Method for manufacturing photocatalyst coating agent

By dispersing rutile-type titanium oxide particles in an aqueous medium using a bead mill and monitoring transmittance, the method ensures the photocatalytic function of titanium oxide is maximized in the coating agent, addressing shape preservation and efficiency issues in conventional dispersion techniques.

JP2024135203AActive Publication Date: 2024-10-04ADERANS CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023045769
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04
Estimated Expiration
2043-03-22

AI Technical Summary

Technical Problem

Conventional dispersion methods for titanium oxide fine particles in aqueous media can damage their shape, leading to insufficient expression of photocatalytic function in photocatalyst coating agents.

Method used

A method involving dispersing rutile-type titanium oxide particles in an aqueous medium using a bead mill and measuring the transmittance of the dispersion to determine the end point, ensuring the particle shape is maintained.

Benefits of technology

The method allows for the production of a photocatalyst coating agent where the original functions of titanium oxide fine particles are fully expressed, achieving high transparency and photocatalytic efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135203000002
    Figure 2024135203000002
  • Figure 2024135203000003
    Figure 2024135203000003
  • Figure 2024135203000004
    Figure 2024135203000004
Patent Text Reader

Abstract

To achieve a manufacturing of a photocatalyst coating agent with which a function inherent in fine particles of titanium oxide can appear sufficiently.SOLUTION: When manufacturing a photocatalyst coating agent containing rutile titanium oxide particles, a transmittance of an aqueous dispersion liquid generated is measured by dispersing the rutile titanium oxide particles in an aqueous medium by a bead mill. A terminal point of a dispersion step is determined by comparing a measurement result of the transmittance with a reference transmittance that indicates a good dispersion state of the rutile titanium oxide particles.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a photocatalytic coating agent. [Background technology]

[0002] Titanium oxide particles are useful as photocatalysts, and can be used as photocatalytic coating agents in the form of an aqueous dispersion in which they are dispersed in an aqueous medium. However, titanium oxide particles tend to aggregate in an aqueous medium. Therefore, in order to express the inherent photocatalytic function of titanium oxide particles in the aqueous dispersion, a technique for finely dispersing titanium oxide particles in an aqueous medium has been investigated.

[0003] Known examples of such techniques include a technique in which titanium oxide fine particles are dispersed in an aqueous medium by a sand mill using zirconia beads in the presence of a dispersant such as condensed phosphate or trimethylsiloxysilicate (see, for example, Patent Documents 1 and 2). Alternatively, known examples of the above techniques include a technique in which titanium oxide fine particles are dispersed in an aqueous medium by using a basic aqueous medium and controlling the rotation speed of a bead mill (see, for example, Patent Document 3). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 7-257923 [Patent Document 2] Japanese Patent Application Publication No. 9-208438 [Patent Document 3] JP 2012-250237 A Summary of the Invention [Problem to be solved by the invention]

[0005] On the other hand, titanium oxide fine particles can have various specific particle shapes. Dispersion by bead mill is a dispersion method carried out under relatively mild conditions, but if it is carried out excessively, the shape of titanium oxide fine particles may be damaged, and as a result, the original photocatalytic function of titanium oxide fine particles may not be fully expressed in the photocatalytic coating agent. Thus, the conventional technology has room for further study from the viewpoint of appropriately dispersing titanium oxide fine particles in an aqueous medium in the production of a photocatalytic coating agent.

[0006] An object of one aspect of the present invention is to realize the production of a photocatalytic coating agent in which the inherent photocatalytic function of titanium oxide fine particles is fully exerted. [Means for solving the problem]

[0007] In order to solve the above problems, a method for producing a photocatalytic coating agent according to one embodiment of the present invention is a method for producing a photocatalytic coating agent of an aqueous dispersion containing rutile-type titanium oxide particles in its dispersoid, the method comprising the steps of dispersing rutile-type titanium oxide particles in an aqueous medium using a bead mill, and measuring the transmittance of the aqueous dispersion produced in the step of dispersing in the aqueous medium, and the end point of the step of dispersing in the aqueous medium is determined by comparing the measurement result of the transmittance of the aqueous dispersion with a pre-specified transmittance of an aqueous dispersion of rutile-type titanium oxide particles dispersed in the aqueous medium while maintaining their particle shape. Effect of the Invention

[0008] According to one aspect of the present invention, it is possible to realize the production of a photocatalytic coating agent in which the inherent functions of titanium oxide fine particles are fully exhibited. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is a flow diagram showing an example of a method for producing a photocatalytic coating agent according to an embodiment of the present invention. [Diagram 2]FIG. 1 is a diagram showing a schematic configuration of an apparatus for producing a dispersion liquid of titanium oxide fine particles using a bead mill, which is used in one embodiment of the present invention. [Diagram 3] FIG. 2 is a flow diagram showing an example of a process for dispersing rutile-type titanium oxide particles in an aqueous medium according to one embodiment of the present invention. [Figure 4] FIG. 2 is a diagram showing an example of the particle size distribution of rutile-type titanium oxide particles in a raw dispersion liquid to be dispersed in one embodiment of the present invention. [Diagram 5] FIG. 2 is a diagram showing an electron microscope photograph of an example of the state of rutile-type titanium oxide particles collected from a raw dispersion liquid to be dispersed in one embodiment of the present invention. [Figure 6] FIG. 2 is a diagram showing an example of the particle size distribution of rutile-type titanium oxide particles in a dispersion liquid in which the rutile-type titanium oxide particles are appropriately dispersed in one embodiment of the present invention. [Figure 7] FIG. 2 is a diagram showing an electron microscope photograph of an example of the state of rutile-type titanium oxide particles collected from a dispersion liquid in which the particles are appropriately dispersed in one embodiment of the present invention. [Figure 8] FIG. 2 is a graph showing the relationship between the titanium oxide particle concentration and the transmittance in an aqueous dispersion of rutile-type titanium oxide particles A. [Figure 9] FIG. 2 is a graph showing the relationship between the titanium oxide particle concentration and the transmittance in an aqueous dispersion of rutile-type titanium oxide particles B. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] An embodiment of the present invention will be described in detail below. A method for producing a photocatalytic coating agent according to an embodiment of the present invention is a method for producing a photocatalytic coating agent of an aqueous dispersion containing rutile-type titanium oxide particles in the dispersoid. The production method includes a dispersion step and a transmittance measurement step.

[0011] [Dispersion process] The dispersing step is a step of dispersing rutile-type titanium oxide particles in an aqueous medium using a bead mill.

[0012] The rutile type titanium oxide particles to be subjected to the dispersion step can be appropriately selected from rutile type titanium oxide particles that can be used as a photocatalyst.

[0013] The particle shape of the rutile titanium oxide particles may be various shapes, and may be a shape having rotational symmetry such as a spherical shape. In this embodiment, even if the rutile titanium oxide particles have a shape having high anisotropy such as a high aspect ratio, the particle shape can be well dispersed in an aqueous medium while maintaining the particle shape. In this embodiment, the rutile titanium oxide particles as a carrier can also be well dispersed while substantially maintaining the particle shape and surface state. The shape of the rutile titanium oxide particles used in this embodiment may be one or more kinds. Examples of the rutile titanium oxide particles include rutile titanium oxide particles carrying a metal, non-spherical rutile titanium oxide particles, and non-spherical rutile titanium oxide particles carrying a metal. The metal can be appropriately selected from the viewpoint of the function as a photocatalyst. Examples of the metal include iron, platinum, copper, silver, palladium, rhodium, gold, and nickel. The component supported by the rutile titanium oxide particles may be a metal oxide such as nickel oxide instead of a metal, or a non-metallic component such as phosphorus or nitrogen.

[0014] The particle size of the rutile-type titanium oxide particles to be subjected to the dispersion step is not limited, and may be, for example, 0.2 to 0.5 μm in volume-based median diameter (D50). In this embodiment, even nano-order fine particles can be dispersed well. From this viewpoint, the particle size of the rutile-type titanium oxide particles may preferably be 0.25 to 0.4 μm in volume-based median diameter (D50). The particle size of the rutile-type titanium oxide particles can be measured by a known method according to the particle size, such as dynamic light scattering, but may be a catalog value.

[0015] As the media particles (beads) of the bead mill, various beads for bead mills can be applied. The material of the beads can be appropriately determined from the viewpoints of the crushing efficiency due to the bulk density of the beads and the allowable contamination from the beads. If the particle size of the beads is too large, the contact with the rutile titanium oxide particles may be insufficient, resulting in insufficient dispersion of the rutile titanium oxide particles. If the particle size of the beads is too small, the energy given to the rutile titanium oxide particles during contact may be small, resulting in insufficient dispersion of the rutile titanium oxide particles. From the viewpoint of sufficiently dispersing the rutile titanium oxide particles, the particle size of the beads is preferably 30 μm or more, preferably 100 μm or less, and more preferably 50 μm or less. From the above viewpoint, it is preferable to use zirconia beads having a particle size of 100 μm or less as the beads in this embodiment.

[0016] The aqueous medium, which is the dispersion medium in the dispersion step, is a liquid containing water as the main component. The aqueous medium may be water itself, or may be a mixed solvent of water and a water-soluble organic solvent. The aqueous medium may further contain an additive within a range in which the effects of the present invention can be obtained. The type and amount of the additive may be appropriately determined within a range in which both the effects of the present invention and the effects of the additive can be obtained.

[0017] The dispersion of rutile-type titanium oxide particles in an aqueous medium in the dispersion step is carried out using a bead mill. For example, the dispersion step is carried out by supplying a raw material slurry in which rutile-type titanium oxide particles are added to an aqueous medium (hereinafter also referred to as "rutile raw dispersion") to a grinding chamber containing beads, and stirring the rutile raw dispersion together with the beads in the grinding chamber by rotating at high speed with a stirring mechanism. Dispersion using a bead mill may be a batch type, but from the viewpoint of improving the efficiency of the dispersion step, it is preferable to use a continuous type in which the rutile raw dispersion is circulated and supplied to the grinding chamber.

[0018] The raw rutile dispersion may be produced by adding rutile-type titanium oxide particles to an aqueous medium during the dispersion step, and may be a commercially available product, a mixture of commercially available products, or a dilution of a commercially available product. Subjecting a commercially available raw rutile dispersion to the dispersion step, i.e., the dispersion step being a step of redispersing the rutile-type titanium oxide particles added to the aqueous medium, is preferred from the viewpoint of easily and stably obtaining an aqueous dispersion having high dispersibility of rutile-type titanium oxide particles.

[0019] [Transmittance measurement process] The transmittance measuring step is a step of measuring the transmittance of the aqueous dispersion produced in the dispersion step. The transmittance of the aqueous dispersion can be measured by a spectrophotometer, and any wavelength may be used as long as it reflects the dispersion state of the rutile-type titanium oxide particles in the aqueous dispersion. From this viewpoint, the wavelength for measuring the transmittance can be appropriately determined, for example, from the range of 380 to 780 nm. On the other hand, in the transmittance measuring step, it is preferable that the state of the aqueous dispersion can be visually confirmed from the viewpoint of improving quality stability and work efficiency. From this viewpoint, the wavelength for measuring the transmittance is preferably a wavelength close to the peak of visible light, and therefore the transmittance is preferably the transmittance of light with a wavelength of 550 nm.

[0020] The transmittance measuring step can be performed by taking a sample of the aqueous dispersion and measuring the transmittance of the sample. Alternatively, the transmittance measuring step may be performed by measuring the transmittance of the aqueous dispersion in the flow path by a spectrophotometer through a transparent window disposed in the flow path.

[0021] [Determining the end point of the dispersion process] The end point of the dispersion process is determined by comparing the measurement result of the transmittance of the aqueous dispersion with a pre-specified transmittance (hereinafter also referred to as "reference transmittance") of the aqueous dispersion of rutile-type titanium oxide particles dispersed in an aqueous medium while maintaining the particle shape. The end point of the dispersion process can be determined when the transmittance of the aqueous dispersion subjected to the dispersion process becomes substantially the same as the reference transmittance. The reference transmittance will be further explained later.

[0022] [Other steps in the manufacturing method] The manufacturing method of this embodiment may further include other steps than the above-mentioned dispersion step and transmittance measurement step within the scope of the effect of the present invention. For example, the manufacturing method of this embodiment may further include a step of mixing the aqueous dispersion obtained in the above-mentioned dispersion step with an aqueous dispersion of anatase type titanium oxide particles (anatase sol). In addition to rutile type titanium oxide particles, anatase type titanium oxide particles are dispersed in the photocatalytic coating agent. Further mixing with an aqueous dispersion of anatase type titanium oxide particles is a preferred embodiment of the present invention.

[0023] The timing of mixing the aqueous dispersion of anatase titanium oxide particles with the aqueous dispersion of rutile titanium oxide particles is not limited. Anatase titanium oxide particles tend to maintain the dispersion state at the time of production in an aqueous medium. Therefore, it is preferable to mix the aqueous dispersion of anatase titanium oxide particles with the aqueous dispersion of rutile titanium oxide particles adjusted to the desired dispersion state after the above-mentioned dispersion step and transmittance measurement step.

[0024] The manufacturing method of the present embodiment may further include a step of adding an optional component in the photocatalytic coating agent. The timing of adding the optional component may be appropriately determined within a range in which the effects of the present invention can be obtained. Therefore, the optional component may be added to the rutile raw dispersion liquid to be subjected to the dispersion step, or may be added to the aqueous dispersion liquid of rutile-type titanium oxide particles adjusted to a desired dispersion state. Alternatively, when an aqueous dispersion liquid of anatase-type titanium oxide particles is further added, the optional component may be added to the aqueous dispersion liquid of anatase-type titanium oxide particles. Alternatively, the optional component may be added to the mixed dispersion liquid after mixing the aqueous dispersion liquid of anatase-type titanium oxide particles with the aqueous dispersion liquid of rutile-type titanium oxide particles. The type and amount of the optional component may be appropriately determined within a range in which both the effects of the present invention and the effects of the optional component in the photocatalytic coating agent can be obtained.

[0025] [Specific Example of Production Method] Hereinafter, one embodiment of the present invention will be further described with reference to the drawings. Fig. 1 is a flow diagram showing an example of a method for producing a photocatalytic coating agent according to one embodiment of the present invention.

[0026] In step S21, rutile-type titanium oxide particles are dispersed in an aqueous medium. In this step S21, the above-mentioned dispersion process and transmittance measurement process are carried out, the end point of the dispersion process is determined, and an aqueous dispersion of rutile-type titanium oxide adjusted to a desired dispersion state (hereinafter also referred to as "rutile dispersion") is obtained.

[0027] Next, in step S22, the rutile dispersion is mixed with an aqueous dispersion of anatase type titanium oxide particles (also called anatase dispersion). The rutile dispersion and the anatase dispersion can be mixed with a normal stirring device capable of mixing slurries.

[0028] [Preparation of rutile dispersion] <Example of dispersion liquid manufacturing equipment> Next, the preparation of a rutile dispersion will be described. Fig. 2 is a diagram showing a schematic configuration of a titanium oxide fine particle dispersion production device using a bead mill, which is used in one embodiment of the present invention. As shown in Fig. 2, the dispersion production device 1 has a holding tank 10, a pump 20, and a bead mill 30. The holding tank 10 has an agitator 11 capable of stirring the inside of the tank.

[0029] The holding tank 10 is connected to the pump 20 by a pipe 41. A valve 51 capable of opening and closing the flow path of the pipe 41 is disposed on the upstream side of the pipe 41.

[0030] The pump 20 is connected to the bead mill 30 by a pipe 42 .

[0031] The bead mill 30 is connected to the holding tank 10 by a pipe 43. A valve 54 capable of opening and closing the flow path of the pipe 43 is disposed downstream of the pipe 43. A pipe 45 branches off from the pipe 43 between the valve 54 and the bead mill 30. A valve 53 capable of opening and closing the flow path of the pipe 45 is disposed in the pipe 45.

[0032] The liquid in the holding tank 10 is supplied to the bead mill 30 via the pump 20, and then returns to the holding tank 10. In this manner, the dispersion liquid producing apparatus 1 is configured to be able to circulate and supply the slurry in the holding tank 10 to the bead mill 30.

[0033] <Example of dispersion preparation> FIG. 3 is a flow diagram showing an example of a process for dispersing rutile-type titanium oxide particles in an aqueous medium according to one embodiment of the present invention.

[0034] In step S211, the rutile dispersion is circulated between the tank and the bead mill. For example, a commercially available aqueous dispersion of rutile-type titanium oxide particles is placed in the holding tank 10 as the raw rutile dispersion, and the agitator 11 is operated. Valve 53 is closed, and valves 51 and 54 are opened. Next, the bead mill 30 is operated. When the rotation speed of the bead mill 30 reaches the dispersion condition, the pump 20 is operated to circulate the raw rutile dispersion. In this way, the dispersion process begins.

[0035] In step S212, the circulating raw rutile dispersion is collected (sampled). For example, valve 53 is opened, and the raw rutile dispersion returning from the bead mill 30 to the holding tank 10 is collected from pipe 45.

[0036] In step S213, the transmittance of the raw rutile dispersion is measured. For example, the sampled raw rutile dispersion is set in a spectrophotometer (not shown), and the transmittance of the raw rutile dispersion at a wavelength of 550 nm is measured with the spectrophotometer.

[0037] In step S214, it is determined whether the transmittance of the raw rutile dispersion is within a specific range. The "specific range" is a range of transmittance that is substantially the same as a pre-specified transmittance (reference transmittance) of an aqueous dispersion of rutile-type titanium oxide particles that are dispersed in an aqueous medium while maintaining their particle shape, for example, a range of a specific transmittance value (%) + 2 (%). The "specific range" will be described later.

[0038] If the transmittance of the raw rutile dispersion measured in step S213 is within a specific range, the dispersion process is terminated, and the raw rutile dispersion is obtained as an aqueous dispersion of rutile-type titanium oxide particles. For example, the bead mill 30 is stopped, the agitator 11 is stopped, valve 54 is closed, valve 53 is opened, and the aqueous dispersion of rutile-type titanium oxide particles is collected from the pipe 45 and stored in a separately prepared container.

[0039] If the transmittance of the raw rutile dispersion measured in step S213 does not fall within the specific range, the process returns to step S211, and steps S211 to S214 are repeated to continue the dispersion process and the transmittance measurement process.

[0040] After the aqueous dispersion of rutile titanium oxide particles is removed from the dispersion production apparatus 1, the dispersion production apparatus 1 is washed. For example, a sufficient amount of distilled water is placed in the holding tank 10, the agitator 11 is operated, and the valve 51 is opened. Next, the pump 20 is operated to circulate the distilled water while the bead mill 30 is operated at an appropriate rotation speed for a certain period of time. Finally, the valve 53 is opened to discharge the liquid in the flow path from the pipe 45.

[0041] The distilled water after washing contains appropriately dispersed rutile-type titanium oxide particles, and therefore may be used as an aqueous dispersion of rutile-type titanium oxide particles as appropriate depending on the concentration of the rutile-type titanium oxide particles.

[0042] [Standard transmittance] The "reference transmittance" is a pre-specified transmittance of an aqueous dispersion of rutile-type titanium oxide particles dispersed in an aqueous medium while maintaining the particle shape. For example, the reference transmittance is the transmittance of an aqueous dispersion of rutile-type titanium oxide particles when the rutile-type titanium oxide particles are dispersed in the best state. The reference transmittance can be determined from the particle size distribution and state of the rutile-type titanium oxide particles in the aqueous dispersion. The particle size distribution of the rutile-type titanium oxide particles in the aqueous dispersion can be measured by a known technique capable of measuring the particle size distribution of the dispersoid in the aqueous dispersion, such as dynamic light scattering. The state of the rutile-type titanium oxide particles in the aqueous dispersion can be confirmed, for example, as follows. First, the aqueous dispersion of rutile-type titanium oxide particles is appropriately diluted as necessary and dropped onto a substrate such as a carbon tape, dried by heat, and coated with osmium to prepare a sample. The state of the rutile-type titanium oxide particles can be confirmed by observing the sample with a scanning electron microscope (SEM).

[0043] The reference transmittance can be determined, for example, as follows. First, the transmittance of the rutile raw dispersion is measured while appropriately adjusting the dispersion conditions using the above-mentioned dispersion production device, and the particle size distribution and particle state at that time are measured. The transmittance when D50 in the particle size distribution is sufficiently reduced and the particle shape is maintained from the SEM image can be determined as the reference transmittance under the dispersion conditions of the dispersion production device. The determination of the reference transmittance will be described in more detail below.

[0044] First, a rutile raw dispersion is prepared. For example, a water dilution of a commercially available aqueous dispersion of rutile titanium oxide particles is prepared. The commercially available rutile titanium oxide particles have a long and slender rod-shaped particle shape, and an iron compound is supported on the surface of the end of the particle in the longitudinal direction. The commercially available product is an aqueous dispersion consisting of only rutile titanium oxide particles and water, and does not contain any additives. The commercially available product is diluted with distilled water, and 1.25% by mass of an anionic surfactant is added as a dispersant for dispersion stability, to prepare an aqueous dispersion containing 1% by mass of rutile titanium oxide particles. The obtained aqueous dispersion is called "rutile raw dispersion 1". It is not necessary to add a dispersant.

[0045] An example of the particle size distribution of the rutile titanium oxide particles in the rutile raw dispersion liquid 1 is shown in FIG. 4. Moreover, the above-mentioned sample was prepared from the rutile raw dispersion liquid 1, and an SEM photograph of an example of the state of the rutile titanium oxide particles in the sample is shown in FIG. 5. As shown in FIG. 4, the D50 of the rutile titanium oxide particles in the rutile raw dispersion liquid 1 is about 0.3 μm, and the D90 is about 0.8 μm. Both are nano-order particles, and at first glance appear to be sufficiently finely dispersed. On the other hand, as shown in FIG. 5, in the rutile titanium oxide particles in the rutile raw dispersion liquid 1, the boundaries of the individual primary particles are partially unclear, and some of the primary particles are in the form of secondary particles in which the primary particles are aggregated.

[0046] The raw rutile dispersion 1 is continuously subjected to a dispersion treatment in the dispersion production apparatus shown in Figure 1. Zirconia beads with a diameter of 0.05 mm are used as the beads. The amount of beads, the operating conditions of the bead mill 30, and the circulation flow rate are fixed, and the raw rutile dispersion during the dispersion treatment is sampled from the tube 45 at specific intervals, for example, 20 minutes. The transmittance of light at 550 nm of the sampled raw rutile dispersion 1 is measured with a spectrophotometer. When measuring the transmittance, the raw rutile dispersion 1 may be diluted as necessary.

[0047] An example of the particle size distribution of rutile-type titanium oxide particles in rutile raw dispersion 1 when dispersed for a specific treatment time t1 is shown in Figure 6. An SEM photograph of an example of the state of rutile-type titanium oxide particles in a sample prepared from rutile raw dispersion 1 at this time is shown in Figure 7. The transmittance of rutile raw dispersion 1 at this time is designated as T1.

[0048] As shown in Figure 6, the rutile titanium oxide particles in the rutile raw dispersion 1 are further finely dispersed, with D50 of about 0.07 μm and D90 of about 0.16 μm. As is clear from the SEM image in Figure 7, the individual rutile titanium oxide particles are rod-shaped and are sufficiently dispersed down to the primary particles. The transmittance T1 at this time can be the reference transmittance.

[0049] Furthermore, the transmittance, particle size distribution, and particle shape of the rutile raw dispersion 1 after dispersion processing up to a processing time t2 (for example, one hour after t1) after a certain time has elapsed are also observed by SEM. In this case, the transmittance T2 is higher (more transparent) than the transmittance T1, but the particle size distribution is slightly decreased, and the state of the primary particles tends to be confirmed from the SEM image. In this case, the transmittance T2 can also be the reference transmittance. In this way, it is possible to determine the above-mentioned "specific range", that is, the range of transmittance that is substantially the same as the pre-specified transmittance (reference transmittance) of the aqueous dispersion of rutile-type titanium oxide particles dispersed in an aqueous medium while maintaining their particle shape.

[0050] The reference transmittance differs depending not only on the type of rutile-type titanium oxide particles but also on the dispersion conditions. Therefore, when the dispersion step is carried out under different dispersion conditions even for the same rutile-type titanium oxide particles, the reference transmittance should be determined according to the dispersion conditions.

[0051] The transmittance of the aqueous dispersion of rutile titanium oxide particles described above correlates with the slurry concentration. Therefore, when determining the reference transmittance or measuring the transmittance of the raw rutile dispersion 1, the sample for the transmittance measurement may be appropriately diluted.

[0052] Fig. 8 is a graph showing the relationship between the titanium oxide particle concentration and the transmittance in an aqueous dispersion of rutile-type titanium oxide particles A. Fig. 9 is a graph showing the relationship between the titanium oxide particle concentration and the transmittance in an aqueous dispersion of rutile-type titanium oxide particles B.

[0053] Rutile titanium oxide particles A are rutile titanium oxide particles carrying a platinum compound on the surface. A commercially available aqueous dispersion of rutile titanium oxide particles A is diluted with distilled water to prepare a rutile raw dispersion A, which is an aqueous dispersion of rutile titanium oxide particles A at 1 mass %. The resulting rutile raw dispersion A is dispersed in a dispersion production apparatus 1 shown in FIG. 1, and the reference transmittance A under the dispersion conditions of the aqueous dispersion of rutile titanium oxide particles A is determined in advance.

[0054] Thus, the aqueous dispersion of rutile-type titanium oxide particles A having the reference transmittance A (slurry concentration: 1% by mass) is diluted 10 times, 25 times, and 50 times with distilled water, and the transmittance of these diluted solutions is measured with a spectrophotometer. The horizontal axis of Fig. 8 represents the dilution ratio at this time, and the black circles in Fig. 8 represent the measured transmittance values ​​of these diluted solutions.

[0055] Meanwhile, as a comparative example, raw rutile dispersion A, i.e., the dispersion before the dispersion step, was similarly diluted 10 times, 25 times, and 50 times with distilled water, and the measured values ​​of the transmittance of these diluted solutions are shown as black triangles in Fig. 8. As is clear from Fig. 8, the plot of black circles has a linear correlation, which differs from the plot of black triangles.

[0056] The rutile titanium oxide particles B are the rod-shaped rutile titanium oxide particles carrying iron described above. A commercially available aqueous dispersion of rutile titanium oxide particles B is diluted with distilled water to prepare a raw rutile dispersion B, which is an aqueous dispersion of 2 mass % rutile titanium oxide particles B. The resulting raw rutile dispersion B is dispersed in the dispersion production apparatus 1 shown in FIG. 1, and the reference transmittance B of the aqueous dispersion under the dispersion conditions of the rutile titanium oxide particles B is determined in advance.

[0057] Thus, the aqueous dispersion of rutile-type titanium oxide particles B having the reference transmittance B (slurry concentration: 2% by mass) is diluted 10 times, 25 times, and 50 times with distilled water, and the transmittance of these diluted solutions is measured with a spectrophotometer. The horizontal axis of Fig. 9 represents the dilution ratio at this time, and the black circles in Fig. 9 represent the measured transmittance values ​​of these diluted solutions.

[0058] Meanwhile, as a comparative example, raw rutile dispersion B, i.e., the dispersion before the dispersion step, was similarly diluted 10 times, 25 times, and 50 times with distilled water, and the measured values ​​of the transmittance of these diluted solutions are shown by black triangles in Fig. 9. As is clear from Fig. 9 as well as Fig. 8, the plot of black circles has a linear correlation, which differs from the plot of black triangles.

[0059] Thus, the transmittance of an aqueous dispersion of rutile titanium oxide particles that satisfies the standard transmittance has a linear correlation with the concentration of rutile titanium oxide particles. By measuring the transmittance at the concentration, it is possible to confirm whether the aqueous dispersion that is the subject of transmittance measurement satisfies the standard transmittance. In this case, the correlation between the transmittance of an aqueous dispersion that satisfies the standard transmittance under specific dispersion conditions and the concentration of rutile titanium oxide particles in the aqueous dispersion is usually determined in advance. However, if the rutile titanium oxide particles and their concentrations in the aqueous dispersion are the same, the above confirmation may be performed based on the correlation between the transmittance and concentration under other dispersion conditions.

[0060] [Uses of photocatalytic coating agents] The photocatalytic coating agent produced as described above is suitable for use as a coating paint that decomposes or renders harmless organic components by irradiation with light such as natural light or indoor light. Therefore, by applying the photocatalytic coating agent as an interior or exterior paint to the surfaces of various articles to form a coating film, it becomes possible to obtain various effects such as deodorization, antifouling, and sterilization.

[0061] In the photocatalytic coating agent produced in this embodiment, the rutile-type titanium oxide particles are dispersed substantially in the state of primary particles. Therefore, compared with photocatalytic coating agents produced from conventional commercially available products, the photocatalytic coating agent in this embodiment is expected to have excellent transparency and photocatalytic function.

[0062] 〔summary〕 As is clear from the above description, the method for producing a photocatalytic coating agent in the first aspect of the present invention is a method for producing a photocatalytic coating agent of an aqueous dispersion containing rutile-type titanium oxide particles in the dispersoid, which includes a step of dispersing rutile-type titanium oxide particles in an aqueous medium by a bead mill, and a step of measuring the transmittance of the aqueous dispersion produced in the step of dispersing in the aqueous medium, and the end point of the step of dispersing in the aqueous medium is determined by comparing the measured transmittance of the aqueous dispersion with a pre-specified transmittance of the aqueous dispersion of rutile-type titanium oxide particles dispersed in the aqueous medium while maintaining the particle shape. According to the first aspect, a photocatalytic coating agent in which the original function of the titanium oxide fine particles is fully expressed can be produced.

[0063] The method for producing a photocatalytic coating agent in the second aspect of the present invention further comprises a step of mixing the aqueous dispersion obtained in the dispersing step in the first aspect with an aqueous dispersion of anatase-type titanium oxide particles, and the dispersing step is a step of redispersing the rutile-type titanium oxide particles added in the aqueous medium. The second aspect is even more effective from the viewpoint of easily and stably producing an aqueous dispersion having high dispersibility of rutile-type titanium oxide particles.

[0064] The method for producing a photocatalytic coating agent in the third aspect of the present invention is the first or second aspect, in which the transmittance is the transmittance of light having a wavelength of 550 nm. The third aspect is more effective in terms of improving the quality stability and work efficiency in the dispersion process.

[0065] The method for producing a photocatalytic coating agent according to the fourth aspect of the present invention is any one of the first to third aspects, in which zirconia beads having a particle size of 100 μm or less are used as media particles for the beads mill. The fourth aspect is even more effective from the viewpoint of sufficiently finely dispersing the rutile-type titanium oxide particles in the dispersing step.

[0066] The method for producing a photocatalytic coating agent in the fifth aspect of the present invention is any one of the first to fourth aspects, in which the rutile-type titanium oxide particles are one or more types of particles selected from the group consisting of rutile-type titanium oxide particles carrying a metal, non-spherical rutile-type titanium oxide particles, and non-spherical rutile-type titanium oxide particles carrying a metal. The fifth aspect is even more effective in terms of enhancing the photocatalytic function of the photocatalytic coating agent.

[0067] According to the above-mentioned configuration, rutile-type titanium oxide particles, which are more difficult to disperse in an aqueous medium than anatase-type titanium oxide particles, can be dispersed in an aqueous medium in a substantially primary particle state, and the photocatalytic function of the photocatalytic coating agent can be maximized. Such an effect is expected to improve hygiene in people's lives, and is expected to contribute to the achievement of Goal 3, which aims to ensure healthy lives for people, among the Sustainable Development Goals (SDGs) advocated by the United Nations.

[0068] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in the different embodiments are also included in the technical scope of the present invention. EXAMPLES

[0069] An embodiment of the present invention will now be described.

[0070] [Example 1] The above-mentioned anionic surfactant was added to a commercially available aqueous dispersion of rutile-type titanium oxide particles B to a concentration of 1.25% by mass, and the resulting raw rutile dispersion B was subjected to a dispersion step using a dispersion production apparatus 1 as shown in Fig. 1 until a predetermined standard transmittance was satisfied. In this manner, an aqueous dispersion of rutile-type titanium oxide particles B was obtained.

[0071] Next, the obtained aqueous dispersion of rutile-type titanium oxide particles B was mixed with an aqueous dispersion of anatase-type titanium oxide particles prepared separately to produce photocatalytic coating agent 1. The content of rutile-type titanium oxide particles B in photocatalytic coating agent 1 was 0.2% by mass, and the content of anatase-type titanium oxide particles was 0.5% by mass. The content of anionic surfactant in photocatalytic coating agent 1 was 0.025% by mass.

[0072] [Comparative Example 1] A photocatalytic coating agent C1 was produced in the same manner as in Example 1, except that the aqueous dispersion of rutile-type titanium oxide particles B was replaced with the raw rutile dispersion B.

[0073] [evaluation] (1) Transmittance The transmittance of each of the photocatalytic coating agents 1 and C1 was measured as follows. First, each of the photocatalytic coating agents 1 and C1 was diluted with pure water to an appropriate ratio (for example, 10 times) that reflects the dispersion state. Then, the transmittance of the obtained diluted solution at a wavelength of 550 nm was measured with a spectrophotometer. If the transmittance is 50% or more, it can be said that the transparency is sufficiently good for practical use. If the transmittance is 50% or more, it is evaluated as "transparent", and if it is less than 50%, it is evaluated as "whitish". The results are shown in Table 1 below.

[0074] The above evaluation standard for the transmittance (transmittance of 50%) is determined as follows. For each of two or more compositions, prepare a dispersed photocatalyst coating agent (corresponding to photocatalyst coating agent 1) that has been subjected to the above-mentioned dispersion process and an undispersed photocatalyst coating agent (corresponding to photocatalyst coating agent C1) that has not been subjected to the dispersion process. Set a plurality of dilution ratios (for example, 10 times, 25 times, and 50 times, etc.) appropriately, and dilute each photocatalyst coating agent at each dilution ratio. Visually check the transparency of the dispersed photocatalyst coating agent and the undispersed photocatalyst coating agent with the same dilution ratio for each composition. In this way, the transmittance that can be said to be substantially transparent for each composition is determined, and is used as the above evaluation standard.

[0075] (2) Photocatalytic function The photocatalytic function of each of the photocatalytic coating agents 1 and C1 was measured as follows. First, a test cell (inner diameter 40 mm, height 3 cm) was fixed with silicon grease to the test plate coated with each photocatalytic coating agent. 35 mL ± 0.3 mL of methylene blue test solution (0.010 ± 0.001 mmol / L) was poured into the test cell, and the cell was covered with a glass cover. The adsorption of methylene blue was repeated until the cell reached a saturated adsorption state. If the absorbance during the adsorption process is lower than that of the methylene blue test solution, the methylene blue adsorption solution (0.020 ± 0.002 mmol / L) was replaced and the process was repeated. If the absorbance is higher than that of the test solution, the adsorption process was completed. After the adsorption process was completed, the measurement process was started. The initial absorption spectrum (λ = 664 nm) of the test solution was measured, and the decomposition of methylene blue due to ultraviolet irradiation was measured as the amount of absorbance reduction using a spectrophotometer. The photocatalytic function was evaluated based on the magnitude of the absorbance decrease when the absorbance decrease amounts of the photocatalytic coating agents 1 and C1 were compared. The results are shown in Table 1 below.

[0076] [Table 1]

[0077] [Consideration] As is clear from Table 1, Photocatalytic coating agent 1 had high transmittance and high photocatalytic function. This is believed to be because the rutile-type titanium oxide particles were dispersed substantially down to the primary particles, the transmittance of the rutile-type titanium oxide particles was the highest, and the surface area of ​​the rutile-type titanium oxide particles in Photocatalytic coating agent 1 was the largest.

[0078] Photocatalytic coating agent C1 had lower transmittance and lower photocatalytic function than photocatalytic coating agent 1. This is thought to be because the rutile-type titanium dioxide particles were insufficiently dispersed and existed in the form of aggregated particles in photocatalytic coating agent C1. [Industrial Applicability]

[0079] The present invention can be utilized in the manufacture of photocatalytic coating agents that are effective in decomposing or removing floating or volatile organic components. [Explanation of symbols]

[0080] 1 Dispersion manufacturing equipment 10. Holding Tank 11 Mixer 20 Pump 30 Bead Mill 41~43, 45 tube 51, 53, 54 valves

Claims

1. A method for producing a photocatalytic coating agent of an aqueous dispersion containing rutile-type titanium oxide particles as a dispersoid, comprising the steps of: Dispersing rutile titanium dioxide particles in an aqueous medium using a bead mill; and measuring the transmittance of the aqueous dispersion produced in the step of dispersing in the aqueous medium, the measurement result of the transmittance of the aqueous dispersion is compared with a predetermined transmittance of an aqueous dispersion of rutile-type titanium oxide particles dispersed in an aqueous medium while maintaining the particle shape, thereby determining an end point of the step of dispersing in the aqueous medium; A method for producing a photocatalytic coating agent.

2. The method further comprises a step of mixing the aqueous dispersion obtained in the dispersing step with an aqueous dispersion of anatase type titanium oxide particles, 2. The method for producing a photocatalytic coating agent according to claim 1, wherein the dispersing step is a step of redispersing rutile-type titanium oxide particles added in an aqueous medium.

3. The method for producing a photocatalytic coating agent according to claim 1, wherein the transmittance is a transmittance of light having a wavelength of 550 nm.

4. The method for producing a photocatalytic coating agent according to claim 1, wherein zirconia beads having a particle size of 100 μm or less are used as media particles in the bead mill.

5. 2. The method for producing a photocatalytic coating agent according to claim 1, wherein the rutile-type titanium oxide particles are one or more types of particles selected from the group consisting of rutile-type titanium oxide particles carrying a metal, non-spherical rutile-type titanium oxide particles, and non-spherical rutile-type titanium oxide particles carrying a metal.

Citation Information

Patent Citations

  • Electrophotographic toner composition and production of surface-treated fine titanium oxide particles used for the same

    JP1995225489A

  • Manufacturing method of photocatalyst coating liquid, coating liquid for antibacterial deodorization dry cleaning, and photocatalyst processed clothing

    JP2010172831A

  • Titanium oxide particle dispersion liquid and method of manufacturing the same, and photocatalyst structure

    JP2010195654A

  • Dispersion liquid of photocatalyst particle and method for preparing the same

    JP2010269266A

  • Dispersion of photocatalyst particles, and method of producing the same

    JP2010274142A