Laminated polyester film, vehicle display, and vehicle electronic component
The laminated polyester film with controlled surface energy and force changes addresses adhesion and transparency issues under moist heat by using a resin layer with specific composition and manufacturing, ensuring durability and clarity.
Patent Information
- Application Number
- JP2023046261
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing laminated polyester films face issues with adhesion and transparency when exposed to moist heat, as reactive compounds in the adhesive layer form surface precipitates that degrade performance.
A laminated polyester film with a resin layer having a surface free energy of 35.0 mN/m to 55.0 mN/m and a controlled change in polar and hydrogen bond forces, achieved through specific composition and manufacturing methods, to maintain adhesion and transparency under moist heat conditions.
The film exhibits excellent adhesion and transparency even after prolonged exposure to high humidity and temperature, minimizing surface precipitates and maintaining performance.
Smart Images

Figure 2024135530000003 
Figure 2024135530000004 
Figure 2024135530000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminated polyester film having excellent coating uniformity and adhesion with a water-based coating material, and to a vehicle display and a vehicle electronic part using the same. [Background technology]
[0002] Thermoplastic resin films, particularly polyester films, have excellent mechanical properties, electrical properties, dimensional stability, transparency, chemical resistance, etc., and are therefore widely used in magnetic recording materials, packaging materials, optical films such as antireflection films and diffusion sheets in flat displays, etc., prism sheets, transparent touch panels, etc. However, when other materials are coated and laminated on the polyester film to form a layer having a desired function in order to suitably use the polyester film for these applications, there is a drawback in that the adhesion is deteriorated depending on the material used.
[0003] In view of this, one method for imparting adhesiveness to the surface of a polyester film is known to be a method of applying various resins to the surface of the polyester film to provide a coating layer having adhesive properties (hereinafter, sometimes referred to as an easy-adhesion layer).Specific examples include a method of improving adhesiveness by providing an easy-adhesion layer on the surface of a polyester film using a coating agent made of polyurethane resin, acrylic resin with a hydrophilic functional group, or polyester resin (Patent Documents 1 and 2).
[0004] In addition, in recent years, the number of automobiles equipped with liquid crystal panels has been increasing. Since the liquid crystal panels installed in such automobiles are often exposed to high temperature and high humidity for long periods of time, the adhesive films constituting the liquid crystal panels are also required to have resistance to moisture and heat and durability at high temperatures.
[0005] When an easily adhesive film is exposed to a humid and hot atmosphere, foreign matter precipitates on the surface from inside the film, causing the following problems. For example, the precipitates scatter light and impair film transparency, when used for lamination with a pressure-sensitive adhesive or hard coat, the precipitates accumulate at the interface and reduce adhesion, and when used as a protective film to which a polarizing plate containing a polarizing element is attached, the precipitates penetrate into the polarizer resin and cause deterioration of properties such as reduced polarization properties and color loss. As a method for solving such problems, an easily adhesive film that has improved hot water resistance and adhesion under high temperature and high humidity conditions by reducing the amount of crosslinking agent is known (Patent Documents 3 and 4). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2009-214531 A [Patent Document 2] JP 2011-140140 A [Patent Document 3] Patent No. 5042161 [Patent Document 4] JP 2014-65887 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, the methods disclosed in Patent Documents 3 and 4 do not provide an easily adhesive film having satisfactory performance in both transparency and adhesion after a wet heat test. When the present inventors investigated the cause of the decrease in transparency and adhesion after a wet heat test, they found that the surface precipitates generated under a wet heat atmosphere are residues of the reactive compound contained in the easily adhesive layer, and that these problems can be improved by reducing the amount of the reactive compound. On the other hand, in the study by the present inventors, it was also found that the reactive compound is strongly related to the strength of the easily adhesive layer and the initial adhesion to the target object, and that sufficient adhesion cannot be obtained by simply reducing the amount of the reactive compound.
[0008] Therefore, an object of the present invention is to overcome the above-mentioned drawbacks and to provide a laminated polyester film which has excellent initial adhesion to an object and can maintain its adhesion and transparency even in a humid and hot atmosphere. [Means for solving the problem]
[0009] In order to solve the above problems, the laminated polyester film of the present invention has the following configuration: That is, the laminated polyester film of the present invention is a laminated polyester film having a resin layer X on at least one outermost layer of a polyester film, characterized in that the surface free energy of the resin layer X is 35.0 mN / m to 55.0 mN / m, and the amount of change in the total value of polar force and hydrogen bonding force in the surface free energy of the resin layer X after wet heat treatment for 500 hours in an environment of a temperature of 85°C and a humidity of 85% is 0.0 mN / m to 3.0 mN / m.
[0010] The laminated polyester film of the present invention may also be in the following form, and a display for a vehicle or an electronic part for a vehicle may also be obtained by using the laminated polyester film of the present invention. (1) A laminated polyester film having a resin layer X on at least one outermost surface of a polyester film, the resin layer X having a surface free energy of 35.0 mN / m to 55.0 mN / m, and a change in the total value of polar force and hydrogen bonding force in the surface free energy of the resin layer X after 500 hours of wet heat treatment in an environment of a temperature of 85°C and a humidity of 85% is 0.0 mN / m to 3.0 mN / m. (2) The domain area in the elastic modulus variation image of the resin layer X of 1 μm square measured by an atomic force microscope (AFM) is 500 nm 2 The laminated polyester film according to (1), which is: (3) A polyester film laminated to (1) or (2), wherein the resin layer X contains a polyester resin. (4) The laminated polyester film according to any one of (1) to (3), wherein the resin layer X is formed from a coating composition that satisfies all of the following characteristics 1 to 3: Feature 1: Contains binder resin, melamine compound, and carbodiimide compound. Feature 2: When the content of the binder resin in the coating composition is taken as 100 parts by mass, the content A of the melamine compound is 10 parts by mass or less, and the content B of the carbodiimide compound is 5 parts by mass to 30 parts by mass. Feature 3: A / B is less than 0.50. (5) The laminated polyester film according to any one of (1) to (4), wherein the resin layer X is formed from a coating composition that satisfies both of the following characteristics 4 and 5: Feature 4: Contains binder resin. Feature 5: 10% by mass or more of the binder resin contained in the coating composition is a resin having a hydroxyl group and a polyfunctional acryloyl group. (6) The laminated polyester film according to any one of (1) to (5), wherein the resin layer X has a thickness of 50 nm or less. (7) The laminate film according to any one of (1) to (6), which is used for a vehicle display. (8) The laminate film according to any one of (1) to (6), which is used for an electronic part for a vehicle. (9) A vehicle display using the laminated polyester film according to any one of (1) to (7). (10) An electronic part for a vehicle, which uses the laminated polyester film according to any one of (1) to (6) and (8). Effect of the Invention
[0011] According to the present invention, it is possible to provide a laminated polyester film which is excellent in transparency and adhesion, particularly after a moist heat treatment. [Brief description of the drawings]
[0012] [Figure 1] 1 is an image showing the variation in elastic modulus of the surface of a resin layer X according to one embodiment (embodiment of Example 1) of the present invention. [Diagram 2] 1 is an image showing the variation in elastic modulus on the surface of a laminated polyester film, which has a problem to be solved by the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The laminated polyester film of the present invention is a laminated polyester film having a resin layer X on at least one outermost layer of the polyester film, characterized in that the surface free energy of the resin layer X is 35.0 mN / m to 55.0 mN / m, and the change in the total value of polar force and hydrogen bonding force in the surface free energy of the resin layer X after wet heat treatment for 500 hours in an environment of a temperature of 85° C. and a humidity of 85% is 0.0 mN / m to 3.0 mN / m. The laminated polyester film of the present invention will be described in detail below.
[0014] It is important that the surface free energy of the resin layer X of the laminated polyester film of the present invention is 35.0 mN / m to 55.0 mN / m. The surface free energy is an index of wettability with a liquid, and is expressed by the sum of three components, namely, dispersion force, polar force, and hydrogen bonding force. The higher the surface free energy of the resin layer X, the higher the affinity between the water-based coating agent and the surface of the resin layer X, and the coating property of the coating agent and the adhesion to the processing layer such as a pressure sensitive adhesive or hard coat are improved. If the surface free energy of the resin layer X is below 35.0 mN / m, the affinity with the water-based coating agent is insufficient, and the adhesion to the processing layer is insufficient. There is no preferred value in terms of characteristics for the upper limit of the surface free energy of the resin layer X, but it is 55.0 mN / m from the range that can be practically achieved by the coating composition and manufacturing method preferred for forming the resin layer X in the laminated polyester film of the present invention.
[0015] The surface free energy of the resin layer X can be calculated by the geometric mean method based on the "extended Fowkes equation" proposed by Hata et al., using the contact angles of four liquids: pure water, ethylene glycol, formamide, and diiodomethane (the detailed measurement method will be described later).
[0016] The method for making the surface free energy of the resin layer X to be 35.0 mN / m to 55.0 mN / m is not particularly limited. For example, a method of applying an easy-adhesion primer (resin layer X described later) to the surface of the polyester film and curing it, or a method of activating the surface by performing a corona discharge treatment or the like can be adopted.
[0017] It is important that the laminated polyester film of the present invention has a change in the total value of polarity and hydrogen bonding strength in the surface free energy of the resin layer X after 500 hours of wet heat treatment in an environment of a temperature of 85°C and a humidity of 85% of 0.0 mN / m to 3.0 mN / m. Here, the polarity in the surface free energy is a parameter that indicates the strength of the interaction between polar groups, and the hydrogen bonding strength is a parameter that indicates the strength of the interaction with water molecules. The resin layer X preferably contains a reactive compound having a polar group or hydrogen bond in order to enhance adhesion to the target, and such a reactive compound precipitates on the outermost surface when stored for a long period of time under a humid heat condition atmosphere. Therefore, we have focused on the change in the surface free energy and found that there is a correlation between the amount of surface precipitate and the change in the total value of polarity and hydrogen bonding strength, and have found that whitening and a decrease in adhesion in a humid heat atmosphere are suppressed when the change in polarity and hydrogen bonding strength in the surface free energy of the resin layer X is in the range of 0.0 mN / m to 3.0 mN / m. If this change is more than 3.0 mN / m, the amount of precipitates on the surface increases, causing problems such as whitening and reduced adhesion. From the above viewpoints, the change is more preferably in the range of 0.0 mN / m to 1.5 mN / m, even more preferably in the range of 0.0 mN / m to 1.4 mN / m, and particularly preferably in the range of 0.0 mN / m to 1.0 mN / m.
[0018] The polar force and hydrogen bond force of the resin layer X can be calculated by the geometric mean method based on the "Fowkes formula (extended Fowkes formula)" proposed by Hata et al., using the contact angles of each of four liquids, namely pure water, ethylene glycol, formamide, and diiodomethane, and the details of the method will be described later. In addition, the change in the polar force and hydrogen bond force in the surface free energy of the resin layer X can be controlled by the components contained in the resin layer X, the method of forming the resin layer X, and a combination thereof. Specifically, it can be adjusted by the functional group type that the resin or compound, which is a constituent, has in the side chain, the molecular weight of the unit structure when a polymer is used, the progress of the crosslinking reaction, and the like. The details of the preferred constituent materials and manufacturing methods will be described later.
[0019] In the laminated polyester film of the present invention, from the viewpoints of reducing the amount of change in the total value of polar force and hydrogen bonding force in the surface free energy of the resin layer X and suppressing a decrease in adhesion after a wet heat treatment, a domain area in an elastic modulus variation image of the resin layer X in a 1 μm square measured by an atomic force microscope (AFM) is 500 nm 2 It is preferable that the elastic modulus is less than 1 μm. The elastic modulus can be measured and calculated by performing analysis based on the JKR contact theory after measurement by the force curve method using an AFM (Atomic Force Microscope), and the detailed method and conditions will be described later. There is a preferable form in the elastic modulus distribution in a 1 μm square measured by AFM, and specifically, there is a preferable form in the "elastic modulus dispersion image" obtained by smoothing the elastic modulus image (i.e., data in the DMT Modulus channel) measured by the measurement method described later in the Flatten mode of the analysis software "NanoScope Analysis V1.40" in Order: 3rd and offsetting the average value to 0 MPa. Specifically, in the above-mentioned "elastic modulus dispersion image," it is preferable that the elastic modulus dispersion width is small, and it is particularly preferable that there is no coarse domain, because this keeps the surface adhesion uniform and minimizes the decrease in adhesion after wet heat treatment.
[0020] FIG. 1 is an "elastic modulus variation image" of the surface of the resin layer X according to one embodiment of the present invention, and FIG. 2 is an "elastic modulus variation image" of a conventional laminated polyester film commercially available for comparison. The black parts of the "elastic modulus variation image" of the surface of the resin layer X ("representative black parts in the elastic modulus variation image" (reference symbol 1) in FIGS. 1 and 2) represent areas with relatively low elastic modulus, and the white parts ("representative white parts in the elastic modulus variation image" (reference symbol 2) in FIGS. 1 and 2) represent areas with relatively high elastic modulus. Each domain in the elastic modulus variation image of the surface of the resin layer X is formed by local aggregation of the binder resin and reactive compound used, and when the domains are coarsened as in FIG. 2, that is, when aggregation of the constituent materials is observed, the adhesion to the resin layer X after the wet heat treatment tends to decrease.
[0021] The elastic modulus variation width corresponds to the Image Rmax obtained by analyzing the above-mentioned "elastic modulus variation image" in Roughness mode, and is preferably less than 5 GPa, and particularly preferably less than 2 GPa. On the other hand, the domain area in the elastic modulus variation image of the resin layer X is expressed as the average area of each domain colored at Bearing Area Percent: 10% in Bearing Analysis mode, and is 500 nm 2 It is preferable that the thickness is less than 300 nm. 2 More preferably, it is 100 nm or less. 2 It is more preferable that the elastic modulus variation width and the method for measuring the domain area are described later in detail. The domain area can be adjusted by the resin constituting the resin layer X, the type of reactive compound, the progress of the crosslinking reaction (which can be increased by thermally curing the coating composition at 170°C or higher), and the like. The preferred coating composition and the production method from the above viewpoint are described later in detail.
[0022] Preferred embodiments of the laminated polyester film of the present invention will be described in detail below.
[0023] <Polyester film> The laminated polyester film of the present invention has a resin layer X on at least one surface of the polyester film. The polyester resin is a general term for polymers having an ester bond as the main bonding chain in the main chain, and preferably has at least one component selected from ethylene terephthalate, propylene terephthalate, ethylene-2,6-naphthalate, butylene terephthalate, propylene-2,6-naphthalate, ethylene-α,β-bis(2-chlorophenoxy)ethane-4,4'-dicarboxylate, etc. as the main structural unit.
[0024] Here, the main constituent unit refers to a constituent unit that is contained in an amount of more than 50 mol% to 100 mol% or less when all the constituent units constituting the resin are taken as 100 mol%. The main constituent component in the polyester resin is preferably contained in an amount of more than 70 mol%. The laminated polyester film refers to a sheet-like molded product having at least two layers and containing polyester resin as the main component. The main component refers to a component that is contained in an amount of more than 50 mass% to 100 mass% or less of all the constituent components of the film. The polyester film refers to a sheet-like material that constitutes the laminated polyester film and contains polyester resin as the main component. The polyester film may be either a single-layer structure or a laminate structure.
[0025] As the polyester film in the laminated polyester film of the present invention, a polyethylene terephthalate film is preferably used from the viewpoint of heat resistance and smoothness. In addition, when heat or shrinkage stress acts on the laminated polyester film, a polyethylene-2,6-naphthalate film having excellent heat resistance and rigidity is preferably used. Here, the polyethylene terephthalate film refers to a film in which polyethylene terephthalate (including copolymers) accounts for more than 50% by mass and not more than 100% by mass of all components constituting the film, and the same can be interpreted for a polyethylene-2,6-naphthalate film.
[0026] From the viewpoint of thermal stability and mechanical strength, the polyester film is preferably biaxially oriented, that is, a biaxially oriented polyester film. A biaxially oriented polyester film refers to a polyester film that shows a pattern oriented along two orthogonal axes in wide-angle X-ray diffraction. In general, a biaxially oriented polyester film is obtained by stretching an unstretched polyester sheet in two orthogonal directions, for example, by stretching the polyester sheet in the longitudinal direction and the width direction by about 2.5 to 5.0 times, and then performing a heat treatment to complete crystal orientation. By using a biaxially oriented polyester film as the polyester film, the thermal stability, particularly the dimensional stability and mechanical strength of the obtained laminated polyester film are improved, and the flatness is also improved. Here, the longitudinal direction refers to the direction in which the film runs during the manufacturing process (in the case of a film roll, this corresponds to the winding direction of the film), and the width direction refers to the direction perpendicular to the longitudinal direction within the film plane.
[0027] The polyester film may also contain various additives, such as antioxidants, heat stabilizers, weather stabilizers, ultraviolet absorbers, organic lubricants, pigments, dyes, organic or inorganic fine particles, fillers, antistatic agents, nucleating agents, etc., to the extent that they do not deteriorate the properties of the film. These additives may be used alone or in combination.
[0028] The thickness of the polyester film is not particularly limited and is appropriately selected depending on the application and type, but is usually preferably 10 μm to 500 μm, more preferably 20 μm to 250 μm, and particularly preferably 30 μm to 150 μm in terms of mechanical strength, handleability, etc. The polyester film may be a composite film obtained by coextrusion, or may be a film obtained by laminating the obtained films by various methods.
[0029] Moreover, the laminated polyester film of the present invention preferably has a haze value of 2.0% or less, and particularly preferably 1.0% or less. By setting the haze value of the laminated polyester film in the above range, the transparency is increased, so that the film can be suitably used for optical films that require transparency. The lower the haze value, the more preferable it is, and there is no particular limit to the lower limit, but from the viewpoint of feasibility, the lower limit is 0.1%. The haze value is also sometimes called "haze".
[0030] The haze value of the laminated polyester film can be measured by a method conforming to JIS "Determination of Haze of Transparent Materials" (K7136 2000 edition), and the details are shown in the Examples. In addition, as a method for making the haze value of the laminated polyester film 2.0% or less, for example, a method of reducing the reflectance at the interface with air by adjusting the surface shape and refractive index of the coating layer formed on the outermost surface of the polyester film can be mentioned.
[0031] Moreover, the laminated polyester film of the present invention preferably has a haze increase of 1.5 or less, more preferably 1.0 or less, before and after a 500-hour wet heat treatment under an environment of a temperature of 85° C. and a humidity of 85%. When the increase is 1.5 or less, the transparency is maintained even when the film is used in a vehicle display, which is preferable.
[0032] <Resin layer X> When another layer (a post-processing layer, which corresponds to the processing layer Y described later) is formed by post-processing, the resin layer X is located between the polyester film and the post-processing layer, and plays a role in enhancing the adhesion between them. From the viewpoint that the resin layer X plays such a role, in the laminated polyester film of the present invention, the outermost layer on at least one side of the polyester film, preferably the outermost layer on one side, is the resin layer X. By adopting such an embodiment, when the polyester film and the post-processing layer are laminated via the resin layer X, the laminate can be easily handled as an integrated laminate. The resin layer X can be designed in consideration of the applicability and adhesion of the water-based coating material (details will be described later).
[0033] In addition, the resin layer X preferably contains various binder resins such as urethane resin, acrylic resin, polyester resin, etc., and more preferably contains a polyester resin, considering that the resin layer X is responsible for adhesion to the polyester film. When the resin layer X contains a polyester resin, the resin layer X has a common chemical structure with the surface of the polyester film, and the adhesion is enhanced.
[0034] In the laminated polyester film of the present invention, the thickness of the resin layer X is preferably 300 nm or less, more preferably 100 nm or less, and even more preferably 50 nm or less. There is no particular limit to the lower limit of the thickness of the resin layer X, but considering the level at which the above-mentioned adhesion can be sufficiently ensured, it is 10 nm. On the other hand, even if the thickness of the resin layer X is made thicker than 300 nm, the adhesion improvement effect is not observed, and rather the amount of precipitates precipitated on the surface increases, which is not preferable. By making the thickness 50 nm or less, the amount of precipitates precipitated on the surface decreases, and it becomes easy to adjust the change in the total value of polar force and hydrogen bond force in the surface free energy to 0.0 mN / m to 3.0 mN / m. The thickness of the resin layer X is the thickness after coating and drying the coating agent, and can be measured from the image obtained by observing the cross section in the direction perpendicular to the film surface (thickness direction) using a transmission electron microscope (TEM) (details will be described later).
[0035] <Coating composition for forming resin layer X> The coating composition for forming the resin layer X of the laminated polyester film of the present invention will be described below. The resin layer X of the laminated polyester film of the present invention is preferably formed from a coating composition containing at least one reactive compound selected from various binder resins such as polyester resins, urethane resins, and acrylic resins, oxazoline compounds, carbodiimide compounds, and melamine compounds.
[0036] The binder resin contained in the coating composition for the resin layer X is preferably a polyester resin from the viewpoint of adhesion to the polyester film, and may be a resin having a hydroxyl group and a polyfunctional acryloyl group from the viewpoint of suppressing the amount of precipitates deposited on the surface and adjusting the change in the total value of polar force and hydrogen bond force in the surface free energy to the range of 0.0 mN / m to 3.0 mN / m. The reactive compound contained in the coating composition for the resin layer X is more preferably a melamine compound and a carbodiimide compound.
[0037] The types of the components constituting the coating composition are selected and their contents adjusted so that the surface free energy of the resin layer X is 35.0 mN / m to 55.0 mN / m, and the change in the total value of the polar force and hydrogen bonding force in the surface free energy of the resin layer X after 500 hours of wet heat treatment in an environment of a temperature of 85°C and a humidity of 85% is 0.0 mN / m to 3.0 mN / m.
[0038] As the dicarboxylic acid component serving as the raw material of the polyester resin, aromatic, aliphatic, and alicyclic dicarboxylic acids can be used. As the aromatic dicarboxylic acid, for example, terephthalic acid, isophthalic acid, orthophthalic acid, phthalic acid, 2,5-dimethylterephthalic acid, 1,4-naphthalenedicarboxylic acid, biphenyldicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 1,2-bisphenoxyethane-p-p'-dicarboxylic acid, and phenylindanedicarboxylic acid can be used. As the aliphatic and alicyclic dicarboxylic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, dodecanedioic acid, dimer acid, 1,3-cyclopentanedicarboxylic acid, 1,2-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, and the like, and their ester-forming derivatives can be used.
[0039] The diol components used as raw materials for polyester resins include ethylene glycol, diethylene glycol, polyethylene glycol, propylene glycol, polypropylene glycol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 2,4-dimethyl-2-ethylhexane-1,3-diol, neopentyl glycol, 2-ethyl-2-butyl-1,3-propanediol, 2-ethyl-2-isobutyl-1,3-propanediol, 3-methyl-1,5-pentanediol, 2,2,4-trimethyl- 1,6-hexanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, 2,2,4,4-tetramethyl-1,3-cyclobutanediol, 4,4'-thiodiphenol, bisphenol A, 4,4'-methylenediphenol, 4,4'-(2-norbornylidene)diphenol, 4,4'-dihydroxybiphenol, o-, m-, and p-dihydroxybenzene, 4,4'-isopropylidenephenol, 4,4'-isopropylidenebindiol, cyclopentane-1,2-diol, cyclohexane-1,2'-diol, cyclohexane-1,2-diol, cyclohexane-1,4-diol, and the like can be used.
[0040] As the polyester resin, in addition to homopolyester, modified polyester copolymers, for example, block copolymers and graft copolymers modified with acrylic, urethane, epoxy, etc., can also be used.
[0041] The polyester resin preferably has a functional group in the side chain from the viewpoint of forming a dense coating film by a crosslinking reaction with a reactive compound described later and easily adjusting the surface free energy of the resin layer X to a range of 35.0 mN / m to 55.0 mN / m. Preferred examples of the functional group in the side chain include a hydroxyl group, a carboxylic acid group, an amide group, a glycidyl group, an isocyanate group, and a sulfonic acid group. The amount of functional groups in the side chain can be selected based on the acid value or the hydroxyl value. For example, if the acid value of the polyester resin is less than 5 KOH / mg, the adhesion to the processing layer Y may decrease, so it is preferable to set the acid value at or above that level.
[0042] The acrylic resin is not particularly limited, but is preferably composed of alkyl methacrylate and / or alkyl acrylate. As the alkyl methacrylate and / or alkyl acrylate, it is preferable to use methacrylic acid, methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-hexyl methacrylate, lauryl methacrylate, 2-hydroxyethyl methacrylate, hydroxypropyl methacrylate, acrylic acid, methyl acrylate, ethyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-hexyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, hydroxypropyl acrylate, maleic acid, itaconic acid, acrylamide, N-methylol acrylamide, diacetone acrylamide, etc. These can be used alone or in combination of two or more.
[0043] Since the acrylic resin is a hydrophobic resin, the surface free energy of the resin layer X acts in a decreasing direction, although it is also affected by the structure of the side chain. In particular, when the resin layer X is formed from a coating composition containing a resin having a hydroxyl group and a polyfunctional acryloyl group, it is preferable in that the change in the total value of the polar force and the hydrogen bond force in the surface free energy of the resin layer X can be suppressed to a low level, while if the weight ratio of the resin having a hydroxyl group and a polyfunctional acryloyl group becomes too large, the initial adhesion tends to decrease. Therefore, when using such a resin, it is preferable that the resin layer X is formed from a coating composition that satisfies both of the following characteristics 4 and 5, in terms of the balance between the two. Feature 4: Contains binder resin. Feature 5: 10% by mass or more of the binder resin contained in the coating composition is a resin having a hydroxyl group and a polyfunctional acryloyl group.
[0044] The resin layer X is "formed from a coating composition" means that the resin layer X is formed by coating and drying the coating composition. The reason why the resin layer X is specified by an expression including the manufacturing method is that after coating and drying, the resin having a hydroxyl group and a polyfunctional acryloyl group forms a crosslinked structure with the reactive compound described later, so that the content of the resin component changes, and since the resin layer X becomes a thin film by drying, it is extremely difficult to analyze and identify the crosslinked structure therein. The reason why the same expression is used for the reactive compound described later is also the same.
[0045] The urethane resin is preferably a resin obtained by reacting a polyhydroxy compound with a polyisocyanate compound by a known urethane resin polymerization method such as emulsion polymerization, suspension polymerization, etc. Examples of the polyhydroxy compound include polyethylene glycol, polypropylene glycol, polyethylene propylene glycol, polytetramethylene glycol, hexamethylene glycol, tetramethylene glycol, 1,5-pentanediol, diethylene glycol, triethylene glycol, polycaprolactone, polyhexamethylene adipate, polyhexamethylene sebacate, polytetramethylene adipate, polytetramethylene sebacate, trimethylolpropane, trimethylolethane, pentaerythritol, polycarbonate diol, and glycerin. Examples of the polyisocyanate compound that can be used include hexamethylene diisocyanate, diphenylmethane diisocyanate, tolylene diisocyanate, isophorone diisocyanate, an adduct of tolylene diisocyanate and trimethylenepropane, and an adduct of hexamethylene diisocyanate and trimethylolethane.
[0046] The above urethane resins and their copolymers (such as acrylic-urethane copolymers and urethane-modified polyesters) have a highly hydrophilic cross-linked structure, and therefore adding an excess amount of them tends to increase the surface free energy of the resin layer X. Although the specific upper limit of the amount added is affected by the combination with other binder resins, if the amount of the urethane resin exceeds 5% by mass of the total binder resin, it may affect adhesion.
[0047] Examples of the epoxy resin include sorbitol polyglycidyl ether crosslinking agents, polyglycerol polyglycidyl ether crosslinking agents, diglycerol polyglycidyl ether crosslinking agents, and polyethylene glycol diglycidyl ether crosslinking agents. Commercially available epoxy resins may be used, such as epoxy compounds "Denacol" (registered trademark) EX-611, EX-614, EX-614B, EX-512, EX-521, EX-421, EX-313, EX-810, EX-830, EX-850, etc., manufactured by Nagase Chemtec Corporation, diepoxy / polyepoxy compounds (SR-EG, SR-8EG, SR-GLG, etc.) manufactured by Sakamoto Pharmaceutical Co., Ltd., epoxy crosslinking agents "EPICLON" (registered trademark) EM-85-75W or CR-5L, manufactured by Dainippon Ink Mfg. Co., Ltd., and among these, those having water solubility are preferably used. Since the above-mentioned epoxy resin is a hydrophilic resin, it acts in the direction of increasing the surface free energy of the resin layer X, although it is also affected by the structure of the side chain.
[0048] The coating composition for forming the resin layer X of the present invention can be composed and used by using polyester resin, acrylic resin, urethane resin, epoxy resin, etc. alone or in combination so as to satisfy the above range. In addition, when these resins are combined, the domain area in the elastic modulus variation image of the resin layer X tends to become large, and the domain area of the elastic modulus variation image of the resin layer X tends to become large. 2 In order to reduce the domain area, it is preferable to use a single resin having the same composition as the binder.
[0049] <Reactive compounds> In the resin layer X of the present invention, the reactive compound plays a role of sufficiently advancing the crosslinking reaction and enhancing the adhesion with the processed layer Y. As the reactive compound, an oxazoline compound, a carbodiimide compound, a melamine compound, an isocyanate compound, etc. can be used alone or in any combination. However, from the viewpoint of easily setting the change in the total value of the polar force and the hydrogen bond force in the surface free energy of the resin layer X after the wet heat treatment for 500 hours in an environment of a temperature of 85°C and a humidity of 85% to the range of 0.0 mN / m to 3.0 mN / m, it is preferable that the resin layer X is formed from a coating composition that satisfies all of the following characteristics 1 to 3. Feature 1: Contains binder resin, melamine compound, and carbodiimide compound. Feature 2: When the content of the binder resin in the coating composition is taken as 100 parts by mass, the content A of the melamine compound is 10 parts by mass or less, and the content B of the carbodiimide compound is 5 parts by mass to 30 parts by mass. Feature 3: A / B is less than 0.50.
[0050] In this case, when there are a plurality of components corresponding to the binder resin, the melamine compound, and the carbodiimide compound, the content of each component is treated as the total content of all the components.
[0051] The reactive compound is essential for increasing the strength of the resin layer X and for increasing the adhesion with the processed layer Y, but it may precipitate on the outermost surface and deteriorate the transparency and adhesion. Therefore, by setting the amount of the reactive compound within the range that satisfies the above requirements, the precipitation on the outermost surface in a high-temperature and high-humidity atmosphere can be reduced, and the deterioration of the transparency and adhesion can be suppressed. In particular, since the melamine compound is more likely to precipitate than other reactive compounds and is more likely to affect the domain area in the elastic modulus variation image of the resin layer X, in consideration of the balance with the adhesion with the processed layer Y and the strength of the resin layer X, it is more preferable to set A / B to 0.05 or more and 0.35 or less, and even more preferably 0.18 or more and 0.35 or less.
[0052] In addition, from the viewpoint of improving the coating property and adhesion, the domain area in the elastic modulus dispersion image of the resin layer X of 1 μm square measured by atomic force microscope (AFM) was easily reduced to 500 nm 2 From the viewpoints below, it is also preferable not to use a melamine compound, but to use an oxazoline compound or a carbodiimide compound alone or in combination in an amount of 5% by mass to 40% by mass of the total components of the coating composition.
[0053] The oxazoline compound is preferably an oxazoline group-containing copolymer obtained by copolymerizing at least one monomer containing an oxazoline group and at least one other monomer, the oxazoline compound having an oxazoline group as a functional group in the compound.
[0054] In the oxazoline compound, at least one other monomer used for the monomer containing an oxazoline group is a monomer copolymerizable with the monomer containing an oxazoline group, and examples thereof include acrylic acid esters or methacrylic acid esters such as methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, 2-ethylhexyl acrylate, and 2-ethylhexyl methacrylate; unsaturated carboxylic acids such as acrylic acid, methacrylic acid, itaconic acid, and maleic acid; unsaturated carboxylic acids such as acrylonitrile and methacrylonitrile; Examples of the monomer include nitriles, unsaturated amides such as acrylamide, methacrylamide, N-methylol acrylamide, and N-methylol methacrylamide, vinyl esters such as vinyl acetate and vinyl propionate, vinyl ethers such as methyl vinyl ether and ethyl vinyl ether, olefins such as ethylene and propylene, halogen-containing α,β-unsaturated monomers such as vinyl chloride, vinylidene chloride, and vinyl fluoride, and α,β-unsaturated aromatic monomers such as styrene and α-methylstyrene. These may be used alone or in combination as long as the scope of the present invention is satisfied.
[0055] Specific examples of monomers containing an oxazoline group include 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-isopropenyl-2-oxazoline, 2-isopropenyl-4-methyl-2-oxazoline, and 2-isopropenyl-5-ethyl-2-oxazoline. These may be used alone or in combination as long as they satisfy the scope of the present invention.
[0056] A carbodiimide compound is a compound having at least one carbodiimide group or a cyanamide group in a tautomeric relationship therewith as a functional group in the molecule. Specific examples of such carbodiimide compounds include dicyclohexylmethane carbodiimide, dicyclohexyl carbodiimide, tetramethylxylylene carbodiimide, and urea-modified carbodiimide, which may be used alone or in combination as long as they satisfy the scope of the present invention. Specific examples of polycarbodiimide compounds include "Carbodilite" (registered trademark) V-02, "Carbodilite" (registered trademark) V-02-L2, "Carbodilite" (registered trademark) SV-02, and "Carbodilite" (registered trademark) V-04 (all manufactured by Nisshinbo Co., Ltd.), which are less colored and have excellent adhesion. In particular, Carbodilite V-02-L2 has high crosslinking properties and is excellent in the effect of suppressing the precipitation of the crosslinking agent on the outermost surface under a high-temperature and high-humidity atmosphere.
[0057] The melamine compound that can be suitably used in the laminated polyester film of the present invention is a melamine compound having one or more triazine rings and one or more methylol groups in one molecule. By using such a melamine compound, a crosslinked structure between methylol groups can be formed in the resin layer X.
[0058] Examples of the melamine compound include melamine, methylolated melamine derivatives obtained by condensing melamine with formaldehyde, compounds obtained by reacting methylolated melamine with a lower alcohol to partially or completely etherify the melamine, and mixtures thereof. The melamine compound may be either a condensate of a monomer or a dimer or higher polymer, or a mixture thereof. Examples of the lower alcohol used for etherification include methyl alcohol, ethyl alcohol, isopropyl alcohol, n-butanol, and isobutanol. Examples of the functional group include an imino group, a methylol group, or an alkoxymethyl group such as a methoxymethyl group or a butoxymethyl group in one molecule, and examples of the methylated melamine compound include an imino group type methylated melamine compound, a methylol group type melamine compound, a methylol group type methylated melamine compound, and a fully alkylated methylated melamine compound. In particular, examples of methylol melamine compounds include monomethylol melamine, dimethylol melamine, trimethylol melamine, tetramethylol melamine, pentamethylol melamine, and hexamethylol melamine. These may be used alone or in combination as long as they satisfy the scope of the present invention.
[0059] In particular, since melamine compounds are materials that are compatible with water as described above, they are likely to precipitate on the surface under a moist and hot atmosphere. When the coating composition contains a melamine compound, the content is preferably 10 parts by mass or less, and more preferably 5 parts by mass or less, relative to 100 parts by mass of the binder resin. By making the content of the melamine compound 10 parts by mass or less relative to 100 parts by mass of the binder resin, it is easy to make the change in the total value of polar force and hydrogen bond force in the surface free energy of the resin layer X after the moist heat treatment 0.0 mN / m to 3.0 mN / m.
[0060] <Method of preparing coating composition> When preparing a coating composition, a solvent or a dispersion medium (hereinafter collectively referred to as a solvent) may be included. That is, various components may be dissolved or dispersed in a solvent to form a coating composition, which may then be applied to a polyester film. When such a method is adopted, a laminated polyester film in which a resin layer X is laminated on a polyester film can be obtained by drying the solvent after application and heating.
[0061] In the laminated polyester film of the present invention, it is preferable to use an aqueous solvent as the solvent. Here, the aqueous solvent refers to a mixture of water or water and an organic solvent soluble in water, such as alcohols such as methanol, ethanol, isopropyl alcohol, butanol, ketones such as acetone, methyl ethyl ketone, glycols such as ethylene glycol, diethylene glycol, propylene glycol, etc., mixed in any ratio. By using an aqueous solvent, it is possible to suppress the rapid evaporation of the solvent during the heating process, and not only can a more uniform resin layer X be formed, but also it is excellent in terms of environmental load.
[0062] In the present invention, a preferred coating composition for forming the resin layer X can be prepared by mixing and stirring the binder resin, which has been water-dispersed or water-soluble as necessary, the reactive compound, and the aqueous solvent in a desired mass ratio in any order. Next, various additives such as a lubricant, inorganic particles, organic particles, surfactants, antioxidants, and thermal initiators can be mixed and stirred in any order as needed to the extent that they do not deteriorate the properties of the resin layer X provided by the coating composition. The mixing and stirring method can be a method of shaking the container by hand, a method of stirring with a magnetic stirrer or stirring blade, a method of using ultrasonic irradiation, vibration dispersion, or the like.
[0063] Examples of the particles used include inorganic particles such as colloidal silica, titanium oxide, aluminum oxide, zirconium oxide, calcium carbonate, carbon black, and zeolite particles, and organic particles such as acrylic particles, silicone particles, polyimide particles, "Teflon" (registered trademark) particles, crosslinked polyester particles, crosslinked polystyrene particles, crosslinked polymer particles, and core-shell particles. These may be used alone or in combination of a plurality of types. Among them, inorganic particles are preferred, and colloidal silica is more preferred, from the viewpoint of hardness for obtaining the effect of suppressing blocking and thermal resistance in a preferred manufacturing method of a laminated polyester film. When the above-mentioned colloidal silica is used as the inorganic particles, the inorganic particles are well dispersed in the resin layer X, and the average roughness Ra of the resin layer X can be easily set to 20 nm or less. As the colloidal silica, for example, the "Snowtex" (registered trademark) series manufactured by Nissan Chemical Industries, Ltd. and the "Cataloid (registered trademark)" series manufactured by JGC Catalysts and Chemicals Co., Ltd. can be suitably used.
[0064] The number average particle diameter of these particles is preferably in the range of 30 nm to 1000 nm. Here, the number average particle diameter is the value (number average) obtained by adding up the particle diameters of primary particles defined as particles generated by the growth of a single crystal nucleus in JIS H7008 (2002) and dividing by the number. The number average particle diameter of the particles is more preferably in the range of 80 nm to 450 nm, and even more preferably in the range of 100 nm to 300 nm. The particles may be monodisperse particles or agglomerated particles in which a plurality of particles are agglomerated. In some cases, a plurality of types of particles with different number average particle diameters may be used in combination. The number average particle diameter of the particles can be measured by particle size distribution analysis using dynamic light scattering in the case of a coating composition, and by shape analysis using SEM-EDX in the case of a laminated polyester film.
[0065] <Method of manufacturing laminated polyester film> The method for forming the resin layer X of the present invention is preferably a method having a step of applying the above-mentioned preferred coating composition to at least one surface of a polyester film and heating (drying) it to form the resin layer X. In this formation method, the coating composition may contain various additives such as various binder resins such as polyester resins, urethane resins, and acrylic resins, at least one compound selected from melamine compounds, oxazoline compounds, and carbodiimide compounds, crosslinking catalysts, lubricants, inorganic particles, organic particles, surfactants, antioxidants, and thermal initiators.
[0066] The coating composition can be applied to a polyester film by either the in-line coating method or the off-coating method, but the in-line coating method is preferred. The in-line coating method is a method in which the coating composition is applied during the polyester film manufacturing process. Specifically, it refers to a method in which the coating is applied at any stage from melt extrusion of a polyester resin to heat treatment after biaxial stretching and winding up. Usually, the coating is applied to any of the following films: an unstretched (unoriented) polyester film (hereinafter sometimes referred to as A film) in a substantially amorphous state obtained by melt extrusion and quenching, a uniaxially stretched (uniaxially oriented) polyester film (hereinafter sometimes referred to as B film) that has been stretched in the longitudinal direction, or a biaxially stretched (biaxially oriented) polyester film (hereinafter sometimes referred to as C film) that has been further stretched in the width direction and before heat treatment.
[0067] In the present invention, it is preferable to adopt a method in which the coating composition is applied to either the A film or the B film of the polyester film before the crystal orientation is completed, the solvent is evaporated, and then the polyester film is stretched in a uniaxial or biaxial direction and heated to complete the crystal orientation of the polyester film, thereby providing the resin layer X. According to this method, the film formation of the polyester film, the coating of the coating composition, the drying of the solvent, and the heating (i.e., the formation of the resin layer X) can be performed in a continuous process. In particular, when the coating is performed on the B film, the heat treatment process (thermal fixation) after stretching in the width direction of the polyester film, the drying of the coating composition, and the heating (i.e., the formation of the resin layer X by thermosetting) can be performed in the same process. Therefore, not only is there an advantage in terms of manufacturing cost, but by completing the crystal orientation of the polyester film after drying, it is possible to perform a high-temperature heat treatment on the coating layer while reducing the deformation and heat shrinkage of the polyester film. As a result, the crosslinking of the resin layer X formed by coating is promoted, and when a water-based functional material is applied, the adhesion effect with the processing layer Y is enhanced. Another advantage is that the resin layer X can be easily and uniformly thinned by stretching after coating.
[0068] In addition, there are preferable temperature conditions for the heat treatment (thermal curing) performed on the coating layer from the viewpoint of sufficiently proceeding the crosslinking reaction of the resin layer X and increasing the adhesion with the processing layer Y. Specifically, the resin layer X is preferably formed by thermal curing at a heat treatment temperature of 170°C or more, and the thermal curing temperature is more preferably 180°C or more, further preferably 200°C or more, and particularly preferably 230°C or more. By increasing the heat treatment temperature, the elastic modulus domain diameter tends to become smaller, and the adhesion after the wet heat treatment is improved. In addition, the upper limit of the heat treatment temperature is preferably 260°C from the viewpoint of the heat resistance temperature of the polyester film. By setting the heat treatment temperature to 260°C or less, deformation of the polyester film is suppressed, making it easier to obtain a more uniform laminated polyester film.
[0069] Among these, a method in which a coating composition is applied to a film (film B) uniaxially stretched in the longitudinal direction, the solvent is dried, and then the film is stretched in the width direction and heated is excellent. This is because, compared with a method in which a coating composition is applied to an unstretched film and then biaxially stretched, this method requires one less stretching step for the layer formed by the coating composition, making it difficult for defects or cracks to occur in the resin layer X due to stretching, and making it possible to form a resin layer X with excellent transparency and smoothness. Another advantage is that process contamination by the coating composition can be reduced.
[0070] On the other hand, the offline coating method is a method in which the coating composition is applied to the film after the A film is uniaxially or biaxially stretched and heat-treated to complete the crystal orientation of the polyester film, or to the A film itself, in a process separate from the film-forming process. In the present invention, it is preferable to use the in-line coating method from the various advantages described above, but even when the resin layer X is formed by the offline coating method, the processing temperature is preferably 170°C or higher, more preferably 180°C or higher, and even more preferably 200°C or higher. By setting the processing temperature to 170°C or higher, the crosslinking reaction can be advanced to sufficiently harden the thin resin layer X. On the other hand, in the offline coating method, in-line coating is preferable because the heating by the resin layer X causes a large deformation in the width direction.
[0071] In particular, from the viewpoint of sufficiently advancing the crosslinking reaction of the resin layer X described above to increase the adhesion with the process layer Y, even when the same binder formulation is used, if the processing temperature is not 170°C or higher, a large amount of unreacted material remains in the resin layer, which may significantly reduce the adhesion with the process layer Y. The upper limit of the processing temperature is preferably 260°C in view of the heat resistance temperature of the polyester film. By keeping the processing temperature at 260°C or lower, deformation of the polyester film is suppressed, making it easier to obtain a uniform laminated polyester film.
[0072] Here, the method of applying the coating composition to the polyester film can be any method selected from known coating methods, such as bar coating, reverse coating, gravure coating, die coating, blade coating, etc., for both in-line coating and offline coating.
[0073] Therefore, a preferred method for forming the resin layer X in the present invention is a method in which a coating composition using an aqueous solvent is applied to a polyester film by in-line coating, followed by drying and heat treatment. More preferably, the coating composition is in-line coated on the B film after uniaxial stretching. In the method for producing the laminated polyester film of the present invention, the drying is preferably carried out at a temperature range of 80°C to 130°C in order to complete removal of the solvent from the coating composition. Moreover, the heat treatment is preferably carried out at a temperature range of 170°C to 260°C in order to complete the crystal orientation of the polyester film and the thermal curing of the coating composition to complete the formation of the resin layer X.
[0074] Next, the method for producing the laminated polyester film of the present invention will be described in more detail using an example in which a polyethylene terephthalate (hereinafter, PET) film is used as the polyester film; however, the laminated polyester film of the present invention and its production method are not limited thereto.
[0075] First, PET pellets are thoroughly vacuum dried, then fed to an extruder, melt-extruded into a sheet at 260°C to 280°C, and cooled and solidified to produce an unstretched (unoriented) PET film (A film). (In this case, the sheet-like material melt-extruded into a sheet is preferably cooled and solidified using a cast drum at a temperature of 10°C to 40°C.) This unstretched PET film is stretched 2.5 to 5.0 times in the longitudinal direction using a roll heated to 80°C to 120°C to obtain a uniaxially oriented PET film (B film). Furthermore, the above-mentioned coating composition prepared to a predetermined concentration is applied to one side of this B film.
[0076] At this time, the surface of the uniaxially oriented PET film to be coated may be subjected to a surface treatment such as a corona discharge treatment before the coating composition is applied. By performing a surface treatment such as a corona discharge treatment, the wettability of the coating composition to the uniaxially oriented PET film is improved, so that the coating composition is prevented from being repelled, and a resin layer X having a more uniform coating thickness can be formed. After the coating composition is applied, the ends of the uniaxially oriented PET film are held with clips and the solvent of the coating composition is dried in a heat treatment zone (preheating zone) at 80 to 130 ° C. Among them, when the uniaxially oriented PET film coated with the coating composition is sent to the heat treatment zone, it is preferable to carry out the process by holding the uncoated parts at both ends of the uniaxially oriented PET film in the width direction with clips and leading it to a tenter. After drying, the film is stretched 1.1 to 5.0 times in the width direction, and then led to a heat treatment zone (thermal fixation zone) at 170 ° C. to 260 ° C. for 1 to 30 seconds to complete the crystal orientation.
[0077] In this heat treatment step (thermal fixation step), a 3% to 15% relaxation treatment may be performed in the width direction or the length direction as necessary. Thereafter, the laminated polyester film is cooled to room temperature, and the laminated polyester film is cut parallel to the length direction with a known razor blade or the like to remove the uncoated parts at both ends in the width direction that were held by the clips, and then the film can be wound into a roll. The laminated polyester film thus obtained is a laminated polyester film that is excellent in the applicability, adhesion, and transparency of water-based coating materials. The uncoated parts of the film at both ends in the width direction cut and removed by the slitter can be used as recycled raw materials as described below.
[0078] The polyester film constituting the laminated polyester film of the present invention is not limited in its layer structure, and examples thereof include a single-layer structure consisting of only Layer A, a laminate structure of Layer A / Layer B, i.e., a two-type two-layer laminate structure, a laminate structure of Layer A / Layer B / Layer A, i.e., a two-type three-layer laminate structure, and a laminate structure of Layer A / Layer B / Layer C, i.e., a three-type three-layer laminate structure.
[0079] The lamination method for the polyester film constituting the laminated polyester film of the present invention is not limited, and examples thereof include a lamination method by coextrusion, a lamination method by lamination, and a combination of these methods. From the viewpoint of transparency and manufacturing stability, however, it is preferable to adopt a coextrusion method. When forming a laminate, different resin structures may be used for the purpose of imparting different functions to each layer. As such a method, for example, a lamination structure of A layer / B layer / A layer, that is, a two-kind three-layer lamination structure, in which B layer is made of homopolyethylene terephthalate from the viewpoint of transparency, and particles are added to A layer to impart easy slippage, can be mentioned.
[0080] <Processing layer Y> Hereinafter, a laminate using the laminate film of the present invention will be described. The laminate has a processed layer Y on the surface of the resin layer X of the laminated polyester film of the present invention. That is, the laminated polyester film of the present invention is preferably used to manufacture a laminate in which a processed layer Y is further formed on the resin layer X. In addition, it is preferable to use a wet coating method for forming the processed layer Y, and the solvent or dispersion medium of the coating material for forming the processed layer Y may be either water or an organic solvent. The process layer Y can be formed by any method selected from known coating methods, such as a bar coating method, a reverse coating method, a gravure coating method, a die coating method, and a blade coating method.
[0081] In addition, the processing layer Y is preferably a function-imparting layer that imparts different physical properties to the polyester film. Examples of the functions that can be imparted include scratch prevention, electrical conductivity and antistatic properties, adhesion, prevention of various adhesions such as dirt, transmission and absorption of various light rays from infrared to visible to ultraviolet, and easy peeling that can be used for protection of adherends and transfer processing. Among these, in the laminate of the present invention, it is particularly preferable for the processing layer Y to contain at least one of a hard coat agent, an adhesive, and a printing ink, for example, for applications of a laminated polyester film having adhesion and transparency.
[0082] The laminated polyester film of the present invention is preferably used for a vehicle display. The vehicle display refers to an image display device that can be attached to or is installed in a vehicle, such as a car navigation system, a display audio, and a head-up display. In particular, transparency is very important for a head-up display, since excellent forward visibility is required. By using the laminated polyester film of the present invention, the problem of reduced visibility is unlikely to occur even if the display is left in a high-temperature, high-humidity vehicle interior for a long period of time. The head-up display of the present invention is a head-up display that uses the laminated polyester film of the present invention.
[0083] The laminated polyester film of the present invention is preferably used for electronic parts for vehicles. The electronic parts for vehicles are electronic parts used in vehicles, such as flexible printed wiring boards (FPCs), flexible flat cables (FFCs), inverter circuit film capacitors for driving motors in electric vehicles, and the like. In recent years, the amount of film mounted in these electronic parts for vehicles has increased due to the shift to EVs and self-driving cars. By using the laminated polyester film of the present invention, adhesion with the deposition layer and adhesive layer is maintained for a long period of time even when placed in a high-temperature and high-humidity environment inside the vehicle. The electronic parts for vehicles of the present invention are electronic parts for vehicles using the laminated polyester film of the present invention. EXAMPLES
[0084] Next, the present invention will be described in more detail with reference to examples, but is not necessarily limited thereto. The methods for measuring the various characteristics and the methods for evaluating the various effects in the present invention are as follows.
[0085] [Methods of measuring characteristics and evaluating effects] (1) Surface free energy of resin layer X First, the laminated polyester film was left for 24 hours in an atmosphere at room temperature of 23°C and relative humidity of 65%. Then, in the same atmosphere, the contact angles of four types of liquids, pure water, ethylene glycol, formamide, and diiodomethane, were measured at five points on the resin layer X using a contact angle meter DM-501 (manufactured by Kyowa Interface Science Co., Ltd.), and the average of the measured values was taken as the contact angle of each liquid. Next, using the contact angles of the four types of liquids obtained, the surface free energy of the solid (γ) was calculated as the dispersion force component (γ S d ), polar force component (γ S p ), and hydrogen bond strength component (γ S h The dispersion force, polar force, hydrogen bonding force, and surface energy, which is the sum of the dispersion force and polar force, were calculated. The specific calculation method is shown below. The meaning of each symbol is explained below. Gamma S L : Surface energy of the resin layer and the known solutions listed in Table 1 Gamma S : Surface energy of resin layer Gamma L : Surface energy of known solutions listed in Table 1 Gamma S d : Dispersion force component of the surface energy of the resin layer Gamma S p : Polar component of the surface energy of the resin layer Gamma S h : Hydrogen bond force component of the surface energy of the resin layer Gamma L d : Dispersion force components of the surface energy of known solutions listed in Table 1 Gamma L p : Polar force components of the surface energy of known solutions listed in Table 1 Gamma L h : Hydrogen bond force component of surface energy of known solutions listed in Table 1 where γS L When is the tension at the interface between a solid and a liquid, equation (1) holds true. Gamma S L =γ S +γ L -2(γ S d ·γ L d ) 1 / 2 -2(γ S p ·γ L p ) 1 / 2 -2(γ S h ·γ L h ) 1 / 2 Formula (1).
[0086] Furthermore, the state when a droplet is in contact with a smooth solid surface at a contact angle (θ) is expressed by the following equation (2) (Young's equation). Gamma S =γ S L +γ L cosθ ··· Equation (2).
[0087] Combining equations (1) and (2), we obtain the following equation. (γ S d ·γ L d ) 1 / 2 +(γ S p ·γ L p ) 1 / 2 +(γ S h ·γ L h ) 1 / 2 =γ L (1+cosθ) / 2 Equation (3).
[0088] In practice, the contact angle (θ) and the surface tension components (γ L d , γL p , γ L h ) into equation (3) and solve the four simultaneous equations. As a result, the surface energy of the solid (γ), the dispersion force component (γ S d ), polar force component (γ S p ), and hydrogen bond strength component (γ S h ) was calculated.
[0089] [Table 1]
[0090] (2) Change in the total value of polarity and hydrogen bonding strength after moist heat treatment The sample was placed in a high-temperature, high-humidity oven (manufactured by Espec, model LHK-113) at 85°C and 90% RH for 500 hours, and the polar component (γ S p ) + hydrogen bond strength component (γ S h )) to (polar force component before treatment (γ S p ) + hydrogen bond strength component (γ S h The value of (a)) was defined as the amount of change in the total value of the polar strength and hydrogen bonding strength of the resin layer X.
[0091] (3) Film thickness of resin layer X The thickness of the resin layer X was determined by observing a sample cut out from a cross section using a microtome under an electron microscope. More specifically, the thickness of the resin layer X on the polyester film was measured by observing the cross section using a transmission electron microscope (TEM) H-7100FA type (manufactured by Hitachi, Ltd.). The thickness of the resin layer was read from an image taken at a magnification of 200,000 times using the TEM. The thickness of the resin layer was measured at a total of 20 points and the average value was taken as the thickness of the resin layer X.
[0092] (4) Domain area using elastic modulus variation images obtained by atomic force microscope (AFM) The elastic modulus of the surface of the resin layer was measured using an AFM (DimensionIcon manufactured by Burker Corporation) in PeakForceQNM mode. The obtained force curve was analyzed based on the JKR contact theory using the attached analysis software "NanoScopeAnalysis V1.40" to obtain the elastic modulus distribution. Specifically, the laminated polyester film was first fixed to the sample stage using double-sided tape so that the measurement surface (resin layer X surface) was on the upper surface. Next, the cantilever's warp sensitivity, spring constant, and tip curvature were configured according to the manual for PeakForceQNM mode, and then measurements were performed under the following conditions, and the data obtained from the DMT Modulus channel was adopted as the elastic modulus of the resin layer. The measurement conditions are shown below. Measurement equipment: Atomic force microscope (AFM) manufactured by Burker Corporation (model number: DimensionIcon) Measurement mode: PeakForceQNM (force curve method) Cantilever: Bruker AXS RTESPA-300 Measurement atmosphere: 23℃ in air Measurement range: 5 (μm) square Resolution: 512×512 Measurement speed: 0.977 Hz Cantilever movement speed: 10 (μm / s) Pressing load (Setpoint): 40 (nN) Poisson's ratio: 0.4.
[0093] The obtained DMT Modulus channel data was then analyzed using the analysis software "NanoScope Analysis V1.40", and the Image Raw Mean value in the Results tab obtained by processing using Roughness was taken as the elastic modulus of the resin layer X. The obtained DMT Modulus channel data was then analyzed using the analysis software "NanoScope Analysis V1.40". First, the data was smoothed using Order:3rd in Flatten mode to obtain an "elastic modulus variation image". The "elastic modulus variation image" was then analyzed in Roughness mode, and Image Rmax was taken as the variation width.
[0094] On the other hand, for the analysis of the domain area, the "elastic modulus variation image" was converted to a grayscale image by selecting Color tabel: 7 from Adjust Image Color Scale in the Commands tab (corresponding to the images shown in Figures 1 and 2). Furthermore, in Bearing Analysis mode, the elastic modulus variation image was colored with Bearing Area Percent: 10%. Next, the colored parts were selected based on the hue using Color Threshold of the image processing software ImageJ / developer: National Institutes of Health (NIH). Furthermore, the average area of each domain was calculated using the Analyze Particles function. Note that the area of noise parts was excluded by setting the Size range to 5-Infinity (Pixel^2) in the measurement condition settings of Analyze Particles. The average area of each domain obtained by the above operations was used as the domain area.
[0095] (5) Haze change after wet heat treatment Five square laminated polyester film samples, each 5 cm on a side, were prepared and the haze was measured using a turbidity meter "NDH5000" manufactured by Nippon Denshoku Industries Co., Ltd. in accordance with the JIS "Determination of Haze for Transparent Materials" (K7136 2000 edition). Next, the samples were subjected to a moist heat treatment under the same conditions as in (2) and the haze was then measured. The amount of haze change after moist heat treatment was determined as (5-point average haze after moist heat treatment - 5-point average haze before moist heat treatment).
[0096] (6) Adhesion of processed layer Y Arakawa Chemical Industries Co., Ltd. UV-curable resin Z7415 (solid content 20%) was applied to the surface of the resin layer X of the laminated polyester film by the wire bar coating method to a thickness of approximately 1 μm, and then dried at 90 °C for 1 minute. After that, an ultraviolet lamp with an irradiation intensity of 120 W / cm was used, the irradiation distance (distance between the lamp and the surface coated with the water-based coating material) was 12 cm, the conveyor speed was 2 m / min, and the cumulative intensity was approximately 300 mJ / cm. 2 The film was irradiated with UV light under the conditions of (the layer thus formed is referred to as processed layer Y). Hereinafter, this film is referred to as hard-coated laminated polyester film. In accordance with JIS5600-5-6 (established in 1999), 25 squares of 5×5 were cut at 2 mm intervals on the processed layer surface of the hard-coated laminated polyester film sample obtained above. Next, 18 mm of "Sellotape" (registered trademark) (manufactured by Nichiban Co., Ltd., product number: CT-18S) was firmly rubbed with a finger on the cut part so that the cut was visible, and pressed down. Then, the "Sellotape" (registered trademark) was instantly peeled off at an angle of about 60° to the hard-coat layer. After that, the number of squares where the hard-coat layer remained was counted. The evaluation was performed five times, and the adhesion of the hard-coat was evaluated using the average value (rounded up to the nearest whole number) according to the following evaluation criteria. S: No peeling at all (pass) A: 99-95 remaining squares (pass) B: Number of remaining squares is 96-90 (pass) C: Number of remaining cells is 89-70 (failed) D: Less than 70 remaining masses (failed).
[0097] (7) Adhesion of processed layer Y after wet heat treatment A hard-coated laminated polyester film was obtained in the same manner as in (6). Next, the obtained hard-coated laminated polyester film sample was placed in a high-temperature and high-humidity chamber at 85°C and 90 RH% for 500 hours, and the adhesion was measured in the same manner as in (6).
[0098] [resin] First, the following resins were obtained for preparing the coating composition.
[0099] (Reference example 1) Resin 1 A water dispersion of polyester resin having the following copolymerization composition was obtained. The following copolymerization components and 0.1 parts of potassium titanium oxalate as a catalyst were added to a reactor, and the temperature was raised to 200°C while stirring and mixing in a nitrogen atmosphere at normal pressure. Next, the reaction temperature was gradually raised to 250°C over 4 hours to terminate the transesterification reaction. 15 parts by mass of the polyester resin thus obtained and 85 parts by mass of water were added to a dissolution tank and dispersed at a temperature of 80 to 95°C over 2 hours with stirring to obtain a 15% by mass water-based dispersion of polyester resin. This was designated resin 1. <Copolymerization component> (Dicarboxylic acid component) Dimethyl 2,6-naphthalenedicarboxylate: 88 mol% Sodium dimethyl 5-sulfoisophthalate: 12 mol% (Diol component) Compound with 2 moles of ethylene oxide added to 1 mole of bisphenol S: 86 mole% 1,3-propanediol: 14 mol% (Reference example 2) Resin 2 Under a nitrogen gas atmosphere and at room temperature (25°C), 100 parts by mass of water, 1 part by mass of sodium lauryl sulfate, and 0.5 parts by mass of ammonium persulfate were charged into a container 1, which was then heated to 70°C to dissolve sodium lauryl sulfate, obtaining a solution 1 at 70°C. Under room temperature (25°C), 30 parts by mass of water and 2 parts by mass of sodium lauryl sulfate were added to a container 2 to dissolve sodium lauryl sulfate, and then 13.3 parts by mass of polyethylene oxide monomethacrylate (10 repeating units of ethylene oxide) was added as an acrylic monomer component having a polyalkylene oxide, and 29.7 parts by mass of ethyl acrylate, 50.0 parts by mass of methyl methacrylate, and 5.0 parts by mass of N-methylol acrylamide were added as other monomer components, and the mixture was stirred to obtain a solution 2. Under a nitrogen gas atmosphere, the solution 1 was transferred to a reactor, and while maintaining the temperature of the solution in the reactor at 70°C, the solution 2 was continuously dripped into the solution 1 over a period of 3 hours. After the dropwise addition was completed, the mixture was stirred at 85° C. for an additional 2 hours, and then cooled to 25° C. to terminate the reaction, yielding an acrylic resin emulsion, designated Resin 2.
[0100] (Reference example 3) Resin 3 Under a nitrogen gas atmosphere and at room temperature (25°C), 66 parts by mass of polyester urethane resin (DIC Corporation's "HYDRAN" (registered trademark) AP-40 (F)), 35 parts by mass of methyl methacrylate, 29 parts by mass of ethyl acrylate, and 2 parts by mass of N-methylol acrylamide were charged into a vessel 3 to obtain a solution 3. Next, 7 parts by mass of an emulsifier (ADEKA Corporation's "REASORP" ER-30) were added, and water was further added so that the solid content of the solution became 50% by mass to obtain a solution 4. Under room temperature (25°C), 30 parts by mass of water was added into the vessel 4, and the temperature was raised to 60°C. Then, while stirring, the solution 4 was continuously dripped into the vessel 4 over a period of 3 hours. At the same time, 3 parts by mass of a 5% by mass aqueous solution of potassium persulfate was continuously dripped into the vessel 4. After the dripping was completed, the mixture was stirred for another 2 hours, cooled to 25°C, and the reaction was terminated to obtain an aqueous dispersion of an acrylic-urethane copolymer resin. This was designated Resin 3.
[0101] (Reference example 4) Resin 4 Similarly to Reference Example 1, an aqueous dispersion of a polyester resin (Tg: 80° C.) composed of terephthalic acid (88 mol%), 5-sodium sulfoisophthalic acid (12 mol%), ethylene glycol (95 mol%), and diethylene glycol (5 mol%) was obtained. This was designated Resin 4.
[0102] (Reference example 5) Resin 5 Similarly to Reference Example 1, an aqueous dispersion of polyester resin 5 (Tg: 66° C.) composed of terephthalic acid (99 mol%), 5-sodium sulfoisophthalic acid (1 mol%), ethylene glycol (70 mol%), and neopentyl glycol (30 mol%) was obtained. This was named resin 5.
[0103] (Reference example 6) Resin 6 Methyl methacrylate, hydroxyethyl methacrylate, and urethane acrylate oligomer (manufactured by Negami Chemical Industries, Ltd., "Art Resin" (registered trademark) UN-3320HA, number of acryloyl groups is 6) were charged in a stainless steel reaction vessel in a ratio of 70:20:5 (mass ratio), and 2 parts by mass of sodium dodecylbenzenesulfonate was added as an emulsifier and stirred to prepare mixed liquid 1. Next, a reaction apparatus equipped with a stirrer, a reflux condenser, a thermometer, and a dropping funnel was prepared, and mixed liquid 1, isopropyl alcohol, and potassium persulfate as a polymerization initiator were charged in the reaction apparatus in a ratio of 60:200:5 (mass ratio), and then heated to 60 ° C. to prepare mixed liquid 2, which was kept heated at 60 ° C. for 20 minutes. Next, mixed liquid 1, isopropyl alcohol, and potassium persulfate were mixed in a ratio of 40:50:5 (mass ratio) to prepare mixed liquid 3. Next, the same amount of mixed solution 3 was dropped into mixed solution 2 over 2 hours using a dropping funnel to prepare mixed solution 4, which was then heated to 60°C and held for 2 hours. The resulting mixed solution 4 was cooled to 50°C or lower, transferred to a container equipped with a stirrer and a pressure reducing device, and 60 parts by mass of 25% ammonia water and 900 parts by mass of pure water were added. The mixture was heated to 60°C while being subjected to reduced pressure to recover isopropyl alcohol and unreacted monomers. The acrylic resin emulsion thus obtained was designated as resin 6.
[0104] [Other ingredients] In addition, the following materials were used as reactive compounds, surfactants, etc. Reactive compound 1: Carbodiimide water-based crosslinker (Nisshinbo Chemical Co., Ltd. "Carbodilite" (registered trademark) V-02-L2) Reactive compound 1-2: Carbodiimide water-based crosslinking agent (Nisshinbo Chemical Co., Ltd. "Carbodilite" (registered trademark) V-04) Reactive compound 2: Oxazoline-containing polymer aqueous dispersion ("Epocross" (registered trademark) WS-500, manufactured by Nippon Shokubai Co., Ltd.) Reactive compound 3: Melamine resin water sol ("WATERSOL" (registered trademark) S-695, manufactured by DIC Corporation) Surfactant: Fluorine-based surfactant ("Pluscoat" (registered trademark) RY-2, manufactured by GOO Chemical Industry Co., Ltd.) Inorganic particles 1: Silica particles having a number average particle diameter of 170 nm ("Snowtex" (registered trademark) MP-2040, manufactured by Nissan Chemical Industries, Ltd.). Inorganic particles 2: Silica particles having a number average particle size of 100 nm ("Snowtex" (registered trademark) MP-1040, manufactured by Nissan Chemical Industries, Ltd.).
[0105] Example 1 <Paint composition> First, resin 1: reactive compound 1: reactive compound 2 were mixed at 100:30:30 (mass ratio), and then 0.1 parts by mass of inorganic particles 1 were added to 100 parts by mass of binder resin (resin 1), and 0.4 parts by mass of inorganic particles 2 were added to 100 parts by mass of binder resin (resin 1). The concentration was adjusted using water as a solvent, and then 0.03 parts by mass of a surfactant was added to a total of 100 parts by mass of water to adjust the coating properties. Here, the method of adjusting the concentration using water will be described in detail. Specifically, the concentration was determined according to the target thickness of the resin layer X by the following method. The thickness of the resin layer X is proportional to the concentration of the coating composition and the coating thickness, and inversely proportional to the stretching ratio in the width direction and the specific gravity of the resin layer X. Of these, the coating thickness is uniquely determined from the number used for the bar coat, and the stretching ratio is uniquely determined from the film-forming conditions. Therefore, a plurality of concentrations of the coating composition were prepared in advance, and a calibration curve was created by measuring the thickness of the resin layer X by the above-mentioned method, and the concentration of the coating composition that matches the target thickness of the resin layer X was determined. The concentration of the obtained coating composition was approximately 2.5% by mass to 4.5% by mass. In this way, the coating composition was obtained.
[0106] <Laminated polyester film> PET pellets (intrinsic viscosity 0.64 dl / g) containing two types of particles (4% by mass of silica particles with a primary particle size of 0.3 μm and 2% by mass of calcium carbonate particles with a primary particle size of 0.8 μm) were thoroughly vacuum dried, fed to an extruder, melted at 280 ° C, extruded into a sheet from a T-shaped die, and wrapped around a mirror-finished casting drum with a surface temperature of 25 ° C by an electrostatic casting method, and cooled and solidified. The unstretched film (A film) thus obtained was heated to 90 ° C and stretched 3.1 times in the longitudinal direction to obtain a uniaxially stretched film (B film). Next, the uniaxially stretched film was subjected to a corona discharge treatment in air, and then the above-mentioned coating composition was applied with a bar coater (wire bar #4). Then, both ends in the width direction of the uniaxially stretched film to which the coating composition was applied were held with clips and introduced into a preheating zone. The atmospheric temperature of the preheating zone was set to 90 to 100 ° C, and the solvent of the coating composition was dried. Subsequently, the film was continuously stretched 3.6 times in the width direction in a 100°C stretching zone, and then heat-treated for 20 seconds in a 240°C heat treatment zone to form a resin layer X. The film was then subjected to a 5% relaxation treatment in the width direction at the same temperature to obtain a laminated polyester film in which the crystal orientation of the polyester film was completed. In the obtained laminated polyester film, the thickness of the PET film (polyester film) was 50 μm, and the thickness (film thickness) of the resin layer X was 80 nm. The evaluation results are shown in Table 2.
[0107] (Examples 2 to 11, Comparative Examples 1 to 4) A laminated polyester film was obtained in the same manner as in Example 1, except that the composition of the coating composition, the drying temperature (maximum processing temperature), and the film thickness of the resin layer were as shown in Table 2. In the obtained laminated polyester film, the thickness of the PET film (polyester film) was 50 μm, and other evaluation results are shown in Table 2.
[0108] Comparative Example 6 Except for not carrying out the coating step of the coating composition, a polyester film having a thickness of 50 μm was obtained in the same manner as in Example 1. The evaluation results are shown in Table 2.
[0109] [Table 2] [Industrial Applicability]
[0110] The present invention relates to an easily adhesive film that exhibits excellent transparency and adhesion even when stored in a hot and humid atmosphere for long periods of time, and can be used in security films, vehicle displays such as car navigation systems, display audio, and head-up displays, flexible printed circuit boards (FPCs) and flexible flat cables (FFCs), and films for vehicle electronic components such as inverter circuit film capacitors for driving the motors of electric vehicles, etc. [Explanation of symbols]
[0111] 1: Representative black area in elastic modulus variation image 2: Representative white area in the elastic modulus variation image
Claims
1. A laminated polyester film having a resin layer X on at least one outermost layer of a polyester film, The surface free energy of the resin layer X is 35.0 mN / m to 55.0 mN / m, A laminated polyester film, characterized in that a change in the total value of polar force and hydrogen bonding force in the surface free energy of the resin layer X after 500 hours of wet heat treatment in an environment of a temperature of 85°C and a humidity of 85% is 0.0 mN / m to 3.0 mN / m.
2. The domain area in the elastic modulus dispersion image of the resin layer X of 1 μm square measured by an atomic force microscope (AFM) is 500 nm 2 The laminated polyester film according to claim 1, wherein:
3. 3. The laminated polyester film according to claim 1, wherein the resin layer X contains a polyester resin.
4. 3. The laminated polyester film according to claim 1, wherein the resin layer X is formed from a coating composition that satisfies all of the following characteristics 1 to 3: Feature 1: Contains binder resin, melamine compound, and carbodiimide compound. Feature 2: When the content of the binder resin in the coating composition is 100 parts by mass, the content A of the melamine compound is 10 parts by mass or less, and the content B of the carbodiimide compound is 5 parts by mass to 30 parts by mass. Feature 3: A / B is 0.50 or less.
5. 3. The laminated polyester film according to claim 1, wherein the resin layer X is formed from a coating composition which satisfies both of the following characteristics 4 and 5. Feature 4: Contains a binder resin. Feature 5: 10% by mass or more of the binder resin contained in the coating composition is a resin having a hydroxyl group and a polyfunctional acryloyl group.
6. The laminated polyester film according to claim 1 or 2, wherein the resin layer X has a thickness of 50 nm or less.
7. The laminated film according to claim 1 or 2, which is used for a vehicle display.
8. The laminated film according to claim 1 or 2, which is used for electronic parts for vehicles.
9. A vehicle display using the laminated polyester film according to claim 1 or 2.
10. 3. An electronic part for a vehicle, comprising the laminated polyester film according to claim 1 or 2.
Citation Information
Patent Citations
JP1975042161A
Easily adhesive film
JP2009214531A
Easily adhesive polyester film for optical use
JP2011140140A
Easily adhesive polyester film for optical use
JP2014065887A