Method for producing chabazite-type zeolite for carbon dioxide adsorption and chabazite-type zeolite

By converting FAU zeolite to CHA zeolite with adjusted SAR and ion exchange, the method addresses the limitations of existing CHA zeolite synthesis, resulting in enhanced CO2 adsorption capacity for carbon dioxide capture.

JP2024136618APending Publication Date: 2024-10-04JGC CATALYSTS & CHEMICALS LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023047775
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing methods for synthesizing chabazite-type zeolite (CHA) struggle with adjusting the SiO2/Al2O3 molar ratio (SAR) and crystal structure, limiting its carbon dioxide (CO2) adsorption capacity.

Method used

A method involving the conversion of faujasite-type zeolite (FAU) to CHA zeolite by adjusting the SAR and replacing sodium ions with potassium ions, using a series of steps including slurry preparation, hydrothermal treatment, and ion exchange processes to enhance CO2 adsorption.

Benefits of technology

The method produces CHA zeolite with improved CO2 adsorption capacity, achieving higher adsorption amounts through optimized SAR and ion exchange, thereby enhancing its effectiveness as a carbon dioxide adsorbent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136618000001
    Figure 2024136618000001
  • Figure 2024136618000002
    Figure 2024136618000002
Patent Text Reader

Abstract

To provide a CHA-type zeolite having a high adsorption amount of CO2.SOLUTION: A method for producing chabazite-type zeolite comprises the steps of: mixing a solvent with FAU-type zeolite to prepare a slurry; and hydrothermally treating the slurry to prepare the chabazite-type zeolite. The method further comprises: a base addition step of adding a salt containing hydroxide ions so that a ratio (OH- / Si) of hydroxide ions (OH-) to Si in the FAU zeolite becomes 0.38 or more before performing the hydrothermal treatment; and a step of adding a salt containing potassium ions before performing the hydrothermal treatment. The method further comprises at least one sodium substitution step of a sodium addition step of adding a salt containing sodium ions before performing the hydrothermal treatment, and an ion exchange step of exchanging ions by adding the salt containing sodium ions to the chabazite-type zeolite.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a chabazite-type zeolite for adsorbing carbon dioxide.

[0002] Carbon dioxide (CO2) is one of the greenhouse gases that causes global warming, and the Paris Agreement mandates that its emissions be reduced. Zeolites are used as CO2 adsorbents to separate and capture CO2 generated at power plants, factories, etc. from other gases. Chabazite-type zeolites (CHA zeolites) are known to be particularly good at adsorbing CO2 (see, for example, Patent Document 1). CHA zeolites can be synthesized using a structure-directing agent (SDA) that serves as a template. CO2 emissions can be reduced by recycling the separated and captured CO2 as a raw material for chemical products, etc. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2015-116532 Summary of the Invention [Problem to be solved by the invention]

[0004] In Patent Document 1, CO2 is adsorbed onto CHA zeolite. However, because CHA zeolite is synthesized using SDA (SDA method), there is a problem in that it is not possible to adjust the SiO2 / Al2O3 molar ratio (SAR) or crystal structure to increase the CO2 adsorption amount. [Means for solving the problem]

[0005] The present inventors have adjusted the SAR and other properties by producing CHA zeolite using FAU-type zeolite (conversion method), and further + A part of the sodium ions (Na +), it has been found that CHA zeolite with a high CO2 adsorption capacity can be produced. That is, the method for producing chabazite-type zeolite includes a step of mixing a solvent and FAU-type zeolite to prepare a slurry, and a step of hydrothermally treating the slurry to prepare chabazite-type zeolite. Furthermore, prior to the hydrothermal treatment, hydroxide ions (OH - ) and the ratio of Si in FAU-type zeolite (OH - The method further comprises a base addition step of adding a salt containing hydroxide ions and a step of adding a salt containing potassium ions before the hydrothermal treatment so that the ratio (kJ / Si) is 0.38 or more. The method further comprises at least one sodium substitution step of a sodium addition step of adding a salt containing sodium ions before the hydrothermal treatment and an ion exchange step of performing ion exchange by adding a salt containing sodium ions to chabazite-type zeolite.

[0006] Furthermore, the chabazite-type zeolite has an SAR of 5 to 9 and contains 1 to 25% by weight of Na in terms of Na2O. DETAILED DESCRIPTION OF THE INVENTION

[0007] The present invention relates to a method (conversion method) for producing chabazite-type zeolite (CHA zeolite) using faujasite-type zeolite (FAU zeolite). CHA zeolite can be produced as follows: First, a solvent and FAU zeolite are mixed to prepare a slurry (slurry preparation step). The slurry is then subjected to hydrothermal treatment to produce CHA zeolite (zeolite production step). Before the hydrothermal treatment, hydroxide ions (OH - ) is added to the solution <hydroxide addition process>. + ) is added to the solution (potassium (K) addition process). + A part of the sodium ions (Na + The sodium (Na) substitution process replaces the salt with cations (cations) and anions (cation anions). This increases the carbon dioxide (CO2) adsorption capacity of CHA zeolite.

[0008] K + A part of which is replaced with Na + There are two methods as follows. The first is the ion exchange method <ion exchange step> by adding a salt containing Na + to the generated CHA zeolite. In this method, K + adsorbed on the sites (cation sites) that adsorb cations in the CHA zeolite is ion-exchanged with Na + . The second is the method <Na addition step> of adding a salt containing Na + before hydrothermal treatment. In this method, Na + adsorbs to the cation sites of the CHA zeolite instead of a part of K + that adsorbs to the cation sites of the CHA zeolite when the CHA zeolite is generated. In the Na substitution step, it is preferable to adjust the Na content in the CHA zeolite to 1 to 25% by weight in terms of Na2O. The higher this Na content, the larger the amount of Na + adsorbed on the cation sites, and the larger the CO2 adsorption amount (hereinafter simply abbreviated as CO2 adsorption amount) per 1 g of the CHA zeolite. Therefore, this Na content rate is preferably 2% by weight or more, and more preferably 5% by weight or more. On the other hand, the lower this Na content, the higher the ratio of Na adsorbed on the cation sites of the CHA zeolite to the total amount of Na in the CHA zeolite. As a result, the excess Na in the CHA zeolite decreases, and the CO2 adsorption amount increases. Therefore, this Na content is preferably 20% by weight or less, and more preferably 15% by weight or less. Here, it can be said that the lower the K content in the CHA zeolite, the larger the amount of Na present in the cation sites of the CHA zeolite. Therefore, it is preferable to adjust the K content in the CHA zeolite to 10% by weight or less (in terms of K) by the Na substitution step. This K content is more preferably 5% by weight or less, and even more preferably 0.5% by weight or less. Also, it is preferable to adjust the molar ratio (K / Na) of K and Na in the CHA zeolite to 0 to 30 by the Na substitution step. This ratio is more preferably 10 or less, and even more preferably 3 or less. This molar ratio is even more preferably 1 or less. Hereinafter, the two methods will be described in detail.

[0009] <Ion exchange process> In this process, Na is added to CHA zeolite. + By adding salts containing + Na + In other words, ion exchange occurs. + Na + To exchange Na with CHA zeolite, Na should be in ionic form and in contact with the zeolite. + A salt containing Na is ionized in water (aqueous solution). + In particular, Na + When normal salt is used as the salt containing Na, the pH of the aqueous solution becomes close to neutral, and the SiO2 / Al2O3 molar ratio (SAR) of CHA zeolite is difficult to change. Therefore, it is easy to adjust the SAR of CHA zeolite. In addition, when CHA zeolite is dispersed in water (CHA zeolite aqueous dispersion), Na + It is preferable to add a salt containing K. + Na + When this method is used, the ion exchange is quicker when the concentration of the aqueous dispersion of CHA zeolite is high. Therefore, this concentration is preferably 5% by weight or more, more preferably 10% by weight or more. On the other hand, the lower this concentration, the easier it is for the aqueous dispersion of CHA zeolite and Na + This makes it easier to mix salts containing Si and Al. Therefore, this concentration is preferably 30% by weight or less, and more preferably 25% by weight or less. Furthermore, the higher the temperature of the aqueous dispersion of CHA zeolite, the faster the ion exchange occurs. Therefore, this temperature is preferably 50°C or higher, and more preferably 60°C or higher. Furthermore, the longer the ion exchange time, the more the ion exchange progresses. Therefore, this time is preferably 1 minute or more, and more preferably 30 minutes or more. On the other hand, if this time is too long, the production efficiency decreases. Therefore, this time is preferably 10 hours or less. Furthermore, the closer the pH of this aqueous dispersion is to neutral, the less Si and Al are eluted, making it easier to adjust the SAR of CHA zeolite. Therefore, this pH is preferably 4 to 10, and more preferably 5 to 9.

[0010] <Sodium addition step> In this step, a salt containing Na is added before the hydrothermal treatment. This makes it easier for Na to fit into the cation sites of the CHA zeolite. As a result, the CO2 adsorption capacity of the CHA zeolite increases. The salts containing Na that can be used are the same as those described in the <Ion exchange step>. When this step is performed, the <Ion exchange step> does not need to be carried out, so the process can be simplified. Also, when using sodium hydroxide, it can be added as a hydroxide in the <Hydroxide addition step>, so the process can be simplified. On the other hand, by performing both this step and the <Ion exchange step>, the proportion of Na adsorbed on the cation sites can be increased. + to fit into the cation sites of the CHA zeolite. As a result, the CO2 adsorption capacity of the CHA zeolite increases. The salts containing Na that can be used are the same as those described in the <Ion exchange step>. When this step is performed, the <Ion exchange step> does not need to be carried out, so the process can be simplified. Also, when using sodium hydroxide, it can be added as a hydroxide in the <Hydroxide addition step>, so the process can be simplified. On the other hand, by performing both this step and the <Ion exchange step>, the proportion of Na adsorbed on the cation sites can be increased. + to fit into the cation sites of the CHA zeolite. As a result, the CO2 adsorption capacity of the CHA zeolite increases. The salts containing Na that can be used are the same as those described in the <Ion exchange step>. When this step is performed, the <Ion exchange step> does not need to be carried out, so the process can be simplified. Also, when using sodium hydroxide, it can be added as a hydroxide in the <Hydroxide addition step>, so the process can be simplified. On the other hand, by performing both this step and the <Ion exchange step>, the proportion of Na adsorbed on the cation sites can be increased. + to fit into the cation sites of the CHA zeolite. As a result, the CO2 adsorption capacity of the CHA zeolite increases. The salts containing Na that can be used are the same as those described in the <Ion exchange step>. When this step is performed, the <Ion exchange step> does not need to be carried out, so the process can be simplified. Also, when using sodium hydroxide, it can be added as a hydroxide in the <Hydroxide addition step>, so the process can be simplified. On the other hand, by performing both this step and the <Ion exchange step>, the proportion of Na adsorbed on the cation sites can be increased. + to fit into the cation sites of the CHA zeolite. As a result, the CO2 adsorption capacity of the CHA zeolite increases. The salts containing Na that can be used are the same as those described in the <Ion exchange step>. When this step is performed, the <Ion exchange step> does not need to be carried out, so the process can be simplified. Also, when using sodium hydroxide, it can be added as a hydroxide in the <Hydroxide addition step>, so the process can be simplified. On the other hand, by performing both this step and the <Ion exchange step>, the proportion of Na adsorbed on the cation sites can be increased.

[0011] The greater the amount of Na added, the more likely the CO2 adsorption capacity of the CHA zeolite is to increase. It is preferable to add a salt containing Na so that the addition amount of Na is 2 parts by mass or more with respect to 100 parts by mass of the FAU zeolite. This addition amount is more preferably 4 parts by mass or more, and even more preferably 6 parts by mass or more. There is no upper limit to this addition amount, but the lower the addition amount, the lower the cost. Therefore, 100 parts by mass or less is preferable, 50 parts by mass or less is more preferable, and 25 parts by mass or less is even more preferable. This addition amount does not include the Na contained in the FAU zeolite. + The greater the amount of Na added, the more likely the CO2 adsorption capacity of the CHA zeolite is to increase. It is preferable to add a salt containing Na so that the addition amount of Na is 2 parts by mass or more with respect to 100 parts by mass of the FAU zeolite. This addition amount is more preferably 4 parts by mass or more, and even more preferably 6 parts by mass or more. There is no upper limit to this addition amount, but the lower the addition amount, the lower the cost. Therefore, 100 parts by mass or less is preferable, 50 parts by mass or less is more preferable, and 25 parts by mass or less is even more preferable. This addition amount does not include the Na contained in the FAU zeolite. + The greater the amount of Na added, the more likely the CO2 adsorption capacity of the CHA zeolite is to increase. It is preferable to add a salt containing Na so that the addition amount of Na is 2 parts by mass or more with respect to 100 parts by mass of the FAU zeolite. This addition amount is more preferably 4 parts by mass or more, and even more preferably 6 parts by mass or more. There is no upper limit to this addition amount, but the lower the addition amount, the lower the cost. Therefore, 100 parts by mass or less is preferable, 50 parts by mass or less is more preferable, and 25 parts by mass or less is even more preferable. This addition amount does not include the Na contained in the FAU zeolite. + The greater the amount of Na added, the more likely the CO2 adsorption capacity of the CHA zeolite is to increase. It is preferable to add a salt containing Na so that the addition amount of Na is 2 parts by mass or more with respect to 100 parts by mass of the FAU zeolite. This addition amount is more preferably 4 parts by mass or more, and even more preferably 6 parts by mass or more. There is no upper limit to this addition amount, but the lower the addition amount, the lower the cost. Therefore, 100 parts by mass or less is preferable, 50 parts by mass or less is more preferable, and 25 parts by mass or less is even more preferable. This addition amount does not include the Na contained in the FAU zeolite.

[0012] Also, the lower the addition ratio [K / Na] of K added in the <Potassium addition step> and Na added in the <Sodium addition step> before the hydrothermal treatment, the more likely the CO2 adsorption capacity of the CHA zeolite is to increase. Therefore, this addition ratio is preferably 10 or less, more preferably 5 or less, and even more preferably 2 or less. This addition ratio is even more preferably 0.5 or less. Here, the Na added in the <Sodium addition step> does not include the Na contained in the raw material FAU zeolite.

[0013] Hereinafter, each step will be described in detail.

[0014] <Slurry preparation process> In this step, a slurry is prepared by mixing a solvent and FAU zeolite. The SAR of the FAU zeolite is preferably 5 or more. When the SAR is within this range, CHA zeolite is easily produced. The SAR of the FAU zeolite is preferably 5 to 10. When the SAR is within this range, the SAR of the CHA zeolite is likely to be 5 to 9, and the CO2 adsorption capacity of the CHA zeolite is likely to be large. Either water or an organic solvent can be used as the solvent. When water is used, hydrothermal synthesis can be performed safely. Furthermore, the smaller the amount of Na ions in the FAU zeolite, the easier it is to produce CHA zeolite. Therefore, the Na content in the FAU zeolite, calculated as Na2O, is preferably 13 wt% or less, more preferably 7.5 wt% or less, and even more preferably 5 wt% or less.

[0015] X-type and Y-type zeolites are known as FAU-type zeolites. Of these, the SAR of Y-type zeolite can be easily adjusted to 5 to 10. Y-type zeolite can be prepared by the method described in Japanese Patent No. 6320658. Examples of Y-type zeolites include NaY-type zeolite, ultrastable Y-type zeolite (USY zeolite), and rare earth ion-exchanged Y-type zeolite (ReY). Of these, it is preferable to use USY zeolite. The SAR of USY zeolite can be easily adjusted to 5 to 10, and the Na content of USY zeolite can easily be reduced.

[0016] The higher the solids concentration of the slurry, the higher the production efficiency. Therefore, the solids concentration of the slurry is preferably 5% by weight or more, and more preferably 10% by weight or more. On the other hand, the lower the solids concentration of the slurry, the easier it is to work with. Therefore, the solids concentration of the slurry is preferably 50% by weight or less, more preferably 30% by weight or less, and even more preferably 20% by weight or less.

[0017] <Hydroxide addition process> In this process, before the hydrothermal treatment, OH - Add a salt containing OH - and Si in FAU zeolite (OH - / Si) to be 0.38 or more.- By adding a salt containing OH, the formation of CHA zeolite becomes easier. - The salt containing OH may be added in small portions or at once. - Examples of the salt containing OH include hydroxides of alkali metals and alkaline earth metals. Using hydroxides of Na or K can simplify the process. In the hydrothermal treatment, the slurry may be stirred or left standing. - The pH tends to increase after adding the salt containing OH. For example, the pH of the slurry becomes 9 or higher.

[0018] <Potassium addition step> In this step, a salt containing K is added before the hydrothermal treatment. + Examples of the salt containing K include potassium carbonate, potassium chloride, potassium nitrate, potassium hydroxide, etc. Especially when using potassium hydroxide, it can be added as a hydroxide in the hydroxide addition step, simplifying the process. + The addition amount of K is preferably 1.6 parts by mass or more. + When the addition amount of K is within this range, CHA zeolite is likely to be formed. + The addition amount of K is preferably 100 parts by mass or less. + When the addition amount of K is within this range, CHA zeolite is likely to be formed. + When the addition amount is within this range, CHA zeolite is likely to be formed.

[0019] <Zeolite formation step> In this step, CHA zeolite is formed by subjecting a slurry containing FAU zeolite, K, and OH to hydrothermal treatment. In the hydrothermal treatment, since the slurry is filled in a sealed container such as an autoclave, the pressure applied to the slurry can be made higher than atmospheric pressure. Therefore, the temperature of the slurry can be made higher than the boiling point of the solvent. The temperature of the hydrothermal treatment is preferably 130°C or higher. On the other hand, when this temperature is 190°C or lower, it is difficult to form crystals other than CHA. Also, the longer the hydrothermal treatment time, the easier it is to form CHA zeolite. Therefore, this time is preferably 12 hours or more. On the other hand, the shorter this time, the lower the cost. Therefore, this time is preferably 96 hours or less. ​​​​

[0020] The X-ray diffraction measurement pattern of the obtained zeolite can be compared with the CHA-type zeolite X-ray diffraction pattern described in "Collection of Simulated XRD Powder Patterns for Zeolites," edited by M.M.J. Treacy and J.B. Higgins, 4th edition, published in 2001, to confirm that CHA-type zeolite has been produced.

[0021] The less the amount of FAU zeolite remaining in the raw material, the greater the CO2 adsorption capacity of CHA zeolite. Here, when the produced CHA zeolite was measured by XRD, the peak intensity I of the (111) plane of the FAU peak was F and the peak intensity of the (100) plane of CHA zeolite I c Ratio to [I F / I c The smaller the ratio, the less FAU zeolite remains. This ratio is preferably 0.1 or less.

[0022] It is preferable to wet-pulverize the slurry before the hydrothermal treatment. When wet-pulverized, the ratio (OH) before the hydrothermal treatment is - Even if the ratio (Hb / Si) is low, CHA zeolite is easily produced. When wet-pulverizing, this ratio is preferably 0.55 or less, more preferably 0.47 or less. A ball mill, a bead mill, or the like can be used for wet-pulverizing. It is preferable to wet-pulverize so that the total intensity (Hb) of the FAU zeolite contained in the slurry after wet-pulverization is half or less (0.5Ha≧Hb) of the total intensity (Ha) of the three peaks [peaks attributed to Miller indices (111), (331), and (533)] that appear in the X-ray diffraction pattern of the FAU zeolite contained in the slurry before wet-pulverization. By pulverizing FAU zeolite in this way, OH - Even if the amount of salt containing hydroxypropyl methyl ketone added is reduced, CHA zeolite is more easily produced. The lower the temperature of the slurry during wet grinding, the higher the yield of CHA zeolite. Therefore, the temperature of the slurry during wet grinding is preferably 65°C or lower, and more preferably 50°C or lower. The lower limit of the slurry temperature should be higher than the boiling point of the solvent. For example, for water, it is 0°C or higher.

[0023] The CHA zeolite will be described below. The SAR of the CHA-type zeolite is 5 to 9. Such a CHA zeolite contains 1% by weight or more of Na. As a result, the CO2 adsorption amount of the CHA zeolite increases. When the Na content of the CHA zeolite is less than 1% by weight, the CO2 adsorption amount of the CHA zeolite is small. The higher this Na content, the greater the CO2 adsorption amount of the CHA zeolite. Therefore, this Na content is preferably 3% by weight or more, and more preferably 5% by weight or more. On the other hand, when this Na content is too high, Na cannot fit into the cation sites of the zeolite, and Na becomes an impurity. Therefore, this Na content is preferably 20% by weight or less, preferably 15% by weight or less, and more preferably 12% by weight or less. When the SAR of the CHA-type zeolite is less than 5, the crystallite size of the CHA zeolite decreases, and the specific surface area of the CHA zeolite becomes small. As a result, the CO2 adsorption amount of the CHA zeolite decreases. When SAR is greater than 9, the cation sites in the CHA zeolite decrease, so the CO2 adsorption amount of the CHA zeolite is small. Examples of the shape of the CHA zeolite include particulate, plate-like, rod-like, and die-like shapes.

[0024] When measuring the CHA-type zeolite by XRD, the peak intensity I of the (100) plane of the Miller index 100 and the peak intensity I of the (211) plane 211 The lower the intensity ratio [I 100 / I 211 , the greater the CO2 adsorption amount of the CHA zeolite. Therefore, this ratio [I 100 / I 211 is preferably 0.8 or less, more preferably 0.65 or less, and even more preferably 0.5 or less. In the zeolite prepared by the conversion method, this ratio [I 100 / I 211 tends to be low. Also, the greater the amount of Na added in the aforementioned <Na addition step>, the more likely this ratio [I 100 / I 211 is to be low.

[0025] A CO2 adsorbent can be manufactured using the chabazite-type zeolite described above. In addition to the chabazite-type zeolite, binders, sintering aids, bulking agents, etc. may be added to the CO2 adsorbent. Examples of binders include celluloses such as methyl cellulose, starch, and polyvinyl alcohol. Examples of sintering aids include inorganic oxides such as silica and alumina.

[0026] A CO2 adsorbent may be produced by molding chabazite-type zeolite. Examples of molding methods include extrusion molding and tablet molding. It is preferable to add a binder and a sintering aid to the CHA zeolite before molding. After molding, it is preferable to dry and calcinate the molded product. The drying temperature is preferably 20 to 150°C, and the calcination temperature is preferably 500 to 700°C.

[0027] The preparation method and properties of CHA zeolite are specifically explained below. The preparation conditions are shown in Table 1.

[0028] [Example 1] <Slurry preparation process (including hydroxide addition process, potassium addition process, and sodium addition process)> 20.7 g of 48.0 mass% NaOH and 2.8 g of 95.5 mass% KOH were added to 416.4 g of pure water, followed by 60.1 g of FAU zeolite (SAR: 7.0, NaO content: 1.14 wt %; the same FAU zeolite is used in the following examples and comparative examples) to obtain a slurry.

[0029] This slurry was wet-pulverized using a bead mill (LMZ015, manufactured by Ashizawa Finetech Co., Ltd.) until the Hb concentration reached 0.5 Ha or higher. The wet-pulverization conditions were zirconia beads of 0.5 mm, a peripheral speed of 10 m / s, and a bead loading of 85% (volume equivalent). The slurry was dried at 180°C for 30 minutes, and the resulting powder was pulverized in a mortar to prepare a sample for X-ray diffraction measurement. This was placed on a sample plate and subjected to X-ray diffraction measurement under the following measurement conditions to determine the peak intensity of each Miller index. (Measurement conditions: Apparatus: MiniFlex (registered trademark), manufactured by Rigaku Corporation; Operating axis: 2θ / θ; Radiation source: CuKα; Measurement method: Continuous; Voltage: 40 kV; Current: 15 mA; Start angle: 2θ = 5°; End angle: 2θ = 50°; Sampling width: 0.020°; Scan rate: 10,000° / min.)

[0030] <Zeolite production process> The wet-milled slurry was hydrothermally treated for 24 hours at 165° C. The hydrothermally treated synthesized slurry was then taken out, filtered, washed, and dried (110° C. for 10 hours) to obtain CHA zeolite (powder).

[0031] The obtained powder (Na-exchanged CHA zeolite when an ion exchange step was performed in the following Examples and Comparative Examples) was measured and evaluated as follows (1) to (3). The measurement and evaluation results of the following Examples and Comparative Examples are also shown in Table 2.

[0032] (1) X-ray diffraction measurement (crystal system, XRD peak ratio) The resulting powder was crushed in a mortar and placed on a sample plate. X-ray diffraction measurements were performed under the same conditions as described above. If the resulting X-ray diffraction pattern contained all peaks attributable to the Miller indices (100), (200), (20-1), (21-1), (211), (3-1-1), (310), and (3-1-2), the sample was determined to have a chabazite crystal structure. The intensity ratio of the peaks attributable to the Miller indices (100) and (211) was calculated.

[0033] (2) Elemental analysis (SAR, K content, Na content) Approximately 0.5 g of CHA zeolite was placed on a platinum dish and 10 ml of hydrofluoric acid and 10 ml of (1 + 1) sulfuric acid were added. The mixture was heated in a sand bath until white sulfuric acid fumes were released, and water was added to dissolve the mixture. The resulting solution was then diluted to volume in a 200 ml volumetric flask. 10 ml of the solution was then diluted to volume in a 100 ml volumetric flask to create the test solution. Na and K were measured using an atomic absorption spectrometer (Hitachi High-Tech Z-2310), and Al was measured using an ICP spectrometer (Shimadzu ICPS-8100). The Na, K, and Al contents were converted to Na2O, K2O, and Al2O3, respectively. The SiO2 value was calculated by subtracting the Al2O3, Na2O, and K2O contents (wt%) from 100 wt%. The SiO2 and Al2O3 contents were converted to molar ratios to calculate the SAR.

[0034] (3) Measurement of CO2 adsorption amount A sample tube was filled with 0.1 g of the resulting powder and heated to 400°C at a rate of 10°C / min in a 100% He (50 SCCM) gas flow. The temperature was then maintained for 60 minutes and then allowed to cool to 30°C. While the test tube was maintained at 30°C, a 1% CO2 / He gas (50 SCCM) mixture was passed through the tube for 25 minutes. The breakthrough point was determined when a detector (TCD, Microtrac-Bell BEL-CAT2) detected CO2. The total amount of CO2 passed from the start of flow to the breakthrough point was calculated. A similar measurement was performed on an empty sample tube to determine the total amount of CO2 passed from the start of flow to the breakthrough point. The difference between the two total amounts was used as the CO2 adsorption amount.

[0035] [Example 2] 18.0 g of 48.0 mass% NaOH and 4.7 g of 95.5 mass% KOH were added to 417.3 g of pure water. Then, 60.0 g of FAU zeolite was added to obtain a slurry. The same procedure as in Example 1 was carried out except that this slurry was used to obtain CHA zeolite.

[0036] [Example 3] 11.4 g of 48.0 mass% NaOH and 9.3 g of 95.5 mass% KOH were added to 419.5 g of pure water. Then, 59.8 g of FAU zeolite was added to obtain a slurry. The same procedure as in Example 1 was carried out except that this slurry was used to obtain CHA zeolite.

[0037] [Example 4] 4.8 g of 48.0 mass% NaOH and 13.9 g of 95.5 mass% KOH were added to 421.6 g of pure water. Then, 59.7 g of FAU zeolite was added to obtain a slurry. The same procedure as in Example 1 was carried out except that this slurry was used to obtain CHA zeolite.

[0038] [Example 5] 11.2 g of 48.0 mass% NaOH and 11.7 g of 95.5 mass% KOH were added to 417.5 g of pure water. Next, 59.6 g of FAU zeolite was added to obtain a slurry. The same procedure as in Example 1 was carried out except that this slurry was used to obtain CHA zeolite.

[0039] [Example 6] 14.6 g of 48.0 mass% NaOH and 11.6 g of 95.5 mass% KOH were added to 414.4 g of pure water. Then, 59.5 g of FAU zeolite was added to obtain a slurry. The same procedure as in Example 1 was carried out except that this slurry was used to obtain CHA zeolite.

[0040] [Example 7] CHA zeolite was obtained using the same recipe as in Example 2.

[0041] <Ion exchange process> 10.0 g of CHA zeolite and 20.0 g of 100% NaCl were added to 200.0 g of pure water, and the mixture was then kept at 80°C for 1 hour, filtered, and washed. This resulted in ion exchange. The same procedure was repeated five more times using the washed CHA zeolite instead of the 10.0 g of CHA zeolite. The resulting CHA zeolite was dried to obtain Na-exchanged CHA zeolite.

[0042] [Example 8] 19.5 g of KOH with a concentration of 95.5 mass% was added to 421.2 g of pure water. Next, 58.7 g of FAU zeolite was added to obtain a slurry. CHA zeolite was obtained in the same manner as in Example 1 except that this slurry was used. Na-exchanged zeolite was obtained by carrying out the ion exchange step in the same manner as in Example 7 except that the CHA zeolite obtained in this example was used.

[0043] [Example 9] 26.0 g of KOH with a concentration of 95.5% by mass was added to 415.3 g of pure water. Next, 58.7 g of FAU zeolite was added to obtain a slurry. CHA zeolite was obtained in the same manner as in Example 1, except that this slurry was used and wet pulverization was not performed. Na-exchanged zeolite was obtained by performing the ion exchange step in the same manner as in Example 7, except that the CHA zeolite obtained in this example was used.

[0044] [Example 10] 60.0 g of FAU zeolite was added to 417.3 g of pure water to obtain a slurry. This slurry was wet-pulverized under the same conditions as in Example 1. 18.0 g of 48.0 mass% NaOH and 4.7 g of 95.5 mass% KOH were added to this slurry, and then hydrothermal synthesis was performed to obtain CHA zeolite.

[0045] [Comparative Example 1] A compounded slurry was obtained by adding and mixing 46.4 g of a 25% N,N,N-trimethyladamantanammonium aqueous solution (manufactured by Seichem Japan), 0.3 g of 95.5 mass% KOH, 25.4 g of a sodium aluminate aqueous solution (AlO concentration 22 mass%, NaO concentration 17 mass%), and 34.7 g of fumed silica (Reolosil (registered trademark) QS40, manufactured by Tokuyama Corporation) to 393.1 g of pure water. This compounded slurry was hydrothermally treated at 150°C for 96 hours. The hydrothermally treated synthesized slurry was then extracted, filtered, washed, and dried to obtain CHA zeolite. The CHA zeolite was calcined at 600°C for 3 hours. A Na-exchanged zeolite was obtained by performing the ion exchange process in the same manner as in Example 7, except that the CHA zeolite obtained in this example was used.

[0046] Comparative Example 2 15.0 g of 95.5 mass % KOH was added to 425.2 g of pure water. Then, 59.8 g of FAU zeolite was added to obtain a slurry. CHA zeolite was obtained in the same manner as in Example 1, except that this slurry was used.

[0047] Comparative Example 3 The CHA zeolite of Example 8 was used.

[0048] Comparative Example 4 26.0 g of 95.5 mass % KOH was added to 415.3 g of pure water. Then, 58.7 g of FAU zeolite was added to obtain a slurry. The slurry was subjected to hydrothermal synthesis to obtain CHA zeolite.

[0049] [Table 1]

[0050] [Table 2]

Claims

1. Mixing a solvent and FAU zeolite to prepare a slurry; preparing chabazite-type zeolite by hydrothermal treatment of the slurry; Prior to the hydrothermal treatment, hydroxide ions (OH - ) to the ratio of Si in the FAU zeolite (OH - a base addition step of adding a salt containing hydroxide ions so that the ratio of the hydroxide ions to the alkali metal salt is 0.38 or more; adding a salt containing potassium ions prior to the hydrothermal treatment; and a sodium addition step of adding a salt containing sodium ions before the hydrothermal treatment, and an ion exchange step of performing ion exchange by adding a salt containing sodium ions to the chabazite-type zeolite. 2 Method for producing chabazite-type zeolite for adsorption.

2. In the sodium substitution step, the sodium content in the chabazite-type zeolite is reduced to Na 2 2. The method according to claim 1, wherein the oxygen content is adjusted to 1 to 25% by weight.

3. 2. The method according to claim 1, wherein the sodium substitution step is a step of adding a salt containing sodium ions prior to the hydrothermal treatment.

4. 2. The method according to claim 1, wherein the sodium substitution step comprises the steps of: adding a salt containing sodium before the hydrothermal treatment; and performing ion exchange by adding a salt containing sodium to the chabazite-type zeolite.

5. The slurry is wet-pulverized prior to the hydrothermal treatment, In the base addition step, the ratio of hydroxide ions to Si in the FAU zeolite (OH -2. The method according to claim 1, wherein the salt containing hydroxide ions is added so that the ratio of the hydroxide ion to the total weight of the silicon dioxide particles is 0.55 or less.

6. A CO2 gas containing chabazite-type zeolite obtained by the method of claim 1. 2 Adsorbent.

7. SAR is 5 to 9; Na to Na 2 Contains 1 to 25% by weight calculated as O, CO 2 Chabazite-type zeolite for adsorption.

8. The Miller indices obtained by XRD are the peak intensity of the (100) plane I 100 and (211) plane peak intensity I 211 The ratio of I 100 / I 211 8. The chabazite-type zeolite according to claim 7, wherein the value of n is 0.8 or less.

9. A CO2 purifying apparatus comprising the chabazite-type zeolite according to claim 7 added thereto. 2 A method for producing an adsorbent.

Citation Information

Patent Citations

  • Method for eliminating carbon dioxide from gas stream

    JP1996252419A

  • Removal of carbon dioxide from gas flow

    JP1999290635A

  • Molecular sieve adsorbent for gas purification and its production method

    JP2002519188A

  • Method for synthesis of chabazite zeolite

    JP2015101506A

  • Chabazite zeolite with high hydrothermal resistance and method for producing same

    JP2017218367A