Diamond and method for manufacturing the same

By synthesizing a pure diamond film followed by a phosphorus-containing film using controlled gas doping, the method addresses quality deterioration in diamond production, achieving smooth surfaces and high quality factors.

JP2024137038APending Publication Date: 2024-10-04NAT UNIV CORP KYUSHU INST OF TECH (JP)
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023048390
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing methods for producing diamond with a smooth surface, such as chemical vapor phase methods, risk deteriorating the quality of the diamond due to impurities added to the gas, necessitating additional processing equipment for surface smoothing.

Method used

A method involving the synthesis of a pure diamond film using a first gas without impurities, followed by a phosphorus-containing diamond film formation using a second gas doped with phosphorus, ensuring an impurity concentration of 0 cm-3 to 1×10^17 cm-3, with specific gas ratios to maintain quality and smoothness.

Benefits of technology

This approach enables the production of diamonds with smooth surfaces and high diamond quality factors of 90% or more, suppressing quality deterioration and enhancing surface smoothness compared to direct synthesis on a substrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137038000001_ABST
    Figure 2024137038000001_ABST
Patent Text Reader

Abstract

To provide a method for manufacturing diamond having a smooth surface, capable of suppressing reduction in quality, and the diamond.SOLUTION: A method for manufacturing diamond comprises: a base formation step of synthesizing pure diamond film by a chemicals vapor phase method using first gas including carbon without including impurities except a material inevitably mixed; and a phosphorus containing film formation step of synthesizing a phosphorus containing diamond film on the pure diamond film by a chemicals vapor phase method by second gas including carbon and having doped phosphorus. The diamond manufactured by the manufacturing method includes the phosphorus containing diamond film including phosphorus and formed on the pure diamond film having an impurity concentration of 0 cm-3 or more and 1×1017 cm-3.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to diamond and a method for producing the same. [Background technology]

[0002] Conventionally, methods of producing diamond with a smooth surface have been considered, such as processing the diamond surface to make it smooth, or synthesizing a diamond film with a smooth surface by chemical vapor deposition. For example, Patent Document 1 discloses a method of smoothing the diamond surface by processing with laser light, and Patent Document 2 discloses a method of synthesizing a diamond film with a smooth surface by chemical vapor deposition. Synthesizing diamond and processing the surface of the synthesized diamond to make it smooth requires processing equipment in addition to the equipment used to synthesize diamond. Therefore, when synthesizing diamond, it is desirable to synthesize diamond with a smooth surface from the standpoint of simplifying the equipment. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2020 / 026393 [Patent Document 2] Japanese Patent Application Publication No. 06-247795 Summary of the Invention [Problem to be solved by the invention]

[0004] However, when synthesizing diamond using the chemical vapor deposition method, if one tries to control the surface of the diamond by adding impurities to the gas used, the quality of the synthesized diamond (the inherent properties of diamond without impurities) is affected by the impurities and reduced, which is a problem. The present invention has been made in view of the above circumstances, and has an object to provide a method for producing diamond having a smooth surface while suppressing deterioration in quality, and to provide such diamond. [Means for solving the problem]

[0005] The diamond manufacturing method of the first invention in line with the above-mentioned object comprises a base formation step of synthesizing a pure diamond film by chemical vapor deposition using a first gas that contains carbon and does not contain any impurities other than substances that are unavoidably mixed in, and a phosphorus-containing film formation step of synthesizing a phosphorus-containing diamond film on the upper side of the pure diamond film by chemical vapor deposition using a second gas that contains carbon and is doped with phosphorus.

[0006] The diamond according to the second invention, which is in accordance with the above object, has an impurity concentration of 0 cm -3 More than 1×10 17 cm -3 A phosphorus-containing diamond film containing phosphorus is formed on the upper side of the following pure diamond film. Effect of the Invention

[0007] The diamond manufacturing method of the first invention includes a base formation process in which a pure diamond film is synthesized by chemical vapor deposition using a first gas that contains carbon and does not contain any impurities other than substances that are unavoidably mixed in, and a phosphorus-containing film formation process in which a phosphorus-containing diamond film is synthesized on the upper side of the pure diamond film by chemical vapor deposition using a second gas that contains carbon and is doped with phosphorus, so that it is possible to produce diamonds with smooth surfaces while suppressing deterioration in quality. Furthermore, the diamond according to the second invention has a phosphorus-containing diamond film formed on the upper side of a pure diamond film, and is therefore a diamond manufactured by the diamond manufacturing method according to the first invention, and has a smooth surface and a certain level of quality or higher. [Brief description of the drawings]

[0008] [Figure 1] Electron microscope photographs of the surfaces of samples D and H. [Diagram 2] Electron microscope photographs of the surfaces of samples A and B. [Diagram 3]Electron microscope photographs of the surfaces of samples C and D. [Figure 4] 1 is an electron microscope photograph of the surface of sample G. [Diagram 5] 1 is a graph showing the relationship between film thickness and surface roughness. [Figure 6] FIG. 1 is an explanatory diagram of measurement results by Raman spectroscopy. [Figure 7] 1 is a graph showing the relationship between the phosphorus to carbon ratio and diamond quality factor. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Next, with reference to the attached drawings, an embodiment of the present invention will be described for understanding the present invention. A method for producing diamond according to one embodiment of the present invention includes a base formation step of synthesizing a pure diamond film by chemical vapor deposition using a first gas that contains carbon and does not contain any impurities other than substances that are inevitably mixed in, and a phosphorus-containing film formation step of synthesizing a phosphorus-containing diamond film on the upper side of the pure diamond film by chemical vapor deposition using a second gas that contains carbon and is doped with phosphorus.

[0010] In addition, the diamond produced by the manufacturing method according to the present embodiment has an impurity concentration of 0 cm -3 More than 1×10 17 cm -3 The phosphorus-containing diamond film is formed on the upper side of the pure diamond film described below. These will be described in detail below.

[0011] In this embodiment, diamond is manufactured through the following steps. First, a pretreatment step is performed on a plate-shaped object made of silicon, silicon carbide, cemented carbide, etc., to attach nanodiamonds that will be growth nuclei when diamonds are synthesized by the chemical vapor deposition method described below (pretreatment step). Instead of attaching nanodiamonds to the plate-shaped object, the surface of the plate-shaped object may be subjected to a treatment to form scratches or fine irregularities so that the growth of diamonds can be started stably. Hereinafter, the plate-shaped object that has undergone the pretreatment step is called a substrate.

[0012] Next, a substrate is placed in a vacuum chamber, and while the substrate is heated by a heater or the like, a first gas containing carbon (e.g., methane) is supplied into the vacuum chamber to grow diamond on the substrate, and a pure diamond film is formed on the substrate by synthesizing diamond in a film-like form (base formation process). A gas mixture of a hydrocarbon gas such as methane (CH4) and hydrogen (H2) gas can be used as the first gas.

[0013] After forming a pure diamond film on the substrate, a second gas containing carbon and doped with phosphorus is supplied into the vacuum chamber while the substrate is heated, to form a phosphorus-containing diamond film doped with phosphorus as an impurity on the pure diamond film (phosphorus-containing film formation process). As the second gas, a gas obtained by mixing a hydrocarbon gas (such as methane gas) with hydrogen gas and a gas containing phosphorus (for example, PMe3 gas or PH3 gas) can be used.

[0014] By going through the above-mentioned pretreatment process, base formation process, and phosphorus-containing film formation process, a diamond is manufactured in which a phosphorus-containing diamond film is formed on the top of a pure diamond film. In order for the diamond to have a certain level of quality and surface smoothness, the concentration of impurities in the pure diamond film must be 0 cm -3 More than 1×10 17 cm -3 It is necessary that the ratio of phosphorus to carbon in the second gas is 0.1 atomic % or more and 2.0 atomic % or less, and it is preferable that the ratio of carbon to hydrogen in the second gas is less than 0.5 atomic %. -3 means substantially free of impurities.

[0015] The concentration of impurities in the pure diamond film is 1×10 17 cm -3 If the concentration exceeds 100%, the quality and surface smoothness of the diamond formed through the base formation process and the phosphorus-containing film formation process may be significantly reduced. In this embodiment, the pure diamond film does not contain impurities other than those substances that are inevitably mixed in. From the viewpoint of efficiently growing diamond nuclei by chemical vapor deposition, it is preferable to set the ratio of carbon to hydrogen in the second gas to 0.1 atomic % or more.

[0016] According to the diamond manufacturing method of the present embodiment, it is possible to stably manufacture diamonds having a diamond quality factor of 90% or more by Raman spectroscopy targeting phosphorus-containing diamond films. From the viewpoint of manufacturing diamonds having a diamond quality factor of 90% or more and a smooth surface, it is necessary to form a diamond film having a phosphorus concentration of 1×10 on the upper side of a pure diamond film. 18 cm -3 It is preferable to synthesize a phosphorus-containing diamond film having a phosphorus concentration of 1×10 or more. Even if a phosphorus-containing diamond film is synthesized on the top of a pure diamond film, the phosphorus concentration of the phosphorus-containing diamond film is not more than 1×10 17 cm -3 If the thickness is below this, then in order to produce a diamond having a smooth surface and a diamond quality factor of 90% or more, it will be necessary to control the thickness of the phosphorus-containing diamond film to a predetermined range.

[0017] In the base formation process and the phosphorus-containing film formation process, the temperature of the heated substrate may be any temperature at which diamond can be synthesized by chemical vapor deposition, for example, 700°C to 1000°C. The temperature of the substrate can be measured without contact using a radiation thermometer. In the base formation process and the phosphorus-containing film formation process, the pressure in the vacuum vessel may be any pressure at which diamond can be vapor-grown on the substrate, for example, 10 Torr to 100 Torr. EXAMPLES

[0018] Next, an experiment conducted to confirm the effects of the present invention will be described. A substrate was prepared by attaching nanodiamonds to a silicon plate, and either or both of a pure diamond film and a phosphorus-containing diamond film were synthesized on the substrate using the hot filament CVD method to produce samples A to O shown in Tables 1 and 2.

[0019] [Table 1]

[0020] [Table 2]

[0021] The hot filament CVD method was performed with tungsten as the filament material, a filament temperature of 2000°C or higher, and a vacuum chamber pressure of 30 Torr. A mixed gas of hydrogen and methane was used to synthesize the pure diamond film, and a mixed gas of hydrogen, methane, and trimethylphosphine was used to synthesize the phosphorus-containing diamond film.

[0022] In addition, samples B to G and samples M to O having pure diamond film and phosphorus-containing diamond film were samples in which phosphorus-containing diamond film was formed on the top of pure diamond film synthesized on substrate. Also, each ratio of CH4 / H2 and PMe3 / CH4 in Tables 1 and 2 means the ratio of molecular weight (CH4 / H2 is the ratio of methane molecules to hydrogen molecules, and PMe3 / CH4 is the ratio of trimethylphosphine molecules to methane molecules).

[0023] Therefore, CH4 / H2 is about twice the atomic weight ratio (atomic %) of carbon to hydrogen in the gas in the vacuum chamber, and PMe3 / CH4 is almost equal to the atomic weight ratio (atomic %) of phosphorus to carbon in the gas in the vacuum chamber. The "film thickness (μm)" values ​​in Tables 1 and 2 refer to the total thickness of the diamond film formed on the substrate (for sample B, the total thickness of the pure diamond film and the phosphorus-containing diamond film), and "n / a" in the grown film thickness in Table 1 indicates that the film thickness was not measured. For samples A to G and samples I to O, the thickness of the pure diamond layer formed on the substrate as the base formation process was about 0.7 μm.

[0024] Electron microscope photographs of samples D and H are shown in Figure 1. Sample D was a sample in which a pure diamond film and a phosphorus-containing diamond film were formed on a substrate, whereas sample H was a sample in which there was no pure diamond film and the phosphorus-containing diamond film was directly formed on the upper side of the substrate. As shown in Figure 1, sample H had more abnormally grown grains on the surface of the phosphorus-containing diamond film than sample D. Therefore, when the phosphorus-containing diamond film was synthesized on the upper side of the pure diamond film, the abnormal growth of diamond grains could be suppressed compared to when the phosphorus-containing diamond film was directly synthesized on the substrate, and as a result, the surface could be made smoother.

[0025] The surface roughness of samples B to H was measured, and the surface roughness was 0.11 μm for samples B and C, 0.08 μm for sample D, 0.07 μm for samples E and F, 0.06 μm for sample G, and 0.09 μm for sample H. In this experiment, the arithmetic mean roughness (Sa) was calculated by performing spline correction on the base value of the surface roughness detected using a three-dimensional scanning electron microscope ERA-8800 by Elionix Co., Ltd. The same applies to the surface roughness below.

[0026] The calculated surface roughness values ​​also revealed that the surface roughness was smoother when the phosphorus-containing diamond film was synthesized on top of the pure diamond film, as the surface roughness of sample D was smaller than that of sample H. In addition, the calculated surface roughness values ​​of samples B to G confirmed that when the phosphorus-containing diamond film was synthesized on top of the pure diamond film, the surface roughness value was smaller as the phosphorus concentration of the gas used in the chemical vapor deposition method was higher.

[0027] Electron microscope photographs of samples A to D and sample G are shown in Figs. 2 to 4. Sample A is a sample in which only a pure diamond film is synthesized on a substrate (specifically, a pure diamond film is further synthesized on the upper side of the pure diamond film), while samples B to D and sample G differ in the ratio of phosphorus to carbon in the gas used when synthesizing the phosphorus-containing diamond film on the upper side of the pure diamond film. From the electron microscope photographs in Figs. 2 to 4, it was confirmed that the higher the ratio of phosphorus to carbon in the gas used in the hot filament CVD method, the more the idiomorphic shape of the crystallites is broken and the smoother the surface (the surface of the upper pure diamond film for sample A, and the surface of the phosphorus-containing diamond film for samples B to D) becomes.

[0028] Next, the thickness and surface roughness of the films grown by the hot filament CVD method were measured for samples I to L, in which a pure diamond film was formed on top of the pure diamond film by the hot filament CVD method, and for samples M and N, in which a phosphorus-containing diamond film was formed on top of the pure diamond film by the hot filament CVD method, and the relationship between film thickness and surface roughness was derived.

[0029] The relationship between the thickness of the diamond film of the samples J to N (the value of "film thickness (μm)" in Table 2) and the surface roughness is shown in FIG. 5. In FIG. 5, the vertical axis Sa (μm) means the surface roughness, and the horizontal axis "Thickness (μm)" value in FIG. 5 is the thickness of the diamond film formed on the substrate. In FIG. 5, the thickness and surface roughness of the pure diamond film formed in the base formation process are indicated by filled circles for reference. From the relationship between the thickness and surface roughness of the film shown in FIG. 5, it was confirmed that the phosphorus-containing diamond film formed on the upper side of the pure diamond film can suppress the magnitude of the surface roughness that increases with the increase in film thickness compared to the upper pure diamond film formed on the upper side of the pure diamond film. In addition, it is known that the surface roughness of the film increases with the increase in film thickness.

[0030] The crystal structure measurement results for samples A to H by Raman spectroscopy are shown in Figure 6. In this measurement, an NRS-5100 from JASCO Corporation was used at a wave number of 900 cm -1 From 1800cm -1 The spectrum was detected in the range of 1000 to 10000. The spectrum was detected by irradiating samples A to H with incident light from a light source with a beam diameter of about 4 μm and an excitation wavelength of about 532 nm, which passed through a 20x objective lens. The grating was 1800.

[0031] In FIG. 6, "Pregrown" indicates the measurement result of sample H, "w / oPMe3" indicates the measurement result of sample A, and "0.1%, "0.4%, "1%, "2%, "4%" and "10%" indicate the measurement results of samples B, C, D, E, F and G, respectively. For samples B, C, D, E, F and G, the baseline was further subtracted based on the measurement result of the crystal structure by Raman spectroscopy, and then peak separation was performed using the Lorentz function, etc., to obtain the peak at 1332 cm -1The area of ​​the nearby diamond peak (referred to as "diaArea") and the area obtained by subtracting the area of ​​the diamond peak from the total area (referred to as "nondiaArea") were calculated, and the diamond quality factor (referred to as "fq") was calculated using the following formula 1. The method of calculating this diamond quality factor is the same for the following diamond quality factors. The unit of diamond quality factor is %.

[0032] fq=100{75.diaArea / (75.diaArea+nondiaArea)} Formula 1

[0033] The results of the diamond quality factor are shown in Figure 7. From these results, it was confirmed that the decrease in the diamond quality factor can be suppressed when the PMe3 / CH4 gas, i.e., the gas used when synthesizing the phosphorus-containing diamond film, is 2.0 atomic % or less, and that the decrease in the diamond quality factor becomes significant when the gas exceeds 2.0 atomic %.

[0034] Moreover, the diamond quality factor of samples I, J, M, and N is 91%, 94%, 92%, and 95%, respectively, as shown in Table 2. Here, samples I and J are samples in which a pure diamond film is formed on the top of a pure diamond film, and samples M and N are samples in which a phosphorus-containing diamond film is formed on the top of a pure diamond film, and the growth time of the upper film is 4 hours for samples I and M, and 8 hours for samples J and N. Therefore, the diamond quality factor of the phosphorus-containing diamond film formed on the top of a pure diamond film is larger than that of the upper pure diamond film formed on the top of a pure diamond film. Therefore, it can be said that the amount of phosphorus added (addition concentration) in samples M and N does not significantly reduce the diamond quality factor.

[0035] Furthermore, since the diamond quality factors of samples N and O were 95% and 79%, respectively, as shown in Table 2, it can be said that the decrease in the diamond quality factor became significant when the ratio of carbon to hydrogen in the gas (second gas) used to synthesize the phosphorus-containing diamond film was 0.5 atomic % or more (the ratio of CH4 / H2 was 1.0%) or more. In addition, the phosphorus concentration of the phosphorus-containing diamond film of sample N was measured by secondary ion mass spectrometry (SISM), and the phosphorus concentration was found to be 2×10 18 cm -3 It was.

[0036] Although the embodiment of the present invention has been described above, the present invention is not limited to the above-mentioned embodiment, and all changes in conditions that do not depart from the gist of the present invention are within the scope of application of the present invention. For example, the ratio of phosphorus to carbon in the second gas may be less than 0.1 atomic % or more than 2.0 atomic %, and the ratio of carbon to hydrogen in the second gas may be 0.5 atomic % or more. In addition, the diamond quality factor of the synthesized phosphorus-containing diamond film by Raman spectroscopy may be less than 90%. Furthermore, the pretreatment step can be omitted, although it is preferable to provide the pretreatment step from the viewpoint of efficiently synthesizing a pure diamond film.

Claims

1. A base forming step of synthesizing a pure diamond film by a chemical vapor deposition method using a first gas containing carbon and not containing impurities other than substances inevitably mixed in; and a phosphorus-containing film formation step of synthesizing a phosphorus-containing diamond film on the top of the pure diamond film by a chemical vapor deposition method using a second gas containing carbon and doped with phosphorus.

2. 2. The method of claim 1, wherein the second gas has a ratio of phosphorus to carbon of 0.1 atomic % or more and 2.0 atomic % or less.

3. 3. The method for producing diamond according to claim 1, wherein the second gas contains hydrogen, and the ratio of carbon to hydrogen in the second gas is less than 0.5 atomic %.

4. Impurity concentration is 0 cm -3 Above 1 x 10 17 cm -3 A diamond comprising a phosphorus-containing diamond film formed on the upper side of a pure diamond film comprising:

5. 5. The diamond according to claim 4, wherein the phosphorus-containing diamond film has a diamond quality factor of 90% or more as determined by Raman spectroscopy.

Citation Information

Patent Citations

  • Formation of diamond single crystal film