Cu-BASED ALLOY POWDER AND MOLDED ARTICLE INCLUDING Cu-BASED ALLOY POWDER
A Cu-based alloy powder with controlled Zr and Ag content, along with minimized impurities, addresses the issues of high laser reflectance and conductivity loss in rapid melting processes, resulting in high-density, conductive shaped objects.
Patent Information
- Application Number
- JP2023045321
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
AI Technical Summary
Conventional Cu-based alloys are not suitable for rapid melting and solidification processes like additive manufacturing due to high laser reflectance, leading to poor bonding, unmelted particles, and low relative density in the shaped objects, and adding alloying elements to suppress reflectance reduces conductivity.
A Cu-based alloy powder containing 0.1 to 3.0% Zr and optionally 0.05 to 3.00% Ag, with controlled impurities such as Al, Fe, and Mn, is used to suppress laser reflectance and improve conductivity, achieved by using high-purity starting materials and specific crucibles to minimize impurity contamination during manufacturing.
The alloy powder achieves a relative density of 80% IACS or higher electrical conductivity, reducing internal voids and ensuring high-density shaped objects with excellent conductivity.
Smart Images

Figure 2024134890000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a Cu-based alloy powder suitable for processes involving rapid melting and rapid solidification, such as three-dimensional additive manufacturing, thermal spraying, laser coating, cladding, etc., and a molded body using this Cu-based alloy powder. In particular, the present invention relates to a powder for three-dimensional additive manufacturing and a three-dimensional additive manufactured body made of a Cu-based alloy powder suitable for three-dimensional additive manufacturing. [Background technology]
[0002] 3D printers are beginning to be used to create metal objects. These 3D printers create objects using additive manufacturing, and typical methods of metal additive manufacturing include the powder bed method (powder bed fusion method) and the metal deposition method (directed energy deposition method). In the powder bed method, the irradiated areas of the spread powder melt and solidify when irradiated with a laser beam or electron beam. This melting and solidification bonds the powder particles together. The laser beam or other irradiation is selectively applied to a portion of the metal powder, and the unirradiated areas do not melt, and a bond layer is formed only in the irradiated areas.
[0003] New metal powder is laid on top of the bonded layer and irradiated with a laser or electron beam. The beam melts and solidifies the metal particles, forming a new bonded layer. The new bonded layer also bonds with the existing bonded layer.
[0004] By repeatedly irradiating the metal powder at desired locations with a beam and melting and solidifying the powder, the bonded layer gradually grows. This growth allows a three-dimensional object to be obtained. By using additive manufacturing in this way, it is possible to easily produce objects with complex shapes that would be difficult to manufacture using conventional methods such as metal molding.
[0005] Meanwhile, alloys used in high-frequency induction heating devices, heat sinks for cooling motors, etc. are required to have excellent electrical and thermal conductivity, and Cu-based alloys are suitable for such applications.
[0006] A copper alloy has been proposed so far, which is obtained by sintering powder containing Cu and 5 to 8 at% Zr by spark plasma, and which contains Cu and a Cu-Zr compound, and in which the two phases of Cu and the Cu-Zr compound have a mosaic structure in which crystals with a size of 10 μm or less are dispersed when viewed in cross section, without containing a eutectic phase (see Patent Document 1).
[0007] Also, a copper alloy powder containing, in mass %, 1.1 to 20% Cr, 0 to 0.2% Zr, and the balance being Cu and unavoidable impurities has been proposed (see Patent Document 2).
[0008] The applicant of the present application has developed a Cu-based alloy comprising, in mass%, 0.1 to 5.0% of a selective component M (one or more of V, Fe, Zr, Nb, Hf, and Ta), and the balance being Cu and unavoidable impurities, and having an average particle diameter D 50 (μm) and the tap density TD (Mg / m 3 ) and the ratio (D 50 / TD) is 0.2×10 -5 m 4 / Mg~20×10 -5 m 4
[0005] Patent Document 3 proposes a Cu-based alloy powder containing Zr and Mg. The Zr content in this proposal is 0.1 to 2.0%.
[0009] The applicant of the present application also provides a Cu-based alloy containing, by mass%, optional components M (one or more of Cr, Fe, Ni, Zr, and Nb): 0.1 to 10.0%, Si: 0.20% or less, P: 0.10% or less, S: 0.10% or less, and unavoidable impurities, and an average particle diameter D 50 (μm) and the tap density TD (Mg / m 3 ) and the ratio (D 50 / TD) is 0.2×10 -5 m 4 / Mg~20×10 -5 m4 has proposed a Cu-based alloy powder having a sphericity of 0.80 to 0.95 (see Patent Document 4). [Prior art documents] [Patent documents]
[0010] [Patent Document 1] International Publication No. 2014 / 069318 [Patent Document 2] JP 2019-44260 A [Patent Document 3] JP 2019-210497 A [Patent Document 4] JP 2021-17639 A Summary of the Invention [Problem to be solved by the invention]
[0011] In the additive manufacturing process, metal materials are rapidly melted and then rapidly cooled to solidify. Conventional Cu-based alloys are not suitable for use as powders in processes involving such rapid melting, rapid cooling, and solidification, and it is difficult to obtain high-density objects even when conventional Cu-based alloy powders are used. Furthermore, conventional Cu-based alloys are not suitable, or even unsuitable, for other rapid melting, rapid cooling, and solidification processes such as thermal spraying, laser coating, and cladding.
[0012] The laser reflectance of pure Cu is higher than that of Fe-based alloys, Ni-based alloys, Co-based alloys, etc. Therefore, when pure Cu powder is used in a process involving rapid melting and rapid solidification, a lot of heat is released into the atmosphere due to the high laser reflectance of Cu. On the other hand, the powder itself does not receive enough heat to melt the powder. Insufficient heat leads to poor bonding between particles. Insufficient heat can also cause unmelted particles to remain inside the molded object obtained from this powder. In this way, the relative density of the molded object obtained from pure Cu powder is likely to be low.
[0013] On the other hand, if a laser with a high energy density is irradiated onto pure Cu powder, the remaining unmelted particles can be suppressed. However, using a laser with a high energy density can lead to bumping of the molten metal. Bumping can cause voids to form inside the molded object, so the energy density cannot be increased easily.
[0014] Therefore, in Cu-based alloys used in rapid melting and rapid solidification processes such as additive manufacturing, alloying elements are added to suppress the laser reflectance, but when the added alloying elements dissolve in Cu, the electrical conductivity is significantly reduced.
[0015] Therefore, an object of the present invention is to provide a Cu-based alloy powder that is suitable for a process involving rapid melting and rapid solidification, and that can give a shaped product with excellent electrical conductivity. [Means for solving the problem]
[0016] As a result of intensive research, the inventors decided to add Zr to Cu in order to suppress the laser reflectance. Zr has a small solid solubility limit in Cu on the equilibrium phase diagram. However, when powder is produced by a process involving rapid solidification such as atomization, Zr is dissolved in Cu in a supersaturated state. Since the laser reflectance is suppressed in this supersaturated solid solution, heat is unlikely to be released into the atmosphere even if the obtained Cu-based alloy powder is subjected to a process involving rapid melting and rapid solidification.
[0017] However, Zr, which is added to suppress the laser reflectivity, also reduces the electrical conductivity of the Cu-based alloy. Therefore, in order to improve the electrical conductivity, it was thought that it would be effective to reduce the impurities that deteriorate the electrical conductivity, and it was decided to control the inclusion of impurities contained in the starting materials. However, it was found that controlling the starting materials alone was not enough. This is because impurities are mixed in not only from the starting materials, but also from the powder manufacturing equipment and the crucible used to melt the raw materials during the production of the powder. Therefore, in addition to increasing the purity of the starting materials, it was decided to suppress the inclusion of impurity elements during production by changing the material of the crucible and lowering the tapping temperature.
[0018] In order to further improve the electrical conductivity, it was decided to add Ag. However, in order for the effect of adding Ag to be significant, it is desirable that the alloy does not contain Al, Fe, Ni, or Mn as impurities, and it was found that if these elements are contained as impurities, the improvement in electrical conductivity is not sufficient. Therefore, when adding Ag, it is useful to remove even more impurities from the Cu-based alloy, and it was found that adding Ag after controlling the impurities improves the electrical conductivity even more.
[0019] A first means for solving the problems of the present invention is a Cu-based alloy powder containing, by mass%, 0.1 to 3.0% Zr, with the remainder being Cu and unavoidable impurities, in which the unavoidable impurities further contain a total of 0.05% or less of Al, Fe, Ni, and Mn.
[0020] Furthermore, the Cu-based alloy powder preferably contains, by mass %, 0.2 to 2.0% Zr.
[0021] The second means is a Cu-based alloy powder containing, by mass%, 0.1-3.0% Zr, 0.05-3.00% Ag, and the balance being Cu and unavoidable impurities, in which the unavoidable impurities further contain a total of 0.05% or less of Al, Fe, Ni, and Mn.
[0022] Furthermore, the Cu-based alloy powder preferably contains, by mass %, 0.2 to 2.0% Zr and 0.05 to 2.00% Ag.
[0023] The third means is a compact using a Cu-based alloy powder containing, by mass%, 0.1 to 3.0% Zr, with the remainder being Cu and unavoidable impurities, and further including unavoidable impurities in which the total content of Al, Fe, Ni, and Mn is 0.05% or less.
[0024] Furthermore, it is preferable that the compact is made of a Cu-based alloy powder containing 0.2 to 2.0% by mass of Zr.
[0025] The fourth means is a compact using a Cu-based alloy powder containing, by mass%, 0.1 to 3.0% Zr, 0.05 to 3.00% Ag, and the balance being Cu and unavoidable impurities, wherein the unavoidable impurities further contain Al, Fe, Ni, and Mn in a total amount of 0.05% or less.
[0026] Furthermore, it is preferable that the compact is made of a Cu-based alloy powder containing, in mass %, 0.2 to 2.0% Zr and 0.05 to 2.00% Ag.
[0027] The fifth aspect of the present invention is a powder for three-dimensional additive manufacturing, which is made of the Cu-based alloy powder according to the first or second aspect of the present invention. The powder for three-dimensional additive manufacturing is used for three-dimensional additive manufacturing by repeating a process of rapid melting, rapid cooling and solidification by irradiating the powder with a beam such as a laser.
[0028] The sixth aspect of the present invention is a three-dimensional additively manufactured object produced by additive manufacturing using the Cu-based alloy powder according to the first or second aspect of the present invention. In other words, it is a three-dimensional additive manufacturing object formed by three-dimensional additive manufacturing by sequentially repeating the process of rapidly melting, rapidly cooling and solidifying a powder for three-dimensional additive manufacturing, which is made of the alloy powder of the first or second means, by irradiating the powder with a beam such as a laser. Effect of the Invention
[0029] In the Cu-based alloy powder containing Zr according to the present invention, impurities such as Al, Fe, Ni, and Mn are controlled and reduced, so that the molded body obtained by molding involving rapid melting and rapid solidification exhibits an excellent electrical conductivity of 80% IACS or more. Furthermore, by adding a small amount of Ag to the Cu-based alloy powder containing Zr and controlling and reducing impurities such as Al, Fe, Ni, and Mn, the molded body exhibits an even better electrical conductivity of 85% IACS or more. In the Cu-based alloy powder containing Zr according to the present invention, Zr is dissolved in a supersaturated state by rapid melting and rapid solidification, so that the laser reflectance is more likely to be reduced. Since the laser reflectance is suppressed in the Cu-based alloy powder, which is a supersaturated solid solution, even if the obtained Cu-based alloy powder is subjected to a process involving rapid melting and rapid solidification, heat is not easily released into the atmosphere, so that unmelted particles are less likely to remain, and since there is no need to use a laser with a high energy density, it is possible to avoid the generation of voids inside due to bumping. Therefore, when the Cu-based alloy of the present invention is subjected to a process involving rapid melting and rapid solidification, a molded body made of Cu-based alloy powder can be appropriately molded, and a molded body that is less likely to have a low relative density can be obtained. In addition, these Cu-based alloy powders have low reflectance, and when used as powders for three-dimensional modeling and layer-by-layer modeling, they become three-dimensional layer-by-layer models with high relative density and excellent electrical conductivity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] The Cu-based alloy powder according to the present invention is an aggregate of many particles. The material of the particles is a Cu-based alloy containing, by mass%, 0.1 to 3.0% Zr, with the remainder being Cu and unavoidable impurities. The Cu-based alloy may further contain 0.05 to 3.00% Ag. These Cu-based alloy powders are characterized in that the total content of Al, Fe, Ni, and Mn among the unavoidable impurities is 0.05% or less. First, before describing the embodiments, the reasons for specifying the additive components and each component of the unavoidable impurities of the Cu-based alloy powder will be described. In the following description of the components, all % refers to mass%.
[0031] [Zr: 0.1-3.0%] Zr is an element with a small solid solubility limit in Cu in the equilibrium diagram. However, when Cu-based alloy powder is manufactured by a method involving rapid melting and rapid solidification such as atomization, the added Zr will be supersaturated in Cu. The laser reflectivity of such Cu-based alloy powder containing a supersaturated solid solution of Zr is suppressed. On the other hand, even when Cu-based alloy powder is subjected to a process involving rapid melting and rapid solidification, the heat is not easily released into the atmosphere. Therefore, in this process, it is not necessary to irradiate the Cu-based alloy powder containing Zr with a laser with an excessively high energy density. Therefore, bumping of the molten metal caused by excessive laser irradiation is suppressed. Since bumping is suppressed, when a shaped body is obtained by additive manufacturing using Cu-based alloy powder containing an appropriate amount of Zr, a shaped body with a high relative density and few internal voids can be obtained.
[0032] When the Zr content in the Cu-based alloy powder is 0.1% or more, the relative density of the molded body using this powder is high, and a molded body with few internal voids can be obtained. From this viewpoint, Zr is more preferably 0.2% or more. On the other hand, if the Zr content exceeds 3.0%, the decrease in electrical conductivity becomes too large. From this viewpoint, Zr is more preferably 2.0% or less. Therefore, Zr in the Cu-based alloy powder is set to 0.1 to 3.0%. Preferably, Zr is 0.2 to 2.0 mass%.
[0033] [Ag:0.05~3.00%] Ag is an element with better electrical conductivity than Cu, so even if it dissolves in Cu, it is an element that is unlikely to hinder the electrical conduction and thermal conduction of the Cu-based alloy. When Ag is added to this molded body that is two-phase, Cu and Zr compounds, the dissolution of Al, Fe, Ni, and Mn, which reduce electrical conductivity, into Cu is suppressed, and they are concentrated in the Zr compound. Such effects are significantly obtained from the addition of 0.05 mass% or more. However, since there is an upper limit to the amount of Al, Fe, Ni, and Mn concentrated in the Zr compound, even if Ag is added without reducing these impurities themselves, the effect is not sufficiently obtained, and the same effect cannot be obtained. If the amount of Ag added exceeds 3.00%, the electrical conductivity will decrease due to the dissolution of Ag in Cu, and the effect of adding Ag will be reduced. From this viewpoint, Ag is more preferably 2.00% or less. Therefore, when Ag is added to a Cu-based alloy, the amount is set to 0.05 to 3.00%. The Ag content is preferably 0.05 to 0.00%.
[0034] [Al, Fe, Ni, Mn: 0.05% or less in total] Among the unavoidable impurities in Cu-based alloy powder, Al, Fe, Ni, and Mn dissolve in Cu and inhibit the electrical and thermal conduction of the Cu-based alloy. Therefore, reducing the total amount of Al, Fe, Ni, and Mn is useful for improving electrical conductivity. From this perspective, the total content of Al, Fe, Ni, and Mn is set to 0.05% or less. Note that Al, Fe, Ni, and Mn are mixed in as impurities contained in the starting materials, and are also mixed in from the powder manufacturing equipment and the crucible used to melt the raw materials during powder production. Therefore, in addition to increasing the purity of the starting materials, the mixing of these impurity elements during powder production can be reduced by appropriately selecting the material of the crucible and lowering the tapping temperature.
[0035] [Powder manufacturing method] Examples of methods for producing powder include water atomization, single roll quenching, twin roll quenching, gas atomization, disk atomization, and centrifugal atomization. Preferred methods are gas atomization and disk atomization. Therefore, the following will explain the method for obtaining Cu-based alloy powder using gas atomization as an example.
[0036] The effects of the present invention will be clarified by the following examples, but it should be noted that the present invention should not be construed as being limited based on the descriptions of these examples.
[0037] [Powder production] The Cu-based alloy powder was produced by gas atomization. In a vacuum, raw materials having a predetermined composition were heated and melted in a predetermined crucible by high-frequency induction heating. Next, the molten metal was dropped at a predetermined melting temperature from a nozzle with a diameter of 5 mm under the crucible. Argon gas or nitrogen gas was sprayed onto the molten metal to obtain the Cu-based alloy powder. The crucibles used in the production of each powder, the melting temperature, and the composition of the obtained Cu-based alloy powder are shown in Table 1 below. All the composition in the table is in mass %. The Zr and Ag components in the Cu-based alloy powder are additive elements and are almost the same as the composition of the starting raw materials. In addition, as the starting raw material Cu, high-purity Cu with very few impurities was used in No. 1 to No. 15, and ordinary purity Cu was used in No. 16 to No. 20.
[0038] [Table 1]
[0039] [Molding] Using this Cu-based alloy powder as a raw material, additive manufacturing was carried out using a three-dimensional additive manufacturing device (EOS-M290 manufactured by EOS Corporation) to obtain a molded body.
[0040] [Measurement of electrical conductivity] A test piece (3 x 2 x 60 mm) of the molded body was created using the additive manufacturing method, and the electrical resistance value (Ω) was measured using the four-terminal method in accordance with Japanese Industrial Standard (JIS) C2525. The measurement was performed using a TER-2000RH model manufactured by ULVAC-RIKO. The measurement conditions were as follows: Temperature: 25℃ Current: 4A Distance between voltage measurement terminals: 40mm The electrical resistivity ρ (Ωm) was calculated based on the following formula. ρ=R / L×S In this formula, R is the electrical resistance of the test piece (Ω), L is the distance between the voltage measurement terminals (m), and S is the cross-sectional area of the test piece (m 2 ) Electrical conductivity (S / m) was calculated from the reciprocal of electrical resistivity ρ. In addition, the electrical conductivity (%IACS) of each test piece was calculated by taking 5.9×107 (S / m) as 100% IACS. The measurement results are shown in Table 1.
[0041] [No.1~No.5: Cu-Zr powder] Inventive examples No. 1 to No. 3 are Cu-Zr powders produced using crucibles (graphite, zirconia, magnesia) that do not contain the impurities Al, Fe, Ni, or Mn as the main raw material. The use of suitable crucibles suppressed the inclusion of impurities, and the electrical conductivity of the molded objects was 82% IACS or higher. Comparative Example No. 4 is a Cu-Zr powder prepared using an alumina crucible and at a pouring temperature of 1400° C., the same temperature as in Invention Examples No. 1 to No. 3. The resulting powder had an increased impurity content and poor electrical conductivity. Inventive Example No. 5 is a Cu-Zr powder obtained by using an alumina crucible and lowering the pouring temperature from 1400° C. to 1350° C. By lowering the pouring temperature, the inclusion of impurities was suppressed, and the electrical conductivity of the molded object was 83% IACS or higher.
[0042] [No.6~No.10: Cu-Zr-Ag powder] Inventive examples No. 6 to No. 8 are Cu-Zr-Ag powders produced using crucibles (graphite, zirconia, magnesia) that do not contain the impurities Al, Fe, Ni, or Mn as main raw materials. The suitable crucibles suppressed the incorporation of impurities, and the addition of Ag further suppressed the dissolution of impurities into Cu, resulting in the electrical conductivity of the molded object reaching 87% IACS or higher. Comparative Example No. 9 is a Cu-Zr-Ag powder prepared using an alumina crucible and at a pouring temperature of 1420° C., the same temperature as Invention Examples No. 6 to No. 8. The resulting powder had an increased impurity content, and the effect of adding Ag to suppress the dissolution of impurities into Cu was not sufficiently obtained, resulting in poor electrical conductivity. Inventive Example No. 10 is a Cu-Zr-Ag powder obtained by using an alumina crucible and lowering the pouring temperature from 1420° C. to 1320° C. Lowering the pouring temperature suppressed the inclusion of impurities, and the addition of Ag further suppressed the dissolution of impurities into Cu, resulting in a conductivity of 88% IACS or more for the molded product.
[0043] [No.11~No.15: Cu-Zr-Ag powder] Inventive examples No. 11 to No. 13 are Cu-Zr-Ag powders produced using crucibles (graphite, zirconia, magnesia) that do not contain the impurities Al, Fe, Ni, or Mn as main raw materials. The suitable crucibles suppressed the incorporation of impurities, and the addition of Ag further suppressed the dissolution of impurities into Cu, resulting in the electrical conductivity of the molded objects reaching 86% IACS or higher. Comparative Example No. 14 is a Cu-Zr-Ag powder prepared using an alumina crucible and at a pouring temperature of 1450° C., the same temperature as Invention Examples No. 11 to No. 13. The resulting powder had an increased impurity content, and the effect of adding Ag to suppress the dissolution of impurities into Cu was not sufficiently obtained, resulting in a deterioration in electrical conductivity. Inventive Example No. 15 is a Cu-Zr-Ag powder obtained by using an alumina crucible and lowering the pouring temperature from 1450° C. to 1350° C. Lowering the pouring temperature suppressed the inclusion of impurities, and the addition of Ag further suppressed the dissolution of impurities into Cu, resulting in the electrical conductivity of the molded object showing a value of 88% IACS or more.
[0044] [No.16~No.20: Uses Cu of normal purity] Comparative Examples No. 16 to No. 20 are Cu-Zr-Ag powders that were produced using Cu of normal purity as the starting material and a crucible (zirconia) that did not contain the impurities Al, Fe, Ni, and Mn as the main raw materials. Although the inclusion of impurities from the crucible was prevented, the impurity content of the obtained Cu-based alloy powder was increased compared to the invention examples due to the influence of the impurities in Cu, so the effect of suppressing the solid solution of impurities in Cu by adding Ag was not sufficiently obtained, and the conductivity deteriorated.
[0045] (Reflectivity) The reflectance of the copper alloy powder was examined for the 1064 nm wavelength of the Yb fiber laser. The reflectance of pure Cu powder for the 1064 nm wavelength Yb fiber laser is 76%. In contrast, in both the examples and comparative examples, the powder with 0.5-0.6% Zr reflected the laser light at about 65%, which was slightly improved. The powder with 1.9-2.1% Zr reflected the laser light at about 45%, making it easier to input heat efficiently.
[0046] (Regarding relative density) The relative density of the shaped body made from pure Cu powder was 88%. In contrast, the relative density of the shaped body made from the Cu-based alloy powder containing 0.5-0.6% Zr of the present invention was 97-99%. Moreover, the relative density of the shaped body made from the Cu-based alloy powder containing 1.9-2.1% Zr of the present invention was 99% or more.
[0047] (About conductivity) As shown in Table 1, the Cu-based alloy powder of the present invention controls the inclusion of impurities in the starting material and during the powder manufacturing process, so that the shaped body obtained from the Cu-based alloy powder of the present invention containing Zr has excellent electrical conductivity. In addition, it was confirmed that when Ag is added to the Cu-based alloy powder of the present invention in addition to Zr, the effect is not diminished by the impurities, and even better electrical conductivity can be obtained than in the case of Zr alone. It was confirmed that the inclusion of impurities can be reduced by using an expensive crucible such as zirconia instead of a general alumina crucible, and that the melting of impurities can be reduced by lowering the tapping temperature from the crucible, thereby obtaining a Cu-based alloy powder in which the decrease in electrical conductivity can be suppressed. On the other hand, in the comparative example, impurities are not controlled in the starting material or the powder manufacturing process, and impurities are mixed in not only from the starting material but also from the crucible during the manufacturing stage. Therefore, impurity components are dissolved in Cu in the Cu-based alloy powder, resulting in poor electrical conductivity. Even when high-purity Cu is used, impurities are mixed in due to the influence of the crucible, and the desired electrical conductivity is not obtained. In addition, in the comparative example, when excessive impurities are mixed in Cu, the effect of adding Ag is reduced, and sufficient effect is not obtained.
[0048] As described above, it has been confirmed that when the Cu-based alloy powder containing Zr in which specific impurities of the present invention are controlled is applied to a rapid melting and rapid solidification process such as additive manufacturing, the obtained shaped body exhibits excellent properties. Furthermore, it has been confirmed that when the Cu-based alloy powder containing Zr and Ag in which specific impurities are controlled is applied to a rapid melting and rapid solidification process such as additive manufacturing, the obtained shaped body exhibits even more excellent properties.
Claims
1. A Cu-based alloy powder containing, by mass%, 0.1 to 3.0% Zr, with the balance being Cu and unavoidable impurities, A Cu-based alloy powder in which the total content of the elements Al, Fe, Ni, and Mn among unavoidable impurities is 0.05% or less.
2. A Cu-based alloy powder containing, by mass%, 0.1 to 3.0% Zr, 0.05 to 3.00% Ag, and the balance being Cu and unavoidable impurities, A Cu-based alloy powder in which the total content of the elements Al, Fe, Ni, and Mn among unavoidable impurities is 0.05% or less.
3. A Cu-based alloy powder containing, by mass%, 0.1 to 3.0% Zr, with the balance being Cu and unavoidable impurities, A compact using a Cu-based alloy powder in which the total content of the elements Al, Fe, Ni, and Mn among unavoidable impurities is 0.05% or less.
4. A Cu-based alloy powder containing, by mass%, 0.1 to 3.0% Zr, 0.05 to 3.00% Ag, and the balance being Cu and unavoidable impurities, A compact using a Cu-based alloy powder in which the total content of the elements Al, Fe, Ni, and Mn among unavoidable impurities is 0.05% or less.
5. A powder for three-dimensional additive manufacturing comprising the Cu-based alloy powder according to claim 1 or 2.
6. A three-dimensional additively manufactured object produced by additive manufacturing using the Cu-based alloy powder according to claim 1 or 2.
Citation Information
Patent Citations
Copper alloy powder, heat treatment method for multilayer shaped structure, method for producing copper alloy shaped structure, and copper alloy shaped structure
JP2019044260A
Cu-BASED ALLOY POWDER
JP2019210497A
Cu-BASED ALLOY POWDER
JP2021017639A
Copper alloy and process for manufacturing same
WO2014069318A1