Planking

A floor plate made of consolidated wood laminas addresses the limitations of iron and resource-intensive alternatives by providing high load capacity, reduced weight, and lower environmental impact, enhancing safety and efficiency.

JP2024135355AInactive Publication Date: 2024-10-04DENKA CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023045988
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing floor plates made of iron are heavy, difficult to handle, and have a significant environmental impact, while alternatives like recycled plastic and eucalyptus wood do not meet high load requirements or are resource-intensive.

Method used

A floor plate made of consolidated wood laminas with specific hardness, density, and surface roughness, manufactured through drying, heat compression, and surface roughening processes, allowing for high load capacity and reduced environmental impact.

Benefits of technology

The floor plate achieves high load capacity, reduced weight, and lower environmental emissions, improving safety and work efficiency by utilizing domestically sourced wood.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135355000001
    Figure 2024135355000001
  • Figure 2024135355000002
    Figure 2024135355000002
  • Figure 2024135355000003
    Figure 2024135355000003
Patent Text Reader

Abstract

To provide a planking suitable for an outrigger in which load resistance is high and which is light compared with an iron plate planking and is low in environmental load.SOLUTION: In a planking containing plies formed by arranging a plurality of plate-shaped wooden laminas in their plate width direction to be bonded, the wooden lamina has a hardness of 20-35 N / mm2, and density of 0.7-1.1 g / cm3, and surface roughness of at least one principal surface is 7-50 μm by arithmetic average height.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a floor plate used in the civil engineering and construction industry and a method for manufacturing the floor plate. [Background technology]

[0002] In various industries, including civil engineering and construction, outriggers are used on cranes, aerial work platforms, concrete pump trucks, and other vehicles when extending their arms or lifting loads, by extending them to the side and grounding them to stabilize the vehicle. Outriggers are used on these vehicles, whose center of gravity moves significantly, to eliminate shaking caused by deflection of the suspension springs and tires and to increase the effective base length. Most outriggers extend straight out to the side, but some are deployed in an X-shape.

[0003] When using outriggers, it is common to place a floor plate between them and the ground surface. A typical floor plate is a steel plate. However, because steel plates are heavy, large ones cannot be laid by hand and often must be lifted by a crane. Even if steel plates are small enough to be carried by a person, there are frequent cases of accidents where they have been dropped on people's feet or fingers have been pinched. Furthermore, steel is a material with a high CO2 emission rate, and it is desirable to replace it with a material that has a lower environmental impact. There is a long awaited need for a durable floor plate that can replace steel plates and has a lower environmental impact.

[0004] Conventionally, as floor plates to replace steel plates, floor plates made from waste plastic and floor plates made from eucalyptus wood as cross-laminated timber (CLT) have been known (see, for example, Non-Patent Documents 1 and 2). The floor plate in Non-Patent Document 1 is lighter than steel plates, is made from recycled waste plastic, and is an environmentally friendly product. The floor plate in Non-Patent Document 2 is made from eucalyptus wood, is lighter than steel plates, and has higher pressure resistance than the floor plate in Non-Patent Document 1, which is made from recycled waste plastic. [Prior art documents] [Non-patent literature]

[0005] [Non-Patent Document 1] internet<URL:https: / / www.yamadabody.co.jp / category / select / pid / 9720 / language / ja> [Non-patent document 2] internet<URL:https: / / jp.misumi-ec.com / vona2 / detail / 223013664344 / > Summary of the Invention [Problem to be solved by the invention]

[0006] However, the floor boards in Non-Patent Document 1 are limited to 4-ton Unic vehicles and cannot be used for loads greater than that. The floor boards in Non-Patent Document 2 use eucalyptus wood, which is a rare and imported wood, and their load-bearing capacity is still insufficient.

[0007] If we could manufacture high-load-bearing floor boards using domestically produced general-purpose wood, without using rare or imported wood, we could increase the number of opportunities to use these floor boards instead of steel plates, which would improve work efficiency and safety. It would also contribute to the widespread use of domestic wood and CO2 reduction.

[0008] In view of the above, an object of the present invention is to provide a floor plate that has a high load-bearing capacity, is lighter than steel floor plates, has a smaller environmental impact, and is suitable for use with outriggers. [Means for solving the problem]

[0009] The present inventors have conducted extensive research to achieve the above object and have discovered that a wooden lamina made of compressed wood and having a specific surface roughness can solve the above problem. The present invention is based on the above findings and has the following gist.

[0010] [1] A floor board including a ply formed by arranging a plurality of plank-shaped wooden laminas in the width direction of the board, wherein the hardness of the wooden laminas is 20 to 35 N / mm 2 and the density is 0.7 to 1.1 g / cm 3 and the surface roughness of at least one of the main surfaces is 7 to 50 μm in arithmetic mean height. [2] The floor board according to [1], wherein the plies are stacked in multiple layers so that the wooden laminas of the plies are arranged perpendicular to each other. [3] At least one of the main surfaces has an area of ​​900 cm 2 ~20,000cm 2 The floor plate according to [1] or [2], having a thickness of 24 mm to 72 mm. [4] A method for manufacturing floor boards, comprising: a drying step of drying raw wood at 40 to 100°C to produce dried wood; a heat compression step of subjecting the dried wood to a pressure compression process of 2 to 5 MPa in the thickness direction at 110 to 210°C multiple times to produce compressed wood; a cooling step of cooling the compressed wood to 40°C while maintaining the pressure of the final pressure compression process to produce a wooden lamina in the shape of a plate; a roughening step of roughening at least one main surface of the wooden lamina; and a ply fabrication step of arranging the roughened wooden laminas together in the width direction to form a ply. [5] A method for manufacturing a floor plate according to [4], including a lamination step of stacking a plurality of the plies so that the lamina arrangement directions of the plies are perpendicular to each other. [6] The method for manufacturing floor boards according to [4], wherein the raw wood material is thinned wood. [7] The method for manufacturing floor boards according to [6], wherein the thinned wood is cedar. [Effects of the Invention]

[0011] According to the present invention, it is possible to provide a floor plate that has a high load-bearing capacity, is lighter than steel floor plates, has a smaller environmental impact, and is suitable for use in outriggers. In particular, the method for manufacturing floor boards of the present invention makes it possible to utilize domestically produced general-purpose wood without using rare or imported wood, and to obtain floor boards that have a high load-bearing capacity, are lighter than steel plates, and have a smaller environmental impact, thereby improving work efficiency and safety. DETAILED DESCRIPTION OF THE INVENTION

[0012] Hereinafter, a floor plate and a method for manufacturing a floor plate according to one embodiment of the present invention (this embodiment) will be described in detail.

[0013] [Sillboard] The floor board according to this embodiment includes a ply formed by arranging and bonding a plurality of plank-shaped wooden lamina together in the width direction of the board. The wooden lamina (hereinafter, simply referred to as "lamina") has a hardness of 20 to 35 N / mm 2 and the density is 0.7 to 1.1 g / cm 3 Specifically, it is made of densified wood that has been densified to achieve the above hardness and density. Densified wood is wood that has been compressed with a powerful press and then fixed by heat treatment, thereby uniformly densifying the entire wood and improving its hardness.

[0014] Here, the term "lamina" refers to the smallest unit of sawn board that constitutes a ply. A "ply" refers to laminas arranged (preferably glued) in the width direction with their fiber directions approximately parallel to each other, and is sometimes called a "lamina layer." In addition, when multiple plies are stacked so that the lamina arrangement directions of the plies are perpendicular to each other, they are sometimes called CLT (Cross Laminated Timber).

[0015] Furthermore, since the lamina according to this embodiment is made of wood, it is a material with a lower CO2 emission per unit compared to steel, and is a material with a smaller environmental impact. Therefore, the environmental impact of the floor board itself can also be reduced. Furthermore, since domestic wood can be used as the raw material, it can contribute to the spread of domestic wood and CO2 reduction.

[0016] As mentioned above, the hardness of the lamina is 20 to 35 N / mm 2 However, 20N / mm 2 If it is less than 35N / mm, the load-bearing capacity will be poor. 2 If the hardness exceeds 20-30N / mm, it becomes difficult to ensure the desired surface roughness. 2 It is preferable that the strength is 25 to 30 N / mm 2 It is more preferable that: Furthermore, the Young's modulus of bending of the lamina is not particularly limited, but is preferably 12 GPa to 22 GPa. When the Young's modulus of bending is 12 GPa or more, it is not necessary to increase the number of plies to ensure bending strength when manufacturing floor boards, and as a result, productivity in manufacturing floor boards can be improved. Furthermore, by making the Young's modulus of bending of the lamina 22 GPa or less, productivity in manufacturing the lamina itself can sometimes be increased. The hardness and bending Young's modulus can be measured and determined according to JIS Z 2101 (testing method for wood).

[0017] As mentioned above, the density of the lamina is 0.7 to 1.1 g / cm 3 However, 0.7g / cm 3 If it is less than 1.1g / cm, the load-bearing capacity will be poor. 3 If the density exceeds this, it becomes impossible to reduce the weight. The density is 0.75 to 1.05 g / cm 3 is preferably 0.8 to 1.0 g / cm 3 It is more preferable that: The density can be determined by measurement according to JIS Z 2101 (testing method for wood).

[0018] Furthermore, the surface roughness of at least one of the main surfaces of the lamina (the surface with the largest area and the surface opposite to it) is 7 to 50 μm in terms of arithmetic mean height (Sa). If the arithmetic mean height is less than 7 μm or exceeds 50 μm, when used for outriggers, the contact surface with the outrigger and / or the contact surface with the ground may become slippery due to vibrations caused by work, which may compromise safety. The reason for this is unclear, but it is thought that if the arithmetic mean height is less than 7 μm, frictional force is not ensured. Conversely, if the arithmetic mean height is more than 50 μm, the contact area is significantly reduced, which is also thought to make the surface more slippery.

[0019] Here, the arithmetic mean height of a surface (Sa) represents the average of the absolute values ​​of the difference in height of each point relative to the average surface of the surface, and is a parameter that extends the arithmetic mean height of a line (Ra) to a surface. Since Ra is information about only a small portion of the lines on the target surface and is not a value that represents the information about the surface, it is not appropriate to use it as a measure. Therefore, in this invention, evaluation is performed using the arithmetic mean height of a surface (Sa).

[0020] The arithmetic mean height (Sa) can be measured and found using the light-section method. The principle is as follows: striped light emitted from the projection lens is diffusely reflected on the surface of the object. When the reflected light is observed from the receiving lens directly above, the striped light appears to be bent according to the uneven shape of the object. This is imaged on a CMOS sensor, and calculations (triangulation method) are performed to measure the height and position of each point.

[0021] From the viewpoint of ensuring friction with the ground and outriggers while maintaining strength, the arithmetic mean height of the surfaces of the lamina that form the contact surface with the ground or the contact surface with the outriggers is preferably 8 to 40 μm. In addition, from the viewpoint of adhesion between the plies when stacking the plies, the arithmetic mean height of both main surfaces of the lamina is preferably 7 to 50 μm.

[0022] The floor boards of this embodiment are preferably made by laminating multiple plies so that the lamina arrangement directions of the plies are perpendicular to each other. In other words, it is preferable to laminate and glue the plies together so that the fiber directions are perpendicular to each other to form CLT. By laminating multiple plies in this way, sufficient load capacity can be achieved and deformation of the wood can be sufficiently suppressed when the outriggers are installed. From the viewpoint of achieving both load-bearing capacity and strength and weight reduction, as well as from the viewpoint of cost reduction, the number of laminated plies is preferably 2 to 6 (2 to 6 layers), and more preferably 2 to 4 (2 to 4 layers).

[0023] The floor plate according to this embodiment has a main surface area of ​​900 cm 2 ~20,000cm 2 and the thickness is preferably 24 mm to 72 mm. 2 ~20,000cm 2 This ensures sufficient dispersion of reaction force and prevents the floorboards from becoming too large, which reduces handling and workability. A thickness of 24mm to 72mm ensures sufficient load-bearing capacity, reduces costs, and maintains good lightness. The area of ​​one main surface is 1,600 to 10,000 cm 2 The thickness is more preferably 30 to 70 mm.

[0024] The lamina constituting one ply preferably has a width of 80 to 480 mm. The thickness is not definitive as it depends on the compressibility, but is preferably 12 to 35 mm. The number of laminas constituting one ply is preferably 1 to 6.

[0025] The hardness of the floor plate according to this embodiment is 20 to 35 N / mm 2 It is preferable that the strength is 20 to 30 N / mm 2 More preferably, it is 25 to 30 N / mm 2 It is more preferable that:

[0026] The floor plate according to the present embodiment as described above can be used, for example, for outriggers, for driving heavy machinery on rough roads, etc., and is particularly preferably used for outriggers (i.e., floor plate for outriggers).

[0027] For example, in the case of outrigger floor plates, the lamina that make up the floor plates are lightweight, allowing for safe handling and excellent workability. Furthermore, the excellent hardness (load-bearing capacity) allows for stable and safe crane work. Furthermore, the contact surfaces of the floor plates with the ground and with the outriggers have a specified surface roughness, so the outriggers will not slip even if vibrations occur during crane work or high-altitude work, allowing for safe work.

[0028] [Method of manufacturing floor boards] The method for manufacturing the floor plate according to this embodiment is as follows: (1) A drying process in which raw wood is dried at 40 to 100°C to produce dried wood; (2) A heating and compressing process in which the dried wood is subjected to a pressure compression treatment of 2 to 5 MPa in the thickness direction at 110 to 210 ° C. multiple times to produce compressed wood; (3) A cooling process in which the compressed wood is cooled to 40°C while maintaining the pressure of the final compression process to form a wooden lamina in the shape of a board. (4) a roughening step of roughening at least one main surface of the wooden lamina; (5) A ply manufacturing process is included in which a plurality of the roughened wooden laminas are arranged in the width direction of the board to form a ply. Each step will be described below.

[0029] (1) Drying process In the drying process, raw wood of a predetermined size is dried at 40 to 100°C to produce dried wood. In the drying process, the raw wood is placed in a dryer set to a drying temperature of approximately 40 to 100°C and a wet-dry bulb temperature difference of approximately 1 to 30°C so that the moisture content averages approximately 10%, and dried to obtain dried wood. The wet-dry bulb temperature difference refers to the temperature difference between the wet-dry temperature and the wet-bulb temperature. The dried wood may be further subjected to a short-term calcination treatment at a high temperature of approximately 300°C. These drying and calcination treatments can be performed using a steam dryer, hot water dryer, pressure dryer, electric dryer, etc.

[0030] The raw wood material is not particularly limited, but thinned wood can be used from the viewpoint of effective use of natural resources, and a representative example is cedar.

[0031] (2) Heat compression process In the heat compression step, the dried wood is subjected to a pressure compression treatment of 2 to 5 MPa in the thickness direction at 110 to 210°C multiple times to produce compressed wood.

[0032] The dried wood heating and compression process involves raising the upper platen relative to the fixed lower platen of the heating and cooling press, placing the dried wood in the compression space formed by the upper and lower platens, and lowering the upper platen relative to the lower platen at a pressure of 0.05 to 0.30 MPa until it contacts the wood's tangential grain. The temperature in the compression space is raised to 110 to 160°C (heating treatment time: 10 to 25 minutes). The compression pressure of the upper platen relative to the fixed lower platen is set to 2.0 to 5.0 MPa, and the dried wood is heated and compressed by the upper and lower platens at a compression speed of 15 to 100 mm / min for a treatment time of 10 to 40 minutes (first heating and compression treatment). The compression ratio in the first heat compression treatment is not particularly limited, but is preferably in the range of 30% to 60%. Furthermore, the compressed wood according to this embodiment is characterized in that it does not return to its original compressed state.

[0033] Next, in order to compress and fix the compressed wood, the compression space is sealed after the first heat compression treatment, and in this state, the compression pressure of the upper press platen against the fixed lower press platen is maintained at 2.0 to 5.0 MPa, the temperature is raised to 150 to 210°C, and the compression is maintained for 40 to 120 minutes, to carry out a second heat compression treatment. The first heat-compression treatment and the second heat-compression treatment described above may be carried out multiple times, or a combination of the treatments may be carried out multiple times, depending on the desired hardness and density.

[0034] (3) Cooling process In the cooling step, the compressed wood is cooled to 40° C. while maintaining the pressure of the final compression treatment among the above-mentioned compression treatments, to form a wooden lamina in the form of a plate.

[0035] In this process, the compression pressure of the upper press platen against the fixed lower press platen is maintained at 2.0 to 5.0 MPa, the same as the pressure during the final heat compression, and the upper and lower press platens are cooled to 40°C or below (10 to 40°C) and held for 30 to 120 minutes. The compression is then released, yielding a lamina made of compressed wood.

[0036] (4) Roughening process In the surface roughening step, at least one main surface of the wooden lamina is subjected to a surface roughening treatment. Examples of roughening treatments include mechanical methods such as using a belt sander or hand sander to carve irregularities into the surface, and methods of processing irregularities using laser processing.This treatment makes the surface roughness of at least one of the main surfaces of the lamina 7 to 50 μm in arithmetic mean height of the surface.

[0037] (5) Ply manufacturing process and lamination process In the ply fabrication process, a plurality of the roughened wooden laminas are aligned widthwise and preferably glued together at their sides to form a ply. In this embodiment, the ply alone may be used as a floor board, but a lamination process may also be carried out to laminate a plurality of plies so that the laminas constituting the ply are aligned perpendicular to each other.

[0038] The adhesive used for bonding the laminas together and for laminating and bonding the plies together in the above steps is not particularly limited, and any adhesive can be used, typical examples of which include aqueous polymer-isocyanate adhesives and resorcinol resin adhesives. [Example]

[0039] The present invention will be specifically explained below with reference to examples, but the present invention is not limited to these examples.

[0040] [Experimental Example 1] (Making floor plate A) Cedar boards (10 cm x 30 cm, 42 mm thick) as raw wood were dried at 80°C in a pressure wood dryer to produce dried wood (drying process). The dried wood was subjected to a pressure compression process (first heat compression process) using a heat compression machine, applying a compression pressure of 2 MPa in the thickness direction at 140°C, and then to a heat compression process (second heat compression process) in which the temperature was increased to 180°C while maintaining the compression pressure at 2 MPa and the compression was maintained for 10 minutes, resulting in compressed wood (heat compression process). The compressed wood was cooled to 40°C while maintaining the pressure of the last compression treatment, and then held for 90 minutes before being released from compression and turned into a wooden lamina (10cm x 30cm, 25mm thick, 22.0N / m hardness). 2 , bending Young's modulus 13.0 GPa) (cooling process). The two main surfaces of the wooden lamina were subjected to the following surface roughening treatment so as to have the surface roughness (arithmetic mean height) shown in Table 1. The surface roughening treatment was carried out using a belt sander. Three wooden laminas prepared as described above were aligned widthwise and glued side-by-side with a resorcinol-based adhesive to form a ply (30 cm x 30 cm, 25 mm thick). Two layers of the resulting plies were then glued together orthogonally to form floor board A, and the hardness, density, surface roughness, and slippage were measured as follows. The results are shown in Table 1.

[0041] Hardness: Measured according to "21 Surface Hardness (Brinell Hardness)" of JIS Z 2101 (Testing Methods for Wood). This test measures the load when a 10mm diameter steel ball is pressed into the surface of the board to a depth of 1 / πmm. Density: Measured according to "5. Density measurement" in JIS Z 2101 (wood testing methods). Surface roughness (arithmetic mean height): Measured by the light cutting method. Slippage: The floor board was placed on a 10-degree inclined surface, and outriggers were installed to apply a load (200 kN). Slippage was observed when a slippage of 2.0 cm or more occurred.

[0042] (Making floor plate B) Cedar boards (10 cm x 30 cm, 72 mm thick) were used as raw wood and dried at 80°C in a pressure wood dryer to produce dried wood (drying process). The dried wood was subjected to a pressure compression process (first heat compression process) using a heat compression machine, applying a compression pressure of 5 MPa in the thickness direction at 140°C, and then to a heat compression process (second heat compression process) in which the temperature was increased to 180°C while maintaining the compression pressure at 5 MPa and the compression was maintained for 60 minutes, resulting in compressed wood (heat compression process). The compressed wood was cooled to 40°C while maintaining the pressure of the last compression treatment, and then held for 90 minutes before being released from compression and turned into a wooden lamina (10cm x 30cm, 25mm thick, 34.0N / m hardness). 2 , bending Young's modulus 21.0 GPa) (cooling process). Both main surfaces of the wooden lamina were subjected to the following surface roughening treatment so as to have the surface roughness shown in Table 1. The surface roughening treatment was carried out using a belt sander. Three wooden laminas prepared as described above were aligned widthwise and glued side-by-side with a resorcinol-based adhesive to form a ply (30 cm x 30 cm, 25 mm thick). Two layers of the resulting plies were then glued together orthogonally to form plank B, which was then measured for hardness, density, surface roughness, and evaluation as described above. The results are shown in Table 1.

[0043] (Making of floor plates C to G) Cedar boards (10 cm x 30 cm, 50 mm thick) as raw wood were dried at 80°C in a pressure dryer to produce dried wood (drying process). The dried wood was subjected to a pressure compression process (first heat compression process) using a heat compression machine, applying a compression pressure of 4 MPa in the thickness direction at 140°C, and then to a heat compression process (second heat compression process) in which the temperature was increased to 180°C while maintaining the compression pressure at 4 MPa and the compression was maintained for 30 minutes, resulting in compressed wood (heat compression process). The compressed wood was cooled to 40°C while maintaining the pressure of the last compression treatment, and then held for 90 minutes before releasing the compression. The wood was then shaped into a wooden lamina (10cm x 30cm, 25mm thick, 27.0N / m hardness). 2 , bending Young's modulus 15.5 GPa) (cooling process). Both main surfaces of the wooden lamina were subjected to the following surface roughening treatment so as to have the surface roughness (arithmetic mean height of the surface) shown in Table 1. The surface roughening treatment was carried out using a belt sander. Three wooden laminas prepared as described above were aligned widthwise and glued side-by-side with a resorcinol-based adhesive to form a ply (30 cm x 30 cm, 25 mm thick). Two of the resulting plies were then crossed and glued together to form planks C to F. Hardness, density, surface roughness, and other properties were measured as described above. Planks C to G differed only in surface roughness (arithmetic mean height of the surface). The surface roughness (arithmetic mean height of the surface) was adjusted by varying the roughness of the sandpaper and the sanding time during belt sanding. The results are shown in Table 1.

[0044] (Comparative floor plate H) For comparison, the previously described measurements and evaluations were carried out using a conventional steel plate floor plate H (30 cm x 30 cm, 10 mm thick).

[0045] [Table 1]

[0046] [Experimental Example 2] Made from cedar wood, the surface roughness (arithmetic mean height of the surface) is 25g / cm 3 Laminae of densified lumber were prepared in the same manner as in "Preparation of lumber C to lumber G" except that the surface was roughened to obtain a lumber with a compression ratio of 50% and a density of 0.78 g / cm. 3 The lamina width is 100mm, the thickness is 12mm, and the hardness is 27.0N / m 2 The Young's modulus of bending was 15.5 GPa. Using this lamina, floor plates were manufactured with the number of layers, thickness, and contact area shown in Table 2. A load of 100 to 300 kN was applied to these floor plates, and the surfaces to which the load was applied were visually inspected for damage. The results are also shown in Table 2.

[0047] [Table 2]

[0048] From Table 2, it can be seen that the floor plate of the present invention can withstand a load of 100 to 300 kN and can be used without being damaged.

[0049] [Experimental Example 3] The mass and CO2 emissions of each of the floor plates in Experiments No. 1 to 8 of Experimental Example 2, as well as the installation work conditions, were compared with the iron plate (Experiment No. 9) shown in Table 3. The results are shown in Table 3. The laying work refers to the work of installing floor plates to protect the outriggers, and involves lowering the floor plates from the truck bed and laying them on the ground at the position where the outriggers will be lowered. Here, the CO2 emissions of the iron plate were calculated by multiplying the CO2 emissions per unit of iron by the volume. For the floor board of the present invention, the CO2 emissions were calculated by multiplying the CO2 emissions per unit of plywood by the volume.

[0050] (CO2 emissions per unit of material) Iron: Blast furnace steel bar, 1,210 kg / ton. Density of iron: 7.85 g / cm 3 When converted to volume, it becomes 9499 kg / m 3 . Flooring: Composite plywood CO2 emissions per unit: 49 kg / m 3 was adopted.

[0051] [Table 3]

[0052] Table 3 shows that the floor plates of the present invention can be installed by one to four people, providing high work efficiency and safety. It also shows that CO2 emissions are extremely low. On the other hand, steel plates are much heavier than the floor plates of the present invention, and require a crane for the installation work itself. Furthermore, work efficiency is poor, and sufficient consideration must be given to ensuring safety. It also shows that CO2 emissions are significantly higher.

Claims

1. A floor board including a ply formed by arranging a plurality of plank-shaped wooden laminas in the width direction of the board, The hardness of the wooden lamina is 20 to 35 N / mm 2 and the density is 0.7 to 1.1 g / cm 3 and at least one of the main surfaces has a surface roughness of 7 to 50 μm in arithmetic mean height.

2. 2. The flooring of claim 1, wherein the plies are laminated together such that the directions of the wooden laminas of the plies are perpendicular to each other.

3. At least one of the main surfaces has an area of ​​900 cm 2 ~20,000cm 2 The floor plate according to claim 1 or 2, wherein the thickness is 24 mm to 72 mm.