Soft nitrided component

A cost-effective nitrocarburized component with optimized C, Si, Mn, P, S, Al, and N composition, along with optional elements, addresses high-temperature embrittlement and cost issues, achieving superior bending fatigue properties.

JP2024137530AActive Publication Date: 2024-10-07JFE STEEL CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023049079
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-07
Estimated Expiration
2043-03-24

AI Technical Summary

Technical Problem

Existing soft-nitriding steels require high amounts of Cu, leading to increased manufacturing costs and high-temperature embrittlement, while shot peening increases costs without addressing bending fatigue properties effectively.

Method used

A nitrocarburized component with a specific composition including C, Si, Mn, P, S, Al, and N, with optional additions of Cr, Mo, Cu, Ni, Ti, Nb, V, Hf, Ta, Sn, Sb, Se, Ca, Pb, and Bi, achieving a maximum inverse pole figure strength distribution of 1.5 or more at a depth of 0.5 mm from the surface.

Benefits of technology

The component achieves excellent bending fatigue properties at a lower cost by optimizing the composition to enhance strength and toughness without relying on expensive metals like Cu and rare elements like V.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137530000002
    Figure 2024137530000002
  • Figure 2024137530000001
    Figure 2024137530000001
Patent Text Reader

Abstract

To provide a cost-efficient soft nitrided component with superior bending fatigue characteristics.SOLUTION: A soft nitrided component has a body composed of steel comprising C: 0.04 mass% or more and 0.35 mass% or less, Si: 0.01 mass% or more and 1.20 mass% or less, Mn: 0.30 mass% or more and 1.80 mass% or less, P: 0.1 mass% or less, S: 0.5 mass% or less, Al: 0.010 mass% or more and 0.300 mass% or less and N: 0.0250 mass% or less, with the balance being Fe and impurities. The body has a nitrided surface layer. At a depth of 0.5 mm from the surface of the body, the maximum strength value in the reverse pole figure intensity distribution, measured in a direction parallel to that surface, is 1.5 or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a nitrocarburized part. [Background technology]

[0002] In order to address environmental issues such as reducing carbon dioxide emissions, there is a demand for weight reduction in various industrial product parts. Nitriding is a heat treatment that improves the fatigue properties of steel parts while having the advantage of less heat treatment distortion compared to carburizing and quenching. Nitriding is applied to various steel parts, including vehicle gears. Improving fatigue properties allows steel parts to be made smaller, thereby realizing weight reduction in industrial products such as vehicles. Therefore, improving fatigue properties is desired for steel parts.

[0003] Patent Document 1 discloses a structural steel for soft nitriding. This structural steel for soft nitriding contains, by weight, 0.20-0.50% C, 0.03-0.50% Si, 0.30-3.00% Mn, 0.10-1.00% Cr, 0.03-1.00% Mo, 0.01-0.10% Al, 0.03-0.50% V, 0.015-0.070% S, 0-0.040% Pb, and 15 ppm or less O, with the balance being Fe and unavoidable impurities. In this structural steel for soft nitriding, a predetermined relationship is specified between the contents of S, Pb, and oxygen and the target material hardness and the target core hardness. This structural steel for soft nitriding is a steel that is machined in the as-rolled, as-forged, normalized, etc. state, and then soft-nitrided and shot peened for use, and is said to have excellent fatigue strength and machinability.

[0004] Patent Document 2 describes a steel for soft nitriding that has excellent bending fatigue strength. This steel for soft nitriding contains, in mass %, the following alloying elements: C: 0.01% to 0.15%, Si: 0.01% to 1.5%, Mn: 0.15% to 2%, Cu: 0.5% to 2%, N: limited to less than 0.005%, and contains one or more of Ti: 0.01% to 0.5%, Nb: 0.005% to 0.5%, and V: 0.05% to 0.5%, with C+N≦Ti / 4.0+Nb / 7.7+V / 4.3, and may further contain, as necessary, one or more of Ni: 0.5% to 2% or less, Cr: 0.1% to 2%, Al: 0.05% to 0.5% or less, S: 0.03% to 0.1%, and Pb: 0.005% to 0.3%, with the balance being Fe and unavoidable impurities. The area ratio of ferrite is 90% or more, and the remainder is made up of carbides and pearlite structures. The average size of pearlite is 20 μm or less. In this soft nitriding steel, Cu is an element that contributes to the age hardening of the core hardness during soft nitriding, and is considered to be essential for obtaining high fatigue strength. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 09-227992 [Patent Document 2] JP 2002-069572 A Summary of the Invention [Problem to be solved by the invention]

[0006] For example, when a large amount of Cu is added as in the case of the steel for nitrocarburizing disclosed in Patent Document 2, not only does it increase the manufacturing cost of the steel, but it also leads to high-temperature embrittlement of the steel, which may lead to a decrease in yield due to an increase in cracks after continuous casting and an additional increase in costs due to maintenance. When shot peening is performed as in the steel for nitrocarburizing disclosed in Patent Document 1, there is a problem that the manufacturing cost of the steel part increases. Therefore, it is desired to provide a low-cost nitrocarburized part with excellent bending fatigue properties and a steel that realizes this.

[0007] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a low-cost soft-nitrided part that is excellent in bending fatigue properties. [Means for solving the problem]

[0008] In order to achieve the above object, the soft nitrided part according to the present invention is as follows.

[0009] [1] The composition is as follows: C: 0.04% by mass or more and 0.35% by mass or less, Si: 0.01% by mass or more and 1.20% by mass or less, Mn: 0.30 mass% or more and 1.80 mass% or less, P: 0.1% by mass or less, S: 0.5% by mass or less, Al: 0.010% by mass or more and 0.300% by mass or less; N: 0.0250% by mass or less, The balance includes a body formed of steel containing Fe and impurities, The body has a nitrided surface layer; A soft nitrided part having a maximum strength value of 1.5 or more in an inverse pole figure intensity distribution measured at a depth of 0.5 mm from the surface of the body in a direction parallel to the surface.

[0010] [2] The steel has the following composition: Cr: 2.0% by mass or less, Mo: 1.0% by mass or less, Cu: 1.0% by mass or less, Ni: 1.0 mass% or less and B: 0.01% by mass or less, The soft nitrided part according to the above [1], further comprising one or more selected from the following:

[0011] [3] The steel has the following composition: Ti: 0.1% by mass or less, Nb: 0.1% by mass or less, V: 0.2% by mass or less, Hf: 0.1% by mass or less and Ta: 0.1% by mass or less, The soft nitrided part according to the above [1] or [2], further comprising one or more selected from the following:

[0012] [4] The steel has the following composition: Sn: 0.1 mass% or less and Sb: 0.1% by mass or less, The soft nitrided part according to any one of the above [1] to [3], further comprising one or more selected from the following:

[0013] [5] The steel has the following composition: Se: 0.3% by mass or less, Ca: 0.1% by mass or less, Pb: 0.3% by mass or less and Bi: 0.3% by mass or less, The soft nitrided part according to any one of the above [1] to [4], further comprising one or more selected from the following: Effect of the Invention

[0014] According to the present invention, it is possible to provide a soft nitrided part having excellent bending fatigue properties at low cost. [Brief description of the drawings]

[0015] [Figure 1] FIG. 2 is a schematic diagram showing the shape of a test piece. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, the soft-nitrided part according to this embodiment will be described.

[0017] First, an overview of the soft nitrided component according to this embodiment will be described.

[0018] The nitrocarburized component according to this embodiment includes a body made of the steel described below, and the body has a nitrided surface layer.

[0019] The steel forming the main body of the soft nitrided part according to this embodiment has a chemical composition (carbon) of 0.04% by mass or more and 0.35% by mass or less, Si (silicon): 0.01% by mass or more and 1.20% by mass or less, Mn (manganese): 0.30% by mass or more and 1.80% by mass or less, P (phosphorus): 0.1% by mass or less, S (sulfur): 0.5% by mass or less, Al (aluminum): 0.010% by mass or more and 0.300% by mass or less, and N (nitrogen): 0.0250% by mass or less, with the remainder being Fe (iron) and impurities.

[0020] In the soft nitrided component according to this embodiment, the maximum strength value in the inverse pole figure intensity distribution measured in a direction parallel to the surface at a depth of 0.5 mm from the surface of the body is 1.5 or more.

[0021] The soft nitrided part according to this embodiment is low cost and has excellent bending fatigue properties.

[0022] The soft-nitrided component according to this embodiment, its body, and the steel forming the body will be described in detail below.

[0023] An example of the soft nitrided part according to the present embodiment is a part forming a vehicle such as an automobile. Examples of parts in the field of automobiles include engine crankshafts, timing gears, etc., transmission gears, ring gears, sun gears, planetary gears, etc., of a transmission, steering pinions, worms, etc., of a suspension, and worms for power windows in an interior.

[0024] Nitriding includes both a nitriding treatment in which only nitrogen is introduced into steel, and a soft nitriding treatment in which nitrogen and carbon are introduced into steel at the same time, and both are treatments that do not cause martensitic transformation of steel. Of these, nitriding in this embodiment refers to soft nitriding.

[0025] The surface of the body of the soft-nitrided component according to this embodiment is nitrided as described above. That is, this body has a surface layer in which steel is nitrided. As an example, this surface layer is about 0.5 mm from the surface of the body. This embodiment also includes cases in which the thickness of this surface layer is greater.

[0026] The soft-nitrided component according to the present embodiment may be a component in which the main body is combined with another structure that is made of a metal or a metal alloy and has a non-nitrided surface. The soft-nitrided component according to the present embodiment may be a component in which the main body is combined with another structure that is not made of metal.

[0027] The component composition of the steel forming the body of the soft-nitrided component according to this embodiment is the composition of base steel into which nitrogen has not penetrated.

[0028] As described above, the steel forming the body of the soft-nitrided component according to this embodiment contains, as a chemical composition, C, Si, Mn, P, S, Al, and N, with the balance containing Fe and impurities. It is not excluded that this steel further contains optional components described later.

[0029] This steel may contain, as optional components, one or more selected from the group consisting of 2.0 mass% or less of Cr (chromium), 1.0 mass% or less of Mo (molybdenum), 1.0 mass% or less of Cu (copper), 1.0 mass% or less of Ni (nickel), and 0.01 mass% or less of B (boron).

[0030] In addition, this steel may contain, as an optional component composition, one or more selected from the group consisting of 0.1 mass% or less of Ti (titanium), 0.1 mass% or less of Nb (niobium), 0.2 mass% or less of V (vanadium), 0.1 mass% or less of Hf (hafnium), and 0.1 mass% or less of Ta (tantalum).

[0031] Furthermore, this steel may contain, as an optional component, at least one selected from the group consisting of 0.1 mass % or less of Sn (tin) and 0.1 mass % or less of Sb (antimony).

[0032] In addition, this steel may contain, as an optional component, one or more selected from the group consisting of 0.3 mass% or less of Se (selenium), 0.1 mass% or less of Ca (calcium), 0.3 mass% or less of Pb (lead), and 0.3 mass% or less of Bi (bismuth).

[0033] The content and effects of each component in the steel will be described in detail below. In the following description, when the content is simply stated, it means the content (mass%) in the steel.

[0034] The C content is 0.04% by mass or more and 0.35% by mass or less. In order to increase the central hardness after nitriding, the C content must be 0.04% by mass or more. If the C content exceeds 0.35% by mass, the load during cold working increases, which may shorten the life of the die. The C content is preferably 0.05% by mass or more and 0.27% by mass or less, more preferably 0.10% by mass or more and 0.25% by mass or less.

[0035] The Si content is 0.01% by mass or more and 1.20% by mass or less. In nitriding steel, Si serves as a deoxidizer. Excessive Si inclusion in steel may reduce the cold workability of the steel material and may also reduce the fatigue strength through a reduction in the toughness of the steel. The Si content is preferably 0.05% by mass or more and 0.70% by mass or less, more preferably 0.10% by mass or more and 0.50% by mass or less.

[0036] The Mn content is 0.30% by mass or more and 1.80% by mass or less. Mn improves hardenability and strengthens the pre-nitriding structure of steel, thereby strengthening the post-nitriding structure (nitrided steel). In order to obtain sufficient fatigue strength, the Mn content must be 0.30% by mass or more. If the steel contains excessive Mn, it may lead to an increase in deformation resistance. The Mn content is preferably 0.40% by mass or more and 1.70% by mass or less, and more preferably 0.50% by mass or more and 1.30% by mass or less.

[0037] The P content is 0.1 mass% or less. Since P segregates at the grain boundaries of nitriding steel and reduces toughness, the lower the P content, the more desirable it is. The P content is permitted up to 0.1 mass%. The P content is preferably 0.02 mass% or less. Although there is no problem if there is no particular limit on the P content, since the inclusion of P is usually unavoidable, unnecessary reduction in P content may increase the refining time and the refining cost. Therefore, it is reasonable and preferable to set the P content to 0.003 mass% or more.

[0038] The S content is 0.5% by mass or less. S exists as sulfide-based inclusions and is an element effective in improving machinability. Excessive S inclusion in steel may lead to a decrease in cold workability. There is no particular limit to the S content, but since the inclusion of S is usually unavoidable, excessive reduction in S content may increase refining costs. Therefore, it is reasonable to set the S content to 0.003% by mass or more. The S content is preferably 0.004% by mass or more and 0.3% by mass or less, and more preferably 0.005% by mass or more and 0.09% by mass or less.

[0039] The Al content is 0.010% by mass or more and 0.300% by mass or less. Al forms oxides and is an element effective in deoxidizing nitrided steel. Furthermore, Al has the effect of suppressing the formation of coarse oxide-based inclusions in nitrided steel. If the Al content is less than 0.010% by mass, these effects may not be obtained. Excessive Al inclusion in steel may lead to an increase in inclusions (Al oxides), which may increase the starting points of fatigue fracture and cause low fatigue strength.

[0040] The N content is 0.0250% by mass or less. N combines with Al to form nitride (AlN). Finely precipitated AlN has the effect of increasing the hardness of steel after nitriding (nitrided steel). Excessive N inclusion in steel may lead to surface cracking of the steel billet after casting. There is no particular limit to the N content, but since the inclusion of N is usually unavoidable, excessive reduction in N content may increase refining costs. The N content is 0.0010% by mass or more, preferably 0.0015% by mass or more. The N content is preferably 0.0180% by mass or less, more preferably 0.0020% by mass or more and 0.0150% by mass or less.

[0041] The optional components of the steel will be described below.

[0042] The Cr content may be 2.0 mass% or less. Cr contributes to improving hardenability and temper softening resistance, and is also a useful element for promoting spheroidization of carbides. If the Cr content exceeds 2.0 mass%, the Cr nitride layer formed on the surface after soft nitriding becomes thick, which may hinder the penetration of N into the inside and lead to insufficient hardness. The Cr content is preferably 0.40 mass% or more and 1.90 mass% or less, and more preferably 0.70 mass% or more and 1.75 mass% or less.

[0043] The Mo content may be 1.0 mass% or less. Mo improves hardenability and strengthens the pre-nitriding structure, thereby strengthening the post-nitriding structure. However, if the Mo content is 1.0 mass% or more, the hardenability becomes excessive, the hardness after rolling increases, and the workability and machinability may decrease. In order to realize the effect of Mo in improving the strength of the steel material, it is preferable to contain Mo in an amount of 0.01 mass% or more in the steel. The Mo content is more preferably 0.03 mass% or more and 0.50 mass% or less, and further preferably 0.05 mass% or more and 0.25 mass% or less.

[0044] The Cu content may be 1.0 mass% or less. Cu improves hardenability and strengthens the pre-nitriding structure, thereby strengthening the post-nitriding structure. In order to obtain this effect, it is preferable to contain Cu in an amount of 0.01 mass% or more in the steel. If the Cu content exceeds 1.0 mass%, the surface of the rolled material may become rough, and there is a concern that these may remain as defects. The Cu content is more preferably 0.015 mass% or more and 0.5 mass% or less, and even more preferably 0.03 mass% or more and 0.3 mass% or less.

[0045] The Ni content may be 1.0 mass% or less. Ni is an element useful for improving toughness. In order to obtain these effects, it is preferable to contain Ni in an amount of 0.01 mass% or more in the steel. Even if the Ni content in the steel exceeds 1 mass%, the above effects are saturated. The Ni content is more preferably 0.015 mass% or more and 0.5 mass% or less, and further preferably 0.03 mass% or more and 0.3 mass% or less.

[0046] The content of B may be 0.01% by mass or less. B segregates at grain boundaries and inhibits diffusion-type transformation, which is effective in improving hardenability, and also has the effect of strengthening grain boundaries, inhibiting the occurrence and progression of fatigue cracks, and improving fatigue strength. In order to obtain this effect of B, it is preferable to contain B in steel at 0.0003% by mass or more. If the content of B exceeds 0.01% by mass, the toughness of the steel decreases, so the content of B is preferably 0.01% by mass or less. The content of B is more preferably 0.0005% by mass or more and 0.005% by mass or less, and even more preferably 0.0007% by mass or more and 0.002% by mass or less.

[0047] The Ti content may be 0.1 mass% or less. Ti improves the strength of the steel by combining with carbon and nitrogen to form fine precipitates during soft nitriding. However, even if the Ti content in the steel exceeds 0.1 mass%, the effect is saturated. The Ti content is preferably 0.005 mass% or more and 0.08 mass% or less, and more preferably 0.01 mass% or more and 0.06 mass% or less.

[0048] The Nb content may be 0.1 mass% or less. Nb improves the strength of the steel by combining with carbon and nitrogen to form fine precipitates during soft nitriding. However, even if the Nb content in the steel exceeds 0.1 mass%, the effect is saturated. The Nb content is preferably 0.005 mass% or more and 0.08 mass% or less, and more preferably 0.01 mass% or more and 0.06 mass% or less.

[0049] The V content may be 0.2 mass% or less. V combines with carbon and nitrogen to form fine precipitates during soft nitriding, thereby improving the strength of the steel. In order to obtain this effect of V, it is preferable to contain at least 0.003 mass% or more of V in the steel. If the V content in the steel exceeds 0.2 mass%, the alloy cost will increase and the effect will saturate. The V content is more preferably 0.005 mass% or more and 0.15 mass% or less, and further preferably 0.01 mass% or more and 0.10 mass% or less.

[0050] The Hf content may be 0.1 mass% or less. Hf improves the strength of steel by combining with carbon and nitrogen and forming fine precipitates during soft nitriding. In order to obtain this effect of Hf, it is preferable to contain at least 0.003 mass% or more of Hf in the steel. If the Hf content in the steel exceeds 0.1 mass%, coarse precipitates may be generated during casting and solidification, which may lead to deterioration of fatigue strength. The Hf content is more preferably 0.005 mass% or more and 0.06 mass% or less, and even more preferably 0.01 mass% or more and 0.05 mass% or less.

[0051] The Ta content may be 0.1% by mass or less. Ta improves the strength of steel by combining with carbon and nitrogen to form fine precipitates during soft nitriding. In order to obtain this effect of Ta, it is preferable to contain Ta in steel at least 0.003% by mass or more. On the other hand, if the Ta content exceeds 0.1% by mass, cracks are likely to occur during casting and solidification, and defects may remain even after rolling and forging. The Ta content is more preferably 0.005% by mass or more and 0.06% by mass or less, and even more preferably 0.01% by mass or more and 0.05% by mass or less.

[0052] The Sn content may be 0.1 mass% or less. Sn is an element effective for improving the corrosion resistance of the steel surface. From the viewpoint of improving the corrosion resistance, it is preferable that the steel contains 0.003 mass% or more of Sn. If the steel contains an excessive amount of Sn, the workability decreases. The Sn content is more preferably 0.0010 mass% or more and 0.050 mass% or less, and further preferably 0.0015 mass% or more and 0.035 mass% or less.

[0053] The Sb content may be 0.1 mass% or less. Sb is an element effective in suppressing decarburization of the steel surface and preventing a decrease in surface hardness. In order to realize this effect, it is preferable to contain Sb in the steel at 0.0003 mass% or more. If an excessive amount of Sb is contained in the steel, the workability of the steel decreases. The Sb content is more preferably 0.001 mass% or more and 0.05 mass% or less, and further preferably 0.0015 mass% or more and 0.035 mass% or less.

[0054] The Se content may be 0.3 mass% or less. Se improves machinability by combining with Mn and Cu and dispersing as precipitates in the steel. To obtain this effect, it is preferable to contain at least 0.001 mass% Se in the steel. Even if the Se content in the steel exceeds 0.3 mass%, the effect is saturated. The Se content is more preferably 0.005 mass% to 0.1 mass%, and further preferably 0.008 mass% to 0.09 mass%.

[0055] The Ca content may be 0.1% by mass or less. Ca improves machinability by combining with S and dispersing in the steel as sulfides. To obtain this effect, it is preferable to contain at least 0.0005% by mass of Ca in the steel. If the Ca content in the steel exceeds 0.1% by mass, the effect is saturated. The Ca content is more preferably 0.0010% by mass or more and 0.0500% by mass or less, and further preferably 0.0015% by mass or more and 0.0300% by mass or less.

[0056] The Pb content may be 0.3% by mass or less. Pb has the effect of refining chips during cutting. Addition of Pb is effective when it is desired to improve chip disposability. To obtain this effect, it is preferable to contain 0.01% by mass or more of Pb in the steel. Even if excessive Pb is contained in the steel, the effect of improving chip disposability becomes saturated. The Pb content is preferably 0.01% by mass or more and 0.2% by mass or less, and more preferably 0.01% by mass or more and 0.1% by mass or less.

[0057] The Bi content may be 0.3 mass% or less. Bi has the effect of refining chips during cutting. Addition of Bi is effective when it is desired to improve chip disposability. To obtain this effect, it is preferable to contain Bi at 0.01 mass% or more. Even if an excessive amount of Bi is contained in the steel, the effect of improving chip disposability becomes saturated. The Bi content is preferably 0.01 mass% or more and 0.2 mass% or less, and more preferably 0.01 mass% or more and 0.1 mass% or less.

[0058] The balance other than the above-described elements is Fe and impurities. The impurities are substances that are mixed in from raw materials such as ore and scrap, or from the manufacturing environment during industrial production of steel material, and are allowed within a range that does not adversely affect the characteristics of this embodiment.

[0059] When steel is cold worked, crystal orientation rotation occurs according to the working style. As the amount of working increases, the crystal orientation rotation becomes more pronounced, and the accumulation of crystal orientations progresses. The inverse pole figure intensity distribution obtained by EBSD (electron backscatter diffraction) is a representative index showing the degree of accumulation of crystal orientations. When the maximum value of strength in the inverse pole figure intensity distribution is 1.5 or more, the fatigue strength of the steel is improved. To sufficiently improve the fatigue strength of steel, the maximum value of strength in the inverse pole figure intensity distribution is preferably 1.7 or more, and more preferably 2.0 or more.

[0060] In the soft nitrided component according to this embodiment, the maximum strength value in the inverse pole figure intensity distribution measured in a direction parallel to the component surface at a depth of 0.5 mm from the surface of the body is 1.5 or more. EXAMPLES

[0061] Hereinafter, the soft-nitrided component according to the present embodiment will be described based on an example. Note that the soft-nitrided component according to the present embodiment is not limited to this example.

[0062] First, steels (steels No. 1 to 31) having the composition shown in Table 1 were melted and formed into round bars having a diameter of 20 mm by hot rolling. Among the values ​​of the composition shown in Table 1, the underlined values ​​are outside the range specified in this embodiment.

[0063] This round bar was then subjected to cold tensile processing (an example of cold processing) to produce a round bar with a diameter of 16 mm, after which an Ono-type rotating bending fatigue test specimen (hereinafter simply referred to as the test specimen) with a diameter of 12 mm at the gripping portion and 10 mm at the parallel portion was cut from the center.

[0064] FIG. 1 shows a schematic diagram of the shape of the test piece of this embodiment. The test piece is a straight rod along the axis G, and the cross section perpendicular to the axis G is a circular rod whose center overlaps with the axis G. Both ends of the rod in the direction along the axis G of the test piece are gripping parts 1,1 described later. A parallel part 2 is disposed between the gripping parts 1,1 in the direction along the axis G. In the test piece shown in FIG. 1, the diameter of the center of the parallel part 2 in the axial direction is 10 mm. The diameter of the gripping parts 1,1 is 12 mm. The length of the gripping part 1 in the direction along the axis G is 25 mm. The length between the gripping parts 1,1 including the parallel part 2 is 30 mm. Both ends of the parallel part 2 in the direction along the axis G are curved with R15 from the end of the gripping part 1 to the center in the axial direction.

[0065] [Table 1]

[0066] Next, this test piece was subjected to a gas soft-nitriding heat treatment (nitriding) at 570°C for 3 hours to obtain a post-treatment test piece (an example of a soft-nitrided part). The nitriding treatment was carried out in a mixed gas containing ammonia and carbon monoxide.

[0067] Furthermore, the treated specimen was measured by EBSD to obtain the inverse pole figure strength distribution and the maximum strength value. The inverse pole figure strength distribution was obtained for the part 0.5 mm deep from the surface of the gripped part of the treated specimen.

[0068] Measurements of the portion 0.5 mm deep from the surface of the gripping portion of the treated test piece were taken at a position 0.5 mm deep from the surface after the cross section perpendicular to the axis G at the centre of the length of the gripping portion (the centre in the direction along the axis G) was mirror polished.

[0069] The calculation of the inverse pole figure intensity distribution based on the measurement results by the EBSD method was performed using the crystal orientation analysis software OIM manufactured by TSL, Inc. For the measurement by the EBSD method, a scanning electron microscope (manufactured by JEOL Ltd., model: JSM-7001F) was used.

[0070] The measurement field of view for the EBSD method was a square region with one side measuring 0.5 mm, and the inverse pole figure intensity distribution was analyzed in the direction parallel to the gripping surface using the spherical harmonics method under the conditions of Series Rank: 13, Gaussian Smoothing: 5.0°, and Sample Symmetry: Triclinic.

[0071] Next, for the treated test pieces of each component composition, the treated test pieces were separated into those with a maximum strength value of 1.5 or more in the inverse pole figure strength distribution and those without. Then, the treated test pieces with a maximum strength value of 1.5 or more in the pole figure strength distribution and those without were subjected to a rotating bending fatigue test, and the fatigue limits (1×10 7 The equivalent stress (stress) was evaluated.

[0072] In this rotating bending fatigue test, if the fatigue limit is 780 MPa or more, it may be evaluated that the fatigue properties are excellent. As shown in Table 1, the test piece (nitrogen-nitrided part) after the treatment according to this embodiment has excellent fatigue properties. Among the fatigue limit values ​​shown in Table 1, the underlined values ​​are less than 780 MPa.

[0073] It is also clear that the test pieces (nitrocarburized parts) treated according to this embodiment have significantly better bending fatigue properties than those not treated according to this embodiment.

[0074] Thus, the steel forming the test piece (main body of the soft-nitrided part) after treatment according to this embodiment has excellent fatigue properties, despite being low cost and not requiring the inclusion of large amounts of relatively expensive metals such as Cu.

[0075] Moreover, the steel forming the post-treatment test piece (main body of the soft-nitrided part) according to this embodiment does not require the addition of a rare metal such as V, is low cost, and yet has excellent fatigue properties.

[0076] In this manner, a soft nitrided part having excellent bending fatigue properties can be provided at low cost.

[0077] It should be noted that the embodiments disclosed in this specification are merely examples, and the present invention is not limited to these embodiments, and can be modified as appropriate without departing from the scope of the present invention. [Industrial Applicability]

[0078] The present invention is applicable to soft-nitrided parts. [Explanation of symbols]

[0079] 1: Grip part 2: Parallel section G: Axial center

Claims

1. The composition of the ingredients is as follows: C: 0.04% by mass or more and 0.35% by mass or less, Si: 0.01% by mass or more and 1.20% by mass or less, Mn: 0.30% by mass or more and 1.80% by mass or less, P: 0.1% by mass or less, S: 0.5% by mass or less, Al: 0.010 mass% or more and 0.300 mass% or less; N: 0.0250 mass% or less, The balance includes a main body formed of steel containing Fe and impurities, The body has a nitrided surface layer; A soft nitrided part having a maximum strength value of 1.5 or more in an inverse pole figure intensity distribution measured at a depth of 0.5 mm from the surface of the body in a direction parallel to the surface.

2. The steel has the following composition: Cr: 2.0% by mass or less, Mo: 1.0% by mass or less, Cu: 1.0% by mass or less, Ni: 1.0 mass% or less; B: 0.01% by mass or less, The nitrocarburized component according to claim 1 , further comprising one or more of the following:

3. The steel has the following composition: Ti: 0.1% by mass or less, Nb: 0.1% by mass or less, V: 0.2% by mass or less, Hf: 0.1% by mass or less and Ta: 0.1% by mass or less, The nitrocarburized component according to claim 1 , further comprising one or more of the following:

4. The steel has the following composition: Ti: 0.1% by mass or less, Nb: 0.1% by mass or less, V: 0.2% by mass or less, Hf: 0.1% by mass or less and Ta: 0.1% by mass or less, The nitrocarburized component according to claim 2 , further comprising one or more selected from the group consisting of:

5. The steel has the following composition: Sn: 0.1 mass% or less; and Sb: 0.1% by mass or less, The soft nitrided part according to any one of claims 1 to 4, further comprising one or more selected from the following:

6. The steel has the following composition: Se: 0.3% by mass or less, Ca: 0.1% by mass or less, Pb: 0.3% by mass or less and Bi: 0.3% by mass or less, The soft nitrided part according to any one of claims 1 to 4, further comprising one or more selected from the following:

7. The steel has the following composition: Se: 0.3% by mass or less, Ca: 0.1% by mass or less, Pb: 0.3% by mass or less and Bi: 0.3% by mass or less, The nitrocarburized component according to claim 5 , further comprising one or more selected from the following:

Citation Information

Patent Citations

  • Steel for machine structure, method for producing the same and method for producing worked component using steel for machine structure

    JP2011236449A

  • Steel for cold forging / nitriding, steel material for cold forging / nitriding and cold-forged / nitrided component

    JP2012087361A

  • Cold forging and nitriding steel, cold forging and nitriding steel material, and cold forged and nitrided component

    JP2013185186A

  • Steel sheet for gas soft nitriding

    WO2022176984A1

  • Soft-nitriding steel for structural purpose

    JP1997227992A