Film for molding and molded article prepared therewith

The molding film with controlled heat shrinkage and layered resin structure addresses cracking and peeling issues, ensuring excellent moldability and thermal stability while maintaining infrared transmittance.

JP2024136653AInactive Publication Date: 2024-10-04TORAY INDUSTRIES INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023047835
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for applying metal-like decoration using films suffer from issues such as cracking on the vapor-deposited surface, deterioration of hiding properties during molding, insufficient infrared transmittance, and peeling within the molding film when heated.

Method used

A molding film configuration with a resin layer on a polyester film, where the heat shrinkage rate is controlled between -1.0% and 2.0% at 150°C, and a layered structure with alternating layers of thermoplastic resins A and B, enhancing moldability and thermal stability.

Benefits of technology

The film provides excellent moldability during processing and maintains thermal stability of the molded product, reducing internal peeling and ensuring high infrared transmittance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136653000001_ABST
    Figure 2024136653000001_ABST
Patent Text Reader

Abstract

To provide a film for molding that exhibits excellent moldability during the molding process, while demonstrating superior heat resistance after being processed into a molded product.SOLUTION: A film for molding has a resin layer (X layer) on at least one side of a polyester film. The polyester film shows a heat shrinkage rate of -1.0% or more to 2.0% or less in the largest direction as measured under the conditions of 150°C for 30 minutes.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a film for molding and a molded article using the same. [Background technology]

[0002] In recent years, with the rise in environmental awareness, there has been an increasing demand for solvent-free painting and alternative plating decoration methods in the fields of building materials, automobile parts, mobile phones, and electrical products, and the introduction of film-based decoration methods is progressing. There is also a high demand for metallic and high-gloss finishes, which can produce high designability. In addition, infrared sensors are often installed in various devices, and there is a need to ensure infrared transparency while making the sensor invisible from the outside.

[0003] Known methods for applying metallic decoration using a film include forming a design layer mainly composed of aluminum, indium, chromium, etc. on a film using deposition methods such as vacuum deposition, sputtering, and ion blading, and then transferring this to a target member (Patent Document 1).Also, as another method for improving the formability of a molding film using an optical interference multilayer film, a method of laminating a polycarbonate resin or an acrylic resin on at least one side of the optical interference multilayer film, and a method of controlling the storage modulus and elongation stress of the entire moldable film are known (Patent Document 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2012-201032 A [Patent Document 2] JP 2018-69552 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the technology described in Patent Document 1 has problems such as cracking of the deposition surface and deterioration of hiding power due to stretching during molding processes such as insert molding and vacuum / pressure molding, and insufficient infrared transmittance. The technology described in Patent Document 2 has problems such as peeling occurring inside the molding film when the molded body is heated after molding processes.

[0006] An object of the present invention is to overcome the problems of the conventional techniques and to provide a film for molding which has excellent moldability during molding and excellent thermal stability of the molded product. [Means for solving the problem]

[0007] In order to solve the above problems, the film for molding of the present invention has the following configuration: That is, the film for molding has a resin layer (X layer) on at least one side of a polyester film, and is characterized in that the heat shrinkage rate of the polyester film under conditions of 150°C for 30 minutes is -1.0% or more and 2.0% or less in the largest direction.

[0008] The film for molding of the present invention can be in the following form, and a molded article can be obtained by using the film for molding of the present invention as follows. (1) A molding film having a resin layer (X layer) on at least one side of a polyester film, characterized in that the heat shrinkage rate of the polyester film at 150°C for 30 minutes is -1.0% or more and 2.0% or less in the largest direction. (2) The film for molding according to (1), wherein the main component of the X layer is a non-crystalline resin. (3) The film for molding according to (1) or (2), characterized in that it has at least one adhesive layer between the X layer and the polyester film. (4) The film for molding according to any one of (1) to (3), characterized in that the polyester film has a structure in which a layer (A layer) mainly composed of thermoplastic resin A and a layer (B layer) containing a thermoplastic resin B different from the thermoplastic resin A are alternately laminated in the thickness direction to form a total of 51 or more layers. (5) The film for molding according to any one of (1) to (4), which has an average reflectance of 30% or more in a wavelength band of 400 nm to 700 nm. (6) A molded article comprising the film for molding according to any one of (1) to (5). Effect of the Invention

[0009] According to the present invention, it is possible to provide a film which has excellent formability during molding and excellent heat resistance after being processed into a molded article. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a cross-sectional view of a molding film according to one embodiment of the present invention, cut along a plane perpendicular to the film surface (X layer on one side, no adhesive layer). [Diagram 2] FIG. 1 is a cross-sectional view of a molding film according to one embodiment of the present invention, cut along a plane perpendicular to the film surface (X layer on one side, with an adhesive layer). [Diagram 3] FIG. 1 is a cross-sectional view of a molding film according to one embodiment of the present invention, cut along a plane perpendicular to the film surface (both sides of the X layer, no adhesive layer). [Figure 4] FIG. 1 is a cross-sectional view of a molding film according to one embodiment of the present invention, cut along a plane perpendicular to the film surface (X layer on both sides, with adhesive layer). [Diagram 5] FIG. 1 is a cross-sectional view of a molding film according to one embodiment of the present invention, cut along a plane perpendicular to the film surface (both sides of X layer, only one side has no adhesive layer). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The film for molding of the present invention is a film for molding having a resin layer (X layer) on at least one side of a polyester film, and is characterized in that the heat shrinkage rate of the polyester film under conditions of 150°C for 30 minutes is -1.0% or more and 2.0% or less in the largest direction. The film for molding of the present invention will be described in more detail below.

[0012] In the film for molding of the present invention, the polyester film refers to a sheet-like material mainly composed of polyester resin, and the main component refers to a component that is contained in an amount of more than 50% by mass to 100% by mass or less when the total components constituting the film are taken as 100% by mass. (In this case, when a plurality of components corresponding to polyester resin are contained, if the total amount exceeds 50% by mass, the polyester resin is regarded as the main component. Hereinafter, the main component can be interpreted in the same manner.) The polyester resin refers to a resin having a molecular structure in which a dicarboxylic acid unit and a diol unit are linked by an ester bond. In addition, the polyester film in the present invention is preferably a biaxially oriented polyester film from the viewpoint of the strength, heat resistance, and versatility of the film. The biaxially oriented polyester film refers to a polyester film having molecular orientation in two orthogonal directions, and is usually obtained by stretching an unstretched polyester sheet in two orthogonal directions, for example, the longitudinal direction and the width direction. The longitudinal direction refers to the direction in which the film runs during the manufacturing process (corresponding to the winding direction in the case of a film roll), and the width direction refers to the direction perpendicular to the longitudinal direction within the film plane.

[0013] In the film for molding of the present invention, from the viewpoint of reducing internal peeling of the film for molding caused by heating, the heat shrinkage rate of the polyester film under 150°C for 30 minutes is -1.0% or more and 2.0% or less in the direction where it is the largest. In the present invention, the heat shrinkage rate (HS) under 150°C for 30 minutes is defined as follows. The gauge length (L0) is measured in advance at room temperature (23°C ± 2°C), and the film is placed in a hot air oven set at 150°C for 30 minutes, and the gauge length (L1) measured after cooling to room temperature (23°C ± 2°C) is obtained, and calculated by the following formula (1) (details of the measurement method will be described later). Hereinafter, the heat shrinkage rate in the direction where the heat shrinkage rate of the polyester film is the largest under 150°C for 30 minutes may be referred to as the maximum heat shrinkage rate of the polyester film, or simply the maximum heat shrinkage rate. Equation (1) HS(%)=(L0-L1) / L0×100%.

[0014] The direction with the largest heat shrinkage rate under the condition of 150°C for 30 minutes can be identified by the following procedure. First, the polyester film is rotated by 15 degrees from any direction as the starting point, and the heat shrinkage rate is measured in 12 directions after placing it in a hot air oven at 150°C for 30 minutes. The direction with the largest measured value is determined to be the direction with the largest heat shrinkage rate.

[0015] The maximum value of the heat shrinkage of the polyester film of the present invention is more preferably 0.0% or more. On the other hand, the maximum value of the heat shrinkage is more preferably 1.5% or less, and even more preferably 1.0% or less. When the maximum value of the heat shrinkage of the polyester film of the present invention is below -0.1% or exceeds 2.0%, the difference in shrinkage with the resin layer X layer becomes large when the molded body after molding is heated. As a result, internal peeling of the molding film occurs and the heat resistance of the molded body is also deteriorated, which is not preferable. Hereinafter, a method for adjusting the maximum value of the heat shrinkage of the polyester film to the above-mentioned range will be described later.

[0016] The thickness of the polyester film constituting the molding film of the present invention is preferably 30 μm or more from the viewpoint of processability when processing is performed to give the molding film a design, and from the viewpoint of expressing design when the polyester film has a structure in which a layer (A layer) mainly composed of thermoplastic resin A and a layer (B layer) containing a thermoplastic resin B different from the thermoplastic resin A are alternately laminated in the thickness direction as described below. From the above viewpoint, it is preferably 60 μm or more, and more preferably 80 μm or more. On the other hand, from the viewpoint of film formability and moldability, the thickness of the polyester film is preferably 500 μm or less. From the above viewpoint, it is preferably 300 μm or less, and more preferably 150 μm or less. The thickness of the polyester film can be reduced by increasing the take-up speed of the cast or reducing the amount of molten resin discharged from the die per unit time, and these means can be used in appropriate combination.

[0017] The film for molding of the present invention has a resin layer (X layer) from the viewpoint of preventing washout during injection molding. The resin that is the main component of the resin layer (X layer) is not particularly limited, but is preferably a thermoplastic resin from the viewpoint of moldability. When the main component of the X layer is a thermoplastic resin, it may be either crystalline or non-crystalline, but it is more preferable that the main component of the X layer is a non-crystalline thermoplastic resin from the viewpoint of moldability. When the main component of the X layer is a non-crystalline thermoplastic resin, it is possible to reduce deterioration of moldability due to crystalline parts when molding the film for molding of the present invention.

[0018] Here, whether a thermoplastic resin is crystalline or non-crystalline is determined by the following procedure. First, using a differential scanning calorimeter (DSC), the temperature is raised from 25°C to 300°C at a heating rate of 10°C / min, and then rapidly cooled to 0°C. After that, the temperature is raised again from 25°C to 300°C at a heating rate of 10°C / min. Thermoplastic resins that do not show an exothermic peak due to crystallization between 100°C and 200°C during the second heating are considered to be non-crystalline thermoplastic resins. On the other hand, thermoplastic resins that show the exothermic peak are considered to be crystalline thermoplastic resins.

[0019] Examples of crystalline thermoplastic resins include polyethylene resin, polypropylene resin, polyamide resin, polyethylene terephthalate resin, polybutylene terephthalate resin, polyethylene naphthalate resin, etc. Examples of non-crystalline thermoplastic resins include polyvinyl chloride resin, modified polyphenylene ether resin, polycarbonate resin (hereinafter sometimes referred to as PC), acrylic resin, etc.

[0020] The main component of the X layer is preferably at least one of polycarbonate resin, acrylic resin, acrylonitrile butadiene styrene resin, and polystyrene resin, among amorphous thermoplastic resins, particularly from the viewpoint of ease of adjusting the glass transition temperature. Note that, when a layer contains multiple polycarbonate resins, the content of the polycarbonate resin is calculated by adding up all the polycarbonate resins, and if the total exceeds 50 mass%, the X layer is considered to be mainly composed of polycarbonate resin. This also applies when the X layer contains multiple acrylic resins, acrylonitrile butadiene styrene resins, or polystyrene resins.

[0021] The polycarbonate resin used in the X layer constituting the molding film of the present invention is not particularly limited as long as it does not impair the effects of the present invention, and examples thereof include polycarbonate resins obtained by using 2,2-bis(4-hydroxyphenyl)propane (bisphenol A), flame-retardant polycarbonate resins obtained by using a mixture of bisphenol A and 2,2-bis(3,5-dibromo-4-hydroxyphenyl)propane (tetrabromobisphenol A), and bisphenol A-based polycarbonate-polyorganosiloxane copolymers.

[0022] The acrylic resin used in the X layer constituting the molding film of the present invention is not particularly limited as long as it does not impair the effects of the present invention. For example, a polymer mainly composed of a methacrylic acid ester, a copolymer of a methacrylic acid ester and another monomer, or a polymer alloy composed of a methacrylic resin and one or more other resins is preferable. Polymethyl methacrylate, polyethyl methacrylate, polybutyl methacrylate, polyethylhexyl methacrylate, polymethyl methacrylate-styrene copolymer, polymethyl methacrylate-polyvinylidene fluoride alloy, etc. are preferable, and from the viewpoints of transparency, moldability, and scratch resistance, it is more preferable to use polymethyl methacrylate.

[0023] The acrylonitrile butadiene styrene resin used in the X layer constituting the molding film of the present invention is not particularly limited as long as it does not impair the effects of the present invention. For example, in addition to a copolymer of acrylonitrile, butadiene, and styrene, an α-methylstyrene-based ABS resin in which α-methylstyrene is polymerized instead of styrene, an ABS resin using phenylmaleimide and modified with imide, an ASA resin in which acrylic rubber is polymerized instead of butadiene, an ACS resin in which chlorinated polyethylene is polymerized instead of butadiene, and an AES resin in which ethylene propylene diene rubber is polymerized instead of butadiene are preferred.

[0024] The polystyrene resin used in the X layer constituting the molding film of the present invention is not particularly limited as long as it does not impair the effects of the present invention. For example, in addition to a polymer of styrene alone, poly-α-methylstyrene, a polymer of a styrene derivative substituted at the meta-position or para-position, a copolymer of the above-mentioned styrene-based monomer, or a copolymer with various olefin-based resins is preferable, and from the viewpoints of transparency and moldability, a styrene homopolymer resin is more preferable.

[0025] The above-mentioned polycarbonate-based resin, acrylic-based resin, acrylonitrile butadiene styrene-based resin, and polystyrene-based resin may contain various additives, such as an ultraviolet absorbing agent for imparting weather resistance, rubber particles for imparting flexibility, and various dyes and pigments for coloring and light blocking.

[0026] If the type of resin in the X layer is unknown, FT-IR, pyrolysis GC-MS, 1 H-NMR, 13 It is possible to identify the type of resin by combining known methods such as C-NMR. In addition, if it is not clear whether the main component is a polycarbonate resin, an acrylic resin, an acrylonitrile butadiene styrene resin, or a polystyrene resin, that is, when the total components constituting the layer are taken as 100 mass%, the above components are contained in an amount of more than 50 mass% to 100 mass% or less, it is possible to separate the above components by known methods such as a solvent extraction method or various types of chromatography, and determine the content (mass%) of the components.

[0027] The thickness of the X layer in the film for molding of the present invention is preferably 50 μm or more and 500 μm or less from the viewpoint of processability as a film for molding. When the thickness of the X layer is 50 μm or more, the processability during molding processing is improved. On the other hand, when the thickness of the X layer is 500 μm or less, for example, warping during the drying process can be suppressed, and at the same time, the increase in manufacturing costs can be reduced. From the above viewpoint, the preferred range of the thickness of the X layer is 100 μm or more and 400 μm or less, more preferably 150 μm or more and 300 μm or less, and even more preferably 200 μm or more and 250 μm or less.

[0028] The film for molding of the present invention is not particularly limited in terms of layer structure as long as it has an X layer on at least one side of the polyester film, but it is preferable that the film for molding has an X layer on both sides. For example, when it is desired to give a metallic look to a part of the molded body rather than the entire surface, the film for molding may be printed. In this case, by providing the X layer on both sides of the polyester film, the adhesion of the ink is improved and warping that occurs during heating in drying the printing ink can be suppressed. When the difference in linear expansion coefficient between the polyester film and the X layer is large, it is particularly effective to provide the X layer on both sides.

[0029] When X layers are provided on both sides, the resins constituting the X layers (referred to as X1 layer and X2 layer) provided on both sides may be the same type of resin, or different resins may be selected. For example, both X1 layer and X2 layer may be layers mainly composed of polycarbonate resin, or X1 layer may be a layer mainly composed of polycarbonate resin, and X2 layer may be a layer mainly composed of acrylic resin. Also, for example, when both X1 layer and X2 layer are mainly composed of polycarbonate resin, the polycarbonate resins mainly composed of both layers may be the same or different.

[0030] Specific examples of the embodiment of the film for molding of the present invention are shown in Figs. 1 to 5. In the embodiment of Fig. 1, in the film for molding 1, an X layer 3 is provided on one side of a polyester film 2. An adhesive layer 4 may be provided between the polyester film 2 and the X layer 3 (embodiment of Fig. 2). The X layer 3 may be provided on both sides of the polyester film 2 (embodiment of Fig. 3), or an adhesive layer 4 may be provided between the polyester film 2 and the X layer on at least one side (embodiments of Figs. 4 and 5). Since the film for molding is subjected to insert molding or vacuum / pressure molding, it is preferable that the polyester film has an X layer on both sides from the viewpoint of reducing warpage of the film during printing and improving the heat resistance of the molded product.

[0031] From the viewpoint of increasing interlayer adhesion, the film for molding of the present invention preferably has at least one adhesive layer between the X layer and the polyester film. The method of laminating the polyester film and the X layer via the adhesive layer is not particularly limited, and known methods, such as using an optical adhesive sheet or laminating by a dry lamination method, are possible. Among them, from the viewpoint of adhesion during molding, it is preferable to use the dry lamination method.

[0032] The adhesive used in the adhesive layer in the film for molding of the present invention is not particularly limited as long as it does not impair the effects of the present invention, but a two-component curing polyurethane adhesive is preferably used from the viewpoint of heat resistance during molding. The two-component curing polyurethane adhesive contains a base agent (polyol) having a hydroxyl group at the polymer end and a curing agent (polyisocyanate) having an isocyanate group, and cures by forming a urethane bond through a reaction between the hydroxyl group and the isocyanate group.

[0033] Examples of polyols include polyether polyols and polyester polyols. Examples of polyether polyols include polyoxyethylene polyols, polyoxypropylene polyols, polyoxyethylene-propylene copolymer polyols, polytetramethylene polyols, and mixtures thereof. Examples of polyester polyols include polyols obtained by polycondensation of dicarboxylic acids (adipic acid, succinic acid, maleic acid, phthalic acid, etc.) and glycols (ethylene glycol, propylene glycol, 1,4-butylene glycol, 1,6-hexane glycol, neopentyl glycol, etc.).

[0034] Examples of the polyisocyanate include 2,4-tolylene diisocyanate, xylylene diisocyanate, 2,6-tolylene diisocyanate, 4,4-diphenylmethane diisocyanate, polymethylene polyphenylene polyisocyanate, carbodiimide-modified MDI, aromatic polyisocyanates such as naphthalene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, 4,4-dicyclohexylmethane diisocyanate, and alicyclic polyisocyanates.

[0035] The adhesive layer may contain various additives such as viscosity modifiers, leveling agents, anti-gelling agents, antioxidants, heat stabilizers, light stabilizers, UV absorbers, lubricants, pigments, dyes, organic or inorganic fine particles, fillers, antistatic agents, and nucleating agents.

[0036] The thickness of the adhesive layer is preferably 0.5 μm or more and 30 μm or less from the viewpoint of achieving both adhesiveness and film appearance. When the thickness of the adhesive layer of the present invention is 0.5 μm or more, the adhesion between the layers is sufficiently maintained. On the other hand, when the thickness of the adhesive layer of the present invention is 30 μm or less, the thickness unevenness of the layer is suppressed, and the deterioration of the film appearance is reduced. From the above viewpoint, the thickness of the adhesive layer is more preferably in the range of 1 μm or more and 20 μm or less, and more preferably in the range of 3 μm or more and 15 μm or less. In addition, when the X layer is formed on both sides via the adhesive layer, the thickness of each adhesive layer may be the same or different, but it is preferable that all of them are in the above preferred range.

[0037] In the film for molding of the present invention, it is preferable that the polyester film has a structure in which a layer (A layer) mainly composed of thermoplastic resin A and a layer (B layer) containing a thermoplastic resin B different from the thermoplastic resin A are alternately laminated in the thickness direction for a total of 51 layers or more. More preferably, the structure has a total of 251 layers or more of A layers and B layers alternately laminated in the thickness direction, and even more preferably, the structure has a total of 801 layers or more. There is no particular upper limit on the number of layers, but from the viewpoints of productivity and cost, 2001 layers or less is preferable. By having 51 or more layers laminated, the uniformity of interference reflection between layers is improved, resulting in a film with excellent design.

[0038] Here, "different thermoplastic resins" refers to cases where the basic skeletons (described later) of the thermoplastic resins are different, and cases where the basic skeletons are the same and the difference is 10 mol% or more and less than 50 mol% when the total repeating units constituting the thermoplastic resins are 100 mol%. In addition, the content of thermoplastic resin B in layer B is preferably 17% by mass or more, more preferably 22% by mass or more, and even more preferably 27% by mass or more, when the total amount of thermoplastic resin in layer B is 100% by mass, from the viewpoint of increasing the refractive index difference between layer A and layer B. On the other hand, there is no particular restriction on the upper limit of the content of thermoplastic resin B in layer B, and it is theoretically 100% by mass, but 50% by mass is preferable from the viewpoint of reducing warping of the film for molding and adhesion between layer A and layer B.

[0039] From the viewpoint of design, the film for molding of the present invention preferably has an average reflectance of 30% or more in the wavelength band of 400 nm to 700 nm. The average reflectance in the wavelength band of 400 nm to 700 nm is a value measured at an incident angle Φ of 10°, and the detailed measurement method will be described later.

[0040] In the polyester film of the present invention, from the viewpoint of making the reflectance of the molding film in the wavelength band of 400 to 700 nm more uniform and expressing the design of a metallic tone, it is preferable that the number of layers with a layer-to-layer thickness of 100 nm or more and less than 200 nm is greater than the number of layers with a layer-to-layer thickness of 200 nm or more and less than 250 nm. Here, the "layer-to-layer thickness" refers to the thickness obtained by adding the layer thicknesses of adjacent A layer and B layer. In addition, the layer-to-layer thickness must be the sum of the layer thickness of the m-th A layer counted from one film surface for only the A layer, and the layer thickness of the m-th B layer counted from the same surface for only the adjacent B layer. Here, m represents an integer. For example, when the layers are arranged in the order of A1 layer / B1 layer / A2 layer / B2 layer / A3 layer / B3 layer... from one film surface to the opposite surface, the A1 layer and the B1 layer are the first layer pair, the A2 layer and the B2 layer are the second layer pair, and the A3 layer and the B3 layer are the third layer pair.

[0041] If the number of layers with a layer-to-layer thickness of 100 nm or more and less than 200 nm is equal to or less than the number of layers with a layer-to-layer thickness of 200 nm or more and less than 250 nm, the reflectance decreases toward the lower wavelength side in the reflection band of the wavelength band of 400 nm to 700 nm, which may result in a reddish appearance. This occurs because the density of the layer pairs that cause reflection on the lower wavelength side becomes thinner. Therefore, it is preferable that the layer-to-layer thickness sequence of the layers constituting the polyester film does not increase or decrease monotonically in an arithmetic progression, but increases or decreases in a geometric progression while satisfying the above conditions. More preferably, the number of layers with a layer-to-layer thickness of 100 nm or more and less than 200 nm is 1.05 times or more and 2.50 times or less than the number of layers with a layer-to-layer thickness of 200 nm or more and less than 250 nm.

[0042] From the viewpoints of strength, heat resistance, transparency and versatility, the thermoplastic resin A and the thermoplastic resin B in the polyester film are preferably polyester resins obtained by polymerization of a monomer mainly composed of an aromatic dicarboxylic acid or an aliphatic dicarboxylic acid and a diol.

[0043] Examples of aromatic dicarboxylic acids include terephthalic acid, isophthalic acid, phthalic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, and 4,4'-diphenylsulfonedicarboxylic acid. Examples of aliphatic dicarboxylic acids include adipic acid, suberic acid, sebacic acid, dimer acid, dodecanedioic acid, cyclohexanedicarboxylic acid, and ester derivatives thereof. Among these, terephthalic acid and 2,6-naphthalenedicarboxylic acid, which have high refractive index, are preferred. These acid components may be used alone or in combination of two or more, or may be partially copolymerized with oxyacids such as hydroxybenzoic acid.

[0044] Examples of the diol component include ethylene glycol, 1,2-propanediol, 1,3-propanediol, neopentyl glycol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-hexanedimethanol, diethylene glycol, triethylene glycol, polyalkylene glycol, 2,2-bis(4-hydroxyethoxyphenyl)propane, isosorbate, and spiroglycol. Among these, ethylene glycol is preferably used. These diol components may be used alone or in combination of two or more.

[0045] Of the polyester resins, from the viewpoint of making the in-plane average refractive index of layer A relatively high and further making it easier to make the difference in the in-plane average refractive index between layer A and layer B 0.005 or more, preferably 0.040 or more, it is preferable to use, as the polyester, polyethylene terephthalate and copolymers thereof, polyethylene naphthalate and copolymers thereof, polybutylene terephthalate and copolymers thereof, polybutylene naphthalate and copolymers thereof, polyhexamethylene terephthalate and copolymers thereof, polyhexamethylene naphthalate and copolymers thereof, etc.

[0046] The in-plane refractive index of the A layer and the B layer can be determined, for example, as follows. First, the resin used for the A layer or the B layer is melted at 290°C in a vented twin-screw extruder, and is introduced into a T-die through a gear pump and a filter to form a sheet. The resin is then rapidly solidified by contacting it with a casting drum whose surface temperature is kept at 25°C by electrostatic application to obtain cast films of the A layer and the B layer. Next, the Abbe refractive index and the refractive index in the longitudinal direction and the width direction of each cast film are measured using sodium D line as a light source, and the average value is taken as the in-plane refractive index (details of the measurement method will be described later). When the polyester film is stretched, the molecules of the crystalline thermoplastic resin are oriented in the stretching direction, so that the refractive index of the A layer of the polyester film and the cast film of the A layer obtained by the above method may differ, but the difference is slight, so the above method can be adopted.

[0047] The combination of thermoplastic resin A and thermoplastic resin B is preferably such that both thermoplastic resins have the same basic skeleton. Here, the "basic skeleton" in the present invention refers to the repeating unit constituting the resin that is contained most frequently, for example, in the case of polyethylene terephthalate, ethylene terephthalate is the basic skeleton. An example of such a combination is one in which one thermoplastic resin is polyethylene terephthalate, and the other thermoplastic resin is a polymer (copolymer) consisting of ethylene terephthalate units and cyclohexane 1,4-dimethylene terephthalate units, and contains ethylene terephthalate units most frequently. When resins with the same basic skeleton are used, problems such as lamination defects such as flow marks and peeling between layers are less likely to occur during the production of a laminated film.

[0048] It is preferable to use a crystalline resin as the thermoplastic resin A from the viewpoint of increasing the resistance to pressure marks (dent resistance) and the stiffness of the polyester film itself. It is preferable to use polyethylene terephthalate or polyethylene naphthalate as the thermoplastic resin A. On the other hand, it is preferable to use a non-crystalline resin as the thermoplastic resin B from the viewpoint of suppressing the increase in the refractive index and forming a non-crystalline film. It is preferable to use a copolymer of polyethylene terephthalate or polyethylene naphthalate as the thermoplastic resin B, which contains isophthalic acid, naphthalenedicarboxylic acid, diphenyl acid, or cyclohexanedicarboxylic acid, or contains spiroglycol, cyclohexanedimethanol, bisphenoxyethanolfluorene, or bisphenol A as a constituent unit.

[0049] In order to adjust the heat shrinkage rate of the polyester film of the present invention under the condition of 150°C for 30 minutes, it is effective to unwind the polyester film obtained as described above, pass it through an oven, and then wind it up, but it is necessary to adjust the film tension in the oven to relieve the residual stress of the polyester film. In particular, when the thermoplastic resin B is a non-crystalline resin, the strength of the polyester film tends to decrease, so it is necessary to more appropriately manage the temperature and tension of the oven.

[0050] An example of a preferred method for producing the polyester film constituting the film for molding of the present invention will be described below, but the method for producing the polyester film is not limited thereto.

[0051] First, thermoplastic resin A and thermoplastic resin B are prepared in the form of pellets. The pellets are dried in hot air or under vacuum as necessary, and then fed to two extruders, respectively. The thermoplastic resins are heated and melted in each extruder to above their melting points, and the amount of resin extruded is made uniform by a gear pump or the like, and extruded. Foreign matter and denatured resins are removed by a filter or the like. Thermoplastic resin A and thermoplastic resin B, which are fed from different flow paths by the two extruders, are fed to a multi-layer lamination device, respectively.

[0052] As the multi-layer lamination device, a multi-manifold die, a feed block, a static mixer, etc. can be used. In particular, in order to efficiently obtain the laminated structure of the polyester film in the present invention, it is desirable to use a feed block containing at least two or more separate members having a large number of fine slits. When such a feed block is used, the device does not become extremely large, so that there is little foreign matter due to thermal degradation, and even if the number of layers is extremely large, lamination can be performed with high precision. In addition, the lamination precision in the width direction is significantly improved compared to the conventional technology, and it is also easy to form an arbitrary layer thickness configuration. In this device, the thickness of each layer can be adjusted by the slit shape (length, width, gap), so that it is possible to easily achieve an arbitrary layer thickness.

[0053] In this case, in order to realize an average reflectance of 30% or more in the wavelength band of 400 nm to 700 nm, which is a preferred embodiment of the film for molding of the present invention, it is preferable to design the layer thickness of each layer of the polyester film based on the following formula 1. The polyester film is capable of reflecting / transmitting light, and the reflectance can be controlled by the refractive index difference between the layer made of thermoplastic resin A and the layer made of thermoplastic resin B and the number of layers. Equation 1: 2×(na·da+nb·db)=λ na: average in-plane refractive index of the layer made of resin A nb: average in-plane refractive index of the layer made of resin B da: Layer thickness of the layer made of resin A (nm) db: Layer thickness of the layer made of resin B (nm). λ: Main reflection wavelength (first reflection wavelength) The molten laminate thus obtained with the desired layer structure is extruded from the slit of the die into a sheet, and the sheet is extruded onto a rotating cooling body such as a casting drum and cooled to solidify, thereby obtaining a cast film (unstretched film). In this case, it is preferable to use a wire-shaped, tape-shaped, wire-shaped, or knife-shaped electrode to bring the sheet into close contact with a rotating cooling body such as a casting drum by electrostatic force, thereby rapidly solidifying the sheet. It is also preferable to blow air from a slit-shaped, spot-shaped, or planar device to bring the sheet into close contact with a rotating cooling body such as a casting drum, thereby rapidly solidifying the sheet, or to bring the sheet into close contact with a rotating cooling body using a nip roll to rapidly solidify the sheet.

[0054] The thus obtained casting film (unstretched film) is preferably stretched biaxially as necessary. Biaxial stretching refers to stretching in two perpendicular directions, for example, the longitudinal direction and the width direction. The stretching may be performed in the biaxial directions successively, or in the two directions simultaneously. The film may also be restretched in the longitudinal direction and / or the width direction.

[0055] First, the case of sequential biaxial stretching will be described. Here, the stretching in the longitudinal direction refers to stretching for giving molecular orientation to the film in the longitudinal direction, and is usually performed by the difference in peripheral speed of the rolls. This stretching may be performed in one step using a pair of stretching rolls, or in multiple steps using a plurality of pairs of stretching rolls. The stretching ratio varies depending on the type of resin, but is usually preferably 2 to 15 times, and when polyethylene terephthalate is used as one of the thermoplastic resins constituting the polyester film, 2 to 7 times is particularly preferably used. In addition, the stretching temperature is preferably the glass transition temperature of the resin having the higher glass transition temperature of the thermoplastic resins A and B constituting the polyester film to the glass transition temperature + 100°C.

[0056] The polyester film may also be provided with an easy-adhesion layer. As a method for providing the easy-adhesion layer, a method of coating with a coating agent and laminating the same is preferred. As a method for coating with a coating agent, there are a method of coating in a separate process from the manufacturing process of the polyester film of the present invention, that is, a so-called offline coating method, and a so-called in-line coating method in which the easy-adhesion layer is laminated at once by coating during the manufacturing process of the polyester film of the present invention. It is preferable to adopt the in-line coating method from the viewpoint of cost and uniformity of the coating thickness, and the solvent of the coating liquid used in this case is preferably aqueous from the viewpoint of environmental pollution and explosion resistance, and the most preferred embodiment is to use water.

[0057] When laminating the easy-adhesion layer by in-line coating, it is preferable to continuously apply the coating agent constituting the easy-adhesion layer to the uniaxially stretched polyester film. For example, the coating agent using water as a solvent (water-based coating agent) can be applied by reverse coating method, spray coating method, bar coating method, gravure coating method, rod coating method, die coating method, etc.

[0058] It is also preferable to subject the surface of the polyester film to corona discharge treatment or the like before applying the water-based coating agent. This is because the adhesion between the polyester film and the coating agent is improved and the coating properties are also improved. The adhesive layer may contain a crosslinking agent, an antioxidant, a heat stabilizer, a weather stabilizer, an ultraviolet absorber, an organic slipper, a pigment, a dye, organic or inorganic particles, a filler, a surfactant, etc., within a range that does not impair the effects of the invention.

[0059] The subsequent stretching in the width direction refers to stretching to give molecular orientation in the width direction of the film, and is usually done by conveying the film while holding both ends with clips using a tenter, applying heat to the film to preheat it, and then stretching it in the width direction. The water-based coating applied just before the tenter is dried during this preheating. The stretching ratio varies depending on the type of resin, but is usually preferably 2 to 15 times, and when polyethylene terephthalate is used as either the thermoplastic resin A or the thermoplastic resin B, it is particularly preferably 2 to 7 times. In addition, the stretching temperature is preferably in the range of the glass transition temperature of the resin having the higher glass transition temperature of the thermoplastic resins A and B constituting the polyester film in the present invention to the glass transition temperature + 120 ° C. In order to impart flatness and dimensional stability, it is preferable that the biaxially stretched polyester film is subjected to a relaxation treatment at a temperature higher than the stretching temperature and lower than the melting point in the tenter. After the relaxation treatment in this way, the film is uniformly cooled slowly, cooled to room temperature, and wound up by a winder. In addition, if necessary, a further relaxation treatment may be performed in combination with the slow cooling.

[0060] Next, the case of simultaneous biaxial stretching will be described. In the case of simultaneous biaxial stretching, the coating agent that forms the easy-adhesion layer is continuously applied to the obtained cast film. As the coating agent (water-based coating agent) that uses water as a solvent, for example, reverse coating method, spray coating method, bar coating method, gravure coating method, rod coating method and die coating method can be suitably used.

[0061] Before applying the water-based coating material, it is preferable to subject the surface of the polyester film in the present invention to a corona discharge treatment or the like. This is because the adhesion between the polyester film and the coating material is improved and the coating property is also good. Next, the cast film coated with the coating material is introduced into a simultaneous biaxial tenter, and the film is conveyed while holding both ends of the film with clips, and is stretched simultaneously and / or stepwise in the longitudinal direction and the width direction. As the simultaneous biaxial stretching machine, there are a pantograph type, a screw type, a drive motor type, and a linear motor type, but the drive motor type or the linear motor type, which can change the stretching ratio at any time and can perform relaxation treatment at any place, is preferable. The stretching ratio varies depending on the type of resin, but usually, an area ratio of 6 to 50 times is preferable, and an area ratio of 8 to 30 times is particularly preferable. In addition, the stretching temperature is preferably the glass transition temperature of the resin having a higher glass transition temperature of the thermoplastic resins A and B to the glass transition temperature + 120°C.

[0062] In order to impart planarity and dimensional stability to the biaxially stretched film, it is preferable to subsequently perform a relaxation treatment in the tenter at a temperature equal to or higher than the stretching temperature and equal to or lower than the melting point of the thermoplastic resin A or B, which has a higher melting point. During this relaxation treatment, in order to suppress the distribution of the main orientation axis in the width direction, it is preferable to perform a relaxation treatment in the longitudinal direction immediately before and / or immediately after entering the relaxation treatment zone. After the relaxation treatment is thus performed, the film is uniformly cooled slowly, cooled to room temperature, and wound up by a winder. In addition, if necessary, additional relaxation treatment may be performed in the longitudinal direction and / or width direction during the slow cooling. It is preferable to perform a relaxation treatment in the longitudinal direction immediately before and / or immediately after entering the relaxation treatment zone. After the relaxation treatment is thus performed, the film is uniformly cooled slowly, cooled to room temperature, and wound up by a winder.

[0063] Furthermore, in order to improve the heat resistance of a molded product using the molding film, the obtained polyester film may be heat-treated at 135°C to 165°C (preferably 145°C to 165°C) for 15 to 60 seconds while applying a tension of 10 N / m to 60 N / m (preferably 15 N / m to 45 N / m) in the longitudinal direction.

[0064] Next, an example of a method for producing the film for molding of the present invention (dry lamination method) will be described below, but the method for producing the film for molding of the present invention is not limited thereto.

[0065] The adhesive coating material is applied to the polyester film obtained as described above.The coating method at this time can be selected from coating methods such as gravure coater, gravure reverse coater, lip coater, flexo coater, blanket coater, roll coater, knife coater, air knife coater, kiss touch coater, kiss touch reverse coater, comma coater, comma reverse coater, micro reverse coater, etc., depending on the viscosity and coating amount of the adhesive coating material, but when using a two-liquid curing polyurethane adhesive, gravure coater is preferably used.

[0066] Next, the film is passed through a drying oven to dry the solvent component of the adhesive. The drying temperature is selected depending on the type of adhesive resin, the type of solvent, the heat resistance of the polyester film, etc., but is preferably 40°C to 120°C.

[0067] Next, the adhesive layer-coated surface of the polyester film coated with the adhesive layer and the resin layer (X layer) previously formed into a sheet are laminated by passing the laminated surface between the two opposing rolls while applying a pressure of, for example, 0.1 to 10 MPa between the two opposing rolls. From the viewpoint of applying pressure uniformly in the width direction, it is preferable that the surface of at least one of the two opposing rolls is covered with rubber, not metal. In addition, from the viewpoint of increasing the adhesion between the adhesive layer and the sheet (X layer) to be attached, it is preferable that at least one of the two opposing rolls is heated to 30°C to 120°C.

[0068] The laminated film thus obtained is wound on a sheet winding core, and, if necessary, the laminated film is wound on a roll and aged at 20 to 60°C for 24 to 168 hours for the purpose of hardening the two-component curing polyurethane adhesive. When such aging is performed, if the temperature is less than 20°C and / or the aging time is less than 24 hours, the adhesive will not be cured sufficiently to obtain sufficient adhesive strength, and the laminated film may become misaligned in the subsequent process. If the temperature exceeds 60°C and / or the aging time exceeds 168 hours, the rolled sheet may have noticeable tightening marks, resulting in streaky appearance defects. In this way, the film for molding of the present invention having an X layer on one side can be obtained.

[0069] When forming the X layer on both sides of the polyester film, the X layer may be formed on the polyester film side of the molding film of the present invention having the X layer on one side by the same method. Also, two or more polyester films manufactured as described above may be used to form the molding film of the present invention. The method of laminating a plurality of polyester films is not particularly limited, and lamination can be performed using the same method as the method of laminating the polyester film and the X layer described above.

[0070] The film for molding of the present invention has a metallic luster tone and is excellent in moldability during molding processing and electromagnetic wave transmittance of the molded body, so it can be suitably used as a molded body. The molded body of the present invention has the film for molding of the present invention. The method for forming the molded body is not particularly limited as long as it does not impair the effects of the present invention, and for example, molding processing methods such as insert molding and vacuum and pressure molding can be used.

[0071] The resin used in the insert molding is not particularly limited as long as it does not impair the effects of the present invention, and examples of resins that can be used include polybutadiene resins, polystyrene resins, polypropylene resins, acrylic resins, polyacrylonitrile-styrene copolymer resins, polyacrylonitrile-butadiene-styrene copolymer resins, polycarbonate resins, and polyacrylonitrile-ethylene propylene-styrene copolymer resins. In addition, various additives may be added as long as they do not impair the effects of the present invention. Examples of additives that can be preferably used include ultraviolet absorbers and pigments for coloring purposes.

[0072] Furthermore, the molding substrate used in vacuum and compressed air molding is not particularly limited as long as it does not impair the effects of the present invention, and examples of the substrate that can be used include resins such as polybutadiene resins, polystyrene resins, polypropylene resins, acrylic resins, polyacrylonitrile-styrene copolymer resins, polyacrylonitrile-butadiene-styrene copolymer resins, polycarbonate resins, and polyacrylonitrile-ethylene propylene-styrene copolymer resins; metals such as aluminum and magnesium; glass; and carbon fiber moldings.

[0073] In order to further improve the design of the molded product, a partial printed layer may be provided on the molding film by a known method prior to insert molding or vacuum / compressed air molding. EXAMPLES

[0074] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0075] [Measurement and evaluation methods] The measurements and evaluations shown in the examples were carried out under the following conditions.

[0076] (1) Thickness of X layer and polyester film Three samples of 1 cm square were cut out from the widthwise center of the molding film, and then each was cut in the thickness direction (perpendicular to the film surface) using a microtome to obtain a slice sample. In order to increase the contrast, the slice sample was subjected to metal sputtering treatment as necessary, and then the cross section of the slice sample was imaged at an appropriate magnification (for example, 200 to 1000 times) using a scanning electron microscope S-3400N (manufactured by Hitachi High-Technologies Corporation). The layer thickness of the X layer and the polyester film was calculated by measuring from the obtained image. The average value of the thickness obtained from each of the three samples was taken as the thickness of the X layer and the polyester film. The presence or absence of the X layer and whether it was present on only one side or both sides of the polyester film were also determined from the image taken here.

[0077] (2) Heat shrinkage rate of polyester film at 150℃ for 30 minutes The adhesive layer was peeled off from the film for molding, and the adhesive layer was removed with a solvent or scraped off with a knife to obtain the X layer and polyester film. However, when the polyester film or X layer used in the film for molding could be prepared as a single film, it was used (the same applies to the following measurements and evaluations). A sample was cut out to a size of 10 mm x 160 mm so that any one direction of the obtained polyester film was the longitudinal direction, and marked lines were drawn at intervals of 100 mm. After leaving it for 2 hours in an environment of 23 ± 3 ° C and 65 ± 10% RH, the distance between the marked lines was read to the nearest 0.01 mm using a universal projector (the read value is L0). Next, it was placed in a hot air oven set at 150 ° C for 30 minutes, cooled for 2 hours in an environment of 23 ± 3 ° C and 65 ± 10% RH, and then the distance between the marked lines was read to the nearest 0.01 mm using a universal projector (the read value is L1). The heat shrinkage was calculated using the formula "(L0-L1) / L0×100(%)", and three samples were evaluated in the same manner, with the average value being designated as HS(0). Next, the polyester film was cut into a size of 10 mm×160 mm by rotating it in the in-plane direction by 15°, 30°, 45°, 60°, 75°, 90°, 105°, 120°, 135°, 150°, and 165° from any one of the above directions, and similarly, HS(15), HS(30), HS(45), HS(60), HS(75), HS(90), HS(105), HS(120), HS(135), HS(150), and HS(165) were calculated, and the largest value, including HS(0), was designated as the heat shrinkage of the polyester film under the condition of 150°C for 30 minutes.

[0078] (3) Presence or absence of an adhesive layer Using a rotary microtome manufactured by Japan Microtome Laboratory Co., Ltd., the molding film was cut in a direction perpendicular to the film surface to prepare a sample. The sample was then observed under a scanning electron microscope (S-3400N manufactured by Hitachi, Ltd.) at magnifications of 1,000x to 10,000x to determine the presence or absence of an adhesive layer.

[0079] (4) Layer structure, layer thickness, number of layers with layer-to-layer thickness of 200 nm or more and less than 250 nm, and number of layers with layer-to-layer thickness of 100 nm or more and less than 200 nm A cross section parallel to the thickness direction was cut out from the sample of the film for molding using a microtome. Next, the cross section of the polyester film was observed at 40,000 times magnification using a transmission electron microscope (TEM) H-7100FA model manufactured by Hitachi, Ltd. at an acceleration voltage of 75 kV, and the cross section was photographed to measure the layer structure and layer thickness. 4 The sample was dyed using a dye. Next, a specific method for determining the layer structure and layer thickness of the polyester film will be described. A cross-sectional photograph taken with a TEM at a magnification of about 40,000 times was captured at an image size of 729 dpi using a "CanonScan" (registered trademark) D123U (manufactured by Canon Inc.). The image was saved in JPEG format, and then the JPEG file was opened using image processing software Imagc-Pro Plus ver.4 (sold by Planetron Co., Ltd.) to perform image analysis. In the image analysis process, the relationship between the average brightness in the area sandwiched between two lines in the thickness direction and width direction was read as numerical data in the vertical thick profile mode. Using a spreadsheet software ("Excel" (registered trademark) 2000 manufactured by Microsoft Corporation), data was collected for the position (nm) and brightness data at sampling step 6 (thinning out 6), and then numerical processing was performed using a three-point moving average. Furthermore, the data of the periodically changing brightness was differentiated, and the maximum and minimum values ​​of the differential curve were read using a VBA (Visual Basic for Applications) program, and the distance between adjacent values ​​was calculated as the layer thickness of one layer. This operation was performed for each photograph, and the layer thickness of all layers was calculated. Of the layer thicknesses obtained, the thin layer was considered to be a layer with a thickness of less than 1 μm. For the thin layer, the average value of the sum of the layer thicknesses of adjacent A and B layers was calculated for all pairs in sequence, and the number of layers with a layer-to-layer thickness of 200 nm or more and less than 250 nm and the number of layers with a layer-to-layer thickness of 100 nm or more and less than 200 nm were counted.

[0080] (5) Average reflectance in the wavelength range of 400 to 700 nm A sample of 5 cm square was cut out from the center of the molding film. Then, the relative reflectance at an incidence angle Φ=10° was measured using a Hitachi U-4100 spectrophotometer. The inner wall of the attached integrating sphere was made of barium sulfate, and the standard plate was made of aluminum oxide. The measurement wavelength was 250 nm to 1200 nm, the slit was 2 nm (visible) / automatic control (infrared), the gain was set to 2, and the measurement was performed at a scanning speed of 600 nm / min. The back side of the sample was painted black with oil-based ink. Next, the average reflectance in the wavelength band of 400 to 700 nm was calculated. The average reflectance was calculated by calculating the area surrounded by the reflection curve and the wavelength band based on the Simpson method formula using the data of the absolute reflectance at every 1 nm wavelength, and dividing it by 300 nm, which is the width of the wavelength band. A detailed explanation of the Simpson method is described in "Numerical Calculation Methods for Electronic Computers I" (Baifukan Publishing, 1965) by Jiro Yamauchi et al.

[0081] (6) Warping evaluation when the print layer is dried Using a screen printing machine and a screen plate with a checkered pattern of 10mm x 10mm, a molding film cut to a size of 200mm x 300mm was coated with an acrylic / urethane black ink on the surface so that the coating thickness after drying would be 20μm, and the film was dried for 10 minutes in a hot air oven set at 80℃. 10 minutes after being placed in the drying process, the warping of the film immediately before being removed from the oven was evaluated according to the following criteria, with a score of B or higher being considered a pass. A: The warpage of the film immediately before it was removed from the oven was less than 15 mm. B: The warpage of the film immediately before being removed from the oven was 15 mm or more and less than 50 mm. C: The warpage of the film immediately before being removed from the oven was 50 mm or more.

[0082] (7) Molding conformity during molding process The molding film sample prepared as described in (6) was set in an injection molding machine manufactured by Japan Steel Works, Ltd., with the mold temperature set to 60°C, and injection molding was performed using polycarbonate resin heated to 230°C to obtain a molded body. The moldability of the molding decorative film was evaluated based on the state in which the obtained molded body was molded along the mold (drawing ratio: molding height / bottom diameter) according to the following criteria, with a score of B or higher being considered a pass. A: Molding was possible with a drawing ratio of 0.3 or more. B: Molding was possible with a drawing ratio of 0.1 or more and less than 0.3, but molding was not possible with a drawing ratio of 0.3 or more. C: The drawing ratio was less than 0.1 and molding was not possible.

[0083] (8) Heat resistance of molded products (7) The sample for moldability evaluation was placed in a hot air oven set at 120℃ for 1 hour, and then cooled to room temperature (23±2℃). The peeling condition inside the molded film was evaluated according to the following criteria, with a grade of C or higher being considered a pass. Samples with a grade of C for moldability were not evaluated. A: No peeling of the molding film was observed over the entire molded body. B: Peeling of the molding film was observed at locations where the drawing ratio was 0.3 or more, but no peeling of the molding film was observed at locations where the drawing ratio was less than 0.3. C: Peeling of the molding film was observed at locations where the drawing ratio was 0.1 or more, but peeling of the molding film was not observed at locations where the drawing ratio was less than 0.1. D: None of A to C applied.

[0084] (9) In-plane refractive index of layer A or B of polyester film The resin used for the A layer was melted at 290°C in a vented twin-screw extruder, and then introduced into a T-die through a gear pump and a filter to form a sheet. The sheet was then rapidly solidified by contacting it with a casting drum whose surface temperature was kept at 25°C by applying static electricity, to obtain a cast film with a thickness of 100 μm. A sample was taken from the center of the width direction of the obtained film, and the refractive index in the flow direction and width direction of the film was measured using an Abbe refractive index NAR 4T manufactured by Atago Co., Ltd. and sodium D line as a light source, and the average value was taken as the in-plane refractive index. Similarly, a cast film was produced using the resin used for the B layer, and the in-plane refractive index was determined.

[0085] [Thermoplastic resins, etc. used in the manufacture of molding films] As the thermoplastic resin for obtaining the polyester film used for the molding film, for example, the following was used.

[0086] (Thermoplastic resin A-1) To a mixture of 100 parts by weight of dimethyl terephthalate and 60 parts by weight of ethylene glycol, 0.09 parts by weight of magnesium acetate and 0.03 parts by weight of antimony trioxide were added relative to the amount of dimethyl terephthalate, and the mixture was heated and heated in a conventional manner to carry out an ester exchange reaction. Next, 0.020 parts by weight of an 85% aqueous solution of phosphoric acid relative to the amount of dimethyl terephthalate was added to the ester exchange reaction product, and then the mixture was transferred to a polycondensation reaction tank. Furthermore, the reaction system was gradually depressurized while heating and heating, and a polycondensation reaction was carried out at 290°C under a reduced pressure of 1 mmHg in a conventional manner to obtain polyethylene terephthalate (hereinafter sometimes referred to as PET) with an intrinsic viscosity (IV) of 0.63. This was designated as thermoplastic resin A-1.

[0087] (Thermoplastic resin A-2) Except for using a mixture of 100 parts by weight of dimethyl 2,6-naphthalenedicarboxylate and 60 parts by weight of ethylene glycol, polymerization was carried out in the same manner as for thermoplastic resin A-1 to obtain a polyethylene naphthalate (hereinafter sometimes referred to as PEN) resin having an intrinsic viscosity (IV) of 0.67. This was designated as thermoplastic resin A-2.

[0088] (Thermoplastic resin B-1) Polymerization was carried out in the same manner as for thermoplastic resin A-1, except that 21 mol% of spiroglycol (SPG) was mixed with ethylene glycol, and 24 mol% of cyclohexanedicarboxylic acid (CHDC) was mixed with dimethyl terephthalate and copolymerized, to obtain a copolymer polyester resin with an intrinsic viscosity (IV) of 0.55. This was designated as thermoplastic resin B-1.

[0089] (Thermoplastic resin B-2) Polymerization was carried out in the same manner as for thermoplastic resin A-1, except that ethylene glycol was mixed with 30 mol% of cyclohexanedimethanol (CHDM) and copolymerized, to obtain a copolymer polyester resin with an intrinsic viscosity (IV) of 0.72. This was designated as thermoplastic resin B-2.

[0090] (Thermoplastic resin B-3) A copolymer polyester resin mixture obtained by mixing the thermoplastic resin A-1 and the thermoplastic resin B-2 in a mass ratio of 65:35 was used as the thermoplastic resin B-3.

[0091] (Thermoplastic resin B-4) A copolymer polyester resin mixture obtained by mixing the thermoplastic resin A-1 and the thermoplastic resin B-2 at a mass ratio of 70:30 was used as the thermoplastic resin B-4.

[0092] (Thermoplastic resin B-5) A copolymer polyester resin mixture obtained by mixing the thermoplastic resin A-1 and the thermoplastic resin B-2 at a mass ratio of 75:25 was used as the thermoplastic resin B-5.

[0093] (Film for forming X-layer) (Film C-1a (PET)) Toray Industries, Inc.'s "Lumirror" (registered trademark) U48, film thickness 125 μm, was used.

[0094] (Film C-1b (PET)) Toray Industries, Inc.'s "Lumirror" (registered trademark) U48, film thickness 250 μm, was used.

[0095] (Film C-2 (PMMA)) The acrylic resin film "Technoloy" (registered trademark) S001 manufactured by Sumika Acrylic Sales Co., Ltd., with a film thickness of 125 μm, was used.

[0096] (Film C-3 (ABS)) An ABS film manufactured by Towa Kako Co., Ltd., having a film thickness of 100 μm, was used.

[0097] (Film C-4 (PS)) "Styrophane" (registered trademark) GL manufactured by Oishi Sangyo Co., Ltd., with a film thickness of 100 μm was used.

[0098] (Film C-5a (PC)) Polycarbonate resin (weight average molecular weight 40,000) polymerized by the phosgene method was molten at 280°C in a twin-screw extruder, then passed through a gear pump and a filter and introduced into a T-die to be molded into a sheet. The sheet was then brought into contact with a casting drum whose surface temperature was kept at 25°C and rapidly cooled and solidified to obtain a cast film. The film with a thickness of 125 μm was then wound up on a winder.

[0099] (Film C-5b (PC)) A 250 μm film was obtained in the same manner as for film C-5a, except for adjusting the speed of the casting drum.

[0100] Example 1 (Manufacture of polyester film) Thermoplastic resin A-1 and thermoplastic resin B-5 were melted at 290°C in separate vented twin-screw extruders, and then merged in a 901-layer feed block having four separate members with 225 slits via a gear pump and a filter. The outermost layers on both sides, which become thick film layers due to the configuration of the feed block, were thermoplastic resin A, and thermoplastic resin A and thermoplastic resin B were alternately laminated, and the layer thickness of the adjacent layer made of thermoplastic resin A and layer made of thermoplastic resin B were made to be almost the same. Next, the film was guided to a T-die and molded into a sheet, and then it was brought into contact with a casting drum whose surface temperature was kept at 25°C by electrostatic application and rapidly cooled and solidified to obtain a cast film. Thereafter, the obtained cast film was heated with a group of rolls set at 75°C, and then stretched 3.3 times in the longitudinal direction (longitudinal direction) while being rapidly heated from both sides of the film by a radiation heater so that the film temperature was 80 to 150°C within a stretching section length of 100 mm, and then cooled once to obtain a uniaxially stretched film. The obtained uniaxially stretched film was introduced into a tenter, preheated with hot air at 100°C, and then stretched 3.5 times in the transverse direction at a temperature of 110 to 150°C. The biaxially stretched film was subjected to a 7% relaxation treatment in the width direction in the tenter at 240°C, cooled to room temperature, and wound up with a winder. The heat shrinkage rate (largest direction) of the film obtained at this stage under a condition of 150°C for 30 minutes was 2.4% (longitudinal direction of the film). Next, the obtained film was passed through a 140°C oven for 30 seconds under a tension of 40N / m in the longitudinal direction, and heat-treated (hereinafter, this process may be referred to as a heat treatment process). The evaluation results of the obtained polyester film are shown in Table 1.

[0101] (Manufacturing of molding film) A two-component polyurethane thermosetting adhesive (Toyo Ink Co., Ltd. dry lamination adhesive BLS-PC21) was reverse-coated on one side of the obtained polyester film using a gravure coater, with a wet coating amount of 5 g / m. 2The coating was applied and dried at a drying temperature of 70°C to 90°C at a speed of 20 m / min. The polyester resin film (film C-1b) having a thickness of 250 μm was then laminated using a nip roll at a nip pressure of 0.4 MPa and a temperature of 40°C to form an X layer (X1 layer), thereby obtaining the intended film for molding. The evaluation results of the obtained polyester film, film for molding, and molded bodies using them are shown in Table 1.

[0102] (Examples 2 to 8) A polyester film and a film for molding were obtained in the same manner as in Example 1, except that the thermoplastic resin A, the thermoplastic resin B, and the film for forming the X1 layer were as shown in Table 1. The evaluation results are shown in Table 1.

[0103] Example 9 A polyester film and a film for molding were obtained in the same manner as in Example 8, except that the oven temperature in the heat treatment step was changed to 150° C. The evaluation results are shown in Table 1.

[0104] Example 10 A polyester film and a film for molding were obtained in the same manner as in Example 8, except that the oven temperature in the heat treatment step was changed to 160° C. and the tension was changed to 20 N / m. The evaluation results are shown in Table 1.

[0105] Example 11 A 250 μm thick PC resin film (film C-5b) was attached to the other surface of the polyester film of the molding film obtained in Example 10 in the same manner to form an X layer (X2 layer), thereby obtaining a molding film. The evaluation results are shown in Table 1.

[0106] Example 12 A polyester film and a film for molding were obtained in the same manner as in Example 11, except that the thermoplastic resin used for the polyester film was changed to Thermoplastic Resin A-2 and Thermoplastic Resin B-1. The evaluation results are shown in Table 1.

[0107] Comparative Example 1 Except for not carrying out the heat treatment step, a film for molding was obtained in the same manner as in Example 1. The evaluation results are shown in Table 1.

[0108] Comparative Example 2 A film for molding was obtained in the same manner as in Example 8, except that the oven temperature in the heat treatment step was 160° C. and the tension was 80 N / m. The evaluation results are shown in Table 1.

[0109] Comparative Example 3 On one side of "Lumirror" (registered trademark) X10S (film thickness 75 μm) manufactured by Toray Industries, Inc., mirror ink silver B manufactured by Seiko Advance Co., Ltd. was printed using a screen printer so that the thickness after drying would be 3 μm, and then dried in a hot air oven at 80° C. for 1 hour. An acrylic resin film (film C-2) was formed on the side with the printed layer, and a PC resin film (film C-5b) was formed on the opposite side in the same manner as in Example 11, thereby forming X1 layer and X2 layer to obtain a film for molding. The evaluation results are shown in Table 1.

[0110] [Table 1] [Industrial Applicability]

[0111] According to the present invention, it is possible to provide a film for molding that has excellent formability during molding processing and excellent heat resistance after processing into a molded product. Since the film for molding of the present invention has excellent properties, it can be suitably used for decorating parts that require high heat resistance, such as molding members for building materials, automobile parts, mobile phones, electrical products, and game machine parts. [Explanation of symbols]

[0112] 1: Molding film 2: Polyester film 3: Resin layer (X layer) 4: Adhesive layer

Claims

1. The molding film has a resin layer (X layer) on at least one side of a polyester film, and is characterized in that the heat shrinkage rate of the polyester film under conditions of 150°C for 30 minutes is -1.0% or more and 2.0% or less in the largest direction.

2. 2. The molding film according to claim 1, wherein the main component of the X layer is a non-crystalline resin.

3. 2. The molding film according to claim 1, further comprising at least one adhesive layer between said X layer and said polyester film.

4. The molding film according to claim 1, characterized in that the polyester film has a structure in which a layer (A layer) mainly composed of thermoplastic resin A and a layer (B layer) containing a thermoplastic resin B different from the thermoplastic resin A are alternately laminated in the thickness direction to a total of 51 or more layers.

5. 2. The film for molding according to claim 1, characterized in that the average reflectance in the wavelength band of 400 nm to 700 nm is 30% or more.

6. A molded body comprising the film for molding according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Three-dimensional molding decorative sheet, method for manufacturing the same, decorative resin molded product using the decorative sheet, and method for manufacturing the same

    JP2012201032A

  • Film for molding, sheet for molding, decorative film for molding and molded body using them

    JP2018069552A