Workpiece processing method and resin composition

By forming a convex pattern on workpieces to address height differences, the method reduces TTV and prevents cracking during back grinding, ensuring uniform thickness and easy peeling of the surface protection sheet.

JP2024136168APending Publication Date: 2024-10-04LINTEC CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023047178
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

The height differences on the surface of workpieces due to bump electrodes or chips protruding from the surface cause suction errors during back grinding, leading to increased Total Thickness Variation (TTV) and potential cracking or processing issues.

Method used

A method involving the formation of a convex pattern on the workpiece surface to mitigate height differences, using a surface protection sheet with specific adhesion and elongation properties to facilitate easy peeling, and a resin composition with controlled adhesive strength and tensile elongation to suppress TTV and ensure residue-free peeling.

Benefits of technology

The method effectively reduces TTV and prevents cracking by ensuring uniform thickness post-grinding, while allowing residue-free peeling of the surface protection sheet and any formed patterns.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136168000001_ABST
    Figure 2024136168000001_ABST
Patent Text Reader

Abstract

To provide a workpiece processing method capable of excellently peeling a pattern formed on a surface together with a surface protective sheet in order to suppress an influence by height difference of the surface.SOLUTION: In a workpiece including a front surface having height difference and a rear surface opposite to the front surface on which a convex pattern for suppressing an influence of the height difference of the front surface is formed, a workpiece processing method includes the steps of: attaching a surface protective sheet to the front surface of the workpiece; and peeling, from the front surface, the surface protective sheet attached to the front surface and at least a part of the convex pattern, where adhesive force at 50°C of the convex pattern to the workpiece on which a polyimide film is formed is 1000 mN / 25 mm or less.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for processing a workpiece and a resin composition. In particular, the present invention relates to a method for processing a workpiece in which a predetermined pattern formed on the surface of the workpiece can be easily peeled off from the surface together with a surface protection sheet attached to the surface, and to a resin composition suitable for forming the pattern. [Background technology]

[0002] A known method for mounting chips with circuits, such as semiconductor chips, at a high density is to bond the chip to electrodes on a substrate via bump electrodes formed on the circuit surface of the chip. The bump electrodes are convex electrodes that protrude in the thickness direction of the chip.

[0003] Such chips are obtained as workpieces by dividing a workpiece such as a wafer on which a circuit is formed. With the rapid progress of miniaturization and multi-functionalization of electronic devices on which such chips are mounted, there is a demand for chips to be smaller, thinner, and more dense. In order to reduce the size and height of a chip, it is common to form a circuit on the front surface of a wafer, and then grind the back surface of the wafer to reduce the thickness of the chip.

[0004] Another known method for mounting chips at high density is the use of chip-on-wafer (CoW), in which multiple chips smaller than the wafer are arranged on the circuit surface of a wafer to obtain a chip-on-wafer, and then the chip-on-wafer is diced to obtain stacked chips.

[0005] Even in the method using chip-on-wafer, in order to reduce the size and height of the stacked chips, it is common to grind the back surface of the wafer as a workpiece to reduce the thickness of the wafer (workpiece), and then place the chip on the wafer (workpiece).

[0006] When grinding the back surface of a workpiece, a surface protection sheet called a backgrind tape is applied to the surface of the workpiece to protect the circuits and chips arranged on the surface of the workpiece and to hold the workpiece.

[0007] Patent Document 1 discloses an adhesive tape for processing semiconductor wafers that has good conformability to the surface of semiconductor wafers having steps and protrusions and can be peeled off without damaging the semiconductor wafer or leaving any adhesive residue. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2017-171896 A Summary of the Invention [Problem to be solved by the invention]

[0009] The bump electrodes are formed to protrude from the surface of the workpiece. Also, in a chip-on-wafer, the chips arranged on the surface of the workpiece protrude from the surface of the wafer (workpiece). Therefore, on the surface of the workpiece, there is a difference in height between the area where the bump electrodes are formed or the area where the chips are arranged and the other areas.

[0010] Such a height difference is reflected as a height difference in the surface protection sheet by attaching the surface protection sheet to the surface of the work. That is, the height of the portion of the surface protection sheet corresponding to the area where the bump electrodes are formed or the area where the chips are arranged is higher than the height of the other portions. Usually, the area where the bump electrodes are formed or the area where the chips are arranged is the inner periphery of the work, and there are no bump electrodes or chips in the outer periphery surrounding the inner periphery.

[0011] When grinding the backside of a workpiece with a surface protection sheet attached, the surface (front side) of the workpiece to which the surface protection sheet is attached is usually placed on a grinding table such as a chuck table and fixed by suction, etc. When the workpiece is placed on the table, the height of the surface protection sheet in the area corresponding to the outer periphery of the workpiece is lower than the height of the area corresponding to the inner periphery of the workpiece, so when the workpiece is placed on the grinding table, the outer periphery of the workpiece and the grinding table are not in sufficient contact with each other, resulting in a gap or the like, which may cause a suction error.

[0012] Also, if the workpiece can be adsorbed, when the workpiece is adsorbed in this state, the outer periphery of the workpiece drops toward the grinding table together with the surface protection sheet and is fixed there. Then, the back surface grinding is performed. When the adsorption is released after the back surface grinding is completed, the outer periphery of the workpiece is released and floats up from the grinding table. In the back surface grinding, the back surface of the workpiece is ground to approximately the same height, but when the outer periphery of the workpiece floats up, the thickness of the outer periphery of the workpiece becomes thicker than the thickness of the inner periphery of the workpiece by the amount of the drop during adsorption. The difference between the thickness of the outer periphery of the workpiece and the thickness of the inner periphery of the workpiece is reflected in the TTV (Total Thickness Variation) of the workpiece, and the TTV of the workpiece tends to be large. If the TTV of the workpiece is large, there are problems such as the workpiece being more likely to crack and problems occurring when the workpiece is divided into individual pieces, so it is preferable that the TTV of the workpiece is small.

[0013] In Patent Document 1, bumps are taken into consideration as steps or protrusions, and the problem of the height difference between the inner and outer peripheries of the wafer is not taken into consideration, so that a height difference occurs between the inner and outer peripheries of the wafer when the adhesive tape for semiconductor wafer processing described in Patent Document 1 is applied. As a result, there is a problem that cracks are likely to occur during backgrinding, or that even if no cracks occur, the TTV of the semiconductor wafer after backgrinding becomes large.

[0014] In order to address this problem and to suppress the effect of the height difference on the surface, a predetermined pattern can be formed on the surface before the surface protection sheet is attached. If such a pattern is formed in a low-height area on the surface of the workpiece so as to protrude from the surface of the workpiece, and then the surface protection sheet is attached, the height difference reflected in the surface protection sheet is suppressed. As a result, even if back grinding is performed, the difference between the thickness of the outer periphery of the workpiece and the thickness of the inner periphery of the workpiece, that is, the TTV, can be reduced.

[0015] On the other hand, after the back grinding, the surface protection sheet is peeled off in order to send the workpiece to the next process. At this time, the surface protection sheet is peeled off so that no residue such as glue remains on the surface of the workpiece. If residue remains on the surface of the workpiece, an extra process such as cleaning is required. Therefore, the pattern previously formed on the surface must also be peeled off together with the surface protection sheet so that no residue remains on the surface of the workpiece. That is, the pattern must be peeled off from the surface together with the surface protection sheet when the surface protection sheet is peeled off. In addition, a predetermined functional film may be formed on the surface of the workpiece in order to protect, insulate, etc. the circuit surface. Therefore, the pattern is required to be peeled off well from such a functional film.

[0016] The present invention has been made in consideration of the above-described situation, and aims to provide a method for processing a workpiece that can effectively peel off a pattern formed on the surface together with a surface protective sheet in order to suppress the effects of differences in height on the surface. [Means for solving the problem]

[0017] The aspects of the present invention are as follows.

[0018] [1] A workpiece having a surface having a height difference and a back surface opposite to the surface, on which a convex pattern for suppressing the effect of the height difference on the surface is formed, comprising: a step of attaching a surface protective sheet to the surface; and peeling off the surface protection sheet attached to the surface and at least a part of the convex pattern from the surface, This is a method for processing a workpiece in which the adhesive strength of a convex pattern on a workpiece having a polyimide film formed thereon at 50°C is 1000 mN / 25 mm or less.

[0019] [2] A method for processing a workpiece as described in [1], wherein the tensile breaking elongation of the convex pattern is 4% or more.

[0020] [3] A method for processing a workpiece according to [1] or [2], wherein the convex pattern is made of a resin composition.

[0021] [4] A method for processing a workpiece according to any one of [1] to [3], further comprising a step of grinding the back surface of the workpiece to which the surface protection sheet is attached.

[0022] [5] A method for machining a workpiece described in any of [1] to [4], wherein the surface has an inner circumference and an outer circumference surrounding the inner circumference, the height of the outer circumference is lower than the height of the inner circumference, and a convex pattern is formed on the outer circumference.

[0023] [6] A method for processing a workpiece according to any one of [1] to [5], wherein a functional film is formed on at least a portion of the surface.

[0024] [7] A method for machining a workpiece according to any one of [1] to [6], wherein the workpiece has a convex electrode formed on its surface.

[0025] [8] A method for machining a workpiece described in any one of [5] to [7], wherein the convex pattern is formed at a distance from the outer edge of the workpiece.

[0026] [9] A method for processing a workpiece according to any one of [1] to [8], wherein the surface protection sheet has a substrate and an adhesive layer.

[0027]

[10] A process for forming a groove on a surface of a workpiece before a process for attaching a surface protective sheet to the surface of the workpiece, A method for processing a workpiece according to any one of [4] to [9], in which, in a process of grinding the back surface of the workpiece, the workpiece is diced into a plurality of workpiece pieces starting from the grooves.

[0028]

[11] A process for forming a modified region inside the workpiece before the process for grinding the back surface of the workpiece, A method for processing a workpiece according to any one of [4] to [9], wherein in a step of grinding the back surface of the workpiece, the workpiece is diced into a plurality of workpiece pieces starting from the modified region.

[0029]

[12] A resin composition having an adhesive strength of 1000 mN / 25 mm or less to a workpiece on which a polyimide film is formed.

[0030]

[13] The resin composition according to

[12] , having a tensile elongation at break of 4% or more.

[0031]

[14] A resin composition according to

[12] or

[13] , which is used to form a convex pattern in a workpiece having a surface with a height difference and a back surface opposite the surface, in order to suppress the effect of the height difference on the surface.

[0032]

[15] The resin composition according to any one of

[12] to

[14] , wherein the resin composition is energy ray-curable and the adhesive strength is the adhesive strength after curing with the energy ray. Effect of the Invention

[0033] According to the present invention, it is possible to provide a method for processing a workpiece that can satisfactorily peel off a pattern formed on a surface together with a surface protection sheet in order to suppress the effects of differences in height on the surface. [Brief description of the drawings]

[0034] [Figure 1A] FIG. 1A is a schematic cross-sectional view of a workpiece having a height difference on its surface, in which a convex electrode is formed on the surface of the workpiece. [Figure 1B]FIG. 1B is a schematic cross-sectional view of a chip-on-wafer as a workpiece having height differences on its surface. [Figure 1C] FIG. 1C is a schematic cross-sectional view of a half-trim wafer as a workpiece having height differences on its surface. [Diagram 2] 2(A) to 2(E) are schematic cross-sectional views for explaining that the TTV of a workpiece increases when the workpiece is machined by a conventional method. [Figure 3A] FIG. 3A is a schematic plan view of a workpiece having a convex electrode on the outer periphery of which a convex pattern is formed in the workpiece machining method according to the present embodiment. [Figure 3B] FIG. 3B is a schematic cross-sectional view taken along line IIIA-IIIA in FIG. 3A. [Figure 3C] FIG. 3C is a schematic cross-sectional view showing another example of the location where a convex pattern is formed on a workpiece. [Figure 4] 4(A) to 4(C) are schematic cross-sectional views for explaining that the TTV of a workpiece is reduced when the workpiece is machined by the method according to this embodiment. [Figure 5A] FIG. 5A is a schematic cross-sectional view of a surface protection sheet that is preferably used in the workpiece processing method according to this embodiment. [Figure 5B] FIG. 5B is a schematic cross-sectional view showing another example of a surface protection sheet that is preferably used in the workpiece processing method according to this embodiment. [Figure 5C] FIG. 5C is a schematic cross-sectional view showing another example of a surface protection sheet that is preferably used in the workpiece processing method according to this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0035] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to the accompanying drawings based on specific embodiments. First, the main terms used in this specification will be explained.

[0036] The work refers to a plate-like body to which a surface protection sheet is attached and then cut into individual pieces. Examples of the work include a circular wafer (including a case having an orientation flat), a rectangular panel level package, and a strip (rectangular substrate) sealed with molded resin. Among them, a wafer is preferable from the viewpoint of easily obtaining the effect of the present invention. The wafer may be, for example, a semiconductor wafer such as a silicon wafer, a gallium arsenide wafer, a silicon carbide wafer, a gallium nitride wafer, or an indium phosphide wafer, or an insulating wafer such as a glass wafer, a lithium tantalate wafer, or a lithium niobate wafer, or may be a reconstructed wafer made of a resin and a semiconductor used for producing a fan-out package or the like. From the viewpoint of easily obtaining the effect of the present invention, a semiconductor wafer or an insulating wafer is preferable, and a semiconductor wafer is more preferable.

[0037] Singulation of a work refers to dividing the work into individual circuits to obtain individual work pieces. For example, if the work is a wafer, the individual work pieces are chips, and if the work is a panel level package or a strip (rectangular substrate) sealed with molded resin, the individual work pieces are semiconductor packages.

[0038] The "front surface" of a workpiece refers to the side on which a circuit or the like is formed or on which the formation of a circuit or the like is planned, and the "back surface" of a workpiece refers to the side on which a circuit or the like is not formed or on which the formation of a circuit or the like is not planned.

[0039] DBG is a method in which a groove of a specified depth is formed on the front side of a workpiece, and then the workpiece is ground from the back side to separate the workpiece by grinding. The grooves formed on the front side of the workpiece are formed by methods such as blade dicing, laser dicing, and plasma dicing.

[0040] LDBG is a modified version of DBG, in which a modified region is created inside the workpiece using a laser, and the workpiece is divided into individual pieces by the stress generated when grinding the back surface of the workpiece.

[0041] The term "group of individual workpieces" refers to a plurality of individual workpieces held on the surface protection sheet of the present invention after the workpiece is singulated. These individual workpieces, as a whole, form a shape similar to that of the workpiece. The term "group of chips" refers to a plurality of chips held on the surface protection sheet of the present invention after the wafer as the workpiece is singulated. These chips, as a whole, form a shape similar to that of the wafer.

[0042] "(Meth)acrylate" is used as the term to refer to both "acrylate" and "methacrylate," and similar terms.

[0043] The term "energy rays" refers to ultraviolet rays, electron beams, etc., and is preferably ultraviolet rays.

[0044] Unless otherwise specified, the "weight average molecular weight" is a polystyrene equivalent value measured by gel permeation chromatography (GPC). Measurements by such a method are performed, for example, using a high-speed GPC device "HLC-8120GPC" manufactured by Tosoh Corporation with a high-speed column "TSK guard column H XL -H", "TSK Gel GMH XL ", "TSK Gel G2000 H XL (All of the above are manufactured by Tosoh Corporation) connected in the above order, the column temperature was 40° C., the liquid flow rate was 1.0 mL / min, and the detector was a differential refractometer.

[0045] The release sheet is a sheet that supports the pressure-sensitive adhesive layer in a releasable manner. The term "sheet" is not limited to a specific thickness, and is used to include a film.

[0046] The mass ratios in the explanations of compositions such as the pressure-sensitive adhesive layer composition are based on the active ingredient (solid content), and do not include the solvent unless otherwise specified.

[0047] (1. Workpiece machining method) The workpiece machined by the method according to the present embodiment is a workpiece having height differences on its surface. Examples of such workpieces include a workpiece having a convex electrode (such as a bump electrode or a pillar electrode) formed on its surface, a chip-on-wafer (CoW) having a chip disposed on its surface, and a half-trim wafer having a part of the edge of the workpiece removed.

[0048] As shown in Fig. 1A, the workpiece with a convex electrode is a workpiece with a convex electrode 2a formed on its surface for electrically connecting a circuit formed on the surface 1a of the workpiece 1 to a substrate or the like. The convex electrode 2a is formed to protrude in the thickness direction of the workpiece. Therefore, there is a height difference D between the tip of the convex electrode and an area on the workpiece where the convex electrode is not formed.

[0049] Chip-on-wafer is used to improve the performance and density of electronic devices. As shown in FIG. 1B, chip-on-wafer is a wafer in which a plurality of chips 2b, smaller in size than the wafer 1, are arranged on the inner periphery of a plate-like body such as a wafer 1. The chip-on-wafer is then diced to form a plurality of high-density stacked packages. The chips 2b are stacked on the surface 1a of the work. Therefore, there is a height difference D between the top surface of the chip and the area on the wafer where the chip is not arranged.

[0050] Half-trim wafers are used to prevent damage to the wafer. Specifically, a half-trim wafer is a wafer in which a part of the front side of the edge of the wafer is removed by trimming in order to prevent chipping, which may cause damage to the wafer, from occurring at the edge of the wafer during back grinding. Therefore, as shown in FIG. 1C, there is a height difference D between the removed area (edge) and the unremoved area of ​​the wafer 1.

[0051] 1A to 1C, the height difference D of the surface 1a corresponds to the height difference between the inner peripheral part and the outer peripheral part of the work (wafer) 1, and the inner peripheral part is surrounded by the outer peripheral part. Therefore, in this embodiment, the height difference of the surface is formed by the inner peripheral part and the outer peripheral part surrounding the inner peripheral part, and it is preferable that the height of the outer peripheral part is lower than the height of the inner peripheral part.

[0052] In the case of a workpiece having a convex electrode, the convex electrodes are formed at a predetermined interval. Therefore, even in the inner peripheral portion, there is a region between the convex electrodes that is approximately the same height as the region (outer peripheral portion) where no convex electrode is formed. However, the height of this region is not the height of the inner peripheral portion, but the height to the tip of the convex electrode is the height of the inner peripheral portion.

[0053] Also, in the case of chip-on-wafer, the chips are usually arranged at a predetermined interval. Therefore, even in the inner periphery, there are areas (usually lattice-shaped areas) between the chips where no chips are arranged, and the height of this area is almost the same as the height of the outer periphery. However, the height of this area is not the height of the inner periphery, but the height of the chip becomes the height of the inner periphery.

[0054] In the case of a half-trim wafer, the outer periphery is the area that has been removed by trimming, and the inner periphery is the area that has not been removed by trimming. Usually, the inner periphery has a uniform height, so that height is the height of the inner periphery.

[0055] The method for machining a workpiece according to this embodiment includes at least the following steps 1 and 2. Step 1: A step of attaching a surface protection sheet to a workpiece having a surface with a height difference and a back surface opposite the surface, the workpiece having a convex pattern formed on the surface to suppress the effect of the height difference on the surface. Step 2: A step of peeling off the surface protection sheet attached to the surface and at least a part of the convex pattern from the surface.

[0056] Furthermore, when a surface protection sheet is applied to a workpiece having circuits or the like formed on one side (front side) and no circuits or the like formed on the other side (back side), for example, the back side of the workpiece may be ground in order to realize a thinner workpiece obtained by dividing the workpiece. In backside grinding of the workpiece, contamination of the circuits or the like due to intrusion of abrasives, cooling water, etc. into the workpiece surface, and damage to the circuits or the like due to the force applied during backside grinding may occur, so that it is useful to apply a surface protection sheet that protects the workpiece surface.

[0057] Therefore, the workpiece machining method according to this embodiment preferably includes the following step 3 in addition to the above steps 1 and 2. In this embodiment, step 3 is performed after step 1 and before step 2. Process 3: Grinding the back surface of the workpiece with the surface protection sheet attached

[0058] In the following, a case will be described in which, in the workpiece machining method including the above steps 1 to 3, the workpiece is a wafer on which convex electrodes are formed, and the workpiece singulated objects are chips.

[0059] (1.1.Process 1) In step 1, a surface protection sheet is attached to the surface of the wafer. As shown in Fig. 1A, a height difference D occurs on the surface 1a of the wafer 1 due to the convex electrode 2a. When a surface protection sheet is attached to this surface 1a, as shown in Fig. 2(A), the surface protection sheet 20 follows the shapes of the surface 1a and the convex electrode 2a, so that the height difference D is reflected in the surface protection sheet 20, and a height difference occurs in the surface protection sheet 20.

[0060] 2B, when the wafer is subjected to back grinding in a state where a height difference occurs in the surface protection sheet, the front side of the wafer, i.e., the surface protection sheet 20, is placed so as to be in contact with the chuck table 100, and the wafer 1 and the surface protection sheet 20 are fixed to the chuck table 100, for example, by suction. At this time, the surface protection sheet 20 present on the convex electrode 2a is in contact with the chuck table 100 when placed on the chuck table 100, but the surface protection sheet 20 present on the area where the convex electrode 2a is not formed, i.e., on the outer periphery of the wafer 1, may not be in sufficient contact with the chuck table 100 or a gap C may be generated between the chuck table 100 and the surface protection sheet 20 when placed on the chuck table 100 due to the height difference.

[0061] When suction is performed in this state, as shown in Fig. 2(C), the surface protection sheet 20 present on the outer periphery of the wafer 1 is deformed by suction and drops toward the chuck table 100 and is fixed there, as shown in Fig. 2(C). Since the outer periphery of the wafer 1 is in close contact with the surface protection sheet 20, the outer periphery of the wafer 1 also deforms as the surface protection sheet 20 deforms. In other words, the outer periphery of the wafer 1 is fixed at a position closer to the chuck table 100 than the inner periphery of the wafer 1 (the region where the convex electrode 2a is formed).

[0062] After the wafer 1 and the surface protection sheet 20 are fixed to the chuck table 100, the back surface 1b of the wafer 1 is ground. The wafer after grinding is shown in FIG. 2(D). Since the back surface of the wafer is ground to approximately the same height, as shown in FIG. 2(D), the thickness of the outer peripheral portion of the wafer 1 is thicker than the thickness of the inner peripheral portion of the wafer 1 by the amount that the outer peripheral portion of the wafer 1 was fixed at a position closer to the chuck table 100. As a result, when the suction is released, the deformation of the surface protection sheet 10 is released as shown in FIG. 2(E), and the height difference between the inner peripheral portion of the wafer 1 and the outer peripheral portion of the wafer 1 becomes apparent. Therefore, in this case, the thickness of the outer peripheral portion of the wafer 1 tends to be the maximum value of the thickness of the wafer 1, and the thickness of the inner peripheral portion of the wafer 1 tends to be the minimum value of the thickness of the wafer 1.

[0063] The difference between the maximum thickness of the wafer and the minimum thickness of the wafer is called TTV (Total Thickness Variation), and the TTV becomes large due to the above-mentioned height difference. If the TTV becomes large, problems such as the wafer being easily cracked and defects occurring during wafer dicing may occur. In other words, the height difference D on the wafer surface that exists when the surface protection sheet is attached may affect the TTV of the wafer after back grinding.

[0064] In order to suppress the influence of the height difference, in this embodiment, as shown in Figures 3A and 3B, a convex pattern 3 is formed on the surface 1a before attaching a surface protection sheet to the surface (step A). ​​That is, step A is performed before step 1.

[0065] (1.2. Convex Pattern) The convex pattern 3 is a pattern formed on the front surface 1a of the wafer 1 so as to protrude in the thickness direction of the wafer 1. The convex pattern 3 is a pattern formed to suppress the influence of the height difference D described above. In this embodiment, as shown in Figures 3A and 3B, the convex pattern is formed on an area where the convex electrodes 2a are not formed. That is, the convex pattern is formed in an area (outer periphery) that is lower in height than the inner periphery of the wafer (area where the convex electrodes 2a are formed).

[0066] Since such a convex pattern 3 is formed on the outer periphery, when the surface protection sheet 10 is attached to the surface of the wafer 1, the portion corresponding to the convex pattern 3 will be elevated in addition to the portion corresponding to the region where the convex electrodes 2a are formed. As a result, the height difference between the region where the convex electrodes 2a are formed (the inner periphery of the wafer) and the region where they are not formed (the outer periphery of the wafer) is suppressed. Therefore, the height difference on the surface of the wafer that exists when the surface protection sheet is attached is suppressed, and problems caused by the height difference are also suppressed.

[0067] In this embodiment, the height of the convex pattern may be set to a height that can suppress the influence of the height difference of the surface. For example, when the workpiece is a wafer on which a convex electrode is formed, it is preferable to set the height of the convex pattern according to the height of the convex electrode. Specifically, when the height of the convex pattern is H1 and the height of the convex electrode is Hb, H1 is set to Hb / 8.

[0068] In addition, when the workpiece is a chip-on-wafer or half-trim wafer, it is preferable to set the height of the convex pattern according to the difference between the height of the inner periphery and the height of the outer periphery of the wafer surface. Specifically, when the height of the convex pattern is H1 and the difference between the height of the inner periphery and the height of the outer periphery is Hd, H1 is expressed as Hd / 1.2

[0069] The reason why H1 differs depending on the type of workpiece is presumed to be, for example, the following reasons. When comparing the convex electrode and the chip constituting the chip-on-wafer, the chip occupies a larger area and volume of the unevenness on the wafer than the convex electrode. In other words, the chip is arranged more densely on the wafer than the convex electrode. Therefore, even if the convex electrode and the chip form unevenness of the same height, the chip is more likely to lift up the surface protection sheet when attached than the convex electrode, especially at the inner periphery of the wafer, and cracks are more likely to occur during back grinding. As a result, H1 is controlled to the above range due to the difference in the ease of cracking.

[0070] ​​The convex pattern may have various patterns. For example, as shown in FIG. 3A, the convex pattern 3 may be formed in a ring shape including the outer edge of the wafer 1. Such a convex pattern is easy to form and can reliably suppress the influence of the height difference on the surface. In addition, the convex pattern 3 shown in FIG. 3A is a continuous pattern, but may be an intermittently formed pattern.

[0071] 3C, the convex pattern 3 may be formed at a distance radially inward from the outer edge of the wafer 1. Such a convex pattern has the advantage that the entire surface of the convex pattern can be covered with a pick-up tape in the step (step 2) of peeling off the surface protection sheet, which will be described later, and therefore the convex pattern can be easily peeled off together with the surface protection sheet.

[0072] Although the convex pattern can be formed over the entire outer periphery (for example, outside the area where the convex electrode is formed, or outside the area where the chip is arranged), it is preferable to form it away from the convex electrode or chip from the viewpoints of the large amount of material required for its formation and the adhesion of the material of the convex pattern to the convex electrode, circuit, chip, etc. In other words, it is preferable for the outer periphery to include an area where the convex pattern is not formed.

[0073] When the workpiece is a chip-on-wafer, a convex pattern can be formed in the area between the chips on the inner periphery (for example, a lattice-shaped area).

[0074] The means for forming the convex pattern may be determined according to the material for forming the convex pattern. For example, when forming the convex pattern using a curable resin composition described later, a means for applying a liquid resin before curing can be used. Specifically, a coating device such as a die coater, curtain coater, spray coater, slit coater, or knife coater; a printing device such as a screen printer or inkjet printer; or a dropping device such as a dispenser can be used.

[0075] (1.3.Step 3) As described above, in this embodiment, step 3 is performed after step 1 and before step 2. As shown in Fig. 4(A), after forming the convex pattern 3 on the front surface 1a of the wafer 1, the surface protection sheet 10 is attached onto the front surface 1a of the wafer and onto the convex pattern 3. Then, the back surface 1b of the wafer 1 is ground.

[0076] 4(B), the front surface side of the wafer 1 with the surface protection sheet 10 attached thereto is placed on the chuck table 100. The chuck table 100 has, for example, a porous holding surface, and the surface protection sheet 10 is adsorbed and fixed to the chuck table 100 by suction from the side opposite to the side on which the wafer 1 is placed.

[0077] At this time, because the convex pattern 3 is formed on the wafer 1, the height difference of the surface protection sheet 10 is suppressed between the inner peripheral portion of the wafer 1 and the outer peripheral portion of the wafer 1. Therefore, even when suction is performed, the outer peripheral portion of the wafer 1 is adsorbed to the chuck table 100 with almost no deformation.

[0078] After the wafer 1 is fixed to the chuck table 100, the back surface 1b of the wafer 1 is ground, for example, by a grinding wheel or the like. The thickness of the wafer after the back surface grinding is, for example, about 25 μm or more and 600 μm or less.

[0079] After grinding, the suction is released and the wafer 1 and surface protection sheet 10 are released from the chuck table 100. In this embodiment, since process A is adopted in step 1, the thickness of the workpiece 1 becomes almost uniform from the inner periphery to the outer periphery as shown in Fig. 4(C). As a result, problems caused by differences in height on the surface, i.e., problems with the TTV of the workpiece 1 after grinding, are suppressed.

[0080] (1.4.Process 2) After step 3, when the wafer is sent to the next step, the surface protection sheet is peeled off from the surface of the wafer. At this time, if residues of the surface protection sheet are generated on the surface, an extra step such as cleaning is required before the wafer is sent to the next step. Therefore, the surface protection sheet needs to be peeled off well from the surface without generating residues or the like. This also applies to the convex pattern formed on the surface as well as the surface protection sheet. That is, when the surface protection sheet is peeled off from the surface of the wafer, the convex pattern also needs to be peeled off well from the surface. In this embodiment, from the viewpoint of residues and the like, it is preferable that the entire convex pattern is peeled off from the surface in the peeling step of the surface protection sheet. In step 2, in order to improve the peelability of the convex pattern, in this embodiment, the physical properties of the convex pattern are controlled as follows.

[0081] (1.5. Physical properties of convex patterns) In this embodiment, the adhesive strength of the convex pattern to the workpiece on which the polyimide film is formed is set to 1000 mN / 25 mm or less at 50° C. When the adhesive strength of the convex pattern is within the above range, good peeling of the convex pattern from the surface is achieved.

[0082] The adhesive strength of the convex pattern is preferably 1000 mN / 25 mm or less, more preferably 800 mN / 25 mm or less, and even more preferably 500 mN / 25 mm or less. On the other hand, from the viewpoint of reliably fixing the convex pattern on the surface when the convex pattern is formed, the lower limit of the adhesive strength of the convex pattern is 10 mN / 25 mm.

[0083] As described above, the wafer is composed of a semiconductor, an insulator, etc., but a predetermined functional film may be formed on the surface of the wafer in order to protect, insulate, etc., circuits formed on the surface of the wafer. When the functional film is formed, the convex pattern is formed on the functional film. Examples of the functional film include organic films such as polyimide films and polybenzoxazole films. Such organic films have a better compatibility with the convex pattern than the material constituting the wafer, and the convex pattern tends to be firmly fixed to the organic film. This tendency is particularly noticeable when the convex pattern is composed of a resin composition.

[0084] Therefore, in this embodiment, the adhesive strength of the convex pattern under conditions where it is difficult to peel off from the wafer surface is set within the above range, thereby ensuring good peelability of the convex pattern regardless of the type and configuration of the wafer. In other words, even if the adhesive strength of a convex pattern to a wafer on which a polyimide film is not formed, for example, a silicon wafer, is 1000 mN / 25 mm or less, the adhesive strength to a wafer on which a polyimide film is formed is greater than the adhesive strength to a silicon wafer, so the adhesive strength of the convex pattern to a wafer on which a polyimide film is formed is not necessarily 1000 mN / 25 mm or less.

[0085] In this embodiment, the tensile elongation at break of the convex pattern is preferably 4% or more. That is, it is preferable that the convex pattern stretches to a certain extent when peeled off. If it does not stretch, the force applied during peeling is not sufficiently alleviated, and it may become prone to cracking due to concentrated force, and peeling may not be completed. Such problems are unlikely to occur when peeling at a low speed, but tend to become evident when peeling at a high speed. Therefore, by having the tensile elongation at break of the convex pattern within the above range, it becomes less likely to crack during peeling, and good peeling can be achieved even when the peeling speed is high.

[0086] The tensile elongation at break of the convex pattern is more preferably 8% or more, and even more preferably 15% or more. The upper limit of the tensile elongation at break of the convex pattern is not particularly limited, but is, for example, 100%.

[0087] (1.6. Composition of Convex Pattern) The material constituting the convex pattern may be any material capable of achieving the above-mentioned physical properties. In this embodiment, from the viewpoint of facilitating the formation of the convex pattern, the material constituting the convex pattern is preferably a resin composition. The resin composition is preferably an adhesive composition that adheres closely to the wafer surface. Examples of the adhesive composition include an acrylic adhesive composition, a silicone adhesive composition, a urethane adhesive composition, an epoxy adhesive composition, a phenolic adhesive composition, a urea adhesive composition, an alkyd adhesive composition, a vinyl acetate adhesive composition, a vinyl chloride adhesive composition, an amide adhesive composition, an imide adhesive composition, a chloroprene rubber, a nitrile rubber, and a styrene butadiene rubber.

[0088] In addition, the resin composition is preferably curable. When the resin composition is curable, the adhesive strength and tensile elongation at break of the convex pattern at 50°C are physical properties after curing. Since the resin composition is curable, it is easy to form a predetermined shape before curing, and it is easy to satisfy the above-mentioned range of adhesive strength after curing. Examples of the curable resin composition include a thermosetting resin composition and an energy ray curable resin composition.

[0089] In this embodiment, from the viewpoint of facilitating the setting of the adhesive strength within the above range, an energy ray-curable resin composition is preferred, and an energy ray-curable acrylic adhesive composition is more preferred. The energy ray-curable acrylic adhesive composition preferably contains the components shown below.

[0090] (1.6.1. Energy ray curable compound) The energy ray-curable compound is preferably a monomer or oligomer which has an unsaturated group in the molecule and can be polymerized and cured by irradiation with energy rays.

[0091] Examples of such energy ray-curable compounds include polyvalent (meth)acrylate monomers such as trimethylolpropane tri(meth)acrylate, pentaerythritol (meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,4-butylene glycol di(meth)acrylate, and 1,6-hexanediol (meth)acrylate; and oligomers such as urethane (meth)acrylate, polyester (meth)acrylate, polyether (meth)acrylate, and epoxy (meth)acrylate.

[0092] Among these, urethane (meth)acrylate and dipentaerythritol hexa(meth)acrylate are preferred in order to adjust the adhesive strength and tensile elongation at break after curing to appropriate ranges.

[0093] The urethane (meth)acrylate may be an oligomer, a polymer, or a mixture thereof. In this embodiment, a urethane (meth)acrylate oligomer is preferred.

[0094] The urethane (meth)acrylate can be obtained, for example, by reacting a polyol compound with a polyisocyanate compound to obtain a terminal isocyanate urethane prepolymer, and then reacting the resulting prepolymer with a hydroxyl group-containing (meth)acrylate. The urethane (meth)acrylate may be used alone or in combination of two or more kinds.

[0095] The content of the urethane (meth)acrylate in the acrylic pressure-sensitive adhesive composition is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more. The content of the urethane (meth)acrylate in the acrylic pressure-sensitive adhesive composition is preferably 80% by mass or less, more preferably 60% by mass or less, and even more preferably 40% by mass or less.

[0096] The content of dipentaerythritol hexa(meth)acrylate in the acrylic pressure-sensitive adhesive composition is preferably 3% by mass or more, more preferably 5% by mass or more, and even more preferably 7% by mass or more. The content of dipentaerythritol hexa(meth)acrylate in the acrylic pressure-sensitive adhesive composition is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 20% by mass or less.

[0097] (1.6.2. Polymerizable Monomers) The polymerizable monomer is preferably a polymerizable compound other than the above-mentioned urethane (meth)acrylate and dipentaerythritol hexa (meth)acrylate, and is a compound that can be polymerized with other components by irradiation with energy rays. In this embodiment, the polymerizable monomer is a compound having one reactive unsaturated double bond group.

[0098] Examples of the polymerizable monomer include (meth)acrylates having an alkyl group having 1 to 30 carbon atoms; (meth)acrylates having a functional group such as a hydroxyl group, an amide group, an amino group, or an epoxy group; (meth)acrylates having an alicyclic structure; (meth)acrylates having an aromatic structure; (meth)acrylates having a heterocyclic structure; and vinyl compounds such as styrene, hydroxyethyl vinyl ether, hydroxybutyl vinyl ether, N-vinyl formamide, N-vinyl pyrrolidone, and N-vinyl caprolactam.

[0099] Examples of the (meth)acrylate having an alkyl group having 1 to 30 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, hexadecyl (meth)acrylate, octadecyl (meth)acrylate, and eicosyl (meth)acrylate.

[0100] Examples of the (meth)acrylate having a functional group include hydroxyl group-containing (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N-butyl (meth)acrylamide, and N-methylol (meth)acrylamide. Examples of the amide group-containing compounds include acrylamide, N-methylolpropane (meth)acrylamide, N-methoxymethyl (meth)acrylamide, and N-butoxymethyl (meth)acrylamide; amino group-containing (meth)acrylates such as primary amino group-containing (meth)acrylates, secondary amino group-containing (meth)acrylates, and tertiary amino group-containing (meth)acrylates; and epoxy group-containing (meth)acrylates such as glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, and allyl glycidyl ether.

[0101] Examples of (meth)acrylates having an alicyclic structure include isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxy (meth)acrylate, cyclohexyl (meth)acrylate, trimethylcyclohexyl (meth)acrylate, and adamantane (meth)acrylate.

[0102] Examples of the (meth)acrylate having an aromatic structure include phenylhydroxypropyl (meth)acrylate, benzyl (meth)acrylate, and 2-hydroxy-3-phenoxypropyl (meth)acrylate.

[0103] Examples of the (meth)acrylate having a heterocyclic structure include tetrahydrofurfuryl (meth)acrylate and morpholine (meth)acrylate.

[0104] In this embodiment, the polymerizable monomer preferably contains a (meth)acrylate having an alicyclic structure. As the (meth)acrylate having an alicyclic structure, isobornyl (meth)acrylate is preferable.

[0105] The content of the polymerizable monomer in the acrylic pressure-sensitive adhesive composition is preferably 10% by mass or more, more preferably 30% by mass or more, and even more preferably 50% by mass or more. The content of the polymerizable monomer in the acrylic pressure-sensitive adhesive composition is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 80% by mass or less.

[0106] (1.6.3. Photopolymerization initiator) When the acrylic pressure-sensitive adhesive composition contains the above-mentioned urethane (meth)acrylate and dipentaerythritol hexa(meth)acrylate, and a polymerizable monomer, the acrylic pressure-sensitive adhesive composition preferably contains a photopolymerization initiator. By containing the photopolymerization initiator, polymerization proceeds reliably, and a convex pattern having the above-mentioned characteristics can be easily obtained.

[0107] Examples of the photopolymerization initiator include photopolymerization initiators such as benzoin compounds, acetophenone compounds, acylphosphinoxide compounds, titanocene compounds, thioxanthone compounds, and peroxide compounds, and photosensitizers such as amines and quinones. Specific examples include 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and 2,2-dimethoxy-1,2-diphenylethan-1-one. These photopolymerization initiators may be used alone or in combination of two or more.

[0108] The amount of the photopolymerization initiator is preferably 0.1 parts by mass or more and 10 parts by mass or less, and more preferably 0.3 parts by mass or more and 5 parts by mass or less, per 100 parts by mass of the total of the urethane (meth)acrylate, dipentaerythritol hexa(meth)acrylate, and polymerizable monomer.

[0109] (1.6.4. Surface tension adjuster) The acrylic pressure-sensitive adhesive composition preferably contains a surface tension modifier, which can reduce the adhesive strength of the pressure-sensitive adhesive composition by energy ray irradiation and can impart flexibility to the composition after energy ray curing.

[0110] Examples of the surface tension adjuster include silicone modified acrylates. In this embodiment, silicone modified acrylates having a functional group number of 1 to 12 are preferred. These surface tension adjusters may be used alone or in combination of two or more.

[0111] The content of the surface tension modifier in the acrylic pressure-sensitive adhesive composition is preferably 0.5% by mass or more, more preferably 1% by mass or more, and even more preferably 5% by mass or more. The content of the surface tension modifier in the acrylic pressure-sensitive adhesive composition is preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 10% by mass or less.

[0112] (1.7. Surface protection sheet) The surface protection sheet attached to the surface may be configured to protect the circuits and the like on the wafer surface. In this embodiment, as shown in FIG. 5A, the surface protection sheet 10 preferably has a base material 11 and an adhesive layer 12. The adhesive layer is attached to the wafer surface, so that the wafer surface is reliably protected. The adhesive layer may or may not conform to the height difference of the wafer surface.

[0113] For example, when the workpiece is a wafer on which a convex electrode is formed, it is preferable that the adhesive layer follows the height difference and embeds the convex electrode. On the other hand, when the workpiece is a chip-on-wafer, the adhesive layer does not have to follow the height difference. That is, the adhesive layer does not have to be inserted between the chips. The convex pattern may be embedded in the surface protection sheet, or a part of the convex pattern may not be embedded in the surface protection sheet and may be exposed to the outside.

[0114] 5B, an intermediate layer 13 may be disposed between the substrate 11 and the adhesive layer 12 in the surface protection sheet 10. The intermediate layer makes it easy to suppress the height difference on the wafer surface. In particular, when the workpiece is a wafer on which a convex electrode is formed, the convex electrode can be reliably embedded.

[0115] The surface protection sheet 10 shown in Fig. 5B is described in detail below. Fig. 5B shows a surface protection sheet 10 having a configuration in which an intermediate layer 13 and a pressure-sensitive adhesive layer 12 are laminated in this order on a substrate 11.

[0116] The surface protective sheet 10 may have other layers. For example, another layer may be formed between the substrate 11 and the intermediate layer 13, or another layer may be formed between the intermediate layer 13 and the pressure-sensitive adhesive layer 12.

[0117] The components of surface protection sheet 10 shown in FIG. 5B will be described in detail below.

[0118] (1.7.1. Base material) The substrate is a member that is responsible for the rigidity of the surface protection sheet. The substrate is not limited as long as it is made of a material that can support the workpiece. For example, various resin films used as substrates for backgrinding tapes are exemplified. By using such a resin film, the workpiece can be held without being damaged even if the thickness of the workpiece becomes thin due to grinding. The substrate may be made of a single-layer film made of one resin film, or may be made of a multi-layer film in which multiple resin films are laminated.

[0119] In this embodiment, examples of the material of the substrate include polyesters such as polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, wholly aromatic polyesters, polyamides, polycarbonates, polyacetals, modified polyphenylene oxides, polyphenylene sulfides, polysulfones, polyether ketones, biaxially oriented polypropylenes, etc. Among these, polyesters are preferred, and polyethylene terephthalate is more preferred.

[0120] The thickness of the substrate affects the rigidity of the surface protection sheet, and may be set according to the material of the substrate. In this embodiment, the thickness of the substrate is preferably 25 μm or more and 200 μm or less, more preferably 35 μm or more and 150 μm or less, and even more preferably 40 μm or more and 150 μm or less.

[0121] At least one of the main surfaces of the substrate may be subjected to an adhesion treatment such as a corona treatment in order to improve adhesion with a layer formed on the main surface. Also, at least one of the main surfaces of the substrate may be provided with an easy-adhesion layer in order to improve adhesion with a layer formed on the main surface.

[0122] (1.7.2. Adhesive Layer) The adhesive layer is attached to the surface of the wafer, and protects the surface and supports the wafer until it is peeled off from the surface. In this embodiment, the adhesive layer is closely attached to the surface of the wafer and fixed thereto. As a result, even if cooling water or the like is used during back grinding, the surface protection sheet can prevent the cooling water from penetrating into the wafer surface, and can adequately protect the wafer surface. Furthermore, even if the wafer is divided into individual pieces, contact between chips can be suppressed. The adhesive layer may be composed of one layer (single layer), or may be composed of two or more layers.

[0123] The thickness of the adhesive layer is not particularly limited as long as it is thick enough to support the wafer. In this embodiment, the thickness of the adhesive layer is preferably 1 μm or more and 100 μm or less, more preferably 5 μm or more and 50 μm or less. The thickness of the adhesive layer means the thickness of the entire adhesive layer. For example, the thickness of an adhesive layer composed of multiple layers means the total thickness of all layers constituting the adhesive layer.

[0124] The composition of the adhesive layer is not limited as long as it has enough adhesiveness to protect the surface of the wafer. In this embodiment, the adhesive layer is preferably composed of, for example, an acrylic adhesive, a urethane adhesive, a rubber adhesive, a silicone adhesive, or the like.

[0125] In addition, the adhesive layer is preferably formed from an energy ray curable adhesive. By forming the adhesive layer of the surface protection sheet from an energy ray curable adhesive, the adhesive layer adheres to the wafer with high adhesive strength when attached to the wafer, and the adhesive strength can be reduced by irradiating energy rays when peeled off from the wafer. Therefore, while appropriately protecting the circuits of the wafer, the circuit on the wafer surface is prevented from being destroyed and the adhesive is prevented from being transferred onto the wafer when the surface protection sheet is peeled off.

[0126] In this embodiment, the energy ray curable adhesive is preferably composed of an adhesive composition containing an acrylic adhesive. As the acrylic adhesive, it is preferable to use an acrylic polymer. As the energy ray curable acrylic adhesive, it may be an acrylic adhesive composed of an acrylic polymer having energy ray curability, or an acrylic adhesive containing an acrylic polymer having energy ray curability and / or an acrylic polymer not having energy ray curability and an energy ray curable compound such as an oligomer having an energy ray curable group. In this embodiment, an acrylic adhesive composed of an acrylic polymer having energy ray curability is preferable.

[0127] The acrylic polymer having energy ray curability may be any known acrylic polymer, but in this embodiment, an acrylic polymer having an energy curable group introduced into a functional group-containing acrylic polymer is preferred. The functional group-containing acrylic polymer may be a homopolymer formed from one type of acrylic monomer, a copolymer formed from multiple types of acrylic monomers, or a copolymer formed from one or multiple types of acrylic monomers and a monomer other than the acrylic monomer.

[0128] In this embodiment, the functional group-containing acrylic polymer is preferably an acrylic copolymer obtained by copolymerizing an alkyl (meth)acrylate with a functional group-containing monomer.

[0129] Examples of the alkyl (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, and n-octyl (meth)acrylate.

[0130] The functional group-containing monomer is a monomer containing a reactive functional group. The reactive functional group is a functional group capable of reacting with other compounds such as a crosslinking agent described later. Examples of the functional group in the functional group-containing monomer include a hydroxyl group, a carboxyl group, and an epoxy group, and a hydroxyl group is preferred.

[0131] Examples of hydroxyl group-containing monomers include hydroxyalkyl (meth)acrylates such as hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; and non-(meth)acrylic unsaturated alcohols (unsaturated alcohols not having a (meth)acryloyl skeleton) such as vinyl alcohol and allyl alcohol.

[0132] Examples of the energy ray curable group include a (meth)acryloyl group and a vinyl group, and a (meth)acryloyl group is preferred. The energy ray curable group is introduced into the acrylic polymer by, for example, adding an energy ray curable compound described later to the functional group-containing acrylic polymer.

[0133] The energy ray-curable compound having an energy ray-curable group is preferably a compound having one or more groups selected from an isocyanate group, an epoxy group, and a carboxy group, and more preferably a compound having an isocyanate group.

[0134] Examples of compounds having an isocyanate group include 2-methacryloyloxyethyl isocyanate, meta-isopropenyl-α,α-dimethylbenzyl isocyanate, methacryloyl isocyanate, allyl isocyanate, 1,1-(bisacryloyloxymethyl)ethyl isocyanate; acryloyl monoisocyanate compounds obtained by reacting a diisocyanate compound or a polyisocyanate compound with hydroxyethyl (meth)acrylate; and acryloyl monoisocyanate compounds obtained by reacting a diisocyanate compound or a polyisocyanate compound with a polyol compound and hydroxyethyl (meth)acrylate. The isocyanate group undergoes an addition reaction with the hydroxyl group of the functional group-containing acrylic polymer.

[0135] The pressure-sensitive adhesive composition preferably further contains a crosslinking agent, which reacts with functional groups, for example, to crosslink resins contained in the functional-group-containing acrylic polymer.

[0136] Examples of the crosslinking agent include isocyanate-based crosslinking agents (crosslinking agents having an isocyanate group) such as tolylene diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, and adducts of these diisocyanates; epoxy-based crosslinking agents (crosslinking agents having a glycidyl group) such as ethylene glycol glycidyl ether; aziridine-based crosslinking agents (crosslinking agents having an aziridinyl group) such as hexa[1-(2-methyl)-aziridinyl]triphosphatriazine; metal chelate-based crosslinking agents (crosslinking agents having a metal chelate structure) such as aluminum chelate; and isocyanurate-based crosslinking agents (crosslinking agents having an isocyanuric acid skeleton).

[0137] The crosslinking agent is preferably an isocyanate-based crosslinking agent from the viewpoints of improving the cohesive strength of the pressure-sensitive adhesive and thereby improving the adhesive strength of the pressure-sensitive adhesive layer, and of easy availability.

[0138] The pressure-sensitive adhesive composition may further contain a photopolymerization initiator. When the pressure-sensitive adhesive composition contains a photopolymerization initiator, the curing reaction proceeds sufficiently even when irradiated with relatively low-energy energy rays such as ultraviolet rays.

[0139] Examples of the photopolymerization initiator include photoinitiators such as benzoin compounds, acetophenone compounds, acylphosphine oxide compounds, titanocene compounds, thioxanthone compounds, and peroxide compounds, and photosensitizers such as amines and quinones.Specific examples include α-hydroxycyclohexyl phenyl ketone, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzyl diphenyl sulfide, benzyl dimethyl ketal, tetramethylthiuram monosulfide, azobisisobutyronitrile, dibenzyl, diacetyl, β-chloroanthraquinone, and 2,4,6-trimethylbenzoyldiphenylphosphine oxide.

[0140] (1.7.3. Middle Layer) The intermediate layer is a layer disposed between the substrate and the pressure-sensitive adhesive layer. In this embodiment, the intermediate layer may be composed of one layer (single layer) or may be composed of two or more layers.

[0141] The thickness of the intermediate layer may be set in consideration of the height difference on the wafer surface. In this embodiment, the thickness of the intermediate layer is preferably 50 μm or more and 600 μm or less, and more preferably 150 μm or more and 500 μm or less. The thickness of the intermediate layer means the thickness of the entire intermediate layer. For example, the thickness of the intermediate layer composed of multiple layers means the total thickness of all layers that compose the intermediate layer.

[0142] In this embodiment, when the surface protective sheet has an intermediate layer, the intermediate layer preferably has the following physical properties.

[0143] (1.7.3.1. Shear storage modulus at 65°C) In this embodiment, the shear storage modulus (G') of the intermediate layer at 65°C is preferably 0.5 MPa or less. The shear storage modulus (G') is one of the indicators of the ease of deformation (hardness) of the intermediate layer. When the shear storage modulus (G') of the intermediate layer at 65°C is within the above range, damage to the wafer or the like during back grinding can be suppressed.

[0144] The shear storage modulus of the intermediate layer at 65° C. is more preferably 0.4 MPa or less, and even more preferably 0.2 MPa or less. Furthermore, from the viewpoint of suppressing exudation of intermediate layer components during storage of the surface protection sheet, the shear storage modulus of the intermediate layer at 65° C. is preferably 0.005 MPa or more.

[0145] The shear storage modulus of the intermediate layer at 65° C. may be measured by a known method. For example, the intermediate layer may be used as a sample of a predetermined size, and the sample may be strained at a predetermined frequency within a predetermined temperature range using a dynamic viscoelasticity measuring device to measure the elastic modulus, and the shear storage modulus may be calculated from the measured elastic modulus.

[0146] (1.7.3.2. Loss tangent at 65°C) In this embodiment, the loss tangent (tan δ) of the intermediate layer at 65° C. is preferably greater than 0.5. The loss tangent is defined as "loss modulus / storage modulus" and is a value measured by the response to stress applied to an object using a dynamic viscoelasticity measuring device. When the loss tangent of the intermediate layer at 65° C. is within the above range, damage to wafers and the like during back grinding can be suppressed.

[0147] The loss tangent of the intermediate layer at 65° C. is more preferably 0.7 or more, and even more preferably 1.0 or more. Also, the loss tangent of the intermediate layer at 65° C. is preferably 2.0 or less.

[0148] The loss tangent of the intermediate layer at 65° C. may be measured by a known method, similar to the shear storage modulus. For example, the intermediate layer is prepared as a sample of a predetermined size, and a dynamic viscoelasticity measuring device is used to apply a strain to the sample at a predetermined frequency within a predetermined temperature range to measure the elastic modulus, and the loss tangent can be calculated from the measured elastic modulus.

[0149] (1.7.4. Composition for intermediate layer) Although the composition of the intermediate layer is not particularly limited, in this embodiment, the intermediate layer is preferably composed of a composition having a resin (intermediate layer composition). The intermediate layer composition preferably contains the following components.

[0150] (1.7.4.1. Urethane (meth)acrylates) The urethane (meth)acrylate is a compound having at least a (meth)acryloyl group and a urethane bond, and has the property of being polymerized by energy ray irradiation. In this embodiment, the urethane (meth)acrylate is a component for imparting flexibility to the intermediate layer.

[0151] The urethane (meth)acrylate may be a monofunctional type or a multifunctional type. In this embodiment, a multifunctional urethane (meth)acrylate is preferred, and a bifunctional urethane (meth)acrylate is preferred.

[0152] The urethane (meth)acrylate may be an oligomer, a polymer, or a mixture thereof. In this embodiment, a urethane (meth)acrylate oligomer is preferred.

[0153] The urethane (meth)acrylate can be obtained, for example, by reacting a polyol compound with a polyisocyanate compound to obtain a terminal isocyanate urethane prepolymer, and then reacting the resulting prepolymer with a hydroxyl group-containing (meth)acrylate. The urethane (meth)acrylate may be used alone or in combination of two or more kinds.

[0154] The content of the urethane (meth)acrylate in the intermediate layer composition is preferably 20% by mass or more, more preferably 25% by mass or more, and even more preferably 30% by mass or more. The content of the urethane (meth)acrylate in the intermediate layer composition is preferably 70% by mass or less, more preferably 65% ​​by mass or less, and even more preferably 50% by mass or less.

[0155] (1.7.4.2. Polymerizable Monomers) The polymerizable monomer is preferably a polymerizable compound other than the above-mentioned urethane (meth)acrylate, and is a compound that can be polymerized with other components by irradiation with energy rays. In this embodiment, the polymerizable monomer is a compound having one reactive unsaturated double bond group.

[0156] Examples of the polymerizable monomer include (meth)acrylates having an alkyl group having 1 to 30 carbon atoms; (meth)acrylates having a functional group such as a hydroxyl group, an amide group, an amino group, or an epoxy group; (meth)acrylates having an alicyclic structure; (meth)acrylates having an aromatic structure; (meth)acrylates having a heterocyclic structure; and vinyl compounds such as styrene, hydroxyethyl vinyl ether, hydroxybutyl vinyl ether, N-vinyl formamide, N-vinyl pyrrolidone, and N-vinyl caprolactam.

[0157] Examples of the (meth)acrylate having an alkyl group having 1 to 30 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, hexadecyl (meth)acrylate, octadecyl (meth)acrylate, and eicosyl (meth)acrylate.

[0158] Examples of the (meth)acrylate having a functional group include hydroxyl group-containing (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N-butyl (meth)acrylamide, and N-methylol (meth)acrylamide. Examples of the amide group-containing compounds include acrylamide, N-methylolpropane (meth)acrylamide, N-methoxymethyl (meth)acrylamide, and N-butoxymethyl (meth)acrylamide; amino group-containing (meth)acrylates such as primary amino group-containing (meth)acrylates, secondary amino group-containing (meth)acrylates, and tertiary amino group-containing (meth)acrylates; and epoxy group-containing (meth)acrylates such as glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, and allyl glycidyl ether.

[0159] Examples of (meth)acrylates having an alicyclic structure include isobornyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxy (meth)acrylate, cyclohexyl (meth)acrylate, trimethylcyclohexyl (meth)acrylate, and adamantane (meth)acrylate.

[0160] Examples of the (meth)acrylate having an aromatic structure include phenylhydroxypropyl (meth)acrylate, benzyl (meth)acrylate, and 2-hydroxy-3-phenoxypropyl (meth)acrylate.

[0161] Examples of the (meth)acrylate having a heterocyclic structure include tetrahydrofurfuryl (meth)acrylate and morpholine (meth)acrylate.

[0162] In this embodiment, the polymerizable monomer preferably includes a (meth)acrylate having an alkyl group with 1 to 30 carbon atoms and a (meth)acrylate having an alicyclic structure. Among (meth)acrylates having an alkyl group with 1 to 30 carbon atoms, (meth)acrylates having an alkyl group with 4 to 14 carbon atoms are preferred, and as (meth)acrylates having an alicyclic structure, isobornyl (meth)acrylate and trimethylcyclohexyl (meth)acrylate are preferred.

[0163] In addition, when the intermediate layer composition contains a crosslinking agent, a (meth)acrylate having a functional group capable of reacting with the crosslinking agent is not preferred. This is because the crosslinked structure formed by the crosslinking reaction may increase the shear storage modulus of the intermediate layer. For example, a composition for the intermediate layer containing a polyisocyanate-based crosslinking agent and a (meth)acrylate having a hydroxyl group is not preferred.

[0164] The content of the polymerizable monomer in the intermediate layer composition is preferably 20% by mass or more, more preferably 30% by mass or more, and is preferably 80% by mass or less, more preferably 70% by mass or less.

[0165] In addition, the mass ratio of the urethane (meth)acrylate to the polymerizable monomer (urethane (meth)acrylate / polymerizable monomer) in a total of 100 parts by mass of the urethane (meth)acrylate and the polymerizable monomer is preferably from 20 / 80 to 80 / 20, and more preferably from 30 / 70 to 70 / 30.

[0166] (1.7.4.3. Photopolymerization initiator) When the intermediate layer composition contains the above-mentioned urethane (meth)acrylate and polymerizable monomer, the intermediate layer composition preferably contains a photopolymerization initiator. By containing the photopolymerization initiator, polymerization proceeds reliably, and an intermediate layer having the above-mentioned characteristics can be easily obtained.

[0167] Examples of the photopolymerization initiator include photopolymerization initiators such as benzoin compounds, acetophenone compounds, acylphosphinoxide compounds, titanocene compounds, thioxanthone compounds, and peroxide compounds, and photosensitizers such as amines and quinones. Specific examples include 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and 2,2-dimethoxy-1,2-diphenylethan-1-one. These photopolymerization initiators may be used alone or in combination of two or more.

[0168] The amount of the photopolymerization initiator is preferably 0.05 to 15 parts by mass, and more preferably 0.5 to 10 parts by mass, per 100 parts by mass of the total of the urethane (meth)acrylate and the polymerizable monomer.

[0169] 1.7.4.4. Chain Transfer Agents The intermediate layer composition preferably contains a chain transfer agent. The chain transfer agent can cause a chain transfer reaction and adjust the progress of the curing reaction of the intermediate layer composition. By containing the chain transfer agent, it becomes possible for components with short molecular chains to remain relatively even after curing, so that the cured polymer has a crosslinked structure with relatively high flexibility. As a result, it becomes easy to set the shear storage modulus of the intermediate layer within the above range.

[0170] Examples of the chain transfer agent include thiol group-containing compounds. Examples of the thiol group-containing compounds include nonyl mercaptan, 1-dodecanethiol, 1,2-ethanedithiol, 1,3-propanedithiol, triazine thiol, triazine dithiol, triazine trithiol, 1,2,3-propane trithiol, tetraethylene glycol-bis(3-mercaptopropionate), trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetraki ... Examples of the chain transfer agent include erythritol tetrakis thioglucolate, dipentaerythritol hexakis (3-mercaptopropionate), tris [(3-mercaptopropionyloxy)-ethyl]-isocyanurate, 1,4-bis (3-mercaptobutyryloxy) butane, pentaerythritol tetrakis (3-mercaptobutyrate), and 1,3,5-tris (3-mercaptobutyloxyethyl)-1,3,5-triazine-2,4,6- (1H,3H,5H)-trione. The chain transfer agent may be used alone or in combination of two or more.

[0171] The amount of the chain transfer agent is preferably 0.1 to 10 parts by mass, more preferably 0.3 to 5 parts by mass, per 100 parts by mass of the total of the urethane (meth)acrylate and the polymerizable monomer.

[0172] (1.7.5. Manufacturing of Surface Protection Sheets) The surface protection sheet can be manufactured by a known method. For example, first, the above-mentioned adhesive layer composition (if necessary, intermediate layer composition) is prepared. Next, the prepared composition is applied to the surface of a release sheet, a substrate, etc., using a known coating method, and then dried and cured to obtain a surface protection sheet having a predetermined structure.

[0173] (1.8. Steps 4A and 4B) The method for processing a workpiece according to this embodiment is also applicable to DBG or LDBG. In this case, it is preferable to use a surface protection sheet 10 shown in FIG. 5C as the surface protection sheet. In the surface protection sheet 10 shown in FIG. 5C, a buffer layer 14 is formed on a main surface 11b of a substrate 11 opposite to a main surface on which an intermediate layer 12 and an adhesive layer 13 are formed.

[0174] The buffer layer is a layer that is softer than the base material and relieves stress during back grinding of the wafer to prevent cracks and chips from occurring in the wafer. Also, the presence of the buffer layer makes it easier for the wafer to be properly held on the chuck table.

[0175] The thickness of the buffer layer is preferably 1 to 200 μm, more preferably 10 to 100 μm, and further preferably 20 to 80 μm. By setting the thickness of the buffer layer within the above range, the buffer layer can appropriately relieve stress during back grinding.

[0176] The buffer layer may be a layer formed from a buffer layer composition containing an energy ray-polymerizable compound, or may be a film such as a polypropylene film, an ethylene-vinyl acetate copolymer film, an ionomer resin film, an ethylene-(meth)acrylic acid copolymer film, an ethylene-(meth)acrylic acid ester copolymer film, an LDPE film, or an LLDPE film.

[0177] When the workpiece processing method according to this embodiment is applied to DBG or LDBG, a step of forming a groove on the surface of the wafer (step 4A: DBG) or a step of forming a modified region inside the wafer (step 4B: LDBG) is included in addition to the above steps 1 to 3. The groove and modified region are formed so as to follow the parting line when the wafer is divided and singulated into chips in the above step 3.

[0178] When grooves are formed on the surface of the wafer by dicing or the like, step 1 (and step A) is performed after step 4A. That is, in step 1, a surface protection sheet is attached to the surface of the wafer having the grooves formed in step 4A described below.

[0179] The grooves formed in step 4A are shallower than the thickness of the wafer. The grooves can be formed by dicing using a conventionally known dicing device or the like. In step 3 described above, the wafer is divided into a plurality of chips along the grooves by the stress applied during back grinding.

[0180] On the other hand, when forming a modified region on the wafer, step 1 (and step A) may be performed before or after step 4 B. In this embodiment, when forming a modified region on the wafer, it is preferable to perform step 1 (and step A) before step 4 B.

[0181] In addition, the modified region is a brittle portion of the wafer, and is the starting point for the wafer to be destroyed and diced into chips when the wafer becomes thinner due to grinding in the grinding process or when stress is applied during backside grinding.

[0182] The modified region is formed inside the wafer by irradiating the laser focused on the inside of the wafer. The laser may be irradiated from the front side or the back side of the wafer. In the embodiment in which the modified region is formed, when step 4B is performed after step 1 and the laser is irradiated from the front side of the wafer, the laser is irradiated to the wafer through the surface protection sheet.

[0183] In DBG, the back grinding in step 3 is performed to thin the wafer at least to the bottom of the grooves. This back grinding turns the grooves into cuts that penetrate the wafer, and the wafer is divided by the cuts into individual chips.

[0184] In LDBG, the grinding surface (wafer back surface) may reach the modified region by grinding, but it does not have to reach the modified region strictly. In other words, it is sufficient to grind to a position close to the modified region so that the wafer is broken and singulated into chips starting from the modified region. For example, the actual singulation of the chips may be performed by attaching a pick-up tape (described later) and then stretching the pick-up tape.

[0185] After the back surface grinding is completed, dry polishing may be performed prior to picking up the chips.

[0186] Step 2 may be performed as described above, but the surface protection sheet is peeled off from the individual wafers. Even in this case, the convex patterns can be easily peeled off.

[0187] The shape of the individualized chips (workpiece individualized products) obtained through step 2 may be square or elongated, such as rectangular. The thickness of the individualized chips is not particularly limited, but is preferably about 5 to 100 μm, and more preferably 10 to 45 μm. LDBG makes it easy to make the thickness of the individualized chips 50 μm or less, and more preferably 10 to 45 μm. The size of the individualized chips is not particularly limited, but the chip size is preferably 600 mm or less. 2 Less than 400mm, more preferably 2 Less than 120mm, more preferably 2 is less than.

[0188] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and may be modified in various aspects within the scope of the present invention. EXAMPLES

[0189] The present invention will be described in more detail below using examples, but the present invention is not limited to these examples.

[0190] Example 1 (1) Convex pattern As materials for forming a convex pattern, 25 parts by mass of bifunctional polyol-modified urethane acrylate (molecular weight 7300), 75 parts by mass of isobornyl acrylate, 10 parts by mass of dipentaerythritol hexaacrylate (DPHA), 10 parts by mass of silicone-modified acrylate (EBECRYL 1360, functional group number: 6, manufactured by Daicel-Allnex Corporation), and 0.5 parts by mass of photopolymerization initiator (Omnirad1173, manufactured by IGM Resin) were mixed to obtain an energy ray-curable acrylic adhesive composition.

[0191] (2) Surface protection sheet As the surface protective sheet, the surface protective sheet shown below was used.

[0192] A composition for an intermediate layer was obtained by blending 48 parts by mass of a urethane acrylate oligomer (CN9021 NS, manufactured by Arkema Co., Ltd.), 26 parts by mass of isobornyl acrylate, 16 parts by mass of trimethylcyclohexyl acrylate, and 10 parts by mass of lauryl acrylate, for a total of 100 parts by mass, with 3.4 parts by mass of a photopolymerization initiator (Omnirad1173, manufactured by IGM Resin Co., Ltd.) and 1.0 part by mass of a chain transfer agent (Karenz MT PE1, manufactured by Showa Denko K.K.).

[0193] The obtained intermediate layer composition was applied by knife coating onto a substrate PET film (manufactured by Toray Industries, Inc., thickness 75 μm) to a thickness of 400 μm to form an intermediate layer composition layer. Immediately after application, a PET-based release film (manufactured by Lintec Corporation, SP-PET752150, thickness 75 μm) was further laminated onto the intermediate layer composition layer. Thereafter, a high-pressure mercury lamp was used to illuminate the intermediate layer composition layer at an illumination intensity of 120 mW / cm. 2 , light intensity 240mJ / cm 2 The intermediate layer composition layer was irradiated with ultraviolet light under the conditions of 330 mW / cm illuminance using a metal halide lamp. 2 , light intensity 1260mJ / cm 2 The intermediate layer composition layer was cured by irradiating ultraviolet light under the above conditions, thereby forming an intermediate layer having a thickness of 400 μm on the PET film substrate.

[0194] Next, 80 parts by mass of 2-ethylhexyl acrylate (2EHA) and 20 parts by mass of 2-hydroxyethyl acrylate (HEA) were copolymerized to obtain an acrylic copolymer, to which 2-isocyanatoethyl methacrylate (MOI) was added so that the addition ratio was 80 equivalents relative to the hydroxyl group (100 equivalents) derived from HEA. To the energy ray curable acrylic copolymer (weight average molecular weight: 800,000) obtained by adding 1.5 parts by mass of trimethylolpropane adduct tolylene diisocyanate (manufactured by Tosoh, Coronate L) as a crosslinking agent and 2.2 parts by mass of 2,2-dimethoxy-2-phenylacetophenone (manufactured by IGM Resin, Omnirad651) as a photopolymerization initiator, toluene was further added to adjust the solid content concentration to 30%, and the mixture was stirred for 30 minutes to prepare a pressure-sensitive adhesive composition.

[0195] Next, the prepared solution of the adhesive composition was applied to a PET-based release film (SP-PET382150, manufactured by Lintec Corporation, thickness 38 μm) and dried to form an adhesive layer with a thickness of 10 μm, thereby producing an adhesive sheet.

[0196] The release film on the intermediate layer obtained above was removed, and the intermediate layer was laminated to the adhesive layer of the adhesive sheet to produce a surface protection sheet having a substrate / intermediate layer / adhesive layer configuration.

[0197] (Adhesive strength of convex pattern at 50℃) To prepare a workpiece on which a polyimide film was formed as a functional film, a photosensitive negative polyimide resin (HD4104, manufactured by HD Microsystems, Inc.) was applied to one side of a 12-inch diameter silicon mirror wafer, which was then heated and dried to form a fully hardened polyimide film with a thickness of 4 μm.

[0198] The energy ray curable acrylic adhesive composition obtained above was applied to the formed polyimide film to a thickness of 100 μm to form an energy ray curable resin layer. Next, a PET film having a thickness of 50 μm was attached to the formed energy ray curable resin layer. This blocked the energy ray curable resin layer from oxygen. Next, a high pressure mercury lamp was used to illuminate the resin layer with an illuminance of 150 mW / cm. 2 , irradiation amount 300mJ / cm 2 The energy ray curable resin layer was cured by irradiating ultraviolet rays under the conditions of 1. The cured product was cut into a 25 mm width on a wafer to obtain a sample for measuring adhesive strength.

[0199] Next, the obtained adhesive strength test sample was peeled off from the wafer (polyimide film) at a peel angle of 180° and a peel speed of 120 mm / min while heating the wafer to 50° C. The results are shown in Table 1.

[0200] (Tensile elongation at break for convex pattern) The energy ray curable acrylic adhesive composition obtained above was applied to a PET release film to a thickness of 100 μm to form an energy ray curable resin layer. Next, a PET film was attached onto the energy ray curable resin layer thus formed. This blocked the energy ray curable resin layer from oxygen. Next, a high pressure mercury lamp was used to illuminate the resin layer with an illuminance of 150 mW / cm. 2 , irradiation amount 300mJ / cm2 The energy ray curable resin layer was cured by irradiating ultraviolet rays under the above conditions to obtain a cured product. The obtained cured product was cut together with a PET-based release film into a width of 15 mm and a length of 100 mm to obtain a sample for measuring tensile elongation at break. The tensile elongation at break of the obtained sample for measuring tensile elongation at break was measured at 23°C in accordance with JISK7161:2014 and JISK7127:1999. Specifically, the sample for measuring tensile elongation at break was subjected to a tensile test at a speed of 200 mm / min using a tensile tester (manufactured by Shimadzu Corporation, product name "Autograph AG-IS500N") with a chuck distance set to 100 mm, and the tensile elongation at break (%) was measured. The results are shown in Table 1.

[0201] (Peelability of convex patterns) A silicon wafer (thickness 760 μm) with bump electrodes, the height of which was 200 μm and the pitch of which was 400 μm, was prepared. A polyimide film (functional film) with a thickness of 4 μm was formed on the surface of this silicon wafer with bump electrodes. The energy ray curable acrylic pressure sensitive adhesive composition obtained above was applied to the outer periphery of this silicon wafer with bump electrodes, where the bump electrodes were not formed, using a dispenser (Musashi Engineering Co., Ltd., shotmaster350DS), to a thickness of 100 μm and a width of 4 mm so that no gap was formed between the outer edge of the wafer and the composition, and then dried to form a convex pattern.

[0202] A surface protection sheet was attached to the silicon wafer with bump electrodes after the convex pattern was formed using a tape laminator (manufactured by Lintec, RAD-3510F / 12) with the lamination table temperature at 65°C. The wafer with the surface protection sheet attached was placed on the chuck table so that the surface protection sheet was in contact with the chuck table, and the wafer was adsorbed and fixed to the chuck table by suction. Next, the back surface of the wafer was ground with a grinding wheel, and grinding was terminated when the wafer thickness reached 150 μm. After grinding was completed, ultraviolet light (illuminance 230 mW / cm) was irradiated to the front surface of the wafer using a peeling device (manufactured by Lintec, RAD-3010F / 12). 2 , 1200mJ / cm 2) was carried out, and peel tests were carried out separately at a peel temperature of 50°C and a peel speed of 2 mm / min (low speed) and 5 mm / min (high speed), and the peeling state of the surface protection sheet and the convex pattern were evaluated. The results are shown in Table 1. ○: No convex patterns remain on the wafer ×: At least a part of the convex pattern remains on the wafer.

[0203] (Examples 2 and 3 and Comparative Example 1) The physical properties and peelability of the convex pattern were evaluated in the same manner as in Example 1, except that the composition of the energy ray-curable acrylic pressure-sensitive adhesive composition constituting the convex pattern was the composition shown in Table 1. The results are shown in Table 1. In Example 2, a silicone-modified acrylate (manufactured by Daicel-Allnex Corporation, EBECRYL 350, number of functional groups: 2) was used instead of the silicone-modified acrylate (manufactured by Daicel-Allnex Corporation, EBECRYL 1360, number of functional groups: 6).

[0204] [Table 1]

[0205] From Table 1, it was confirmed that when the convex pattern satisfies the above-mentioned physical properties, the peelability of the convex pattern is good. [Explanation of symbols]

[0206] 1...Work (wafer) 2a...Convex electrode, 2b...Chip 3…Convex pattern 10...Surface protection sheet 11...Base material 12...Adhesive layer 13. Middle class 14...Buffer layer

Claims

1. A workpiece having a surface having a height difference and a back surface opposite to the surface, the surface having a convex pattern formed thereon to suppress the effect of the height difference of the surface, comprising: a step of attaching the surface protective sheet to the surface; and peeling off the surface protective sheet attached to the surface and at least a part of the convex pattern from the surface, A method for processing a workpiece, wherein the adhesive strength of the convex pattern to a workpiece having a polyimide film formed thereon at 50°C is 1000 mN / 25 mm or less.

2. The method for machining a workpiece according to claim 1 , wherein the tensile elongation at break of the convex pattern is 4% or more.

3. 3. The method for machining a workpiece according to claim 1, wherein the convex pattern is made of a resin composition.

4. 3. The method for machining a workpiece according to claim 1, further comprising a step of grinding the back surface of the workpiece to which the surface protection sheet is attached.

5. A method for machining a workpiece as described in claim 1 or 2, wherein the surface has an inner circumference and an outer circumference surrounding the inner circumference, the height of the outer circumference is lower than the height of the inner circumference, and the convex pattern is formed on the outer circumference.

6. The method for machining a workpiece according to claim 1 or 2, wherein a functional film is formed on at least a part of the surface.

7. 3. The method for machining a workpiece according to claim 1, wherein the workpiece has a convex electrode formed on the surface thereof.

8. The method for machining a workpiece according to claim 5 , wherein the convex pattern is formed at a distance from an outer edge of the workpiece.

9. The method for processing a workpiece according to claim 1 or 2, wherein the surface protection sheet has a base material and an adhesive layer.

10. A step of forming a groove on the surface of the workpiece before the step of attaching a surface protection sheet to the surface of the workpiece, 5. The method for machining a workpiece according to claim 4, wherein in the step of grinding the rear surface of the workpiece, the workpiece is diced into a plurality of workpiece pieces starting from the grooves.

11. A process for forming a modified region inside the workpiece before the process for grinding the back surface of the workpiece, The method for machining a workpiece according to claim 4 , wherein in the step of grinding the rear surface of the workpiece, the workpiece is diced into a plurality of workpiece individual pieces starting from modified regions.

12. A resin composition having an adhesive strength of 1000 mN / 25 mm or less to a workpiece having a polyimide film formed thereon.

13. The resin composition according to claim 12, having a tensile elongation at break of 4% or more.

14. The resin composition according to claim 12 or 13, which is used to form a convex pattern in a workpiece having a surface with a height difference and a back surface opposite the surface, in order to suppress the effect of the height difference on the surface.

15. The resin composition according to claim 12 or 13, wherein the resin composition is energy ray curable, and the adhesive strength is the adhesive strength after curing with the energy ray.

Citation Information

Patent Citations

  • Method of manufacturing semiconductor device, sealing member used for method, and feeder of sealing member

    JP2004288725A

  • Surface protection sheet and method for grinding semiconductor wafer

    JP2005123382A

  • Thermosensitive pressure-sensitive adhesive

    JP2012087218A

  • Method for sticking surface protective tape

    JP2013247133A

  • Temperature-sensitive adhesive

    JP2015187238A