with other nitride semiconductor layers. For this reason, the thickness of the current confinement layer 101 is preferably equal to or less than the critical film thickness.

[0021] The current confinement layer 101 is provided in the p-type semiconductor layer 105. As for its position within the p-type semiconductor layer 105, the current confinement layer 101 may be disposed at a position in contact with the active layer 102, which is the lowermost part of the p-type semiconductor layer 105, or at the uppermost part of the p-type semiconductor layer 105, as long as the evaporation of In is not impeded during the manufacturing process of the nitride semiconductor structure 100.

[0022] Next, a method for manufacturing the nitride semiconductor structure 100 according to the first embodiment will be described. FIGS. 2A to 2D are cross-sectional views showing a method for manufacturing the nitride semiconductor structure 100 according to the first embodiment. In this manufacturing method, the nitride semiconductor layer included in the nitride semiconductor structure 100 is epitaxially grown on a substrate 103. Examples of the epitaxial growth method include metal organic chemical vapor deposition (MOCVD), molecular beam epitaxy (MBE), plasma chemical vapor deposition (PCVD), and hydride vapor phase epitaxy (HVPE). In the following, a case where the MOCVD method is used will be described as an example.

[0023] First, as shown in FIG. 2A, an n-type semiconductor layer 104, an active layer 102, a lower semiconductor layer 105a, an intermediate semiconductor layer 101x, and an upper semiconductor layer 105b are formed on a substrate 103. The intermediate semiconductor layer 101x contains In and has the same composition as the first region 101a. The lower semiconductor layer 105a, the intermediate semiconductor layer 101x, and the upper semiconductor layer 105b are doped with Mg as an impurity. In the MOCVD method, hydrogen atoms of ammonia (NH3) are taken in together with Mg to form Mg-H bonds. This inactivates Mg. As a result, the lower semiconductor layer 105a, the intermediate semiconductor layer 101x, and the upper semiconductor layer 105b are in a state of high electrical resistance.

[0024] Next, a first heat treatment is performed to activate the lower semiconductor layer 105a, the intermediate semiconductor layer 101x, and the upper semiconductor layer 105b. By performing the heat treatment in an atmosphere that does not contain hydrogen atoms, hydrogen atoms bonded to Mg in the lower semiconductor layer 105a, the intermediate semiconductor layer 101x, and the upper semiconductor layer 105b are released, and Mg is activated as an acceptor. As a result, the lower semiconductor layer 105a, the intermediate semiconductor layer 101x, and the upper semiconductor layer 105b function as p-type electrical conductors.

[0025] 2B, a protective mask 106 is formed on the upper semiconductor layer 105b to cover the region where the first region 101a is to be formed. The protective mask 106 may be formed of, for example, a silicon oxide film (SiO2 film), a silicon nitride film (SiN film), or the like, as long as it can block hydrogen.

[0026] Then, a second heat treatment is performed. The second heat treatment is performed at a temperature of 500° C. or higher in an atmosphere containing hydrogen. This heat treatment causes In to evaporate from the intermediate semiconductor layer 101x that does not overlap with the protective mask 106, and hydrogen atoms penetrate into the intermediate semiconductor layer 101x that does not overlap with the protective mask 106, thereby inactivating Mg. As a result, as shown in FIG. 2C, a second region 101b is formed in which the In composition is lower than that of the intermediate semiconductor layer 101x and the inactivation rate of Mg is high. The remaining part of the intermediate semiconductor layer 101x becomes a first region 101a in which the In composition does not change from that of the intermediate semiconductor layer 101x. In this way, a current confinement layer 101 having a first region 101a and a second region 101b is formed. Furthermore, hydrogen atoms also penetrate into the lower semiconductor layer 105a located below the second region 101b and the upper semiconductor layer 105b located above the second region 101b, and Mg contained in each layer is inactivated. The process of incorporating hydrogen atoms into nitride semiconductor layers such as the intermediate semiconductor layer 101x, the lower semiconductor layer 105a, and the upper semiconductor layer 105b is an example of a "hydrogen penetration treatment process".

[0027] For this second heat treatment, for example, a film forming apparatus such as an MOCVD apparatus used for forming the n-type semiconductor layer 104, the active layer 102, the lower semiconductor layer 105a, the intermediate semiconductor layer 101x, and the upper semiconductor layer 105b can be used. A heat treatment apparatus or the like may also be used.

[0028] The protective mask 106 is then removed, as shown in FIG. 2D.

[0029] In this manner, the nitride semiconductor structure 100 according to the first embodiment can be manufactured.

[0030] According to this method, the intermediate semiconductor layer 101x has an in-plane band gap distribution and a hydrogen atom concentration distribution based on the difference in In composition. In other words, an electrical resistance distribution caused by the difference in Mg deactivation rate is formed in the intermediate semiconductor layer 101x. Also, an electrical resistance distribution caused by the difference in Mg deactivation rate is generated in the lower semiconductor layer 105a and the upper semiconductor layer 105b, and a very stable current confinement structure characteristic can be obtained. Furthermore, the distribution of In composition generates a refractive index difference in the plane, and light generated in the active layer 102 can be confined.

[0031] In the above description, the intermediate semiconductor layer 101x is disposed in the p-type semiconductor layer 105. However, if the upper semiconductor layer 105b is too thick, in the manufacturing method of this embodiment, the detachment of hydrogen atoms due to the Mg activation treatment in the first heat treatment and the penetration of hydrogen atoms due to the second heat treatment are not so problematic, but In becomes difficult to evaporate in the second heat treatment. Therefore, the thickness of the upper semiconductor layer 105b is preferably 100 nm or less. More preferably, it is 50 nm or less, and further preferably, it is 10 nm or less.

[0032] Second embodiment Next, a second embodiment will be described. The second embodiment relates to a nitride semiconductor structure. Fig. 3 is a cross-sectional view showing the nitride semiconductor structure according to the second embodiment.

[0033] 3, the nitride semiconductor structure 200 according to the second embodiment includes an n-type semiconductor layer 104, an active layer 102, a p-type semiconductor layer 105, a tunnel junction layer 107, and an upper n-type semiconductor layer 108. The p-type semiconductor layer 105 includes a current confinement layer 101 as a nitride semiconductor layer containing Mg as an impurity. The upper n-type semiconductor layer 108, the tunnel junction layer 107, the p-type semiconductor layer 105, the current confinement layer 101, the active layer 102, and a part of the n-type semiconductor layer 104 are etched to form a mesa structure 211.

[0034] There is no particular limitation on the planar shape of the mesa structure 211. For example, when the nitride semiconductor structure 200 is used in an edge-emitting laser, the mesa structure 211 is formed in a stripe shape. For example, when the nitride semiconductor structure 200 is used in a surface-emitting laser, the mesa structure 211 is formed in a circular or rectangular shape.

[0035] Next, a method for manufacturing the nitride semiconductor structure 200 according to the second embodiment will be described. Figures 4A to 4C are cross-sectional views showing the method for manufacturing the nitride semiconductor structure 200 according to the second embodiment. In this manufacturing method, the nitride semiconductor layers included in the nitride semiconductor structure 200 are epitaxially grown on the substrate 103.

[0036] 4A, an n-type semiconductor layer 104, an active layer 102, a lower semiconductor layer 105a, an intermediate semiconductor layer 101x, an upper semiconductor layer 105b, a tunnel junction layer 107, and an upper n-type semiconductor layer 108 are formed on a substrate 103. The tunnel junction layer 107 has a two-layer structure of a p-type semiconductor and an n-type semiconductor doped with a high concentration of impurities, with the substrate side being the p-type semiconductor and the surface side being the n-type semiconductor.

[0037] Next, as shown in FIG. 4B, the upper n-type semiconductor layer 108, the tunnel junction layer 107, the lower semiconductor layer 105a, the intermediate semiconductor layer 101x, the upper semiconductor layer 105b, the intermediate semiconductor layer 101x, the active layer 102, and a portion of the n-type semiconductor layer 104 are removed by lithography and dry etching, thereby forming a mesa structure 211.

[0038] Thereafter, the lower semiconductor layer 105a, the intermediate semiconductor layer 101x, and the upper semiconductor layer 105b are activated by a first heat treatment. It is known that when an n-type nitride semiconductor layer is formed on the upper part of a p-type nitride semiconductor layer, hydrogen atoms bonded to Mg in the p-type nitride semiconductor layer are less likely to pass through the n-type nitride semiconductor layer during activation. Therefore, a mesa structure 211 is formed to remove hydrogen atoms from the sidewall of the mesa structure 211.

[0039] Next, as the second heat treatment, heat treatment is performed at a temperature of 500° C. or more in an atmosphere containing hydrogen. This heat treatment causes hydrogen atoms to penetrate from the sidewall of the mesa structure 211, so that In of the intermediate semiconductor layer 101x evaporates from the sidewall, and the p-type semiconductor layer 105 is also passivated from the sidewall side. As a result, as shown in FIG. 4C, a second region 101b is formed in which the In composition is lower than that of the intermediate semiconductor layer 101x and the passivation rate of Mg is high. The remaining part of the intermediate semiconductor layer 101x becomes the first region 101a in which the In composition does not change from the In composition of the intermediate semiconductor layer 101x. In this way, the current confinement layer 101 having the first region 101a and the second region 101b is formed.

[0040] In this manner, the nitride semiconductor structure 200 according to the second embodiment can be manufactured.

[0041] According to this method, a band gap distribution and a hydrogen atom concentration distribution are formed in the intermediate semiconductor layer 101x in the plane based on the difference in In composition. In other words, an electrical resistance distribution is formed in the plane of the intermediate semiconductor layer 101x due to the difference in the passivation rate of Mg. Also, an electrical resistance distribution is generated due to the difference in the passivation rate of Mg in the plane of the lower semiconductor layer 105a and the upper semiconductor layer 105b, and very stable characteristics of the current confinement structure can be obtained. Furthermore, a refractive index difference is generated in the plane due to the distribution of the In composition, and light generated in the active layer 102 can be confined.

[0042] The mesa structure 211 may be formed so that at least the sidewall of the p-type semiconductor layer 105 is exposed.

[0043] Furthermore, the In composition does not need to change abruptly and discontinuously between the first region 101a and the second region 101b, and there may be a region between the first region 101a and the second region 101b in which the In composition changes continuously.

[0044] In the first and second embodiments, the atmosphere of the second heat treatment may be an atmosphere of only hydrogen gas, or an atmosphere of a mixed gas of hydrogen gas and an inert gas such as nitrogen gas. The evaporation rate of In can be controlled according to the ratio of the inert gas. The atmosphere of the second heat treatment may also be an atmosphere containing ammonia in addition to hydrogen gas. During the heat treatment, nitrogen in the nitride semiconductor layer may be desorbed, causing the exposed surface to become rough. However, when the atmosphere contains ammonia, it is easy to suppress the desorption of nitrogen and keep the exposed surface flat. Furthermore, ammonia also contains hydrogen atoms, so that it can inactivate Mg.

[0045] The heat treatment temperature of the second heat treatment is not limited as long as it is a temperature at which In can evaporate, and is, for example, 500°C or higher as described above. When the temperature at which the intermediate semiconductor layer 101x that becomes the current confinement layer can be formed with good crystallinity is T (°C), the heat treatment temperature is preferably T-200 (°C) or higher, and more preferably T-100 (°C) or higher. On the other hand, the heat treatment temperature is preferably a temperature at which the intermediate semiconductor layer 101x decomposes or lower. For example, when the intermediate semiconductor layer 101x is an InGaN layer, Ga starts to evaporate in a temperature range of 1100°C to 1200°C. Therefore, if the heat treatment temperature exceeds 1200°C, the intermediate semiconductor layer 101x decomposes before the current confinement layer 101 is formed. Therefore, when the intermediate semiconductor layer 101x is an InGaN layer, the heat treatment temperature is preferably 1200°C or lower, and more preferably 1100°C. For example, when the intermediate semiconductor layer 101x is an AlInN layer or an AlGaInN layer, the Al contained in the intermediate semiconductor layer 101x suppresses thermal decomposition of the intermediate semiconductor layer 101x, and the heat treatment temperature can be increased to 1400° C. The temperature T depends on the In composition of the intermediate semiconductor layer 101x, and the temperature T tends to be higher as the In composition is lower.

[0046] The order of the steps of activating Mg by the first heat treatment and evaporating In by the second heat treatment may be reversed, and a step of infiltrating hydrogen atoms may be introduced separately, thereby forming a third region between the first region 101a and the second region 101b, in which the In composition is lower than the first region 101a and the hydrogen atom concentration is lower than the second region 101b, or a third region in which the In composition is higher than the second region 101b and the hydrogen atom concentration is higher than the first region 101a, and the in-plane electrical resistance distribution and the refractive index distribution can be controlled separately.

[0047] For example, after fabricating the nitride semiconductor structure 100 of FIG. 1, if a protective mask 106 is formed on the upper semiconductor layer 105b and a second heat treatment is performed to evaporate In without performing a first heat treatment for activating Mg, as shown in FIG. 5A, In evaporates from the region of the intermediate semiconductor layer 101x where the protective mask 106 is not formed, and an in-plane distribution of the In composition of the first region 101a and the second region 101b is formed in the intermediate semiconductor layer 101x, but the distribution of the concentration of hydrogen atoms bonded to Mg in the p-type semiconductor layer 105 does not change.

[0048] On the other hand, when the first heat treatment is performed, as shown in FIG. 5B, hydrogen atoms in the p-type semiconductor layer 105 are detached, and the hydrogen atom concentration in the entire surface is reduced. Next, a protective mask 106 is newly formed on the surface of the p-type semiconductor layer 105, and hydrogen atoms are penetrated to form a distribution of hydrogen atom concentration in the surface. For example, as shown in FIG. 5C, when the width of the protective mask 106 is narrowed and hydrogen atoms are penetrated to the center of the intermediate semiconductor layer 101x, a third region 101c is formed between the first region 101a and the second region 101b, in which the In composition is higher than that of the second region 101b and the hydrogen atom concentration is higher than that of the first region 101a. At this time, if heat treatment is performed under a hydrogen atmosphere, In in the third region 101c evaporates, so the penetration of hydrogen atoms is performed by, for example, proton injection.

[0049] 5D, when the width of the protective mask 106 is made larger than the first region 101a, a third region 101c having a lower In composition than the first region 101a and a lower hydrogen atom concentration than the second region 101b is formed between the first region 101a and the second region 101b. In this example, the third region 101c is protected by the protective mask 106, and evaporation of In due to penetration of hydrogen atoms does not occur, so that heat treatment can be performed under a hydrogen atmosphere in addition to proton injection.

[0050] In the nitride semiconductor structure 200 of the second embodiment, after the mesa structure is formed, the order of the steps of activating Mg by the first heat treatment and evaporating In by the second heat treatment is reversed, and a hydrogen penetration step is separately introduced, so that the in-plane electrical resistance distribution and the refractive index distribution can be separately controlled in the same manner.

[0051] As described above, the electrical resistance distribution due to Mg passivation and the refractive index distribution due to differences in the In composition can be separately formed within the plane to obtain desired characteristics.

[0052] (Third embodiment) Next, a third embodiment will be described. The third embodiment relates to a light-emitting diode having a nitride semiconductor structure. A light-emitting diode is an example of a light-emitting device. Fig. 6 is a cross-sectional view showing a light-emitting diode according to the third embodiment.

[0053] 6, a light emitting diode 350 according to the third embodiment includes a sapphire substrate 302 and a light emitting diode (LED) structure 300 on the sapphire substrate 302. The LED structure 300 includes an n-GaN layer 303, a multiple quantum well layer 304, and a p-Al 0.20 Ga 0.80 The N layer 305, the p-GaN layer 306a, the current confinement layer 301, the p-GaN layer 306b, and the p ++The LED structure 300 includes a p-GaN layer 307. The p-GaN layer 306a is an example of a lower semiconductor layer, the p-GaN layer 306b is an example of an upper semiconductor layer, and the current confinement layer 301 is an example of a nitride semiconductor layer containing Mg as an impurity. The LED structure 300 is an example of a nitride semiconductor structure.

[0054] The n-GaN layer 303 is formed on a sapphire substrate 302. The thickness of the n-GaN layer 303 is, for example, 5 μm.

[0055] The multiple quantum well layer 304 is formed on the n-GaN layer 303. The multiple quantum well layer 304 is, for example, an InN layer having a thickness of 2.5 nm. 0.15 Ga 0.85 It has a structure in which N layers and GaN layers with a thickness of 7.5 nm are alternately stacked for five periods. The multiple quantum well layer 304 is an example of an active layer.

[0056] p-Al 0.20 Ga 0.80 The N layer 305 is formed on the multiple quantum well layer 304. 0.20 Ga 0.80 The thickness of the N layer 305 is, for example, 20 nm.

[0057] The p-GaN layer 306a is p-Al 0.20 Ga 0.80 It is formed on the N layer 305. The p-GaN layer 306a has a thickness of, for example, 50 nm.

[0058] The current confinement layer 301 is formed on the p-GaN layer 306a. The thickness of the current confinement layer 301 is, for example, 50 nm. The current confinement layer 301 is made of p-Al 0.70 In 0.30 The N layer 301a and the p-Al 0.70 In 0.30 The p-AlN layer 301b surrounds the N layer 301a. 0.70 In 0.30 The In composition is smaller than that of the N layer 301a. 0.70 In 0.30The N layer 301a is an example of a first region, and the p-AlN layer 301b is an example of a second region.

[0059] The p-GaN layer 306b is formed on the current confinement layer 301. The thickness of the p-GaN layer 306b is, for example, 50 nm.

[0060] p ++ The -GaN layer 307 is formed on the p-GaN layer 306b. ++ The thickness of the -GaN layer 307 is, for example, 5 nm. ++ The GaN layer 307 contains 1×10 Mg as an acceptor. 20 cm -3 It is doped at a concentration of

[0061] p ++ -GaN layer 307, p-GaN layer 306b, current confinement layer 301, p-GaN layer 306a, and p-Al 0.20 Ga 0.80 An isolation trench 312 is formed in the N layer 305 , the multiple quantum well layer 304 , and a part of the n-GaN layer 303 .

[0062] p ++ A p-side electrode 309 is formed on the surface of the -GaN layer 307. An n-side electrode 310 is formed on the surface of the portion of the n-GaN layer 303 exposed from the element isolation trench 312. The p-side electrode 309 is, for example, ++ The n-side electrode 310 has, for example, a Ni film and an Au film stacked in this order from the n-GaN layer 307 side. The n-side electrode 310 has, for example, a Ti film and an Al film stacked in this order from the n-GaN layer 303 side.

[0063] In the light-emitting diode 350, as described above, the current confinement layer 301 is p-Al 0.70 In 0.30 The p-AlN layer 301a and the p-AlN layer 301b are 0.70 In 0.30 The band gap of the p-AlN layer 301a is 3.59 eV, and the band gap of the p-AlN layer 301b is 6.2 eV. 0.70 In0.30 The band gap of the p-AlN layer 301b is 1.0 eV or more larger than that of the p-AlN layer 301a. 0.70 In 0.30 A large band offset is formed between the N layer 301a, the p-GaN layer 306a, and the p-GaN layer 306b.

[0064] Furthermore, by the manufacturing method described later, the hydrogen atom concentration in the region where the p-AlN layer 301b is formed among the p-GaN layer 306a and the p-GaN layer 306b is p-Al 0.70 In 0.30 In the plane of the N layer 301a, the p-GaN layer 306a, and the p-GaN layer 306b, 0.70 In 0.30 The hydrogen atom concentration is higher than that of the region in which the N layer 301a is formed. Therefore, in the current confinement layer 301, the current flows through the p-Al 0.70 In 0.30 It selectively flows through the N layer 301a.

[0065] Next, a method for manufacturing the light emitting diode 350 according to the third embodiment will be described. Figures 7A to 7D are cross-sectional views showing the method for manufacturing the light emitting diode 350 according to the third embodiment. In this manufacturing method, the nitride semiconductor layers included in the LED structure 300 are epitaxially grown on a sapphire substrate 302.

[0066] First, using an MOCVD apparatus, an n-GaN layer 303, a multiple quantum well layer 304, and a p-Al layer 305 were deposited on a sapphire substrate 302 as shown in FIG. 7A. 0.20 Ga 0.80 N layer 305, p-GaN layer 306a, and p-Al 0.70 In 0.30 N layer 301x are formed in this order. Before the n-GaN layer 303 is formed, a GaN buffer layer (not shown) may be formed on the sapphire substrate 302 with a thickness of, for example, 20 nm.

[0067] p-Al 0.20 Ga 0.80 N layer 305, p-GaN layer 306a, p-Al0.70 In 0.30 N layer 301x, p-GaN layer 306b, p ++ Mg in the GaN layer 307 (hereinafter collectively referred to as a p-type layer) is ++ - 1 × 10 for GaN layer 307 20 cm -3 and 2×10 19 cm -3 The p-type layer is doped with hydrogen. Hydrogen atoms from the ammonia gas used in film formation in the MOCVD apparatus are incorporated into the p-type layer at the same concentration as the Mg in the p-type layer, making it inactive (inactivation rate 1.0). Therefore, as the first heat treatment, the structure shown in FIG. 7A is placed in a heat treatment apparatus and heat-treated at a temperature of 900°C in a nitrogen atmosphere. For example, the heat treatment time is set to 10 minutes. Depending on the heat treatment temperature, time, and atmospheric gas, this heat treatment causes 70% of the hydrogen atoms to be desorbed from the p-type layer (inactivation rate 0.30), resulting in p-type conductivity.

[0068] The structure shown in FIG. 7A is then removed from the MOCVD apparatus, and as shown in FIG. ++ On the GaN layer 307, p-Al 0.70 In 0.30 As a protective mask covering the region where the N layer 301a is to be formed, a SiO2 film 308 having a thickness of, for example, 100 nm is formed. The SiO2 film 308 can be formed by, for example, photolithography.

[0069] Thereafter, the structure shown in FIG. 7B is placed in a heat treatment device, and heat treatment is performed in a hydrogen atmosphere at a temperature of 800° C. as a second heat treatment. The heat treatment time is, for example, 10 minutes. This heat treatment causes hydrogen atoms to penetrate from the front surface side of the sapphire substrate 302 into the area not protected by the SiO2 film 308, and the p-Al 0.70 In 0.30 In evaporates from the portion of the N layer 301x that is not protected by the SiO2 film 308. As a result, as shown in FIG. 7C, p-Al 0.70 In 0.30 The area of ​​the N layer 301x that is not protected by the SiO2 film 308 changes to a p-AlN layer 301b. 0.70 In0.30 The remainder of the N layer 301x has an In composition of p-Al 0.70 In 0.30 p-Al, which has not changed from the In composition of N layer 301x 0.70 In 0.30 In this way, the p-Al N layer 301a is formed. 0.70 In 0.30 A current confinement layer 301 having an N layer 301a and a p-AlN layer 301b is formed. Furthermore, hydrogen atoms are introduced at the same concentration as Mg in the p-type layer in the region where the SiO2 film 308 is not formed, and Mg is inactivated. As a result, an electrical resistance distribution is formed in the p-type layer.

[0070] Next, the structure shown in Fig. 7C is removed from the heat treatment device, and the SiO2 film 308 is removed as shown in Fig. 7D. The SiO2 film 308 can be removed using, for example, buffered hydrofluoric acid.

[0071] Then, as shown in FIG. ++ -GaN layer 307, p-GaN layer 306b, current confinement layer 301, p-GaN layer 306a, and p-Al 0.20 Ga 0.80 An isolation trench 312 is formed in the N layer 305 , the multiple quantum well layer 304 , and a part of the n-GaN layer 303 .

[0072] The element isolation trench 312 can be formed by, for example, lithography and dry etching. ++ A p-side electrode 309 is formed on the surface of the -GaN layer 307, and an n-side electrode 310 is formed on the surface of the portion of the n-GaN layer 303 exposed from the element isolation trench 312. ++ A Ni film and an Au film are laminated in this order from the -GaN layer 307 side. In forming the n-side electrode 310, for example, a Ti film and an Al film are laminated in this order from the n-GaN layer 303 side.

[0073] In this manner, the light emitting diode 350 according to the third embodiment can be manufactured.

[0074] According to this method, p-Al0.70 In 0.30 In the N layer 301x, a distribution of band gap and a distribution of hydrogen atom concentration are formed in the plane due to the difference in In composition. In other words, an electrical resistance distribution is formed due to the difference in Mg passivation rate. Furthermore, an electrical resistance distribution occurs due to the difference in Mg passivation rate between the p-GaN 306a and the p-GaN 306b, and the characteristics of a very stable current confinement structure can be obtained.

[0075] (Fourth embodiment) Next, a fourth embodiment will be described. The fourth embodiment relates to a surface emitting laser having a nitride semiconductor structure. The surface emitting laser is an example of a light emitting device. Fig. 8 is a cross-sectional view showing the surface emitting laser according to the fourth embodiment.

[0076] 8, a surface-emitting laser 450 according to the fourth embodiment has an n-GaN substrate 402 and a laser structure 400 on the n-GaN substrate 402. The laser structure 400 includes a lower multilayer reflector 403, an n-GaN layer 404, a multiple quantum well layer 405, and a p-Al 0.20 Ga 0.80 The N layer 406, the p-GaN layer 407, the current confinement layer 401, and the p ++ The p-GaN layer 407 is an example of a lower semiconductor layer, and the p-GaN layer 408 is an example of a lower semiconductor layer. ++ The -GaN layer 408 is an example of an upper semiconductor layer, and the current confinement layer 401 is an example of a nitride semiconductor layer containing Mg as an impurity. The laser structure 400 is an example of a nitride semiconductor structure.

[0077] The lower multilayer reflector 403 is formed on an n-GaN substrate 402. The lower multilayer reflector 403 has a structure in which high-refractive index layers and low-refractive index layers are alternately stacked for 46 periods. The high-refractive index layers are, for example, 50 nm thick In 0.05 Ga 0.95 The low refractive index layer has a multilayer structure in which, for example, two AlN layers with a thickness of 6 nm are inserted between three GaN layers with a thickness of 6 nm.

[0078] The n-GaN layer 404 is formed on the lower multilayer reflector 403. The thickness of the n-GaN layer 404 is, for example, 1.1 μm.

[0079] The multiple quantum well layer 405 is formed on the n-GaN layer 404. The multiple quantum well layer 405 is, for example, an InN layer having a thickness of 4 nm. 0.10 Ga 0.90 It has a structure in which N layers and GaN layers with a thickness of 6 nm are alternately stacked for five periods. The multiple quantum well layer 405 is an example of an active layer.

[0080] p-Al 0.20 Ga 0.80 The N layer 406 is formed on the multiple quantum well layer 405. 0.20 Ga 0.80 The thickness of the N layer 406 is, for example, 20 nm.

[0081] The p-GaN layer 407 is p-Al 0.20 Ga 0.80 The p-GaN layer 407 is formed on the N layer 406. The thickness of the p-GaN layer 407 is, for example, 75 nm. The p-GaN layer 407 contains 2×10 Mg as an acceptor. 19 cm -3 It is doped at a concentration of

[0082] The current confinement layer 401 is formed on the p-GaN layer 407. The thickness of the current confinement layer 401 is, for example, 35 nm. The current confinement layer 401 is made of p-Al 0.70 In 0.30 The N layer 401a and the p-Al 0.70 In 0.30 The p-Al layer surrounding the N layer 401a 0.90 In 0.10 In this way, the p-Al 0.90 In 0.10 The In composition of the N layer 401b is p-Al 0.70 In 0.30 The In composition is smaller than that of the N layer 401a. 0.70 In 0.30 The N layer 401a is an example of the first region, and is a p-Al 0.90 In0.10 N layer 401b is an example of the second region.

[0083] p ++ The -GaN layer 408 is formed on the current confinement layer 401. ++ The thickness of the -GaN layer 408 is, for example, 10 nm. ++ The GaN layer 408 contains 1×10 Mg as an acceptor. 20 cm -3 It is doped at a concentration of

[0084] In the laser structure 400, p ++ -GaN layer 408, current confinement layer 401, p-GaN layer 407, and p-Al 0.20 Ga 0.80 The N layer 406 , the multiple quantum well layer 405 , and a portion of the n-GaN layer 404 are etched to form a mesa structure 409 .

[0085] A SiN film 410 is formed as a passivation film so as to cover the surface and side surfaces of the mesa structure 409 and the surface of the n-GaN layer 404. The SiN film 410 contains p ++ An opening 410a exposing a part of the surface of the -GaN layer 408 and an opening 410b exposing a part of the surface of the n-GaN layer 404 are formed. 0.70 In 0.30 The N layer 401a is located inside the opening 410a.

[0086] p ++ An indium tin oxide (ITO) film 411 is formed on the surface of the -GaN layer 408 so as to protrude above the SiN film 410 through the opening 410a. An upper electrode 412 having a ring-shaped planar shape is formed on the SiN film 410 and the ITO film 411 above the mesa structure 409. Inside the upper electrode 412, a dielectric distributed Bragg reflector (DBR) 414 is formed on the ITO film 411. A lower electrode 413 is formed on the surface of the n-GaN layer 404 so as to protrude above the SiN film 410 through the opening 410b.

[0087] The upper electrode 412 has, for example, a Ti film and an Au film stacked in this order from the SiN film 410 and the ITO film 411 side. The lower electrode 413 has, for example, a Ti film and an Al film stacked in this order from the n-GaN layer 404 side. The DBR 414 includes, for example, a tantalum oxide film (Ta2O5 film) and a SiO2 film. The lower multilayer film reflector 403 and the DBR 414 are included in the resonator structure.

[0088] In the surface emitting laser 450, as described above, the current confinement layer 401 is made of p-Al 0.70 In 0.30 N layer 401a and p-Al 0.90 In 0.10 N layer 401b. 0.70 In 0.30 The band gap of the N layer 401a is 3.59 eV, and the band gap of the p-Al 0.90 In 0.10 The band gap of the N layer 401b is 5.24 eV.

[0089] The current confinement layer 401 is sandwiched between the p-GaN layer 407 and the p ++ The band gap of the p-GaN layer 408 is 3.4 eV. 0.90 In 0.10 The band gap of the N layer 401b is 0.70 In 0.30 N layer 401a, p-GaN layer 407, p ++ The band gap of the p-Al GaN layer 408 is 1.0 eV or more larger than that of the p-Al GaN layer 408. 0.90 In 0.10 N layer 401b and p-Al 0.70 In 0.30 N layer 401a, p-GaN layer 407, p ++ A large band offset is formed between the GaN layer 408 and the GaN layer 408 .

[0090] Furthermore, by the manufacturing method described later, p-Al 0.90 In 0.10 N layer 401b and p-Al 0.70 In 0.30The N layer 401a and the p-GaN layer 407, ++ Within the plane of the GaN layer 408, p-Al 0.90 In 0.10 The hydrogen atom concentration in the region where the N layer 401b is formed is p-Al 0.70 In 0.30 N layer 401a, p-GaN layer 407 and p ++ Within the plane of the GaN layer 408, p-Al 0.70 In 0.30 This is higher than the hydrogen atom concentration in the region where the N layer 401a is formed.

[0091] Therefore, inside the current confinement layer 401, p-Al 0.90 In 0.10 The current is blocked by the N layer 401b, and the current is 0.70 In 0.30 It selectively flows through the N layer 401a.

[0092] In addition, p-Al 0.90 In 0.10 The refractive index of the N layer 401b is p-Al 0.70 In 0.30 Since the refractive index is lower than that of the N layer 401a, a light confinement effect can be obtained in the in-plane direction of the substrate.

[0093] Next, a method for manufacturing the surface-emitting laser 450 according to the fourth embodiment will be described. Figures 9A to 9D are cross-sectional views showing the method for manufacturing the surface-emitting laser 450 according to the fourth embodiment. In this manufacturing method, the nitride semiconductor layers included in the laser structure 400 are epitaxially grown on an n-GaN substrate 402.

[0094] First, using an MOCVD apparatus, a lower multilayer reflector 403, an n-GaN layer 404, a multiple quantum well layer 405, and a p-Al 0.20 Ga 0.80 N layer 406, p-GaN layer 407, and p-Al 0.70 In 0.30 N-layer 401x and p ++ -GaN layer 408 is then formed.

[0095] p-Al 0.20 Ga 0.80 N layer 406, p-GaN layer 407, p-Al 0.70 In 0.30 N-layer 401x, p ++ The Mg in the GaN layer 408 (hereinafter collectively referred to as the p-type layer) is ++ - 1 × 10 for GaN layer 408 20 cm -3 and 2×10 19 cm -3 Doping with.

[0096] Hydrogen atoms originating from the ammonia gas used in film formation in the MOCVD apparatus are incorporated into the p-type layer at the same concentration as Mg in the p-type layer, causing it to be inactivated (inactivation rate 1.0). Therefore, as the first heat treatment, the structure shown in FIG. 9A is placed in a heat treatment apparatus and heat-treated at 600°C in an oxygen atmosphere. The heat treatment time is, for example, 10 minutes. Depending on the heat treatment temperature, time, and atmospheric gas, this heat treatment causes 90% of the hydrogen atoms to be desorbed from the p-type layer (inactivation rate 0.10), resulting in p-type conductivity.

[0097] The structure shown in FIG. 9A is then removed from the MOCVD apparatus, and as shown in FIG. ++ On the GaN layer 408, p-Al 0.70 In 0.30 As a protective mask covering the region where the N layer 401a is to be formed, for example, a SiO2 film 415 having a diameter of 10 μm and a thickness of 100 nm is formed. The SiO2 film 415 can be formed by, for example, photolithography.

[0098] Thereafter, the structure shown in FIG. 9B is placed in an MOCVD apparatus and heat-treated at 800° C. in a mixed gas atmosphere of hydrogen and ammonia. The heat treatment time is, for example, 30 minutes. By this heat treatment, p-Al 0.70 In 0.30 Hydrogen atoms penetrate into the portion of the N layer 401x exposed from the SiO2 film 415, and In evaporates from this portion.

[0099] As a result, as shown in FIG. 9C, p-Al 0.70 In 0.30 The portion of the N layer 401x exposed from the SiO2 film 415 is p-Al 0.90 In 0.10 It changes to N layer 401b. 0.70 In 0.30 The remainder of the N layer 401x has an In composition of p-Al 0.70 In 0.30 p-Al, which has not changed from the In composition of N layer 401x 0.70 In 0.30 In this way, the p-Al 0.70 In 0.30 N layer 401a and p-Al 0.90 In 0.10 A current confinement layer 401 having an N layer 401b is formed. Furthermore, hydrogen with the same concentration as Mg in the p-type layer in the region where the SiO2 film 415 is not formed is taken into the p-type layer in the region where the SiO2 film 415 is not formed, and Mg is inactivated, so that a resistance distribution is formed in the p-type layer.

[0100] Next, the structure shown in FIG. 9C is removed from the MOCVD apparatus, and the SiO2 film 415 is removed. The SiO2 film 415 can be removed, for example, using buffered hydrofluoric acid. Then, the p ++ -GaN layer 408, current confinement layer 401, p-GaN layer 407, and p-Al 0.20 Ga 0.80 By removing the N layer 406, the multiple quantum well layer 405, and a part of the n-GaN layer 404, a mesa structure 409 is formed for device isolation.

[0101] Then, as shown in FIG. ++An ITO film 411 is formed on the surface of the n-GaN layer 408 so as to rise above the SiN film 410 through the opening 410a, and an upper electrode 412 having a ring-like planar shape is formed on the SiN film 410 and the ITO film 411 above the mesa structure 409. A lower electrode 413 is formed on the surface of the n-GaN layer 404 so as to rise above the SiN film 410 through the opening 410b. The upper electrode 412 is formed, for example, by stacking a Ti film and an Au film in order from the SiN film 410 and ITO film 411 side. The lower electrode 413 is formed, for example, by stacking a Ti film and an Al film in order from the n-GaN layer 404 side. Next, a DBR 414 is formed on the ITO film 411 inside the upper electrode 412.

[0102] In this manner, the surface-emitting laser 450 according to the fourth embodiment can be manufactured. 0.70 In 0.30 In the N layer 401x, a distribution of the band gap in the plane due to the difference in the In composition and a distribution of the hydrogen atom concentration are formed. In other words, a distribution of the electrical resistance is formed due to the difference in the passivation rate of Mg. ++ -The difference in the Mg passivation rate in each plane of GaN 408 results in an electrical resistance distribution, which makes it possible to obtain very stable current confinement structure characteristics. Furthermore, the refractive index distribution is formed in the plane of the current confinement layer 401, which strengthens the light confinement in the in-plane direction, resulting in a surface-emitting laser with good characteristics.

[0103] Fifth embodiment Next, a fifth embodiment will be described. The fifth embodiment relates to a surface emitting laser having a nitride semiconductor structure. The surface emitting laser is an example of a light emitting device. Fig. 10 is a cross-sectional view showing the surface emitting laser according to the fifth embodiment.

[0104] 10, a surface-emitting laser 550 according to the fifth embodiment has an n-GaN substrate 502 and a laser structure 500 on the n-GaN substrate 502. The laser structure 500 includes a lower multilayer reflector 503, an n-GaN layer 504, a multiple quantum well layer 505, a p-AlGaN layer 506, a p-GaN layer 507, a current confinement layer 501, and a n ++ The current confinement layer 501 and the n-GaN layer 502 are disposed on the n-GaN substrate 501. ++ A tunnel junction is formed between the p-GaN layer 507 and the -GaN layer 508. The p-GaN layer 507 is an example of a p-type semiconductor layer, and the current confinement layer 501 is an example of a nitride semiconductor layer containing Mg as an impurity. The laser structure 500 is an example of a nitride semiconductor structure.

[0105] The lower multilayer reflector 503 is formed on an n-GaN substrate 502. The lower multilayer reflector 503 has a structure in which high-refractive index layers and low-refractive index layers are alternately stacked for 46 periods. The high-refractive index layers are, for example, 50 nm thick In 0.05 Ga 0.95 The low refractive index layer has a multilayer structure in which, for example, two AlN layers with a thickness of 6 nm are inserted between three GaN layers with a thickness of 6 nm.

[0106] The n-GaN layer 504 is formed on the lower multilayer reflector 503. The thickness of the n-GaN layer 504 is, for example, 1.1 μm.

[0107] The multiple quantum well layer 505 is formed on the n-GaN layer 504. The multiple quantum well layer 505 is, for example, an InN layer having a thickness of 4 nm. 0.10 Ga 0.90 It has a structure in which N layers and GaN layers with a thickness of 6 nm are alternately stacked for five periods. The multiple quantum well layer 505 is an example of an active layer.

[0108] The p-AlGaN layer 506 is formed on the multiple quantum well layer 505. The thickness of the p-AlGaN layer 506 is, for example, 20 nm.

[0109] The p-GaN layer 507 is formed on the p-AlGaN layer 506. The thickness of the p-GaN layer 507 is, for example, 100 nm.

[0110] The current confinement layer 501 is formed on the p-GaN layer 507. The thickness of the current confinement layer 501 is, for example, 10 nm. ++ -Al 0.70 In 0.30 The N layer 501a and the current confinement layer 501 are parallel to each other. ++ -Al 0.70 In 0.30 p surrounding N layer 501a ++ -Al 0.90 In 0.10 and N layer 501b.

[0111] In this way, p ++ -Al 0.90 In 0.10 The In composition of the N layer 501b is p ++ -Al 0.70 In 0.30 The In composition is smaller than that of the N layer 501a. ++ -Al 0.70 In 0.30 The N layer 501a is an example of the first region. ++ -Al 0.90 In 0.10 The N layer 501b is an example of the second region. ++ -Al 0.70 In 0.30 N layers 501a and p ++ -Al 0.90 In 0.10 The N layer 501b contains 1×10 Mg as an acceptor. 20 cm -3 It is doped at a concentration of

[0112] n ++ The -GaN layer 508 is formed on the current confinement layer 501. ++ The thickness of the -GaN layer 508 is, for example, 10 nm. ++ The GaN layer 508 has 3×10 Si as a donor. 20 cm -3It is doped at a concentration of

[0113] A tunnel junction is formed between the current confinement layer 501 highly doped with Mg and the n-GaN layer 508 highly doped with Si. ++ The n-GaN layer 509 is formed on the n-GaN layer 508. The n-GaN layer 509 has a thickness of, for example, 440 nm.

[0114] The laser structure 500 includes an n-GaN layer 509 and ++ The -GaN layer 508, the current confinement layer 501, the p-GaN layer 507, the p-AlGaN layer 506, the multiple quantum well layer 505, and a portion of the n-GaN layer 504 are etched to form, for example, a mesa structure 510 having a circular planar shape.

[0115] A SiN film 511 is formed as a passivation film so as to cover the surface and side surfaces of the mesa structure 510 and the surface of the n-GaN layer 504. The SiN film 511 has an opening 511a exposing a part of the surface of the n-GaN layer 508 and an opening 511b exposing a part of the surface of the n-GaN layer 504. For example, when viewed from above, ++ -Al 0.70 In 0.30 The N layer 501a is located inside the opening 511a.

[0116] A ring-shaped upper electrode 512 is formed on the surface of the n-GaN layer 509 except for the central portion of the opening 511a, so as to rise above the SiN film 511 through the opening 511a. Inside the upper electrode 512, a dielectric DBR 514 is formed on the n-GaN layer 509. On the surface of the n-GaN layer 504, a lower electrode 513 is formed on the surface of the n-GaN layer 504, so as to rise above the SiN film 511 through the opening 511b. The upper electrode 512 and the lower electrode 513 have, for example, a Ti film and an Al film laminated in this order from the n-GaN layer 504 side and the n-GaN layer 509 side. The DBR 514 includes, for example, a tantalum oxide film (Ta2O5 film) and a SiO2 film. The lower multilayer film reflector 503 and the DBR 514 are included in the resonator structure.

[0117] In the surface emitting laser 550, as described above, the current confinement layer 501 is p ++ -Al 0.70 In 0.30 N layer 501a and p ++ -Al 0.90 In 0.10 N layer 501b. ++ -Al 0.70 In 0.30 The band gap of the N layer 501a is 3.59 eV, and ++ -Al 0.90 In 0.10 The band gap of the N layer 501b is 5.24 eV. ++ The band gap of the -GaN layer 508 is 3.4 eV. ++ -Al 0.90 In 0.10 The band gap of the N layer 501b is the p ++ -Al 0.70 In 0.30 N layer 501a, p-GaN layer 507, n ++ -1.0 eV larger than any band gap of the GaN layer 508. ++ -Al 0.90 In 0.10 N layer 501b and p ++ -Al 0.70 In 0.30 N layer 501a, p-GaN layer 507, n ++ A large band offset is formed between the GaN layer 508 and the GaN layer 509 .

[0118] Furthermore, by the manufacturing method described later, p ++ -Al 0.90 In 0.10 N layer 501b and p ++ -Al 0.70 In 0.30 Within the plane of the N layer 501a and the p-GaN layer 507, ++ -Al 0.90 In 0.10 The hydrogen atom concentration in the region where the N layer 501b is formed is p ++ -Al 0.70 In 0.30The N layer 501a and the p-GaN layer 507 are ++ -Al 0.70 In 0.30 This is higher than the hydrogen atom concentration in the region where the N layer 501a is formed.

[0119] Therefore, inside the current confinement layer 501, the current is p ++ -Al 0.90 In 0.10 It is blocked by the N layer 501b, and p ++ -Al 0.70 In 0.30 It flows selectively through the N layer 501a. ++ -Al 0.90 In 0.10 The refractive index of the N layer 501b is p ++ -Al 0.70 In 0.30 Since the refractive index is lower than that of the N layer 501a, a light confinement effect can be obtained in the in-plane direction.

[0120] Next, a method for manufacturing the surface-emitting laser 550 according to the fifth embodiment will be described. Figures 11A to 11D are cross-sectional views showing a method for manufacturing the surface-emitting laser 550 according to the fifth embodiment. In this manufacturing method, the nitride semiconductor layers included in the laser structure 500 are epitaxially grown on an n-GaN substrate 502.

[0121] First, using an MOCVD apparatus, as shown in FIG. 11A, a lower multilayer reflector 503, an n-GaN layer 504, a multiquantum well layer 505, a p-AlGaN layer 506, a p-GaN layer 507, and a p ++ -Al 0.70 In 0.30 N-tier 501x ​​and n ++ A -GaN layer 508 and an n-GaN layer 509 are formed in this order.

[0122] Next, the structure shown in FIG. 11A is taken out of the MOCVD apparatus, and as shown in FIG. 11B, the n-GaN layer 509 and the n ++ -GaN layer 508 and p ++ -Al 0.70 In0.30 The N layer 501x, the p-GaN layer 507, the p-AlGaN layer 506, the multiple quantum well layer 505, and a portion of the n-GaN layer 504 are removed to form a mesa structure 510.

[0123] Thereafter, the structure shown in FIG. 11B is subjected to a first heat treatment at a temperature of 800° C. in an oxygen atmosphere. The heat treatment time is, for example, 30 minutes. By this heat treatment, the p-AlGaN layer 506, the p-GaN layer 507, and the p ++ -Al 0.70 In 0.30 90% (inactivation rate: 0.10) of the hydrogen atoms bonded to Mg in the N layer 501x ​​are desorbed from the sidewall of the mesa structure 510, and the Mg is activated, exhibiting p-type conductivity.

[0124] Next, the structure shown in FIG. 11B is placed in an MOCVD apparatus and heat-treated at 800° C. in a mixed gas atmosphere of hydrogen and ammonia. The heat treatment time is, for example, 30 minutes. By this heat treatment, p ++ -Al 0.70 In 0.30 As hydrogen atoms penetrate into the N layer 501x, In evaporates from this portion. As a result, as shown in FIG. ++ -Al 0.70 In 0.30 The side wall of the N layer 501x ​​is p ++ -Al 0.90 In 0.10 It changes to N layer 501b. ++ -Al 0.70 In 0.30 The remainder of the N layer 501x ​​is p ++ -Al 0.70 In 0.30 The In composition of the N layer 501x ​​is unchanged. ++ -Al 0.70 In 0.30 In this way, the N layer 501a is formed. ++ -Al 0.70 In 0.30 N layer 501a and p ++ -Al 0.90 In 0.10A current confinement layer 501 having an N layer 501b is formed.

[0125] p ++ -Al 0.90 In 0.10 The range in which the N layer 501b is formed is, for example, within about 10 μm from the sidewall. Furthermore, hydrogen atoms penetrate from the sidewall into the p-AlGaN layer 506 and the p-GaN layer 507, and the layers are passivated. Hydrogen atoms are taken in at the same concentration as Mg in the p-type layer on the sidewall side (passivation rate 1.0), and the Mg is passivated, forming an electrical resistance distribution in the p-type layer.

[0126] 11D, a SiN film 511 is formed to cover the surface and side surfaces of mesa structure 510 and the surface of n-GaN layer 504. Next, an opening 511a exposing a part of the surface of n-GaN layer 509 and an opening 511b exposing a part of the surface of n-GaN layer 504 are formed in SiN film 511.

[0127] Thereafter, a ring-shaped upper electrode 512 is formed on the surface of n-GaN layer 509 except for the center of opening 511a, so as to protrude above SiN film 511. Also, a lower electrode 513 is formed on the surface of n-GaN layer 504, so as to protrude above SiN film 511 through opening 511b. In forming upper electrode 512 and lower electrode 513, for example, a Ti film and an Al film are laminated in this order from the n-GaN layer 504 side and the n-GaN layer 509 side. Next, a DBR 514 is formed inside upper electrode 512.

[0128] In this manner, the surface-emitting laser 550 according to the fifth embodiment can be manufactured. The composition, conductivity type, and impurity concentration of the current confinement layer are not limited to those in these embodiments. Furthermore, the application of the nitride semiconductor structure having a current confinement layer is not limited to optical elements, and the nitride semiconductor structure having a current confinement layer can also be used in other electronic devices.

[0129] Sixth embodiment Next, a sixth embodiment will be described. The sixth embodiment relates to a projection device that draws an image by scanning a laser. The projection device is an example of a light source device. FIG. 12 is a diagram showing the layout of the projection device according to the sixth embodiment.

[0130] The projection device 1000 according to the sixth embodiment includes a light source 1001 and an optical scanning unit 1002. The light source 1001 includes, for example, one or more of the surface-emitting laser 450 according to the fourth embodiment and the surface-emitting laser 550 according to the fifth embodiment. When there is one surface-emitting laser 450 or one surface-emitting laser 550, the projection device 1000 projects a monochromatic image onto the object 1003. When there are multiple surface-emitting lasers 450 or 550, the projection device 1000 can project images of multiple colors onto the object 1003 by aligning the optical axes of the surface-emitting lasers on the same axis and emitting light from the emission surface and changing the oscillation wavelength for each surface-emitting laser.

[0131] The optical scanning unit 1002 includes an element for scanning the laser light emitted from the light source 1001 and projecting it onto the target 1003. As such an element, a micro electro mechanical systems (MEMS) mirror movable in two axial directions or an element combining two MEMS mirrors movable in one axial direction can be used. The optical scanning unit 1002 is an example of an optical element that adjusts the traveling direction of the laser light emitted from the light source 1001.

[0132] When generating an image, the intensity of the laser light is modulated in accordance with the scanning of the optical scanning unit 1002, and the laser light is irradiated onto the object 1003. In this manner, an image can be generated directly on the object 1003.

[0133] When a single or a small number of surface emitting lasers are used as the light source 1001, a laser beam of the order of μW to several mW can be output and an image can be drawn in a minute area. Such a projection device 1000 can be used as, for example, a retinal display.

[0134] When a two-dimensional array light source in which a number of surface-emitting lasers are arrayed is used as the light source 1001, it is possible to output laser light of the order of mW to the order of kW and draw an image in a large area. Such a projection device can be used as, for example, a projector.

[0135] Seventh embodiment Next, a seventh embodiment will be described. The seventh embodiment relates to a floodlight device. The floodlight device is an example of a light source device. Fig. 13 is a diagram showing a layout of the floodlight device according to the seventh embodiment.

[0136] A light projecting device 1100 according to the seventh embodiment includes a light source 1101, a fluorescent member 1102, and a light projecting member 1103. As the light source 1101, for example, a two-dimensional array light source in which a plurality of the surface-emitting lasers 450 according to the fourth embodiment and the surface-emitting lasers 550 according to the fifth embodiment are arrayed is used, and the fluorescent member 1102 is excited with light emitted from the light source 1101. The light emitted from the light source 1101 and the light emitted by the excited fluorescent member 1102 are two-dimensionally expanded by the light projecting member 1103 and projected. FIG. 13 illustrates a reflecting mirror as an example of the light projecting member 1103.

[0137] As the fluorescent member 1102, for example, when the light emitted from the light source 1101 is blue light, a fluorescent member emitting yellow light is used, and when the light emitted from the light source 1101 is ultraviolet light, a fluorescent member emitting white light is used. The fluorescent member 1102 is an example of an optical element that adjusts the wavelength of the laser light emitted from the light source 1101. Moreover, the light projecting member 1103 is an example of an optical element that adjusts the traveling direction of the laser light emitted from the light source 1101 and whose wavelength has been adjusted by the fluorescent member 1102.

[0138] The light source 1101 is, for example, a two-dimensional array light source in which several thousand to several tens of thousands of surface-emitting lasers are arranged in a two-dimensional array on a surface, and electrodes are connected so that a plurality of surface-emitting laser groups can be driven individually. The surface-emitting laser group may have a plurality of surface-emitting lasers, or may have a single surface-emitting laser.

[0139] By selecting a group of surface-emitting lasers to which a voltage is applied, it is possible to project light to any location or space with one light source 1101. For example, when the light projecting device 1100 is used as an in-vehicle headlight module, it can be used as a variable light distribution headlamp.

[0140] Eighth embodiment Next, an eighth embodiment will be described. The eighth embodiment relates to a projection device. The projection device is an example of a light source device. Fig. 14 is a diagram showing a layout of the projection device according to the eighth embodiment.

[0141] The projection device 1200 according to the eighth embodiment includes a light source 1201 and a projection optical unit 1202. The light source 1201 includes a two-dimensional array light source in which a plurality of the surface-emitting lasers 450 according to the fourth embodiment and the surface-emitting lasers 550 according to the fifth embodiment are arrayed.

[0142] The projection optical unit 1202 includes at least a fluorescent member 1203, a filter 1204, and an image generating element 1205, and may further include lenses such as a projection lens 1206, mirrors, and the like, as necessary.

[0143] The fluorescent member 1203 produces white light by being excited by a portion of the light incident on the projection optical unit 1202 from the light source 1201. As the fluorescent member 1203, for example, when the light emitted from the light source 1201 is blue light, a fluorescent member that emits yellow light is used, and when the light emitted from the light source 1201 is ultraviolet light, a fluorescent member that emits white light is used.

[0144] The filter 1204 is a filter that separates colors from white light and also has a movable part. As the filter 1204, for example, a color wheel that transmits red, blue, and green light is used.

[0145] The image generating element 1205 is an element that generates an image from the light that has passed through the filter 1204. As the image generating element 1205, for example, a MEMS device having fine mirrors in a two-dimensional array, a reflective liquid crystal element, or the like is used.

[0146] The projection lens 1206 enlarges the image generated by the image generating element 1205 to a desired magnification and projects it onto an object. The projection optical unit 1202 is an example of an optical element that adjusts the wavelength, traveling direction, etc. of the laser light emitted from the light source 1201.

[0147] In this embodiment, the projection optical unit 1202 includes a filter 1204, but a prism or a dichroic mirror may be used instead of the filter 1204. When a prism or a dichroic mirror is used, it is possible to configure the system so that light is separated into, for example, red, green, and blue, images of each color are generated by three image generating elements, and the images are finally combined by a prism or the like.

[0148] Ninth embodiment Next, a head mounted display according to a ninth embodiment will be described with reference to Fig. 15 and Fig. 16. Fig. 15 is a perspective view for explaining an example of the configuration of a head mounted display 60 according to this embodiment. Fig. 16 is a cross-sectional view for explaining an example of the configuration of the head mounted display 60.

[0149] The head mounted display 60 is an example of a head mounted display device that can be worn on a human head, and may have a shape similar to glasses. Note that hereinafter, the head mounted display will be abbreviated to HMD.

[0150] 15, the HMD 60 is composed of a front 60a and a temple 60b, which are provided approximately symmetrically on the left and right sides. The front 60a can be composed of, for example, a light guide plate 61, and the optical system, control device, etc. can be built into the temple 60b.

[0151] Fig. 16 shows a part of the configuration of the HMD 60. Note that, although Fig. 15 shows an example of the configuration for the left eye, the HMD 60 has a similar configuration for the right eye.

[0152] The HMD 60 includes a control device 11, a light source unit 930, a light amount adjustment section 907, a movable device 13 having a reflecting surface 14, a light guide plate 61, and a half mirror 62. The HMD 60 is an example of a display device.

[0153] The light source unit 930 is a unit made up of a red laser light source, a green laser light source, a blue laser light source, a plurality of collimating lenses, and a plurality of dichroic mirrors, all of which are integrated into an optical housing. In the light source unit 930, the three color laser lights from the red laser light source, the green laser light source, and the blue laser light source are combined by a dichroic mirror, which serves as a combining section. The light source unit 930 emits a combined parallel light. The light source unit 930 is an example of a light source device.

[0154] Each laser light source includes, for example, one or more surface emitting lasers 450, 550 according to the fourth or fifth embodiment, and irradiates laser light. Note that, although the oscillation wavelength is specified in the fourth and fifth embodiments, the oscillation wavelength can be changed by selecting the material and optical thickness of the semiconductor layer.

[0155] The light from the light source unit 930 is adjusted in amount by the light amount adjustment section 907, and then enters the movable device 13. The movable device 13 moves the reflection surface 14 in the XY directions based on a signal from the control device 11, and performs two-dimensional scanning with the light from the light source unit 930. The drive control of the movable device 13 is performed in synchronization with the emission timing of the red laser light source, the green laser light source, and the blue laser light source.

[0156] The scanning light from the movable device 13 is incident on a light guide plate 61. The light guide plate 61 reflects the scanning light on its inner wall surface and guides the light to a half mirror 62. The light guide plate 61 is made of a resin or the like that is transparent to the wavelength of the scanning light.

[0157] The half mirror 62 reflects the light from the light guide plate 61 to the rear side of the HMD 60 and emits it in the direction of the eyes of a wearer 63 of the HMD 60. The half mirror 62 has, for example, a free curved surface shape. An image formed by the scanning light is formed on the retina of the wearer 63 by reflection from the half mirror 62. Alternatively, an image is formed on the retina of the wearer 63 by reflection from the half mirror 62 and the lens effect of the crystalline lens in the eyeball. Furthermore, spatial distortion of the image is corrected by reflection from the half mirror 62. The wearer 63 can visually recognize the image formed by the light scanned in the XY directions.

[0158] Since the half mirror 62 is used, an image based on light from the outside world and an image based on the scanning light are superimposed and viewed by the wearer 63. By providing a mirror instead of the half mirror 62, it is possible to eliminate light from the outside world and to configure so that only the image based on the scanning light can be viewed.

[0159] In this embodiment, compared to when an edge-emitting laser is used as the light source, a small, lightweight HMD can be realized that requires fewer parts such as ND filters and consumes less power.

[0160] (Tenth embodiment) Next, a biometric authentication device using a human pupil response according to the tenth embodiment will be described with reference to FIG. 17. FIG. 17 is a diagram for explaining an example of the configuration of the biometric authentication device according to this embodiment. The biometric authentication device 20 includes a light source 21, an optical scanning unit 22, a first optical element 23, a second optical element 24, an image sensor 25, and a control device 27. The light source 21 includes, for example, one or more surface-emitting lasers 450, 550 according to the fourth or fifth embodiment, and the light emitted from the light source 21 is incident on the optical scanning unit 22. The optical scanning unit 22 moves a reflecting surface based on a signal from the control device 27, and scans the light from the light source 21. The scanning light from the optical scanning unit 22 is irradiated to the pupil 26 via the first optical element 23 and the second optical element 24. The size of the pupil is controlled by the intensity of the light irradiated to the pupil 26, and iris information is acquired by the image sensor 25. Then, the control device 27 acquires information on the pupil 26 of the person (living body) based on the output of the imaging element 25. The biometric authentication device 20 is an example of a biometric information acquisition device, the light source 21 is an example of a light source device, the imaging element 25 is an example of a light receiving device, and the control device 27 is an example of an information acquisition unit.

[0161] For example, the first optical element 23 is a waveguide that guides the light scanned by the optical scanning unit 22 to the second optical element 24, and the second optical element 24 is a mirror that changes the path of the light emitted from the first optical element 23 to the pupil 26. Although the present embodiment has been described as being divided into two optical elements, other methods may be used as long as they are optical elements that emit the scanned light to the pupil 26.

[0162] The light source 21 can be equipped with multiple elements, for example, a module mounted so that lasers of four wavelengths, red, blue, green, and infrared, are emitted on the same axis. Since the pupil reaction to blue and green wavelengths is more sensitive than other wavelengths, it is possible to obtain detailed iris information by narrowing the pupil. In addition, by using multiple wavelengths, biometric information for each iris wavelength can be obtained, resulting in higher authentication accuracy.

[0163] For example, by using the surface emitting lasers 450 and 550 according to the fourth and fifth embodiments, a highly accurate biometric authentication device 20 can be realized.

[0164] Although the preferred embodiments have been described in detail above, the present invention is not limited to the above-described embodiments, and various modifications and substitutions can be made to the above-described embodiments without departing from the scope of the claims.

[0165] For example, aspects of the present invention are as follows. <1> A nitride semiconductor layer containing Mg as an impurity is provided. The nitride semiconductor layer is A first area; a second region surrounding the first region in a plane parallel to the nitride semiconductor layer; having the second region has an In composition smaller than the first region; A nitride semiconductor structure, wherein the hydrogen atom concentration in the second region is at least twice as high as the hydrogen atom concentration in the first region. <2> The Mg deactivation rate of the second region is 0.5 or more. <1> The nitride semiconductor structure according to claim 1. <3> The first region is made of AlInN or AlGaInN containing Mg as an impurity. <1> or the above <2> The nitride semiconductor structure according to claim 1, <4> The above <1> ~The above <3> The nitride semiconductor structure according to any one of the above items is provided. The light-emitting device, wherein the nitride semiconductor structure further comprises an active layer. <5> The nitride semiconductor structure has a resonator structure that resonates light emitted from the active layer. <4> The light-emitting element according to claim 1. <6> The above <4> or the above <5> A light source device comprising the light emitting element according to claim 1. <7> forming a nitride semiconductor layer containing Mg as an impurity; a first heat treatment step of activating Mg in the nitride semiconductor layer by heat treatment in an inert gas atmosphere; a hydrogen permeation treatment step of incorporating hydrogen atoms into the nitride semiconductor layer to form a first region in the nitride semiconductor layer and a second region that surrounds the first region in a plane parallel to the nitride semiconductor layer and prevents current from passing therethrough; having The hydrogen permeation treatment step is carried out after the first heat treatment step, the second region has an In composition smaller than the first region; 13. A method for manufacturing a nitride semiconductor structure, wherein the hydrogen atom concentration in the second region is at least twice as high as the hydrogen atom concentration in the first region. [Explanation of symbols]

[0166] 100, 200 Nitride semiconductor structure 101, 201, 301, 401, 501 Current confinement layer 101a First Area 101b Second Area 300 LED structure 350 Light Emitting Diode 301a p-Al 0.70 In 0.30 N layer 301b p-AlN layer 401a p-Al 0.70 In 0.30 N layer 401b p-Al 0.90 In 0.10 N layer 400, 500 laser structure 450, 550 Surface Emitting Laser 501a p ++ -Al 0.70 In 0.30 N layer 501b p ++ -Al 0.90 In 0.10 N layer 1000, 1200 projection device 1001, 1101, 1201 light source 1002 Optical scanning unit 1003 Object 1100 Floodlight 1102, 1203 Fluorescent materials 1103 Light-emitting components 1202 Projection optics section 1204 Filter 1205 Image generating element 1206 Projection Lens 60 Head-mounted display 930 Light source unit 20 Biometric authentication device 21 Light source [Prior art documents] [Patent documents]

[0167] [Patent Document 1] JP 2020-120051 A

Claims

1. A nitride semiconductor layer containing Mg as an impurity, The nitride semiconductor layer is A first region; and a second region surrounding the first region in a plane parallel to the nitride semiconductor layer; having the second region has an In composition smaller than the first region; A nitride semiconductor structure, wherein the hydrogen atom concentration in the second region is at least twice as high as the hydrogen atom concentration in the first region.

2. 2. The nitride semiconductor structure according to claim 1, wherein the Mg passivation ratio of the second region is 0.5 or more.

3. 3. The nitride semiconductor structure according to claim 1, wherein the first region is made of AlInN or AlGaInN containing Mg as an impurity.

4. The nitride semiconductor structure according to claim 1 or 2, The light-emitting device, wherein the nitride semiconductor structure further comprises an active layer.

5. The light emitting device according to claim 4 , wherein the nitride semiconductor structure has a resonator structure that resonates the light emitted from the active layer.

6. A light source device comprising the light emitting device according to claim 5 .

7. forming a nitride semiconductor layer containing Mg as an impurity; a first heat treatment step of activating Mg in the nitride semiconductor layer by performing heat treatment in an inert gas atmosphere; a hydrogen permeation treatment step of incorporating hydrogen atoms into the nitride semiconductor layer to form a first region in the nitride semiconductor layer and a second region that surrounds the first region in a plane parallel to the nitride semiconductor layer and prevents current from passing therethrough; having The hydrogen permeation treatment step is carried out after the first heat treatment step, the second region has an In composition smaller than the first region; 2. A method for manufacturing a nitride semiconductor structure, wherein the hydrogen atom concentration in the second region is at least twice as high as the hydrogen atom concentration in the first region.

Citation Information

Patent Citations

  • Nitride semiconductor multilayer structure, light-emitting element, light source device, and method of manufacturing nitride semiconductor multilayer structure

    JP2020120051A