Composition for colloidal crystal and printed matter

The composition for colloidal crystals, with fine resin particles and specific additives, addresses low fluidity and plate clogging issues, ensuring excellent color development and printability for large-scale production.

JP2024135663APending Publication Date: 2024-10-04TOYO INK MFG CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023046460
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Conventional compositions for colloidal crystals suffer from low fluidity, leading to plate clogging and printing defects, limiting their ability to produce printed matter in large quantities.

Method used

A composition for colloidal crystals containing fine resin particles, water, and specific additives with a thixotropic index of 1.00 to 2.00, along with a hydrophilic solvent and nonionic surfactant, enhances fluidity and reduces plate clogging, ensuring excellent color development and printability.

Benefits of technology

The composition achieves good resolubility during printing, minimizes plate clogging, and produces a coating film with superior color development, enabling large-scale production of printed matter.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135663000001
    Figure 2024135663000001
  • Figure 2024135663000002
    Figure 2024135663000002
  • Figure 2024135663000003
    Figure 2024135663000003
Patent Text Reader

Abstract

To provide a composition for a colloidal crystal which has good re-melting property in printing, hardly causes plate clogging, and is excellent in color development property of a coating film after printing.SOLUTION: A composition for a colloidal crystal contains resin fine particles (A) and water, and has a thixotropy index (TI value) measured by an E type viscometer of 1.00 to 2.00. The composition for the colloidal crystal contains a hydrophilic solvent (B) having a boiling point at 1 atom of 95 to 250°C. The composition for the colloidal crystal further contains a nonionic surface active agent (C) having an HLB value of 3.0 to 15.0.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composition for colloidal crystals and a printed matter. [Background technology]

[0002] Photonic crystals are artificial crystals with a nano-periodic structure in which materials with different refractive indices are arranged at intervals equivalent to the wavelength of light. They have various interesting optical properties, such as the reflection of light of a specific wavelength known as Bragg reflection, the light trapping effect due to the photonic band gap, and the light amplification effect, and have been actively studied in recent years. Among them, colloidal crystals, in which colloid-sized particles are regularly arranged, are one of the photonic crystals that can be produced relatively easily. However, when a composition for colloidal crystals is printed, the composition for colloidal crystals has poor resolubility and printing defects such as clogging occur, so that it has not yet been possible to mass-produce them. Therefore, a composition for colloidal crystals that combines color development and printability is required.

[0003] Patent Document 1 discloses a coating composition for forming a structural color film, which can easily arrange fine particles in an ordered manner and the resulting fixed crystal structure can exhibit sufficient mechanical strength and visual effects, and a method for producing the same. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2017-223915 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the composition described in Patent Document 1 has low fluidity, which causes problems such as clogging during printing. As described above, conventional compositions for colloidal crystals have problems such as low fluidity and printing defects such as clogging and plate fogging, and therefore have not yet reached a state where they can be used to mass-produce printed matter.

[0006] An object of the present invention is to solve the problems of providing a composition for colloidal crystals which has good re-solubility during printing, is less likely to cause plate clogging, and provides a coating film with excellent color development properties after printing. [Means for solving the problem]

[0007] The present invention relates to a composition for colloidal crystals, which contains resin fine particles (A) and water, and has a thixotropy index (TI value) of 1.00 to 2.00 as measured with an E-type viscometer.

[0008] The present invention also relates to the above composition for colloidal crystals, which contains a hydrophilic solvent (B) having a boiling point of 95 to 250° C. at 1 atmospheric pressure.

[0009] The present invention also relates to the above composition for colloidal crystals, which contains a nonionic surfactant (C) having an HLB value of 3.0 to 15.0.

[0010] The present invention also relates to the above composition for colloidal crystals, wherein the hydrophilic solvent (B) contains at least one solvent selected from the group consisting of monohydric lower alcohol solvents, glycol solvents, and glycol ether solvents.

[0011] The present invention also relates to the above composition for colloidal crystals, wherein the content of the hydrophilic solvent (B) is 0.5 to 30% by mass based on the total mass of the composition for colloidal crystals.

[0012] The present invention also relates to the above-mentioned composition for colloidal crystals, wherein the nonionic surfactant (C) comprises at least one selected from the group consisting of polyoxyalkylene alkyl ether surfactants, polyglycerol fatty acid ester surfactants, acetylene surfactants, and siloxane surfactants.

[0013] The present invention also relates to the above composition for colloidal crystals, wherein the content of the nonionic surfactant (C) is 0.5 to 5 mass % based on the total mass of the composition for colloidal crystals.

[0014] The present invention also relates to the above-mentioned composition for colloidal crystals, which is for use in gravure printing.

[0015] The present invention also relates to a printed matter comprising a colloidal crystal layer made of the above-mentioned composition for colloidal crystals.

[0016] The present invention also relates to a laminate comprising a substrate, a primer layer, and a colloidal crystal layer made of the above-mentioned composition for colloidal crystals. Effect of the Invention

[0017] According to the present invention, it is possible to provide a composition for colloidal crystals which has good re-solubility during printing, is less likely to cause plate clogging, and provides a coating film with excellent color development after printing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] <Composition for colloidal crystals> The composition for colloidal crystals of the present invention contains resin fine particles (A) and water, and is characterized in that it has a thixotropy index (TI value) measured by an E-type viscometer of 1.00 to 2.00. The composition of the present invention contains resin fine particles (A) and water, and since the TI value is within the above range, it has high fluidity and is less likely to cause printing defects such as clogging during printing. The elements constituting the present invention will now be described in detail.

[0019] <Resin fine particles (A)> The resin fine particles (A) may be of a core-shell type (core layer: inner layer, shell layer: outer layer) or may have a uniform structure (core layer only). The resin fine particles (A) are present in the form of a dispersion in the composition for colloidal crystals, and in the process of being applied to a substrate and dried, they are regularly arranged and laminated in a densely packed form due to an advection accumulation phenomenon accompanying the evaporation of water. Then, the voids are replaced by air from the water, forming a colloidal crystal layer. The colloidal crystal layer is a layer that exhibits structural colors derived from Bragg reflection, and various colors can be exhibited by controlling the periodic interval by controlling the particle diameter of the resin fine particles (A).

[0020] The average particle size of the resin fine particles (A) is preferably in the range of 100 to 500 nm. The above range is preferable because the color development of the colloidal crystal layer becomes clear and a colloidal crystal coating film with better color development can be obtained. The average particle size in this specification can be measured by dynamic light scattering, and the peak of the obtained volume particle size distribution data (histogram) is taken as the average particle size. The coefficient of variation (Cv value) of the average particle size of the resin fine particles is preferably 30% or less, more preferably 20% or less. By having a coefficient of variation of 30% or less, the regularity of the particle arrangement is improved, the color development of the laminate is improved, and the amount of coarse particles is reduced, so that plate fogging is less likely to occur during printing. The coefficient of variation is a value that indicates the uniformity of the particle size, and can be calculated by the following formula. Formula: Coefficient of variation Cv value (%) = standard deviation of particle size / average particle size × 100 [In the formula, the units of standard deviation and average particle size are the same]

[0021] [Polymer of ethylenically unsaturated monomer (a)] The type and manufacturing method of the resin fine particles (A) are not particularly limited, and any monodispersible resin fine particles can be used, but the resin fine particles (A) are preferably polymers of ethylenically unsaturated monomers (a) in terms of easy control of the refractive index and monodispersity of the fine particles (A) and excellent color development properties, and more preferably resin fine particles made of acrylic resin or styrene acrylic resin.

[0022] The resin fine particles which are a polymer of the ethylenically unsaturated monomer (a) can be produced, for example, by the following emulsion polymerization. First, an aqueous medium and a surfactant are charged into a reaction tank and the temperature is raised to a predetermined temperature. Meanwhile, water, a surfactant, and an ethylenically unsaturated monomer (a) are charged into a dropping tank and stirred to prepare an emulsion of the ethylenically unsaturated monomer (a). Then, under a nitrogen atmosphere, a radical polymerization initiator is added while dropping the prepared emulsion into the reaction tank. After the reaction starts, polymer particle nuclei are generated, and the particles gradually grow to form resin fine particles.

[0023] Examples of the ethylenically unsaturated monomer (a) include styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, m-methylstyrene, vinylnaphthalene, benzyl(meth)acrylate, phenoxyethyl(meth)acrylate, phenoxydiethylene glycol(meth)acrylate, phenoxytetraethylene glycol(meth)acrylate, phenoxyhexaethylene glycol(meth)acrylate, phenoxyhexaethylene glycol(meth)acrylate, phenyl(meth)acrylate, acrylate and other aromatic ethylenically unsaturated compounds; methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, heptyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, lauryl (meth)acrylate , tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, behenyl (meth)acrylate, and other linear or branched alkyl group-containing ethylenically unsaturated monomers; cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyl (meth)acrylate ethylenically unsaturated monomers containing an alicyclic alkyl group, such as adamantyl (meth)acrylate; ethylenically unsaturated monomers containing a fluorinated alkyl group, such as trifluoroethyl (meth)acrylate, heptadecafluorodecyl (meth)acrylate; ethylenically unsaturated monomers containing a carboxy group, such as maleic acid (anhydride), fumaric acid, itaconic acid, citraconic acid, or alkyl or alkenyl monoesters thereof, succinic acid β-(meth)acryloxyethyl monoester, acrylic acid, methacrylic acid, crotonic acid, cinnamic acid, etc.Sulfo group-containing ethylenically unsaturated monomers such as 2-acrylamido 2-methylpropanesulfonate sodium, methallylsulfonic acid, methallylsulfonic acid, sodium methallylsulfonate, allylsulfonic acid, sodium allylsulfonate, ammonium allylsulfonate, and vinylsulfonic acid; (meth)acrylamide, N-methoxymethyl-(meth)acrylamide, N-ethoxymethyl-(meth)acrylamide, N-propoxymethyl-(meth)acrylamide, N-butoxymethyl-(meth)acrylamide, N-pentoxy Methyl-(meth)acrylamide, N,N-di(methoxymethyl)acrylamide, N-ethoxymethyl-N-methoxymethylmethacrylamide, N,N-di(ethoxymethyl)acrylamide, N-ethoxymethyl-N-propoxymethylmethacrylamide, N,N-di(propoxymethyl)acrylamide, N-butoxymethyl-N-(propoxymethyl)methacrylamide, N,N-di(butoxymethyl)acrylamide, N-butoxymethyl-N-(methoxymethyl)methacrylamide, N,N-di(pentoxymethyl)acrylamide ethylenically unsaturated monomers containing an amide group, such as N-methoxymethyl-N-(pentoxymethyl)methacrylamide, N,N-dimethylaminopropylacrylamide, N,N-diethylaminopropylacrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide, and diacetone acrylamide; ethylenically unsaturated monomers containing a hydroxyl group, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, glycerol mono(meth)acrylate, 4-hydroxyvinylbenzene, 1-ethynyl-1-cyclohexanol, and allyl alcohol; ethylenically unsaturated monomers containing a polyoxyethylene group, such as methoxypolyethylene glycol (meth)acrylate and polyethylene glycol (meth)acrylate; ethylenically unsaturated monomers containing an amino group, such as dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, methylethylaminoethyl (meth)acrylate, dimethylaminostyrene, and diethylaminostyrene;Epoxy group-containing ethylenically unsaturated monomers such as glycidyl (meth)acrylate and 3,4-epoxycyclohexyl (meth)acrylate; ketone group-containing ethylenically unsaturated monomers such as diacetone (meth)acrylamide, acetoacetoxy (meth)acrylate and 2-acetoacetoxyethyl (meth)acrylate; allyl (meth)acrylate, 1-methylallyl (meth)acrylate, 2-methylallyl (meth)acrylate, 1-butenyl (meth)acrylate, (meth)acrylate, 2-butenyl (meth)acrylate, 3-butenyl (meth)acrylate, 1,3-methyl-3-butenyl (meth)acrylate, 2-chloroallyl (meth)acrylate, 3-chloroallyl (meth)acrylate, o-allylphenyl (meth)acrylate, 2-(allyloxy)ethyl (meth)acrylate, allyl lactyl (meth)acrylate, citronellyl (meth)acrylate, geranyl (meth)acrylate, Ethylenically unsaturated monomers having two or more ethylenically unsaturated groups, such as rosinyl (meth)acrylate, cinnamyl (meth)acrylate, diallyl maleate, diaryl itaconic acid, vinyl (meth)acrylate, vinyl crotonate, vinyl oleate, vinyl linoleate, 2-(2'-vinyloxyethoxy)ethyl (meth)acrylate, ethylene glycol di(meth)acrylate, triethylene glycol (meth)acrylate, tetraethylene glycol (meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, 1,1,1-trishydroxymethylethane diacrylate, 1,1,1-trishydroxymethylethane triacrylate, 1,1,1-trishydroxymethylpropane triacrylate, divinylbenzene, divinyl adipate, diallyl isophthalate, diallyl phthalate, and diallyl maleate;Examples of the ethylenically unsaturated monomer include alkoxysilyl group-containing ethylenically unsaturated monomers such as γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropyltriethoxysilane, γ-methacryloxypropyltributoxysilane, γ-methacryloxypropylmethyldimethoxysilane, γ-methacryloxypropylmethyldiethoxysilane, γ-acryloxypropyltrimethoxysilane, γ-acryloxypropyltriethoxysilane, γ-acryloxypropylmethyldimethoxysilane, γ-methacryloxymethyltrimethoxysilane, γ-acryloxymethyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltributoxysilane, and vinylmethyldimethoxysilane; and methylol group-containing ethylenically unsaturated monomers such as N-methylol(meth)acrylamide, N,N-dimethylol(meth)acrylamide, and alkyl etherified N-methylol(meth)acrylamide. These monomers may be used alone or in combination of two or more.

[0024] The resin fine particles (A) may have a reactive group for forming crosslinks, and in order to obtain such resin fine particles (A), an ethylenically unsaturated monomer having a reactive group may be used as the ethylenically unsaturated monomer (a). The resin fine particles (A) having reactive groups can introduce crosslinks into the colloidal crystal layer, further improving the abrasion resistance and solvent resistance of the pattern portion in gravure printing. Also, the resin fine particles (A) having reactive groups can introduce crosslinks between the colloidal crystal layer and a primer layer described below, further improving the conformability to the substrate and the abrasion resistance.

[0025] Crosslinking of the colloidal crystal layer can be introduced by a method of reacting reactive groups of the resin fine particles (A) with each other, a method of reacting reactive groups of the resin fine particles (A) with each other via a polyfunctional crosslinking agent, etc. Crosslinking between the colloidal crystal layer and a primer layer described below can be introduced by a method of reacting reactive groups of the resin fine particles (A) with reactive groups of the primer layer, a method of crosslinking reactive groups of the resin fine particles (A) with reactive groups of the primer layer via a polyfunctional crosslinking agent, etc.

[0026] The reactive group that the resin fine particles (A) may have is preferably an epoxy group, a carboxy group, a hydroxyl group, a ketone group, a hydrazide group, etc., and more preferably a ketone group. In particular, when the reactive group is a ketone group and the crosslinking agent is a hydrazide crosslinking agent, a ketone-hydrazide crosslinking can be formed. The ketone-hydrazide crosslinking is preferably used because it does not adversely affect the physical properties of colloidal crystals and can form crosslinks at low temperatures and in a short time by volatilization of water, and is effective when using a film substrate that is easily damaged by heating. In addition, since the ketone group is highly hydrophilic, when an ethylenically unsaturated monomer having a ketone group is used in the copolymerization composition, the ketone group is introduced to the outside of the resin fine particles (A), i.e., near the interface with the aqueous medium, and is considered to be able to efficiently form crosslinks with the hydrazide crosslinking agent.

[0027] When the resin fine particles (A) have a ketone group, the content of the ketone group is preferably in the range of 0.05 to 0.3 mmol / g based on the mass of the resin fine particles (A). By incorporating the ketone group in the range of 0.05 to 0.3 mmol / g, the film strength of the colloidal crystal layer is improved and the abrasion resistance is improved without adversely affecting the color development.

[0028] [Radical polymerization initiator] In the polymerization reaction of the ethylenically unsaturated monomer (a), it is preferable to use a radical polymerization initiator. As the radical polymerization initiator, a known oil-soluble polymerization initiator or water-soluble polymerization initiator can be used, and these may be used alone or in combination of two or more kinds.

[0029] The oil-soluble polymerization initiator is not particularly limited, and examples thereof include organic peroxides such as benzoyl peroxide, tert-butyl peroxybenzoate, tert-butyl hydroperoxide, tert-butyl peroxy(2-ethylhexanoate), tert-butylperoxy-3,5,5-trimethylhexanoate, and di-tert-butyl peroxide; and azobis compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis-2,4-dimethylvaleronitrile, 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), and 1,1'-azobis-cyclohexane-1-carbonitrile. In the emulsion polymerization, it is preferable to use a water-soluble polymerization initiator. As the water-soluble polymerization initiator, for example, conventionally known ones such as ammonium persulfate (APS), potassium persulfate (KPS), hydrogen peroxide, and 2,2'-azobis(2-methylpropionamidine) dihydrochloride can be suitably used.

[0030] [Surfactants] When the resin microparticles (A) are produced by emulsion polymerization, surfactants such as low molecular weight surfactants and polymer dispersants can be used. By using a surfactant, the stability and monodispersibility of the resin microparticles can be improved. From the viewpoint of excellent monodispersibility of the resin microparticles, a low molecular weight surfactant is preferable as the surfactant. The low molecular weight surfactant may be anionic or nonionic, more specifically, anionic reactive surfactant, anionic nonreactive surfactant, nonionic reactive surfactant, nonionic nonreactive surfactant, preferably anionic surfactant. These surfactants may be used alone or in combination of two or more.

[0031] Here, the reactive surfactant refers to one that can polymerize with the above-mentioned ethylenically unsaturated monomer. More specifically, it refers to one that has a reactive group that can polymerize with an ethylenically unsaturated bond. Here, examples of the reactive group include alkenyl groups such as vinyl groups, allyl groups, and 1-propenyl groups, and (meth)acryloyl groups. The use of a reactive surfactant is preferable because it reduces free emulsifier components that adversely affect the particle arrangement and weather resistance (humidity resistance) of colloidal crystals, and further improves the color development of the colloidal crystals.

[0032] (anionic surfactant) Examples of the anionic reactive surfactant include polyoxyethylene alkyl ether sulfates (commercially available products include Aqualon KH-05, KH-10, and KH-20 manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., Adeka Reasoap SR-10N and SR-20N manufactured by ADEKA Corporation, and Latemul PD-104 manufactured by Kao Corporation); polyoxyalkylene styrenated phenyl ether sulfates (commercially available products include Aqualon AR-10 and AR-20 manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.); and sulfosuccinates (commercially available products include Latemul S- manufactured by Kao Corporation). 120, S-120A, S-180P, S-180A, Eleminol JS-2 manufactured by Sanyo Chemical Industries, Ltd., etc.); polyoxyethylene alkylphenyl ether sulfates or polyoxyethylene alkylphenyl ester sulfates (commercially available products include Aqualon HS-10, HS-20, HS-30, BC-10, BC-20 manufactured by Daiichi Kogyo Seiyaku Co., Ltd., Adeka Reasoap SDX-222, SDX-223, SDX-232, SDX-233, SDX-259, SE-10N, SE-20N manufactured by ADEKA Corporation, etc.); (meth)acrylates sulfate ester-based (commercially available products include Antox MS-60 and MS-2N manufactured by Japan Surfactant Co., Ltd., and Eleminol RS-30 manufactured by Sanyo Chemical Industries, Ltd.); and phosphate ester-based (commercially available products include H-3330PL manufactured by Daiichi Kogyo Seiyaku Co., Ltd., and Adeka Reasop PP-70 manufactured by ADEKA Corporation).

[0033] Examples of anionic non-reactive surfactants include higher fatty acid salts such as sodium oleate; alkylarylsulfonates such as sodium dodecylbenzenesulfonate; alkyl sulfate ester salts such as sodium lauryl sulfate; and polyoxyethylene alkyl ether sulfates such as sodium polyoxyethylene lauryl ether sulfate (commercially available products include Hitenol LA-10, LA-12, LA-16, etc., manufactured by Daiichi Kogyo Seiyaku).

[0034] (Nonionic surfactant) Examples of nonionic reactive surfactants include polyoxyalkylene alkyl ethers (commercially available products include ADEKA REASOAP ER-10 (HLB 12.3), ER-20 (HLB 15.1), ER-30 (HLB 16.4), and ER-40 (HLB 17.1), manufactured by ADEKA CORPORATION, and LATEMURU PD-420 (HLB 12.6), PD-430 (HLB 14.4), and PD-450 (HLB 16.2), manufactured by Kao Corporation; polyoxyalkylene styrenated phenyl ethers (commercially available products include AQUALON AN-10 (HLB 13.0), AN-20 (HLB 18.0), manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.; and polyoxyethylene alkyl phenyl ethers (commercially available products include AQUALON RN-20 (HLB 14.2), RN-30 (HLB 16.7), manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.).

[0035] Examples of nonionic non-reactive surfactants include polyoxyalkylene alkyl ethers (commercially available products include Noigen XL-50 (HLB 11.6), XL-100 (HLB 14.7), XL-1000 (HLB 19.3), TDS-50 (HLB 10.5), TDS-70 (HLB 12.1), TDS-80 (HLB 13.3), TDS-120 (HLB 14.8), Noigen TDX-80 (HLB 13.1), TDX-140 (HLB 14.4), and Emulgen 106 (HLB 10.5), 108 (HLB 12.1), 1108 (HLB 13.5), and 1135S-7, all manufactured by Daiichi Kogyo Seiyaku Co., Ltd. 0 (HLB 17.9), etc.; polyoxyalkylene styrenated phenyl ethers (commercially available products include Noigen EA-87 (HLB 87), EA-127 (HLB 11.7), EA-157 (HLB 14.3), and Kao Corporation's Emulgen A-60 (HLB 12.8), A-90 (HLB 14.5), and A-500 (HLB 18.0), etc.); polyoxyethylene alkyl phenyl ethers (commercially available products include Aoki Oil Industries Co., Ltd.'s Brannow N-505 (HLB 10.0), Brannow NK-8055 (HLB 10.8), etc.); polyglycerin fatty acid esters (commercially available products include Nikko Chemicals Co., Ltd.'s NIKKOL Hexaglyn1-L (HLB14.5), Decaglyn-1-L (HLB15.5), Decaglyn-1-M (HLB14.0), Decaglyn-1-LN (HLB12.0), etc.; polyoxyethylene glycerin fatty acid esters (commercially available products include NIKKOL TMGS-5V (HLB9.5), TMGS-15V (HLB13.5), TMGO-5 (HLB9.5), TMGO-15 (HLB14.5), etc., manufactured by Nikko Chemicals; polyoxyethylene sorbitan fatty acid esters (commercially available products include NIKKOL TL-10 (HLB 16.9), TP-10EX (HLB 15.6), TS-10V (HLB 14.9), TS-30V (HLB 10.5), TO-10V (HLB 15.0), TO-106V (HLB 10.0), Kao Leodor TW-L120 (HLB 16.7), TW-L106 (HLB 13.3), TW-P120 (HLB 15.6), TW-S120V (HLB 14.9), TW-S-106 (HLB 9.5), TW-O-106 (HLB 10.0); polyoxyethylene sorbitol fatty acid esters (commercially available products include NIKKOL GL-1 (HLB 15.5), GS-460 (HLB 13.0), GO-440V (HLB 12.5), and GO-460V (HLB 14.0) manufactured by Nikko Chemicals Co., Ltd., and Rheodol 430V (HLB 10.5), 440V (HLB 11.8), and 460V (HLB 13.8) manufactured by Kao Corporation; polyethylene glycol fatty acid esters (commercially available products include EMALEX-810 (HLB 11.0), 820 (HLB 14.0), 830 (HLB 15.0), and 840 (HLB 16.0) manufactured by Nippon Emulsion Co., Ltd., and EMANON 1112 (HLB 13.7), EMANON 31 (HLB 15.0), and EMANON 41 (HLB 16.0) manufactured by Kao Corporation); 99V (HLB 19.4), etc.; sucrose fatty acid esters (commercially available products include Mitsubishi Chemical Foods' S-970 (HLB 9.0), S-1170 (HLB 11.0), S-1570 (HLB 15.0), S-1670 (HLB 16.0), P=1570 (HLB 15.0), P-1670 (HLB 16.0), M-1695 (HLB 16.0), O-1570 (HLB 15.0), L-1695 (HLB 16.0), LWA-1570 (HLB 15.0), etc.); polyoxyethylene lanolins (commercially available products include Nikko Chemicals' NIKKOL TW-10 (HLB 12.0), TW-20 (HLB 13.0), BWA-5 (HLB 12.5), BWA-10 (HLB 15.5), BWA-20 (HLB 16.0), etc.; polyoxyethylene hydrogenated castor oils (commercially available products include NIKKOL HCO-20 (HLB 10.5), HCO-30 (HLB 11.0), HCO-40 (HLB-12.5), HCO-100 (HLB 16.5), etc., manufactured by Nikko Chemicals; polyoxyethylene sterols (commercially available products include NIKKOL HCO-20 (HLB 10.5), HCO-30 (HLB 11.0), HCO-40 (HLB-12.5), HCO-100 (HLB 16.5), etc., manufactured by Nikko Chemicals; Examples of such compounds include BPS-5 (HLB 9.5), BPS-10 (HLB 12.5), BPS-20 (HLB-30), and BPSH-25 (HLB 14.5); acetylenes (commercially available products include SURFYNOL 420 (HLB 4.0) manufactured by Evonik); and siloxanes (commercially available products include KF-351A (HLB 12.0) manufactured by Shin-Etsu Silicone Co., Ltd.).

[0036] (Polymer dispersant) Examples of the polymer dispersing agent include polyvinyl alcohol, polyvinylpyrrolidone, polyoxyethylene-polyoxypropylene block copolymers, (meth)acrylic acid-(meth)acrylic acid alkyl ester copolymers, styrene-(meth)acrylic acid-(meth)acrylic acid alkyl ester copolymers, styrene-(meth)acrylic acid copolymers, maleic acid-(meth)acrylic acid alkyl ester copolymers, styrene-maleic acid copolymers, styrene-maleic acid copolymers, styrene-maleic acid-(meth)acrylic acid alkyl ester copolymers, styrene-maleic acid half ester copolymers, vinylnaphthalene-(meth)acrylic acid copolymers, vinylnaphthalene-maleic acid copolymers, vinylpyrrolidone-(meth)acrylic acid alkyl ester copolymers, vinylpyrrolidone-styrene copolymers, vinylpyrrolidone-vinyl acetate copolymers, vinyl acetate-crotonic acid copolymers, vinyl acetate-(meth)acrylic water-soluble vinyl copolymers such as vinyl acetate-crotonic acid copolymer, polyvinyl sulfonic acid, sodium polyvinyl sulfonate, polystyrene sulfonic acid, sodium polystyrene sulfonate (Polynas PS-1, Polynas PS-5, etc., manufactured by Tosoh Corporation), styrene sulfonic acid-maleic acid copolymer, polyitaconic acid, polyhydroxyethyl (meth)acrylate, poly(meth)acrylamide, (meth)acrylamide-(meth)acrylic acid copolymer, polyvinyl methyl ether, methyl vinyl ester, and carboxyvinyl polymer; water-soluble polyurethane resins which are urethane resins obtained by a polyaddition reaction of polyisocyanate and polyol, and in which the entire resin is made water-soluble by the introduction of hydrophilic groups; and water-soluble polyester resins which are polyester resins obtained by a polycondensation reaction of polycarboxylic acid and polyol, and in which the entire resin is made water-soluble by the introduction of hydrophilic groups.

[0037] When the resin microparticles (A) are produced by emulsion polymerization, the emulsion polymerization may be a two-stage polymerization in which the monomer composition is changed between the first and second stages and then dropped, or a multi-stage polymerization in which the monomer composition is changed in three or more stages and then dropped. For example, the resin microparticles can be produced by the following procedure. (1) First, an aqueous medium and a surfactant are charged into a reaction vessel and the temperature is raised. Then, a radical polymerization initiator is added while an emulsion of an ethylenically unsaturated monomer is dropped under a nitrogen atmosphere. After the reaction starts, the particles gradually grow according to the amount of the drop.

[0038] The refractive index of the resin fine particles (A) is preferably 1.45 or more, more preferably 1.45 to 3.00, and further preferably 1.45 to 2.00. When the refractive index is 1.45 or more, the color development property of the colloidal crystal becomes good, which is preferable.

[0039] The content of the resin fine particles (A) is preferably 20 to 60% by mass, more preferably 35 to 50% by mass, based on the total mass of the composition for colloidal crystals. When the content of the resin fine particles (A) is within this range, the resin fine particles (A) are well ordered and the composition for colloidal crystals has good leveling properties.

[0040] <Water> The composition for colloidal crystals of the present invention contains water. Water may be included when the resin fine particles are obtained as a dispersion, or may be added by mixing with a hydrophilic solvent (B) described below, or both. The water content is preferably 40 to 70 mass %, more preferably 50 to 60 mass %, based on the total mass of the composition for colloidal crystals. When the water content is within this range, the resin fine particles (A) are well ordered, and the composition for colloidal crystals has appropriate leveling properties.

[0041] <Hydrophilic Solvent (B)> The composition for colloidal crystals of the present invention preferably contains a hydrophilic solvent as a liquid medium other than water, and more preferably contains a hydrophilic solvent (B) having a boiling point of 95 to 250°C at 1 atmospheric pressure. When the boiling point is 95°C or higher, rapid drying of the composition for colloidal crystals is prevented during gravure printing, and at the same time, the leveling ability on the substrate is improved. Furthermore, by delaying the drying of the composition for colloidal crystals, the re-dissolving ability of the composition for colloidal crystals when printed is increased. By making the boiling point 250° C. or less, the amount of residual solvent is reduced, and adverse effects on color development, such as swelling of particles due to the residual solvent, are prevented. The boiling point of the hydrophilic solvent (B) is more preferably in the range of 100 to 240°C.

[0042] Examples of the hydrophilic solvent (B) include monohydric lower alcohol solvents such as 1-propanol (bp 97°C), 1-butanol (bp 118°C), 2-methyl-1-propanol (bp 108°C), and 2-butanol (bp 100°C); ethylene glycol (bp 197.0°C), 1,3-propanediol (bp 230°C), propylene glycol (bp 188°C), 1,2-butanediol (bp 192°C), 1,4-butanediol (bp 230°C), pentylene glycol (bp 188°C), and 1,2-hexyl alcohol (bp 188°C). Glycol solvents such as Sandiol (bp 230°C), 1,6-hexanediol (bp 208°C), and diethylene glycol (bp 245°C); ethylene glycol monomethyl ether (bp 124°C), diethylene glycol monomethyl ether (bp 194°C), triethylene glycol monoethyl ether (bp 249°C), ethylene glycol monoethyl ether (bp 134°C), diethylene glycol monoethyl ether (bp 202°C), ethylene glycol monoisopropyl ether (bp 144°C), diethylene glycol monoisopropyl ether (bp 230°C), ethylene glycol monobutyl ether (bp 171°C), diethylene glycol monobutyl ether (bp 230°C), ethylene glycol monoisobutyl ether (bp 160°C), ethylene glycol monohexyl ether (bp 208°C), diethylene glycol dimethyl ether (bp 162°C), triethylene glycol dimethyl ether (bp 216°C), and propylene glycol monomethyl ether glycol ether solvents such as propylene glycol monomethyl ether (bp 120°C), dipropylene glycol dimethyl ether (bp 194°C), tripropylene glycol monomethyl ether (bp 243°C); lactam solvents such as N-methyl-2-pyrrolidone (bp 202°C), N-hydroxyethyl-2-pyrrolidone (bp 175°C), 2-pyrrolidone (bp 245°C); formamide (bp 210°C), 3-methoxy-N,N-dimethylpropionamide (bp215°C), 3-butoxy-N,N-dimethylpropanamide (bp 252°C), and other amide solvents. These hydrophilic solvents (B) may be used alone or in combination of two or more.

[0043] Among the above solvents, the hydrophilic solvent (B) is preferably at least one selected from the group consisting of monohydric lower alcohol solvents, glycol solvents, and glycol ether solvents. By including such a hydrophilic solvent, the leveling property of the composition for colloidal crystals and the re-dissolving property when printing the composition for colloidal crystals are improved.

[0044] The content of the hydrophilic solvent (B) is preferably in the range of 0.5 to 30 mass %, and more preferably in the range of 2 to 20 mass %, based on the total mass of the composition for colloidal crystals. When the content of the hydrophilic solvent (B) is in the above range, the leveling property of the composition for colloidal crystals and the re-dissolving property when the composition for colloidal crystals is printed are improved without affecting the ordered arrangement of the resin fine particles (A).

[0045] [Nonionic surfactants (C)] The composition for colloidal crystals of the present invention preferably contains a nonionic surfactant (C) having an HLB value of 3.0 to 15.0. By containing the nonionic surfactant (C), the fluidity of the composition for colloidal crystals is improved, and thus the resolubility is improved. By the nonionic surfactant (C) having an HLB value of 3.0 or more, the composition has excellent solubility in water and excellent leveling properties with respect to the substrate. In addition, there are no adverse effects such as disrupting the regular arrangement of the resin fine particles (A) or swelling of the resin fine particles (A) by the surfactant. This allows the composition to exhibit excellent printability and color development. By having an HLB value of 15.0 or less, the surface tension of the composition for colloidal crystals is lowered to an appropriate range.

[0046] The HLB value is a numerical representation of the hydrophilicity and lipophilicity of a material, and the smaller the HLB value, the higher the lipophilicity. In this specification, the HLB value is calculated by the Griffin method shown in the following formula (1). Formula (1) HLB value = 20 x (sum of formula weights of hydrophilic parts) ÷ (molecular weight of material)

[0047] As the nonionic surfactant (C), those having an HLB value of 3.0 to 15.0 as mentioned above in the section (Nonionic Surfactants) can be used. The nonionic surfactant (C) is preferably at least one selected from the group consisting of polyoxyalkylene alkyl ether surfactants, polyglycerol fatty acid ester surfactants, acetylene surfactants, and siloxane surfactants. By including such a surfactant, the resolubility of the composition for colloidal crystals is improved.

[0048] It is important that the content of the nonionic surfactant (C) is in the range of 0.5 to 5 mass % based on the total mass of the composition for colloidal crystals, and more preferably in the range of 0.5 to 1.5 mass %. When the content of the nonionic surfactant (C) is in such a range, the resolubility of the composition for colloidal crystals is improved without affecting the regular arrangement of the resin fine particles (A).

[0049] The composition for colloidal crystals of the present invention similarly exhibits the excellent effects of the present invention even when it contains both the hydrophilic solvent (B) and the nonionic surfactant (C).

[0050] <Thixotropy index (TI value)> The thixotropy index (TI value) can be calculated by dividing the viscosity (mPa·s) at 6 rpm measured with an E-type viscometer under 25°C conditions by the viscosity (mPa·s) at 60 rpm. The thixotropy index can be adjusted by selecting additives and appropriate solvents. When the thixotropy is weak, the viscosity becomes closer to Newtonian. It is important that the composition for colloidal crystals of the present invention has a TI value measured with an E-type viscometer of 1.00 to 2.00, preferably 1.00 to 1.60, and more preferably 1.00 to 1.40. When the TI value is in the above range, the ink has good fluidity, and printing defects such as plate fogging and plate clogging due to reduced ink fluidity are less likely to occur.

[0051] From the viewpoint of printability, the viscosity of the composition for colloidal crystals is preferably 3.0 mPa·s to 200 mPa·s.

[0052] <Crosslinking agent> As described above, the composition for colloidal crystals of the present invention may contain a crosslinking agent in order to form crosslinks within the colloidal crystal layer and between the colloidal crystal layer and a primer layer, which will be described later. The crosslinking agent is not particularly limited and can be appropriately selected depending on the reactive groups possessed by the colloidal crystal layer and / or the primer layer. Examples of the crosslinking agent include hydrazide compounds (polyhydrazides) having two or more hydrazino groups that react with active carbonyl groups to form keto-hydrazide crosslinks; isocyanate compounds that react with hydroxyl groups or amino groups to form urethane bonds or urea bonds; and epoxy compounds that react with carboxy groups, amino groups, etc., and can be appropriately selected depending on the application. More specifically, for example, when the resin fine particles (A) and / or the component constituting the primer layer have a carboxyl group, crosslinking can be formed via an epoxy crosslinking agent. Also, for example, when the resin fine particles (A) and / or the component constituting the primer layer have a hydroxyl group, crosslinking can be formed via a polyisocyanate crosslinking agent. Also, for example, when the resin fine particles (A) and / or the component constituting the primer layer have a ketone group, crosslinking can be formed via a hydrazide crosslinking agent. As the crosslinking agent, it is preferable to use a hydrazide crosslinking agent to form a ketone-hydrazide crosslink as described above. Examples of the hydrazide crosslinking agent include adipic acid dihydrazide and a water-soluble resin modified with a polyfunctional hydrazide group.

[0053] The colloidal crystal composition may contain various additives within the range that does not impair the effects of the present invention. For example, colorless black fine particles, antifoaming agents, leveling agents, thickening agents, and preservatives may be blended.

[0054] <Printed matter and laminates> A printed matter can be obtained by printing a colloidal crystal composition on a substrate to form a colloidal crystal layer. Alternatively, for example, a primer layer, which will be described later, can be formed on a substrate, and a colloidal crystal layer can be formed on the primer layer to obtain a laminate.

[0055] The printing method for printing the composition for colloidal crystals of the present invention onto a substrate, a primer layer, etc. is not particularly limited, but suitable examples include gravure printing, flexographic printing, and inkjet printing. The composition for colloidal crystals is preferably printed by gravure printing, since the regular arrangement of colloidal particles is not hindered and color development is good.

[0056] When the composition for colloidal crystals is gravure printed, various cell types (conventional type, screen gravure type, laser type, etc.) prepared by engraving or etching can be used for gravure printing. The composition for colloidal crystals applied to the substrate by transfer can form a colloidal crystal layer by drying. There are no particular limitations on the drying method, and examples include heat drying, hot air drying, infrared drying, microwave drying, and drum drying. From the viewpoint of the effect on the regular arrangement of the resin fine particles (A) and productivity, the drying temperature is preferably in the range of 20 to 80°C.

[0057] The thickness of the colloidal crystal layer in the printed matter is preferably in the range of 1.0 to 20 μm. By being in the above range, excellent printability and color development are sufficiently ensured, and a printed matter having excellent substrate conformability, abrasion resistance, and solvent resistance can be obtained.

[0058] <Base material> The substrate is not particularly limited and can be appropriately selected depending on the application. Examples of the substrate include thermoplastic resin substrates such as polyvinyl chloride sheet, polyethylene terephthalate (PET) film, polypropylene film, polyethylene film, nylon film, polystyrene film, and polyvinyl alcohol film; metal substrates such as aluminum foil; glass substrates, paper substrates such as coated paper, and cloth substrates.

[0059] The substrate may have a smooth or uneven coating surface. The substrate may be transparent, semi-transparent, or opaque, and a substrate that has been colored in advance, such as black, may be used to make the color of the colloidal crystal coating film more distinct. The substrate may be one type alone, or may be a laminate of two or more types of substrates bonded together.

[0060] <Primer layer> When printing the colloidal crystal composition, it may be printed directly on the substrate, or a primer layer may be provided on the substrate and printed on the primer layer. However, in order to further increase the fixation of the colloidal crystal layer on the substrate, it is preferable to print on the primer layer. The primer layer can be formed, for example, by applying a primer layer forming composition on the substrate in advance. The primer layer forming composition is not particularly limited, and examples thereof include acrylic resin, styrene acrylic resin, urethane resin, olefin resin, polyester resin, and composite resins obtained by compounding these resins. These resins may be used alone or in combination of two or more. From the viewpoints of excellent adhesion to the substrate and colloidal crystal layer, resistance of the primer layer, etc., the composition for forming the primer layer preferably contains one or more resins selected from the group consisting of acrylic resins, styrene acrylic resins, and urethane resins.

[0061] The primer layer may contain additives as long as the effects of the present invention are not impaired. Examples of such additives include surfactants, achromatic black fine particles, and neutralizing amines. Examples of surfactants are as described above. The primer layer may further include The primer may contain fatty acid amide and / or silica particles as an anti-blocking agent for preventing blocking (sticking) between primers.

[0062] <Thermal recording medium> A printed matter comprising a colloidal crystal layer made of a substrate and the composition for colloidal crystals of the present invention, or a laminate further comprising a primer layer or the like, is characterized in that the particles in the colloidal crystal layer dissolve and become fluid upon heat treatment, filling in voids. This causes the color of the colloidal crystal layer to fade and produce a clear change in color, and the printed matter or laminate can therefore be used as a thermal recording medium. The heat treatment method can be appropriately selected as long as it does not impair the effects of the present invention, and examples of the heat treatment method include a method in which a thermal head of a thermal printer is applied to the laminate to heat it; a method in which laser light is irradiated to cause the photothermal conversion material in the laminate to absorb the light and heat adjacent resin particles; oven heating, microwave heating, and boiling treatment.

[0063] Among them, image formation by laser is preferred because it can form an image without damaging the substrate, the resin layer, or the non-image forming area. In addition, it is preferred to use an infrared laser because it has little adverse effect on the substrate, the resin forming the primer layer, and the resin particles. Examples of infrared laser markers include CO2 laser markers (wavelength 10600 nm), YVO4 laser markers (wavelength 1064 nm), YAG laser markers (wavelength 1064 nm), and fiber laser markers (wavelength 1090 nm).

[0064] (Photothermal conversion materials) When the laminate is irradiated with laser light, the photothermal conversion material absorbs the laser light, converts it into heat, and promotes heating of the resin particles in the adjacent colloidal crystal layer. Examples of photothermal conversion materials include organic materials, inorganic materials, and carbon materials that have an absorption range in the infrared region. EXAMPLES

[0065] The present invention will be described below with reference to examples, but the present invention is not limited thereto. In the examples and comparative examples, "parts" and "%" mean "parts by mass" and "% by mass" unless otherwise specified.

[0066] <Thixotropy index (TI value)> The thixotropy index (TI value) of the composition for colloidal crystals was calculated from the viscosity (mPa·s) at 6 rpm measured with an E-type viscometer at 25°C divided by the viscosity (mPa·s) at 60 rpm.

[0067] <Average particle size, Cv value> The average particle size was measured by diluting the microparticle dispersion 500 times with water and measuring about 5 ml of the diluted solution using a dynamic light scattering measurement method (measuring device manufactured by Nanotrack UPA Co., Ltd., Microtrack Bell Co., Ltd.). The peak of the volumetric particle size distribution data (histogram) obtained at this time was taken as the average particle size. In addition, the coefficient of variation Cv value, which represents the uniformity of the particle size, was calculated using the following formula. Formula: Cv value (%) = standard deviation of particle size / average particle size x 100 [In the formula, the units of standard deviation and average particle size are the same]

[0068] <Preparation of Resin Fine Particle (A) Dispersion> [Production Example 1] 79.0 parts of styrene, 20.0 parts of isobornyl methacrylate, 1.0 parts of acrylic acid, 4.0 parts of 25% aqueous solution of Aqualon AR-10 (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., anionic reactive surfactant (polyoxyethylene styrenated phenyl ether sulfate salts) (solid content 1.0 part), and 39.0 parts of ion-exchanged water were mixed and stirred to prepare an emulsion of ethylenically unsaturated monomers in the first stage. 95.0 parts of ion-exchanged water and 1.5% of the emulsion in the first stage were added to a reaction vessel equipped with a stirrer, thermometer, dropping funnel, and reflux condenser. The internal temperature of the reaction vessel was raised to 70°C and sufficiently replaced with nitrogen, and then 6.0 parts of a 2.5% aqueous solution of potassium persulfate (solid content 0.15 parts) was added as an initiator to start polymerization. The internal temperature was raised to 80° C. and while maintaining the temperature, the remainder of the emulsion and 4.2 parts of a 2.5% aqueous solution of potassium persulfate (solid content 0.11 part) were added dropwise over 2 hours to react them, synthesizing core particles. Next, 27.6 parts of styrene, 13.2 parts of n-butyl acrylate, 2.2 parts of methacrylic acid, 1.7 parts of 25% aqueous solution of Aqualon AR-10 (0.4 parts solids), and 16.7 parts of ion-exchanged water were mixed and stirred to prepare the second stage emulsion of ethylenically unsaturated monomer. 20 minutes after the completion of the first stage dripping, the dripping of the second stage emulsion was started. While maintaining the internal temperature at 80°C, the reaction was allowed to proceed while dripping the second stage emulsion and 1.6 parts of a 2.5% aqueous solution of potassium persulfate (0.04 parts solids) over 2 hours, to obtain an aqueous dispersion of resin fine particles. After the reaction, water was added to adjust the solid content to 45.0%. Then, 1.7 parts of 25% ammonia water (NH3(aq)) was added to neutralize the resin particles, and an aqueous dispersion of resin particles (A-1) was obtained. The average particle size of the obtained resin particles was 248 nm, and the Cv value was 12.9%.

[0069] [Production Example 2] A reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, and a reflux condenser was charged with 68.9 parts of water. Next, 3% of an emulsion of ethylenically unsaturated monomers, which had been previously prepared by mixing and stirring 80.0 parts of methyl methacrylate, 9.0 parts of n-butyl methacrylate, 8.0 parts of 2-ethylhexyl acrylate, 1.0 parts of acrylic acid, 1.0 parts of diacetone acrylamide, 1.0 parts of 3-methacryloxypropyltriethoxysilane, 5.0 parts of a 20% aqueous solution of Aqualon KH-10 (Dai-ichi Kogyo Seiyaku, an anionic reactive surfactant of polyoxyethylene alkyl ether sulfate salt), and 40.4 parts of water, was further added to the reaction vessel. After the internal temperature of the reaction vessel was raised to 70°C and the atmosphere was fully replaced with nitrogen, 2.0 parts of a 5% aqueous solution of potassium persulfate was added as an initiator to initiate emulsion polymerization. The internal temperature was raised to 80°C, and while maintaining the temperature, the remaining emulsion of ethylenically unsaturated monomer and 2.0 parts of a 5% aqueous solution of potassium persulfate were added dropwise over 3 hours, and the mixture was allowed to react for another 4 hours. The solid content was then adjusted to 45.0% with water, and an aqueous dispersion of resin fine particles (A-2) was obtained. The average particle size of the obtained resin fine particles was 201 nm, and the Cv value was 25.8%.

[0070] [Production Example 3] A reaction vessel equipped with a stirrer, a thermometer, a dropping funnel, and a reflux condenser was charged with 95.0 parts of water. Next, 1.5% of the emulsion of ethylenically unsaturated monomers in the first stage, which had been separately prepared by mixing and stirring 97.0 parts of styrene, 2.0 parts of acrylic acid, 1.0 part of 3-methacryloxypropyltrimethoxysilane, 5.0 parts of a 20% aqueous solution of Aqualon KH-10, and 39.1 parts of water, was further added to the reaction vessel. After the internal temperature of the reaction vessel was raised to 70°C and the vessel was thoroughly purged with nitrogen, 5.7 parts of a 2.5% aqueous solution of potassium persulfate was added as an initiator to initiate polymerization. The internal temperature was raised to 80°C and while maintaining the temperature, the remaining emulsion of the ethylenically unsaturated monomer from the first stage was reacted with 4.0 parts of a 2.5% aqueous solution of potassium persulfate while being added dropwise over a period of 2 hours to synthesize particles. 20 minutes after the completion of the first drop, the drop of the emulsion of the ethylenically unsaturated monomer of the second step, which was prepared by mixing and stirring 15.0 parts of methyl methacrylate, 23.1 parts of n-butyl acrylate, 0.9 parts of acrylic acid, 2.1 parts of a 20% aqueous solution of Aqualon KH-10, and 16.8 parts of water, was started. The reaction was further advanced while dropping the emulsion of the ethylenically unsaturated monomer of the second step and 2.1 parts of a 2.5% aqueous solution of potassium persulfate over 2 hours while keeping the internal temperature at 80°C, and water was added to adjust the solid content concentration to 45.0%, to obtain an aqueous dispersion of resin fine particles (A-3). The average particle diameter of the obtained resin fine particles was 255 nm, and the Cv value was 26.1%.

[0071] [Production Example 4] <Production of Resin for Primer Layer> 30.7 parts of styrene, 64.2 parts of n-butyl acrylate, 5.0 parts of methacrylic acid, 5.6 parts of 25% aqueous solution of Aqualon AR-10 (1.4 parts solids), and 40.4 parts of ion-exchanged water were mixed and stirred in advance to prepare an emulsion of ethylenically unsaturated monomers. 68.9 parts of ion-exchanged water and 3% of the emulsion were added to a reaction vessel equipped with a stirrer, thermometer, dropping funnel, and reflux condenser, and the internal temperature was raised to 80°C and sufficiently replaced with nitrogen, after which 6.0 parts of a 2.5% aqueous solution of potassium persulfate (0.15 parts solids) was added as an initiator to start emulsion polymerization. While maintaining the internal temperature at 80°C, the remaining emulsion and 6.0 parts of a 2.5% aqueous solution of potassium persulfate (0.15 parts solids) were dropped over 3 hours, and the mixture was allowed to react for another 4 hours to obtain an aqueous dispersion of styrene-acrylic resin. After the reaction was completed, 3.9 parts of 25% ammonia water was added for neutralization, and the solid content of the aqueous dispersion was adjusted to 45.0% with ion-exchanged water to obtain an aqueous dispersion of styrene-acrylic resin.

[0072] <Preparation of primer layer-forming composition> [Production Example 5] A primer layer-forming composition was prepared by adding 1.0 part of Emulgen 1108 (manufactured by Kao Corporation, an ether-based nonionic surfactant) as a surfactant to 100.0 parts of the styrene-acrylic resin water dispersion of Production Example 4 and stirring the mixture.

[0073] The abbreviations in Table 1 stand for the following: Silica: Water dispersion of KE-P30 (spherical silica fine particle powder) (manufactured by Nippon Shokubai Co., Ltd.) Solids concentration 35 wt.% (solvent: water) Particle size 0.3 μm Emulgen 1108: Kao Corporation polyoxyalkylene alkyl ether surfactant Noigen XL-1000: Polyoxyalkylene alkyl ether surfactant manufactured by Daiichi Kogyo Seiyaku Co., Ltd. Emulgen 1135S-70: Kao Corporation polyoxyalkylene alkyl ether surfactant Hexaglyn1-L: Polyglycerin fatty acid ester surfactant manufactured by Nikko Chemicals Decaglyn 1-L: Polyglycerin fatty acid ester surfactant manufactured by Nikko Chemicals SURFYNOL420: Evonik acetylene surfactant KF-351A: Siloxane surfactant manufactured by Shin-Etsu Silicone Co., Ltd. Noigen EA-87: Polyoxyethylene styrenated phenyl ether surfactant manufactured by Daiichi Kogyo Seiyaku Co., Ltd. SN Thickener 612: Thickener manufactured by San Nopco Ltd.

[0074] [Example 1] The composition for forming the primer layer prepared in Production Example 5 was applied to the corona-treated surface of a biaxially oriented polypropylene (OPP) film (Futamura FOR, thickness 20 μm) using a bar coater so that the thickness after drying would be 2 μm, and then dried in an oven at 80°C for 3 minutes to form a primer layer. Furthermore, a gravure cylinder (engraving method: helio, cell shape: compressed, number of lines: 70 lines / cm) made by Toyo FPP was set in a simple gravure coater (Nissho Gravure GRAVO-PROOF MINI), and the aqueous dispersion of the resin fine particles (A-1) from Production Example 1 was printed on the primer layer of the film substrate having a primer layer, and then dried in an oven at 50°C for 3 minutes to obtain a laminate with a printed pattern. The thickness of the colloidal crystal layer was 5 μm.

[0075] [Examples 2 to 3] A laminate including a colloidal crystal layer made of a composition for colloidal crystals was produced in the same manner as in Example 1, except that the materials were changed as shown in Table 1.

[0076] [Example 4] 5.0 parts of ethanol was added to 95 parts of the aqueous dispersion of the resin fine particles (A-1) of Production Example 1 and stirred to prepare a composition for colloidal crystals. Then, the resin composition for primer layer prepared in Production Example 5 was applied to the corona-treated surface of a biaxially oriented polypropylene (OPP) film (Futamura FOR, thickness 20 μm) using a bar coater so that the thickness after drying would be 2 μm, and then dried in an oven at 80°C for 3 minutes to form a primer layer. Furthermore, a gravure cylinder (engraving method: helio, cell shape: compressed, number of lines: 70 lines / cm) made by Toyo FPP was set in a simple gravure coater (Nissho Gravure GRAVO-PROOF MINI), and the above composition for colloidal crystals was printed on the primer layer of the film substrate having a primer layer, and dried in an oven at 50°C for 3 minutes to obtain a laminate with a printed pattern. The thickness of the colloidal crystal layer was 5 μm.

[0077] [Examples 5 to 28, Comparative Examples 1 to 9] Except for changing the blending composition to that shown in Table 1, compositions for colloidal crystals were prepared in the same manner as in Example 4. Thereafter, using the compositions for colloidal crystals, laminates having colloidal crystal layers were produced in the same manner as in Example 4.

[0078] The obtained compositions for colloidal crystals and laminates having a colloidal crystal layer were evaluated as follows. The evaluation results are shown in Table 1.

[0079] [Plate jam] For the laminates obtained in the above Examples and Comparative Examples, printed areas with a dot percentage of 100% to 3% were evaluated according to the following evaluation criteria. ○: Tone reproducibility is good from the printed area with 100% dot percentage to the printed area with 3% dot percentage, and No change in size (good) △: Tone reproduction is possible from the printed area with 100% dot percentage to the printed area with 10% dot percentage, and There is a slight change in dot size (usable) ×: There is no gradation reproducibility below the print area with a dot percentage of 70%, and there is no change in dot size. (unavailable)

[0080] [Resolubility] The compositions for colloidal crystals of Examples 1 to 28 and Comparative Examples 1 to 9 were printed on OPP films using the method described in Example 1, and the plate was stopped for 30 minutes to allow the ink to dry on the plate. The plate was then run idle for 1 minute, and then printed on an OPP film, and the resolubility of the ink was evaluated based on the reproducibility of the image. ○: The image was restored within 10 seconds. (Good) △: The image recovered in more than 10 seconds but less than 20 seconds. (Usable) ×: It took more than 20 seconds to reproduce the image. (Not available)

[0081] [Color development (△R)] The reflection spectrum of the pattern portion of the laminate obtained in the above Examples and Comparative Examples was measured in the wavelength range of 250 to 850 nm using an ultraviolet-visible near-infrared spectrophotometer (V-770D manufactured by JASCO Corporation, integrating sphere unit ISN-923). The reflectance at each wavelength is a relative reflectance measured using a standard white board with a known reflectance (SRS-99-010 manufactured by Labsphere) as a reference. For the obtained reflection spectrum, the difference (ΔR) between the maximum reflectance derived from colloidal crystals and the baseline reflectance not due to colloidal crystals was calculated. The larger ΔR is, the better the color development is. The color development was evaluated according to the following criteria. ○: △R is 10% or more (good) △: △R is 5% or more and less than 10% (usable) ×: △R is less than 5% (unusable)

[0082] [Table 1]

[0083] [Table 1]

[0084] [Table 1]

[0085] From the above, the compositions for colloidal crystals of the present invention having a specified TI value had good color development, and the resolubility and degree of clogging were also at a usable level. On the other hand, the compositions of the comparative examples were all inferior in gravure printing suitability, and clogging occurred during printing.

Claims

1. A composition for colloidal crystals, comprising fine resin particles (A) and water, and having a thixotropy index (TI value) of 1.00 to 2.00 as measured by an E-type viscometer.

2. 2. The composition for colloidal crystals according to claim 1, further comprising a hydrophilic solvent (B) having a boiling point of 95 to 250° C. at 1 atmospheric pressure.

3. 3. The composition for colloidal crystals according to claim 1, further comprising a nonionic surfactant (C) having an HLB value of 3.0 to 15.

0.

4. 3. The composition for colloidal crystals according to claim 2, wherein the hydrophilic solvent (B) contains at least one solvent selected from the group consisting of monohydric lower alcohol solvents, glycol solvents, and glycol ether solvents.

5. 3. The composition for colloidal crystals according to claim 2, wherein the content of said hydrophilic solvent (B) is 0.5 to 30% by mass based on the total mass of the composition for colloidal crystals.

6. 4. The composition for colloidal crystals according to claim 3, wherein the nonionic surfactant (C) comprises at least one selected from the group consisting of polyoxyalkylene alkyl ether surfactants, polyglycerol fatty acid ester surfactants, acetylene surfactants, and siloxane surfactants.

7. 4. The composition for colloidal crystals according to claim 3, wherein the content of said nonionic surfactant (C) is 0.5 to 5% by mass based on the total mass of the composition for colloidal crystals.

8. 3. The composition for colloidal crystals according to claim 1 or 2, which is for gravure printing.

9. A printed matter comprising a substrate and a colloidal crystal layer made of the composition for colloidal crystals according to claim 1 or 2.

10. A laminate comprising a substrate, a primer layer, and a colloidal crystal layer made of the composition for colloidal crystals according to claim 1 or 2.

Citation Information

Patent Citations

  • Coating composition for forming structural color film, structural color film and method for producing the same

    JP2017223915A