Bio-electrode composition, bio-electrode, and method for manufacturing bio-electrode
The bioelectrode composition with a urethane bond and sulfonamide salts addresses conductivity and biocompatibility issues, enabling stable, long-term health monitoring by maintaining conductivity and adhesion, suitable for wearable medical devices.
Patent Information
- Application Number
- JP2024028068
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-23
- Filing Date
- 2024-02-28
- Publication Date
- 2024-10-07
AI Technical Summary
Existing bioelectrodes used in wearable medical devices face challenges with conductivity loss due to drying, skin allergies from certain materials, and the trade-off between biocompatibility and conductivity, making them unsuitable for long-term, continuous health monitoring.
A bioelectrode composition with a urethane bond in the main chain and ammonium, sodium, or potassium sulfonamide salts in the side chain, combined with resins and conductive materials like carbon nanotubes and metal powders, to create a soft, stretchable, and adhesive biocontact layer.
The bioelectrode maintains conductivity and biocompatibility, is lightweight, and can be manufactured at low cost, ensuring stable signal collection even when wet or dry, without significant conductivity loss.
Smart Images

Figure 2024137755000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a bioelectrode composition, a bioelectrode, and a method for producing a bioelectrode. [Background technology]
[0002] In recent years, the development of wearable devices has progressed with the spread of IoT (Internet of Things). Typical examples are watches and glasses that can connect to the Internet. In addition, wearable devices that can constantly monitor the condition of the body are needed in the medical and sports fields, and these are expected to be growth fields in the future.
[0003] In the medical field, wearable devices that monitor the state of the body's organs by sensing weak currents, such as in electrocardiograms, which detect the movement of the heart through electrical signals, are being considered. In electrocardiograms, electrodes coated with a water-soluble gel conductive paste are attached to the body to perform the measurement, but this is a one-time, short-term measurement. In contrast, the development of medical wearable devices such as those mentioned above aims to develop devices that constantly monitor the health state for several weeks. Therefore, the bioelectrodes used in medical wearable devices are required to have no change in conductivity even when used for long periods of time and to be free of skin allergies. In addition to these, they are also required to be lightweight and to be able to be manufactured at low cost.
[0004] Wearable medical devices include those that are attached to the body and those that are incorporated into clothing. As a type that is attached to the body, a bioelectrode that uses a water-soluble gel containing water and electrolytes, which are the materials for the conductive paste mentioned above, has been proposed (Patent Document 1). The water-soluble gel contains sodium, potassium, and calcium as electrolytes in a water-soluble polymer that holds water, and converts changes in ion concentration from the skin into electricity. On the other hand, as a type that is incorporated into clothing, a method has been proposed in which a conductive polymer such as PEDOT-PSS (Poly-3,4-ethylenedioxythiophene-Polystyrenesulfonate) or cloth with silver paste incorporated into the fibers is used as an electrode (Patent Document 2).
[0005] However, when using the above-mentioned water-soluble gel containing water and electrolytes, there is the problem that the conductivity is lost when the water evaporates due to drying. When using metals with a high tendency to ionize, such as copper, there is the problem that there is a risk of causing skin allergies in some people. Even when using conductive polymers such as PEDOT-PSS, there is the problem that there is a risk of causing skin allergies due to the strong acidity of the conductive polymer, and there is the problem that the conductive polymer peels off from the fibers during washing.
[0006] In addition, because of their excellent electrical conductivity, the use of metal nanowires, carbon black, carbon nanotubes, and the like as electrode materials has also been considered (Patent Documents 3, 4, 5). Metal nanowires have a high probability of contact between wires, so they can conduct electricity with a small amount of additive. However, metal nanowires are thin materials with sharp tips, which can cause skin allergies. Thus, even if the material itself does not cause an allergic reaction, the shape and irritation of the material can cause the material to have poor biocompatibility, making it difficult to achieve both electrical conductivity and biocompatibility.
[0007] Wristwatches sold by Apple Inc. can obtain dielectric biosignals by touching the metal on the skin side of the watch, which is always in contact with the skin, and a metal button called the digital crown with the fingers of the hand not wearing the watch (Patent Document 6).
[0008] Metals are highly conductive, so one would think they would function as excellent bioelectrodes, but this is not necessarily the case. When the heart beats, not only a weak current is released from the skin, but also sodium ions, potassium ions, and calcium ions. For this reason, it is necessary to convert the change in ion concentration into an electric current, but precious metals, which are difficult to ionize, are inefficient at converting ions from the skin into an electric current. Therefore, bioelectrodes using precious metals have a high impedance, and there is a high resistance to electrical current passing through the skin. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] International Publication No. 2013 / 039151 [Patent Document 2] JP 2015-100673 A [Patent Document 3] Japanese Patent Application Publication No. 05-095924 [Patent Document 4] JP 2003-225217 A [Patent Document 5] JP 2015-019806 A [Patent Document 6] Patent Publication No. 2021-093127 Summary of the Invention [Problem to be solved by the invention]
[0010] The present invention has been made to solve the above problems, and aims to provide a bioelectrode composition that is excellent in electrical conductivity and biocompatibility, lightweight, can be manufactured at low cost, does not significantly decrease in electrical conductivity whether wetted with water or dried, and can form a biocontact layer for a bioelectrode that is soft, stretchable, and strong; a bioelectrode in which a biocontact layer is formed from the bioelectrode composition; and a method for manufacturing the same. [Means for solving the problem]
[0011] In order to solve the above problems, the present invention provides a bioelectrode composition, which contains, as component (A), a resin having a urethane bond in its main chain and one or more salts selected from ammonium salts, sodium salts, potassium salts, and silver salts of sulfonamide in its side chains.
[0012] Such a bioelectrode composition has excellent electrical conductivity and biocompatibility, is lightweight, and can be produced at low cost. Its electrical conductivity does not decrease significantly whether it is wetted with water or dried, and it is a bioelectrode composition that can form a biocontact layer for a bioelectrode that is soft, stretchable, and strong.
[0013] In the present invention, the component (A) is preferably represented by the following general formula (1). [ka] (In general formula (1), R 1 , R 3 R is a single bond or a linear or branched alkylene group having 1 to 6 carbon atoms, which may have an ether bond or a bromine atom. 2 R is a hydrogen atom, a hydroxyl group, a linear or branched alkyl group having 1 to 6 carbon atoms, or an alkoxy group. 4 represents a single bond or a linear, branched or cyclic hydrocarbylene group having 1 to 20 carbon atoms, which may have a carbonyl group, an ether group or an ester group; R 1 R may be bonded to form a ring. 5is a linear, branched, or cyclic alkyl group having 1 to 10 carbon atoms, which may be substituted with a fluorine atom, or an alkenyl group having 2 to 6 carbon atoms, an alkynyl group having 2 to 6 carbon atoms, or an aryl group having 6 to 10 carbon atoms, which may have a fluorine atom, a trifluoromethyl group, a cyano group, a nitro group, a hydroxy group, an alkoxy group having 1 to 6 carbon atoms, or an alkyl group having 1 to 6 carbon atoms. M + is an ammonium ion, a sodium ion, a potassium ion, or a silver ion.
[0014] Such component (A) can provide a bioelectrode composition capable of forming a biocontact layer for a bioelectrode having superior electrical conductivity and biocompatibility.
[0015] In the present invention, the component (A) preferably contains, as the ammonium ion constituting the ammonium salt, an ammonium ion represented by the following general formula (2). [ka] (In general formula (2), R 101d , R 101e , R 101f , and R 101g R is a hydrogen atom, a linear, branched, or cyclic alkyl group having 1 to 15 carbon atoms, a linear, branched, or cyclic alkenyl or alkynyl group having 2 to 12 carbon atoms, or an aromatic group having 4 to 20 carbon atoms, and may have one or more groups selected from an ether group, a carbonyl group, an ester group, a hydroxy group, an amino group, a nitro group, a sulfonyl group, a sulfinyl group, a halogen atom, and a sulfur atom. 101d and R 101e , or R 101d , R 101e and R 101f may form a ring together with the nitrogen atom to which they are attached, and when they form a ring, R 101d and R 101e , or R 101d , R 101e and R 101fis an alkylene group having 3 to 10 carbon atoms, or forms a heteroaromatic ring having the nitrogen atom in the general formula (2) in the ring.
[0016] If the component (A) containing such ammonium ions is included, it is possible to obtain a bioelectrode composition capable of forming a biocontact layer for a bioelectrode having even better electrical conductivity and biocompatibility.
[0017] In the present invention, it is preferable that the bioelectrode composition further contains, as component (B), a resin other than the component (A).
[0018] By including such a component (B), it is possible to prevent the elution of salt due to compatibility with the component (A) and improve adhesion.
[0019] In this case, the component (B) is preferably at least one selected from a silicone resin, a (meth)acrylate resin, and a urethane resin.
[0020] Such a component (B) can further improve the adhesiveness.
[0021] In the present invention, it is preferable that the bioelectrode composition further contains, as component (C), either or both of a carbon material and a metal powder.
[0022] By including such a component (C), electronic conductivity can be increased.
[0023] In this case, the carbon material is preferably either or both of carbon black and carbon nanotubes.
[0024] By including such a carbon material, higher electrical conductivity can be provided.
[0025] In the present invention, the metal powder is preferably a metal powder selected from the group consisting of gold, silver, platinum, copper, tin, titanium, nickel, aluminum, tungsten, molybdenum, ruthenium, chromium, and indium.
[0026] Such metals can be used as the metal powder.
[0027] In this case, the metal powder is preferably silver powder.
[0028] Silver powder is generally preferred from the standpoints of electrical conductivity, cost, and biocompatibility.
[0029] In the present invention, it is preferable that the bioelectrode composition further contains an organic solvent as component (D).
[0030] By including such a component (D), high coatability can be exhibited.
[0031] The present invention also provides a bioelectrode having a conductive substrate and a biocontact layer formed on the conductive substrate, the bioelectrode being a cured product of the bioelectrode composition described above.
[0032] Such a bioelectrode has excellent electrical conductivity and biocompatibility, is lightweight, and can be manufactured at low cost. Its electrical conductivity does not decrease significantly whether it is wet or dried, and it is a soft bioelectrode with excellent elasticity and strength.
[0033] In this case, it is preferable that the conductive substrate contains one or more selected from gold, silver, silver chloride, platinum, aluminum, magnesium, tin, tungsten, iron, copper, nickel, stainless steel, chromium, titanium, carbon, and a conductive polymer.
[0034] As the conductive substrate, such a conductive substrate can be used.
[0035] The present invention also provides a method for manufacturing a bioelectrode having a conductive substrate and a biocontact layer formed on the conductive substrate, in which the bioelectrode composition described above is applied to the conductive substrate and cured to form the biocontact layer.
[0036] This method of manufacturing a bioelectrode makes it possible to easily manufacture a bioelectrode that is excellent in conductivity and biocompatibility, lightweight, and can be manufactured at low cost, and that does not significantly decrease in conductivity whether wet or dry, and that is soft, stretchable, and strong.
[0037] In this case, it is preferable to use, as the conductive substrate, one or more selected from gold, silver, silver chloride, platinum, aluminum, magnesium, tin, tungsten, iron, copper, nickel, stainless steel, chromium, titanium, carbon, and conductive polymers.
[0038] As the conductive substrate, such a conductive substrate can be used. Effect of the Invention
[0039] As described above, the bioelectrode composition, bioelectrode, and manufacturing method thereof of the present invention can provide a bioelectrode composition that is excellent in electrical conductivity and biocompatibility, lightweight, and can be manufactured at low cost, and that does not significantly decrease in electrical conductivity whether wetted with water or dried, and can form a biocontact layer for a bioelectrode that is soft, stretchable, and strong; a bioelectrode in which a biocontact layer is formed from the bioelectrode composition; and a manufacturing method thereof. [Brief description of the drawings]
[0040] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of a bioelectrode of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing an example of the bioelectrode of the present invention attached to a living body. [Diagram 3] FIG. 2 is a schematic diagram of a bioelectrode produced in an example of the present invention after printing. [Figure 4]FIG. 2 is a schematic diagram of one of the bioelectrodes produced in the examples of the present invention, cut out and with an adhesive layer and an electric wire attached. [Diagram 5] FIG. 2 is a diagram showing the locations where electrodes and a ground are attached to the human body when measuring a biosignal in an embodiment of the present invention. [Figure 6] 1 is an electrocardiogram waveform obtained using a bioelectrode according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0041] As described above, there has been a demand for the development of a bioelectrode composition capable of forming a biocontact layer for a bioelectrode that is excellent in electrical conductivity and biocompatibility, lightweight, can be produced at low cost, is soft, stretchable, and strong, and can be in contact with the skin for a long period of time and can stably collect biosignals even when wetted with water such as during bathing or dried; a bioelectrode in which a biocontact layer is formed from the bioelectrode composition; and a method for producing the same.
[0042] Sodium, potassium, and calcium ions are released from the skin surface in tandem with the heartbeat. Bioelectrodes need to convert the increase or decrease in the ions released from the skin into an electrical signal. To do this, materials with excellent ionic conductivity are required to transmit the increase or decrease in ions.
[0043] As mentioned above, the electrodes of wristwatch-type vital signs monitors use metal. Metal not only has low sensitivity to vital signs, but there are a certain number of people who have allergic reactions to it. If the rubber band of a wristwatch could function as a vital electrode, the problem of metal allergies would be solved. However, rubber bands are generally insulating and do not function as a vital electrode.
[0044] The bioelectrodes in the rubber band of the watch must have high strength to prevent them from falling off or cracking due to friction with the skin, and they also need to have high adhesive strength with the metal wiring inside the rubber band and flexibility.
[0045] On the other hand, bioelectrodes that are attached to the body require high adhesiveness in order to be attached for long periods of time and to be able to follow the movements of those involved in sports.
[0046] Polyurethane is an example of a material with high strength, high elasticity, and high adhesion. Since polyurethane is insulating, it is possible to add additives to it to develop ionic or electronic conductivity. To improve ionic conductivity, it is possible to add neutralizing salts.
[0047] When the acidity of the acid that forms the neutralized salt is high, the ions are strongly polarized, improving ionic conductivity. This is why lithium salts of bis(trifluoromethanesulfonyl)imide acid and tris(trifluoromethanesulfonyl)methide acid show high ionic conductivity in lithium-ion batteries. On the other hand, the higher the acid strength of the acid before it becomes a neutralized salt, the stronger the bioirritation of the salt. In other words, there is a trade-off between ionic conductivity and bioirritation. However, salts to be applied to bioelectrodes must have both high ionic conductivity and low bioirritation.
[0048] The larger the molecular weight of an ionic compound, the less permeable it is to the skin, and the less irritating it is to the skin. For this reason, it is preferable for the ionic compound to be a high molecular weight polymer. Therefore, the present inventors have avoided the problem of irritating the skin by introducing this ionic compound into polyurethane.
[0049] That is, the present invention is a bioelectrode composition that contains, as component (A), a resin having a urethane bond in its main chain and one or more salts selected from ammonium salts, sodium salts, potassium salts, and silver salts of sulfonamide in its side chains.
[0050] The present invention will be described in detail below, but the present invention is not limited thereto.
[0051] <Bioelectrode composition> The bioelectrode composition of the present invention contains, as component (A), a resin having a urethane bond in the main chain and one or more salts selected from ammonium salts, sodium salts, potassium salts, and silver salts of sulfonamide in the side chain. Each component will be described in more detail below.
[0052] [(A) A resin having a urethane bond in its main chain and one or more salts selected from ammonium salts, sodium salts, potassium salts, and silver salts of sulfonamide in its side chain] The bioelectrode composition of the present invention contains, as component (A), a resin having a urethane bond in its main chain and one or more salts selected from ammonium salts, sodium salts, potassium salts, and silver salts of sulfonamide in its side chains.
[0053] The component (A) is preferably represented by the following general formula (1). [ka] (In general formula (1), R 1 , R 3 R is a single bond or a linear or branched alkylene group having 1 to 6 carbon atoms, which may have an ether bond or a bromine atom. 2 R is a hydrogen atom, a hydroxyl group, a linear or branched alkyl group having 1 to 6 carbon atoms, or an alkoxy group. 4 represents a single bond or a linear, branched or cyclic hydrocarbylene group having 1 to 20 carbon atoms, which may have a carbonyl group, an ether group or an ester group; R 1 R may be bonded to form a ring. 5 is a linear, branched, or cyclic alkyl group having 1 to 10 carbon atoms, which may be substituted with a fluorine atom, or an alkenyl group having 2 to 6 carbon atoms, an alkynyl group having 2 to 6 carbon atoms, or an aryl group having 6 to 10 carbon atoms, which may have a fluorine atom, a trifluoromethyl group, a cyano group, a nitro group, a hydroxy group, an alkoxy group having 1 to 6 carbon atoms, or an alkyl group having 1 to 6 carbon atoms. M +is an ammonium ion, a sodium ion, a potassium ion, or a silver ion.
[0054] The repeating unit represented by general formula (1) can be obtained by reacting a monomer having a dihydroxy group represented by the following general formula (1)-1 with a compound having an isocyanate group. [ka] (In general formula (1)-1, R 1 ~R 5 , M + is as mentioned above.)
[0055] Specific examples of the monomer having a dihydroxy group represented by the general formula (1)-1 include the following.
[0056] [ka]
[0057] [ka]
[0058] [ka]
[0059] [ka]
[0060] [ka]
[0061] [ka]
[0062]
change
[0063]
change
[0064]
change
[0065]
change
[0066]
change
[0067]
change
[0068]
change
[0069]
change
[0070]
change
[0071]
change
[0072]
change
[0073] As a method for synthesizing the above dihydroxy group-containing n-carbonylsulfonamide salt, an acid chloride is synthesized from a carboxylic acid compound described in paragraph
[0176] of JP 2022-078861 A, and this is reacted with a sulfonamide described in paragraph
[0132] of JP 2019-011454 A, which can be obtained.
[0074] The dihydroxy group-containing sulfonamide salt can be synthesized by synthesizing sulfonamide by the method described in paragraph
[0177] of JP 2022-078861 A, and then neutralizing or ion exchanging it with ammonium hydroxide, ammonium chloride, sodium hydroxide, sodium chloride, potassium hydroxide, potassium chloride, silver hydroxide, silver chloride, silver nitrate, etc.
[0075] The component (A) preferably contains, as the ammonium ion constituting the ammonium salt, an ammonium ion represented by the following general formula (2). [ka] (In general formula (2), R 101d , R 101e , R 101f , and R 101g R is a hydrogen atom, a linear, branched, or cyclic alkyl group having 1 to 15 carbon atoms, a linear, branched, or cyclic alkenyl or alkynyl group having 2 to 12 carbon atoms, or an aromatic group having 4 to 20 carbon atoms, and may have one or more groups selected from an ether group, a carbonyl group, an ester group, a hydroxy group, an amino group, a nitro group, a sulfonyl group, a sulfinyl group, a halogen atom, and a sulfur atom. 101d and R 101e , or R 101d , R 101e and R 101f may form a ring together with the nitrogen atom to which they are attached, and when they form a ring, R 101d and R 101e , or R 101d , R 101e and R101f is an alkylene group having 3 to 10 carbon atoms, or forms a heteroaromatic ring having the nitrogen atom in the general formula (2) in the ring.
[0076] Specific examples of the ammonium ion represented by the above general formula (2) include the following.
[0077] [ka]
[0078] [ka]
[0079] [ka]
[0080] [ka]
[0081] [ka]
[0082] [ka]
[0083] [ka]
[0084] [ka]
[0085] [ka]
[0086] [ka]
[0087] [ka]
[0088] [ka]
[0089] [ka]
[0090] [ka]
[0091] [ka]
[0092] [ka]
[0093] As the ammonium ion represented by the above general formula (2), a tertiary or quaternary ammonium ion is particularly preferred.
[0094] The repeating unit represented by the above general formula (1) can be obtained by reacting a monomer having a dihydroxy group represented by the above general formula (1)-1 with a compound having an isocyanate group. Examples of the compound having an isocyanate group include the following.
[0095] [ka]
[0096] [ka] (In the formula, t is an integer of 1 or more.)
[0097] The repeating unit represented by the above general formula (1) can be obtained by reacting a monomer having a dihydroxy group represented by the above general formula (1)-1 with a compound having an isocyanate group, but it may also be reacted with a compound having a hydroxy group other than the above general formula (1)-1.
[0098] Examples of compounds having a hydroxy group other than those of the above general formula (1)-1 include compounds having a polyol terminal, as exemplified below.
[0099] [ka]
[0100] [ka] Here, the brackets are the repeating units.
[0101] [ka]
[0102] Examples of the diol compound obtained from a polyester compound having a copolymerizable terminal diol as a raw material include those shown below.
[0103] [ka]
[0104] [ka]
[0105] [ka] Here, the brackets are the repeating units.
[0106] It can also be copolymerized with the following polycarbonate compound having a diol terminal.
[0107] [ka] Here, the brackets are the repeating units.
[0108] Furthermore, it can also be copolymerized with the following diol compounds having a fluoroalkyl group or a fluoroalkylene group.
[0109] [ka] Here, m and n are in the range of 0 to 20.
[0110] [ka] Here, m ranges from 1 to 20.
[0111] [ka] Here, n and q are in the ranges of 1 to 20, 2≦n+q≦21, and 1≦p≦40.
[0112] [ka] Here, n and q are in the ranges of 1 to 20, 2≦n+q≦21, and 1≦p≦40.
[0113] [ka] Here, n and q are in the ranges of 1 to 20, 2≦n+q≦21, and 1≦p≦40.
[0114] [ka] Here, n and q are in the ranges of 1 to 20, 2≦n+q≦21, and 1≦p≦40.
[0115] [ka] Here, n and q are in the ranges of 1 to 20, 2≦n+q≦21, and 1≦p≦40.
[0116] [ka] Here, n and q are in the ranges of 1 to 20, 2≦n+q≦21, and 1≦p≦40.
[0117] [ka] Here, m ranges from 1 to 20.
[0118] [ka] Here, m ranges from 1 to 20.
[0119] [ka] Here, m, r, s, and t are in the range of 0 to 20.
[0120] Furthermore, it can also be copolymerized with a diol compound having a fluoroalcohol group or a sulfonamide group, as described in JP-A-2022-078861.
[0121] It can also be copolymerized with the silicon-pendant diol compounds described below.
[0122] [ka]
[0123] [ka]
[0124] [ka]
[0125] [ka]
[0126] [ka]
[0127] [ka]
[0128] [ka]
[0129] [ka]
[0130] [ka]
[0131] [ka]
[0132] [ka]
[0133] [ka] Here, m, n, and p are in the range of 1 to 20.
[0134] Among the above isocyanate compounds, in particular, an isocyanate compound having a (meth)acrylate group can be reacted with a compound represented by general formula (1)-1 or other hydroxy compounds to obtain a compound having a (meth)acrylate group at the end. A compound having a (meth)acrylate group at the end can also be obtained by reacting a compound having a hydroxy group and a (meth)acrylate group with an isocyanate compound.
[0135] Among the above-mentioned isocyanate compounds, in particular, an isocyanate compound having a maleimide group can be reacted with a compound represented by the general formula (1)-1 or other hydroxy compounds to obtain a compound having a maleimide group at its terminal. A compound having a maleimide group at its terminal can also be obtained by reacting a compound having a hydroxy group and a maleimide group with an isocyanate compound.
[0136] The above-mentioned isocyanate compounds have high reactivity with hydroxyl group-containing compounds, and it may be difficult to control this. In addition, since the isocyanate compounds may react with moisture in the air during storage and the isocyanate group may be deactivated, sufficient care must be taken during storage, such as preventing humidity. Therefore, in order to prevent these events, a compound having a blocked isocyanate group in which the isocyanate group is protected by a substituent may be used.
[0137] The blocked isocyanate group is a group in which the blocking group is deprotected by heating to become an isocyanate group. Specific examples of the blocked isocyanate group include isocyanate groups substituted with alcohol, phenol, thioalcohol, imine, ketimine, amine, lactam, pyrazole, oxime, β-diketone, etc.
[0138] A catalyst can be added to lower the deprotection temperature of the blocked isocyanate group. Known examples of such catalysts include organotins such as dibutyltin dilaurate, bismuth salts, and zinc carboxylates such as zinc 2-ethylhexanoate and zinc acetate.
[0139] In particular, JP 2012-152725 A discloses that the deprotection reaction can be carried out at a lower temperature by using an α,β-unsaturated carboxylate zinc salt as a carboxylic acid and a blocked isocyanate dissociation catalyst.
[0140] In the polyurethane polymerization, it is preferable to add a catalyst as necessary in order to promote the urethane bond forming reaction.
[0141] The urethanization catalyst can be appropriately selected from known catalysts, and examples of such catalysts include amine catalysts, ammonium salt catalysts, potassium salt catalysts, and organometallic catalysts.
[0142] Examples of the amine catalyst include triethylamine, N,N-dimethylcyclohexylamine, triethylenediamine, 2-methyltriethylenediamine, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethylpropylenediamine, N,N,N',N",N"-pentamethyldiethylenetriamine, N,N,N',N",N"-pentamethyl-(3-aminopropyl)ethylenediamine, N,N,N',N",N"-pentamethyldipropylenetriamine, N,N,N',N'-tetramethylhexamethylenediamine, bis(2-dimethylaminoethyl)ether, dimethylethanolamine, dimethylisopropanolamine, dimethylaminoethoxyethanol, N,N-dimethylhexanolamine, N,N-dimethyl-N'-(2-hydroxyethyl)ethyl Examples of the dimethylaminoethyl ether include dimethylaminoethyl ether, N,N-dimethyl-N'-(2-hydroxyethyl)propanediamine, N,N,N'-trimethylaminoethylethanolamine, bis(dimethylaminopropyl)amine, bis(dimethylaminopropyl)isopropanolamine, N-methyl-N'-(2-dimethylaminoethyl)piperazine, N-methyl-N'-(2-hydroxyethyl)piperazine, N-methylmorpholine, N-ethylmorpholine, 1-methylimidazole, 1,2-dimethylimidazole, 1-isobutyl-2-methylimidazole, 1-dimethylaminopropylimidazole, 1-(2-hydroxyethyl)imidazole, 1-(2-hydroxypropyl)imidazole, 1-(2-hydroxyethyl)-2-methylimidazole, and 1-(2-hydroxypropyl)-2-methylimidazole.
[0143] Examples of the ammonium salt catalyst include quaternary ammonium salts such as tetraethylhydroxylammonium, and ammonium salts of 1,8-diazabicyclo(5,4,0)-undecene-7 or 1,5-diazabicyclo(4,3,0)-nonene-5 with octylic acid, oleic acid, p-toluenesulfonic acid, formic acid, phenolic acid, orthophthalic acid, acetic acid, maleic acid, or boric acid.
[0144] Examples of potassium salt catalysts include potassium carbonate, potassium acetate, and potassium octylate.
[0145] Examples of the organometallic catalyst include organotin compounds such as tin acetate, tin octoate (tin 2-ethylhexanoate), tin oleate, tin laurate, dibutyltin diacetate, dimethyltin dilaurate, dibutyltin dilaurate, dibutyltin dimercaptide, dibutyltin maleate, dibutyltin dineodecanoate, dioctyltin dimercaptide, dioctyltin dilaurate, and dibutyltin dichloride; organolead compounds such as lead octoate and lead naphthenate; organonickel compounds such as nickel naphthenate; organocobalt compounds such as cobalt naphthenate; organocopper compounds such as copper octoate; and organobismuth compounds such as bismuth octoate and bismuth neodecanoate.
[0146] These urethanization catalysts may be used alone or in combination of two or more. The amount of the urethanization catalyst used is preferably in the range of 0 to 5 parts by mass, more preferably 0.1 to 2 parts by mass, per 100 parts by mass of the total amount of the polyurethane constituents.
[0147] In the bioelectrode composition of the present invention, the amount of the component (A) is not particularly limited, but is preferably 10 to 10,000 parts by mass, and more preferably 20 to 2,000 parts by mass, per 100 parts by mass of the component (B). The component (A) may be used alone or in combination of two or more kinds.
[0148] [(B) Resin] The (B) resin blended in the bioelectrode composition of the present invention is a component that is compatible with the above-mentioned (A) component to prevent the elution of salt, holds a conductivity enhancer such as metal powder, carbon powder, silicon powder, lithium titanate powder, and further improves adhesion. If the (A) component has sufficient adhesion, the (B) resin is not necessarily required. The (B) resin may be any resin other than the above-mentioned (A) component, and is preferably either a thermosetting resin or a photocurable resin, or both, and is particularly preferably one or more selected from silicone resins, (meth)acrylate resins, and urethane resins.
[0149] The adhesive silicone resin may be of an addition reaction curing type or a radical crosslinking reaction curing type. Examples of the addition reaction curing type include diorganopolysiloxane having an alkenyl group, RSiO, which is described in JP-A-2015-193803. 0.5 and SiO2 units, organohydrogenpolysiloxane having a plurality of SiH groups, platinum catalyst, addition reaction inhibitor, and organic solvent. In addition, as the radical crosslinking reaction curing type, for example, diorganopolysiloxane which may or may not have alkenyl groups, R3SiO 0.5 and those containing an MQ resin having SiO2 units, an organic peroxide, and an organic solvent, where R is a substituted or unsubstituted monovalent hydrocarbon group having 1 to 10 carbon atoms.
[0150] It is also possible to use a polysiloxane-resin integrated compound formed by condensing polysiloxane with silanols at the polymer end or side chain with MQ resin. MQ resin contains a lot of silanols, so adding this improves adhesive strength, but since it is not crosslinkable, it is not molecularly bonded to the polysiloxane. By integrating polysiloxane and resin as described above, adhesive strength can be increased.
[0151] In addition, modified siloxanes having a group selected from amino groups, oxirane groups, oxetane groups, polyether groups, hydroxy groups, carboxy groups, mercapto groups, methacryl groups, acrylic groups, phenol groups, silanol groups, carboxylic anhydride groups, aryl groups, aralkyl groups, amide groups, ester groups, and lactone rings can be added to the silicone resin. By adding modified siloxanes, the dispersibility of component (A) in the silicone resin is improved. The modified siloxane may be modified at one end, both ends, or the side chain of the siloxane.
[0152] The adhesive (meth)acrylate resin may be, for example, one having a hydrophilic (meth)acrylic acid ester or a long-chain hydrophobic (meth)acrylic acid ester as a repeating unit, as described in JP 2016-011338 A. In some cases, a (meth)acrylic acid ester having a functional group or a (meth)acrylic acid ester having a siloxane bond may be copolymerized.
[0153] As the adhesive urethane resin, for example, one having a urethane bond and a polyether or polyester bond, a polycarbonate bond, or a siloxane bond, as described in JP 2016-065238 A, can be used.
[0154] In addition, in order to prevent the decrease in conductivity due to the detachment of the (A) component from the biocontact layer, in the bioelectrode composition of the present invention, it is preferable that the (B) resin has high compatibility with the above-mentioned (A) component. In addition, in order to prevent the peeling of the biocontact layer from the conductive substrate, it is preferable that the (B) resin has high adhesion to the conductive substrate in the bioelectrode composition of the present invention. In order to make the (B) resin highly compatible with the conductive substrate and salt, it is effective to use a resin with high polarity. Examples of such resins include resins having one or more selected from ether bonds, ester bonds, amide bonds, imide bonds, urethane bonds, thiourethane bonds, and thiol groups, or polyacrylic resins, polyamide resins, polyimide resins, polyurethane resins, and polythiourethane resins. On the other hand, since the biocontact layer contacts the living body, it is easily affected by sweat from the living body. Therefore, in the bioelectrode composition of the present invention, it is preferable that the (B) resin has high water repellency and is not easily hydrolyzed. In order to make the (B) resin highly water repellent and not easily hydrolyzed, it is effective to use a resin containing a silicon atom.
[0155] Silicon-atom-containing polyacrylic resins include polymers having silicone in the main chain and polymers having silicon atoms in the side chain, and both can be used suitably. As the polymer having silicone in the main chain, siloxane or silsesquioxane having a (meth)acrylpropyl group can be used. In this case, the (meth)acryl portion can be polymerized and cured by adding a photoradical generator.
[0156] Suitable examples of polyamide resins containing silicon atoms include polyamide silicone resins described in JP 2011-079946 A and U.S. Patent No. 5,981,680 A. Such polyamide silicone resins can be synthesized by combining, for example, a silicone having amino groups at both ends or a non-silicone compound having amino groups at both ends with a non-silicone having carboxy groups at both ends or a silicone having carboxy groups at both ends so as to contain silicon atoms.
[0157] Alternatively, polyamic acid obtained by reacting a carboxylic anhydride with an amine before cyclization may be used. An epoxy or oxetane crosslinking agent may be used to crosslink the carboxyl groups of the polyamic acid, or the carboxyl groups may be esterified with hydroxyethyl (meth)acrylate to perform photoradical crosslinking of the (meth)acrylate portion.
[0158] As the polyimide resin containing silicon atoms, for example, the polyimide silicone resin described in JP-A-2002-332305 can be suitably used. Polyimide resins have a very high viscosity, but the viscosity can be reduced by blending a (meth)acrylic monomer as a solvent and a crosslinking agent.
[0159] Examples of polyurethane resins containing silicon atoms include polyurethane silicone resins. In such polyurethane silicone resins, crosslinking by urethane bonds can be performed by blending and heating a compound having isocyanate groups at both ends and a compound having hydroxyl groups at the ends. In this case, it is necessary to contain silicon atoms (siloxane bonds) in either or both of the compound having isocyanate groups at both ends and the compound having hydroxyl groups at the ends. Alternatively, as described in JP 2005-320418 A, a urethane (meth)acrylate monomer can be blended with polysiloxane to perform photocrosslinking. In addition, a polymer having both siloxane bonds and urethane bonds and a (meth)acrylate group at the end can also be photocrosslinked. In particular, materials having silicone chains attached to side chains and polyurethane main chains described in JP 2018-123304 A and JP 2019-070109 A are preferred because they have high strength and high elasticity.
[0160] The polythiourethane resin containing silicon atoms can be obtained by reacting a compound having a thiol group with a compound having an isocyanate group, and any one of them may contain a silicon atom. In addition, if the compound has a (meth)acrylate group at the end, it can be photocured.
[0161] In the silicone resin, the above-mentioned diorganopolysiloxane having an alkenyl group, RSiO 0.5 In addition to MQ resins having SiO2 units and organohydrogenpolysiloxanes having multiple SiH groups, the addition of modified siloxanes having groups selected from amino groups, oxirane groups, oxetane groups, polyether groups, hydroxy groups, carboxy groups, mercapto groups, methacryl groups, acrylic groups, phenol groups, silanol groups, carboxylic anhydride groups, aryl groups, aralkyl groups, amide groups, ester groups, and lactone rings increases compatibility with the above-mentioned component (A).
[0162] Diorganopolysiloxanes having alkenyl groups and organohydrogenpolysiloxanes having a plurality of SiH groups can be crosslinked by an addition reaction in the presence of a platinum catalyst.
[0163] Examples of platinum catalysts include platinum catalysts such as chloroplatinic acid, alcohol solutions of chloroplatinic acid, reaction products of chloroplatinic acid and alcohol, reaction products of chloroplatinic acid and olefin compounds, reaction products of chloroplatinic acid and vinyl group-containing siloxane, platinum-olefin complexes, platinum-vinyl group-containing siloxane complexes, platinum group metal catalysts such as rhodium complexes and ruthenium complexes, etc. Furthermore, these catalysts may be used in the form of a solution or dispersion in an alcohol-based, hydrocarbon-based, or siloxane-based solvent.
[0164] The amount of the platinum catalyst added is preferably within a range of 5 to 2,000 ppm, and particularly preferably 10 to 500 ppm, per 100 parts by mass of the resin consisting of components (A) and (B) combined.
[0165] In the bioelectrode composition of the present invention, the blending amount of the (B) component is preferably 0 to 2,000 parts by mass, and more preferably 10 to 1000 parts by mass, per 100 parts by mass of the (A) component. Moreover, the (A) component and the (B) component may each be used alone or in combination of two or more kinds.
[0166] When an addition-curing silicone resin is used, an addition reaction inhibitor may be added as a quencher to prevent the platinum catalyst from acting in the solution and in a low-temperature environment before heat curing after coating formation. Specific examples include 3-methyl-1-butyn-3-ol, 3-methyl-1-pentyn-3-ol, 3,5-dimethyl-1-hexyn-3-ol, 1-ethynylcyclohexanol, 3-methyl-3-trimethylsiloxy-1-butyne, 3-methyl-3-trimethylsiloxy-1-pentyne, 3,5-dimethyl-3-trimethylsiloxy-1-hexyne, 1-ethynyl-1-trimethylsiloxycyclohexane, bis(2,2-dimethyl-3-butynoxy)dimethylsilane, 1,3,5,7-tetramethyl-1,3,5,7-tetravinylcyclotetrasiloxane, and 1,1,3,3-tetramethyl-1,3-divinyldisiloxane.
[0167] The amount of the addition reaction inhibitor added is preferably within a range of 0 to 10 parts by mass, and particularly preferably 0.05 to 3 parts by mass, per 100 parts by mass of the resin consisting of components (A) and (B) combined.
[0168] When component (B) has a radical-crosslinkable double bond, it is effective to add a radical generator, which can be classified into photoradical generators and thermal radical generators.
[0169] Examples of photoradical generators include acetophenone, 4,4'-dimethoxybenzyl, benzil, benzoin, benzophenone, 2-benzoylbenzoic acid, 4,4'-bis(dimethylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin butyl ether, benzoin isobutyl ether, 4-benzoylbenzoic acid, 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 2-benzoylbenzoic acid methyl ester, 2-(1,3-benzodioxol-5-yl)-4,6-bis(trichloromethyl)-1,3,5-triazine, 2-benzoylbenzoic acid methyl ester ... Examples of suitable acetophenones include 2-(dimethylamino)-4'-morpholinobutyrophenone, 4,4'-dichlorobenzophenone, 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,4-diethylthioxanthen-9-one, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide (BAPO), 1,4-dibenzoylbenzene, 2-ethylanthraquinone, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methylpropiophenone, 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone, 2-isonitrosopropiophenone, and 2-phenyl-2-(p-toluenesulfonyloxy)acetophenone.
[0170] It can also be cured by adding a thermally decomposable radical generator. Examples of thermal radical generators include 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(methylpropionamidine) hydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane]hydrochloride, 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(cyclohexane-1-carbonitrile), 1[(1-cyano-1-methylethyl)azo]formamide, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl )propionamide], 2,2'-azobis[N-(2-propenyl)-2-methylpropionamide], 2,2'-azobis(N-butyl-2-methylpropionamide), dimethyl-2,2'-azobis(isobutyrate), 4,4'-azobis(4-cyanopentanoic acid), dimethyl-2,2'-azobis(2-methylpropionate), benzoyl peroxide, tert-butyl hydroperoxide, cumene hydroperoxide, di-tert-butyl peroxide, di-tert-amyl peroxide, di-n-butyl peroxide, dicumyl peroxide, and the like.
[0171] The amount of the radical generator added is preferably within a range of 0.1 to 50 parts by mass per 100 parts by mass of the resin, which is the combined total of the components (A) and (B).
[0172] As described later, the biocontact layer is a cured product of the bioelectrode composition. By curing, the adhesion of the biocontact layer to both the skin and the conductive substrate is improved. The curing method is not particularly limited, and a general method can be used, for example, heat and / or light, or a crosslinking reaction using an acid or base catalyst. The crosslinking reaction can be carried out by appropriately selecting a method described in, for example, Crosslinking Reaction Handbook, Nakayama Hiroharu, Maruzen Publishing (2013), Chapter 2, p. 51 to p. 371.
[0173] [Ionic polymer] In addition to the component (A), an ionic polymer can be added to the bioelectrode composition of the present invention. The ionic polymer may be the polymer described in JP 2018-099504 A, JP 2018-110845 A, or JP 2018-130533 A. The amount of the ionic polymer added is preferably in the range of 0.1 to 100 parts by mass per 100 parts by mass of the resin, which is the combined total of the components (A) and (B).
[0174] [(C) Carbon materials and metal powders] It is also preferable that the bioelectrode composition further contains, as component (C), either or both of a carbon material and a metal powder.
[0175] [Metal powder] In order to enhance electronic conductivity, the bioelectrode composition of the present invention may contain a metal powder selected from gold, silver, platinum, copper, tin, titanium, nickel, aluminum, tungsten, molybdenum, ruthenium, chromium, and indium. The amount of metal powder added is preferably within the range of 1 to 50 parts by mass per 100 parts by mass of the resin, which is the combined total of the (A) and (B) components.
[0176] As for the types of metal powder, gold, silver, and platinum are preferred from the viewpoint of electrical conductivity, and silver, copper, tin, titanium, nickel, aluminum, tungsten, molybdenum, ruthenium, and chromium are preferred from the viewpoint of cost. From the viewpoint of biocompatibility, precious metals are preferred, and from these viewpoints overall, silver (silver powder) is the most preferred.
[0177] The shape of the metal powder can be spherical, disk-like, flake-like, or needle-like, but the addition of flake-like powder is the most conductive and is preferred. The size of the metal powder is 100 μm or less, and the tap density is 5 g / cm. 3 Below, the specific surface area is 0.5m 2 Flakes with a relatively low density and large specific surface area of 100 / g or more are preferred.
[0178] [Carbon materials] A carbon material can be added as a conductivity improver. Examples of the carbon material include carbon black, graphite, carbon nanotubes, carbon fibers, graphene, etc., and it is particularly preferable to use either or both of carbon black and carbon nanotubes. The carbon nanotubes may be either single-walled or multi-walled, and the surface may be modified with an organic group. The amount of the carbon material added is preferably in the range of 1 to 50 parts by mass per 100 parts by mass of the resin, which is the combined resin of components (A) and (B).
[0179] [Silicon powder] Silicon powder can be added to the bioelectrode composition of the present invention in order to increase the sensitivity of ion reception. Examples of silicon powder include powders made of silicon, silicon monoxide, and silicon carbide. The particle size of the powder is preferably smaller than 100 μm, and more preferably 1 μm or less. Since finer particles have a larger surface area, they can receive more ions, resulting in a highly sensitive bioelectrode. The amount of silicon powder added is preferably in the range of 1 to 50 parts by mass per 100 parts by mass of the resin, which is the combined resin of components (A) and (B).
[0180] [Lithium titanate powder] Lithium titanate powder can be added to the bioelectrode composition of the present invention in order to increase the sensitivity of ion reception. Lithium titanate powder includes Li2TiO3, LiTiO2, and Li4Ti5O with a spinel structure. 12 The molecular formula of the lithium titanate powder is as follows, and a spinel structure is preferable. Lithium titanate particles composited with carbon can also be used. The particle size of the powder is preferably smaller than 100 μm, more preferably 1 μm or less. Since finer particles have a larger surface area, they can receive more ions, resulting in a highly sensitive bioelectrode. These may be composite powders with carbon. The amount of lithium titanate powder added is preferably in the range of 1 to 50 parts by mass per 100 parts by mass of the resin (A) and (B) combined.
[0181] [Crosslinking agent] An epoxy-based crosslinking agent can be added to the bioelectrode composition of the present invention. In this case, the crosslinking agent is a compound having multiple epoxy groups or oxetane groups in one molecule. The amount of the crosslinking agent added is preferably 1 to 30 parts by mass per 100 parts by mass of the resin, which is the combined resin of components (A) and (B).
[0182] [Crosslinking catalyst] A crosslinking catalyst for crosslinking epoxy groups or oxetane groups can also be added to the bioelectrode composition of the present invention. In this case, the catalyst described in paragraphs
[0027] to
[0029] of JP2019-503406A can be used. The amount of addition is preferably 0.01 to 10 parts by mass per 100 parts by mass of the resin (A) and (B) combined.
[0183] [Ionic additives] An ionic additive for increasing ionic conductivity can be added to the bioelectrode composition of the present invention. In consideration of biocompatibility, sodium chloride, potassium chloride, calcium chloride, magnesium chloride, saccharin sodium salt, acesulfame potassium, sodium carboxylate, potassium carboxylate, calcium carboxylate, sodium sulfonate, potassium sulfonate, calcium sulfonate, sodium phosphate, potassium phosphate, calcium phosphate, magnesium phosphate, betaine, and salts of JP2018-044147A, JP2018-059050A, JP2018-059052A, and JP2018-130534A can be mentioned. The amount of additive is preferably 0.1 to 50 parts by mass per 100 parts by mass of the resin consisting of the (A) component and the (B) component combined.
[0184] [(D) Organic solvent] The bioelectrode composition of the present invention may further contain an organic solvent as component (D). Specific examples of the organic solvent (D) include toluene, xylene, cumene, 1,2,3-trimethylbenzene, 1,2,4-trimethylbenzene, 1,3,5-trimethylbenzene, styrene, α-methylstyrene, butylbenzene, sec-butylbenzene, isobutylbenzene, cymene, diethylbenzene, 2-ethyl-p-xylene, 2-propyltoluene, 3-propyltoluene, 4-propyltoluene, 1,2,3,5-tetramethyltoluene, 1,2,4,5-tetramethyltoluene, ... 1,2-diisopropylbenzene, 1,3-diisopropylbenzene, 4-phenyl-1-butene, 1,4-isopropylbenzene, 2-tert-butyltoluene, 3-tert-butyltoluene, 4-tert-butyltoluene, 5-isopropyl-m-xylene, 3-methylethylbenzene, 1,4-tert-butyl-o-xylene, 5-tert-butyl-m-xylene, 1,4-isopropyl-p-xylene, 1,2-diisopropylbenzene, 1,3-diisopropylbenzene, 1,4 -Aromatic hydrocarbon solvents such as diisopropylbenzene, dipropylbenzene, pentamethylbenzene, hexamethylbenzene, hexylbenzene, and 1,3,5-triethylbenzene, n-heptane, isoheptane, 3-methylhexane, 2,3-dimethylpentane, 3-ethylpentane, 1,6-heptadiene, 5-methyl-1-hexyne, norbornane, norbornene, dicyclopentadiene, 1-methyl-1,4-cyclohexadiene, 1-heptyne, 2-heptyne, cycloheptane, and cyclo Heptene, 1,3-dimethylcyclopentane, ethylcyclopentane, methylcyclohexane, 1-methyl-1-cyclohexene, 3-methyl-1-cyclohexene, methylenecyclohexane, 4-methyl-1-cyclohexene, 2-methyl-1-hexene, 2-methyl-2-hexene, 1-heptene, 2-heptene, 3-heptene, n-octane, 2,2-dimethylhexane, 2,3-dimethylhexane, 2,4-dimethylhexane, 2,5-dimethylhexane, 3,3-dimethylhexane, 3,4-Dimethylhexane, 3-ethyl-2-methylpentane, 3-ethyl-3-methylpentane, 2-methylheptane, 3-methylheptane, 4-methylheptane, 2,2,3-trimethylpentane, 2,2,4-trimethylpentane, cyclooctane, cyclooctene, 1,2-dimethylcyclohexane, 1,3-dimethylcyclohexane, 1,4-dimethylcyclohexane, ethylcyclohexane, vinylcyclohexane, isopropylcyclopentane, 2,2-dimethyl-3-hexene, 2,4-dimethyl-1-hexene, 2,5-dimethyl-1- Hexene, 2,5-dimethyl-2-hexene, 3,3-dimethyl-1-hexene, 3,4-dimethyl-1-hexene, 4,4-dimethyl-1-hexene, 2-ethyl-1-hexene, 2-methyl-1-heptene, 1-octene, 2-octene, 3-octene, 4-octene, 1,7-octadiene, 1-octyne, 2-octyne, 3-octyne, 4-octyne, n-nonane, 2,3-dimethylheptane, 2,4-dimethylheptane, 2,5-dimethylheptane, 3,3-dimethylheptane, 3,4-dimethylheptane, 3,5-dimethylheptane, 4-ethylhexene, ethylheptane, 2-methyloctane, 3-methyloctane, 4-methyloctane, 2,2,4,4-tetramethylpentane, 2,2,4-trimethylhexane, 2,2,5-trimethylhexane, 2,2-dimethyl-3-heptene, 2,3-dimethyl-3-heptene, 2,4-dimethyl-1-heptene, 2,6-dimethyl-1-heptene, 2,6-dimethyl-3-heptene, 3,5-dimethyl-3-heptene, 2,4,4-trimethyl-1-hexene, 3,5,5-trimethyl-1-hexene, 1-ethyl-2-methylcyclohexane, 1-ethyl-3 -Methylcyclohexane, 1-ethyl-4-methylcyclohexane, propylcyclohexane, isopropylcyclohexane, 1,1,3-trimethylcyclohexane, 1,1,4-trimethylcyclohexane, 1,2,3-trimethylcyclohexane, 1,2,4-trimethylcyclohexane, 1,3,5-trimethylcyclohexane, allylcyclohexane, hydrindane, 1,8-nonadiene, 1-nonyne, 2-nonyne, 3-nonyne, 4-nonyne, 1-nonene, 2-nonene, 3-nonene, 4-nonene, n-decane, 3,3-dimethyloctane, 3,5-Dimethyloctane, 4,4-Dimethyloctane, 3-Ethyl-3-methylheptane, 2-Methylnonane, 3-Methylnonane, 4-Methylnonane, tert-Butylcyclohexane, Butylcyclohexane, Isobutylcyclohexane, 4-Isopropyl-1-methylcyclohexane, Pentylcyclopentane, 1,1,3,5-Tetramethylcyclohexane, Cyclododecane, 1-Decene, 2-Decene, 3-Decene, 4-Decene, 5-Decene, 1,9-Decadiene, Decahydronaphthalene, 1-Decyne, 2-Decyne, 3-Decyne, 4-Decyne, 5-Decyne, 1,5,9-Decyne katriene, 2,6-dimethyl-2,4,6-octatriene, limonene, myrcene, 1,2,3,4,5-pentamethylcyclopentadiene, α-phellandrene, pinene, terpinene, tetrahydrodicyclopentadiene, 5,6-dihydrodicyclopentadiene, dicyclopentadiene, 1,4-decadiyne, 1,5-decadiyne, 1,9-decadiyne, 2,8-decadiyne, 4,6-decadiyne, n-undecane, amylcyclohexane, 1-undecene, 1,10-undecadiene, 1-undecyne, 3-undecyne, 5-undecyne, tricyclo[6.2.1.0, 2,7]Undec-4-ene, n-dodecane, n-tridecane, n-pentadecane, n-hexadecane, 2-methylundecane, 3-methylundecane, 4-methylundecane, 5-methylundecane, 2,2,4,6,6-pentamethylheptane, 1,3-dimethyladamantane, 1-ethyladamantane, 1,5,9-cyclododecatriene, 1,2,Aliphatic hydrocarbon solvents such as 4-trivinylcyclohexane and isoparaffin; ketone solvents such as cyclohexanone, cyclopentanone, 2-octanone, 2-nonanone, 2-heptanone, 3-heptanone, 4-heptanone, 2-hexanone, 3-hexanone, diisobutyl ketone, methylcyclohexanone, and methyl n-pentyl ketone; alcohol solvents such as 3-methoxybutanol, 3-methyl-3-methoxybutanol, 1-methoxy-2-propanol, and 1-ethoxy-2-propanol; propylene glycol monomethyl ether, ethylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, propylene glycol dimethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monobutyl ether, diethylene glycol monopentyl ether, and diethylene glycol monoheptyl Examples of the solvent include ether solvents such as ether, diethylene glycol diethyl ether, diethylene glycol dipropyl ether, diethylene glycol dibutyl ether, diisopropyl ether, diisobutyl ether, diisopentyl ether, di-n-pentyl ether, methylcyclopentyl ether, methylcyclohexyl ether, di-n-butyl ether, di-sec-butyl ether, diisopentyl ether, di-sec-pentyl ether, di-tert-amyl ether, di-n-hexyl ether, and anisole; ester solvents such as propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ethyl lactate, ethyl pyruvate, butyl acetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, tert-butyl acetate, tert-butyl propionate, and propylene glycol monotert-butyl ether acetate; lactone solvents such as γ-butyrolactone; and water.
[0185] The amount of the (D) organic solvent added is preferably within a range of 10 to 50,000 parts by mass per 100 parts by mass of the resin, which is the combined total of the (A) and (B) components.
[0186] [Other additives] The bioelectrode composition of the present invention can also be mixed with silica particles, polyether silicone, polyether, polyglycerin, and polyglycerin silicone. Silica particles have a hydrophilic surface, and are compatible with hydrophilic ionic polymers, polyether silicone, and polyglycerin silicone, and can improve the dispersibility of ionic polymers, polyether silicone, and polyglycerin silicone in hydrophobic silicone adhesives. Silica particles can be used preferably in either dry or wet methods.
[0187] [Silicone compounds having polyglycerin structure] In the bioelectrode composition of the present invention, a silicone compound having a polyglycerin structure can be added in order to improve the moisture retention of the membrane and improve the sensitivity and ion conductivity of ions released from the skin. The amount of the silicone compound having a polyglycerin structure is preferably 0.01 to 100 parts by mass, more preferably 0.5 to 60 parts by mass, per 100 parts by mass of the resin (A) and (B) components combined. The silicone compound having a polyglycerin structure may be used alone or in a mixture of two or more kinds.
[0188] The silicone compound having a polyglycerin structure is preferably any one of those represented by the following general formulas (4)' and (5)'. [ka] (In the formula, R 1 are each independent and may be the same or different, each independently represent a hydrogen atom, a linear or branched alkyl group having 1 to 50 carbon atoms, or a phenyl group, each independently represent a silicone chain represented by the general formula (6)' ... 2 R′ is a group having a polyglycerin structure represented by general formula (4)′-1 or general formula (4)′-2, 3' are each independent and may be the same or different, 1 ' or the R 2 ' and R 4 ' are each independent and may be the same or different, 1 ', said R 2 ' or an oxygen atom. 4 If ' is an oxygen atom, R 4 a' may be bonded to each other to form a single ether group and form a ring together with the silicon atom. a' may be the same or different and is 0 to 100, b' is 0 to 100, and a'+b' is 0 to 200. However, when b' is 0, R 3 At least one of the R 2 '. R 5 ' is an alkylene group having 2 to 10 carbon atoms or an aralkylene group having 7 to 10 carbon atoms; R 6 ', R 7 ', and R 8 ' is an alkylene group having 2 to 6 carbon atoms, and R 7 ' may be an ether bond, c' is 0 to 20, and d' is 1 to 20.
[0189] Examples of such silicone compounds having a polyglycerin structure include the following.
[0190] [ka]
[0191] [ka]
[0192] [ka]
[0193] [ka]
[0194] [ka]
[0195] [ka]
[0196] [ka]
[0197] [ka]
[0198] [ka]
[0199] [ka] (wherein a', b', c' and d' are as defined above).
[0200] A bioelectrode composition containing a silicone compound having such a polyglycerin structure can exhibit better moisturizing properties, and as a result, can form a biocontact layer that can exhibit better sensitivity to ions released from the skin.
[0201] As described above, the bioelectrode composition of the present invention is a bioelectrode composition that can form a biocontact layer for a bioelectrode that has high adhesion, has sufficient adhesion even when peeled off from the skin and reattached, can efficiently transmit electrical signals from the skin to the device (i.e., has excellent conductivity), is not likely to cause allergies even when worn on the skin for a long period of time (i.e., has excellent biocompatibility), is lightweight, can be manufactured at low cost, and does not significantly decrease in conductivity even when wet or dried. In addition, the conductivity can be further improved by adding a carbon material, and a bioelectrode with particularly high adhesion and high elasticity can be manufactured by combining it with a resin having adhesiveness and elasticity. Furthermore, the elasticity and adhesiveness to the skin can be improved by additives, and the elasticity and adhesiveness can be adjusted by appropriately adjusting the composition of the resin and the thickness of the biocontact layer.
[0202] <Bioelectrode> The present invention also provides a bioelectrode having a conductive substrate and a biocontact layer formed on the conductive substrate, the bioelectrode being a cured product of the bioelectrode composition described above.
[0203] The bioelectrode of the present invention will be described in detail below with reference to the drawings, but the present invention is not limited thereto.
[0204] Fig. 1 is a schematic cross-sectional view showing an example of the bioelectrode of the present invention. The bioelectrode 1 in Fig. 1 has a conductive substrate 2 and a biocontact layer 3 formed on the conductive substrate 2. The biocontact layer 3 is made of a cured product of the bioelectrode composition of the present invention. The biocontact layer 3 contains an ionic urethane resin 5. The biocontact layer 3 may further contain a resin 6 other than the ionic urethane resin 5, and a conductive powder 4. Hereinafter, with reference to Figs. 1 and 2, a case where the biocontact layer 3 is a layer in which the ionic urethane resin 5 and the conductive powder 4 are dispersed in the resin 6 will be described, but the bioelectrode of the present invention is not limited to this embodiment.
[0205] When using such a bioelectrode 1 of Fig. 1, as shown in Fig. 2, the biocontact layer 3 (i.e., a layer in which ionic urethane resin 5 and conductive powder 4 are dispersed in resin 6) is brought into contact with a living body 7, and an electrical signal is extracted from the living body 7 by the ionic urethane resin 5 and the conductive powder 4, and this is conducted to a sensor device or the like (not shown) via the conductive base material 2. In this way, with the bioelectrode of the present invention, the above-mentioned ionic urethane resin (component (A)) can achieve both electrical conductivity and biocompatibility, and since it also has adhesiveness, the contact area with the skin is constant, and electrical signals from the skin can be obtained stably and with high sensitivity.
[0206] Each of the constituent materials of the bioelectrode of the present invention will be described in more detail below.
[0207] [Conductive base material] The bioelectrode of the present invention has a conductive substrate. This conductive substrate is usually electrically connected to a sensor device or the like, and conducts an electrical signal extracted from a living body via a living body contact layer to the sensor device or the like.
[0208] The conductive substrate is not particularly limited as long as it is conductive, but it is preferable that the conductive substrate contains at least one material selected from the group consisting of gold, silver, silver chloride, platinum, aluminum, magnesium, tin, tungsten, iron, copper, nickel, stainless steel, chromium, titanium, carbon, and conductive polymers.
[0209] The conductive substrate is not particularly limited and may be a hard conductive substrate, a flexible conductive film, a fabric coated with a conductive paste, or a fabric with a conductive polymer kneaded in. The conductive substrate may be flat or uneven, or may be a mesh of woven metal wires, and may be appropriately selected depending on the application of the bioelectrode.
[0210] [Bio-contact layer] The bioelectrode of the present invention has a biocontact layer formed on a conductive substrate. This biocontact layer is the part that actually comes into contact with the living body when the bioelectrode is used, and is conductive and, in some cases, adhesive. The biocontact layer is a cured product of the bioelectrode composition of the present invention described above, that is, an adhesive resin layer made of a cured product of a composition containing the above-mentioned component (A) and, if necessary, components (B), (C), (D), and other components.
[0211] The living body contact layer may or may not have adhesiveness, but if it does have adhesiveness, the adhesive strength is preferably in the range of 0.01 N / 25 mm to 20 N / 25 mm. The adhesive strength is generally measured by the method shown in JIS Z 0237, and a metal substrate such as SUS (stainless steel) or a PET (polyethylene terephthalate) substrate can be used as the substrate, but it can also be measured using human skin. The surface energy of human skin is lower than that of metals and various plastics, and is close to that of Teflon (registered trademark), making it difficult to adhere to the skin.
[0212] The thickness of the biocontact layer of the bioelectrode is preferably 1 μm to 5 mm, more preferably 2 μm to 3 mm. The thinner the biocontact layer, the weaker the adhesive strength, but the more flexible it is, the lighter it is, and the better it fits to the skin. The thickness of the biocontact layer can be selected based on the balance between adhesiveness and texture on the skin.
[0213] In addition, in the bioelectrode of the present invention, similar to conventional bioelectrodes (for example, the bioelectrode described in JP 2004-033468 A), a separate adhesive film may be provided on the biocontact layer to prevent the bioelectrode from peeling off from the living body during use. When providing a separate adhesive film, it is sufficient to form the adhesive film using an adhesive film material such as an acrylic type, a urethane type, or a silicone type. In particular, the silicone type has high oxygen permeability, so that the skin can breathe while it is attached, and has high water repellency, so that the adhesiveness is less likely to decrease due to sweat, and further, is less irritating to the skin, so it is preferable. In addition, in the bioelectrode of the present invention, as described above, peeling off from the living body can be prevented by adding an adhesive imparting agent to the bioelectrode composition or using a resin that has good adhesiveness to the living body, so that the above-mentioned separate adhesive film is not necessarily required.
[0214] When the bioelectrode of the present invention is used as a wearable device, the wiring between the bioelectrode and the sensor device and other components are not particularly limited, and for example, those described in JP 2004-033468 A can be applied.
[0215] As described above, the bioelectrode of the present invention has a biocontact layer formed of the cured product of the bioelectrode composition of the present invention, so that the bioelectrode can efficiently transmit electrical signals from the skin to the device (i.e., has excellent electrical conductivity), is not likely to cause allergies even when worn on the skin for a long period of time (i.e., has excellent biocompatibility), is lightweight, can be manufactured at low cost, and does not significantly decrease in electrical conductivity even when wet or dried. In addition, the electrical conductivity can be further improved by adding conductive powder, and a bioelectrode with particularly high adhesive strength and high elasticity can be manufactured by combining it with a resin having adhesiveness and elasticity. Furthermore, the elasticity and adhesiveness to the skin can be improved by additives, and the elasticity and adhesiveness can be adjusted by appropriately adjusting the composition of the resin and the thickness of the biocontact layer. Therefore, such a bioelectrode of the present invention is particularly suitable as a bioelectrode used in a medical wearable device.
[0216] <Manufacturing method of bioelectrodes> The present invention also provides a method for manufacturing a bioelectrode having a conductive substrate and a biocontact layer formed on the conductive substrate, in which the bioelectrode composition described above is applied to the conductive substrate and cured to form the biocontact layer.
[0217] The conductive substrate and the like used in the method for producing a bioelectrode of the present invention may be the same as those described above. As the conductive substrate, for example, one or more selected from gold, silver, silver chloride, platinum, aluminum, magnesium, tin, tungsten, iron, copper, nickel, stainless steel, chromium, titanium, carbon, and conductive polymers are preferably used.
[0218] The method for applying the bioelectrode composition onto the conductive substrate is not particularly limited, but suitable methods include, for example, dip coating, spray coating, spin coating, roll coating, flow coating, doctor coating, screen printing, flexographic printing, gravure printing, and inkjet printing.
[0219] The resin curing method is not particularly limited and may be appropriately selected depending on the components (A) and (B) used in the bioelectrode composition, but it is preferable to cure the resin by, for example, heat or light, or both. In addition, a catalyst that generates an acid or base may be added to the bioelectrode composition to cause a crosslinking reaction and cure the resin.
[0220] The temperature for heating is not particularly limited and may be appropriately selected depending on the components (A) and (B) used in the bioelectrode composition, but is preferably about 50 to 250°C, for example.
[0221] In addition, when heating and light irradiation are combined, heating and light irradiation may be performed simultaneously, or heating may be performed after light irradiation, or light irradiation may be performed after heating. In addition, air drying may be performed before heating after coating in order to evaporate the solvent.
[0222] After the film has hardened, applying water droplets or spraying water vapor or mist on the surface improves its compatibility with the skin, allowing for quick biosignals to be obtained. Water mixed with alcohol can also be used to reduce the size of the vapor or mist droplets. The film surface can also be wetted by contacting it with absorbent cotton or cloth soaked in water.
[0223] The water that wets the surface of the cured film may contain a salt, and the water-soluble salt that is mixed with the water is selected from sodium salts, potassium salts, calcium salts, magnesium salts, and betaines.
[0224] Specifically, the water-soluble salt may be a salt selected from sodium chloride, potassium chloride, calcium chloride, magnesium chloride, sodium saccharin, acesulfame potassium, sodium carboxylate, potassium carboxylate, calcium carboxylate, sodium sulfonate, potassium sulfonate, calcium sulfonate, sodium phosphate, potassium phosphate, calcium phosphate, magnesium phosphate, and betaine. Note that the above-mentioned component (A) is not included in the water-soluble salt.
[0225] More specifically, in addition to the above, sodium acetate, sodium propionate, sodium pivalate, sodium glycolate, sodium butyrate, sodium valerate, sodium caproate, sodium enanthate, sodium caprylate, sodium pelargonate, sodium caprate, sodium undecylate, sodium laurate, sodium tridecylate, sodium myristate, sodium pentadecylate, sodium palmitate, sodium margarate, sodium stearate, sodium benzoate, disodium adipate, disodium maleate, disodium phthalate, sodium 2-hydroxybutyrate, sodium 3-hydroxybutyrate, sodium 2-oxobutyrate, sodium gluconate, methanesulfonate, sodium glycer ... Examples of betaines include sodium sulfonate, sodium 1-nonanesulfonate, sodium 1-decanesulfonate, sodium 1-dodecanesulfonate, sodium 1-undecanesulfonate, sodium cocoyl isethionate, sodium lauroyl methylalanine, sodium cocoyl methyl taurate, sodium cocoyl glutamate, sodium cocoyl sarcosine, sodium lauroyl methyl taurate, laumidpropyl betaine, potassium isobutyrate, potassium propionate, potassium pivalate, potassium glycolate, potassium gluconate, potassium methanesulfonate, calcium stearate, calcium glycolate, calcium gluconate, calcium 3-methyl-2-oxobutyrate, and calcium methanesulfonate. Betaine is a general term for intramolecular salts, specifically a compound in which three methyl groups are added to the amino group of an amino acid, and more specifically, trimethylglycine, carnitine, and proline betaine can be mentioned.
[0226] The water-soluble salt may further contain a monohydric alcohol or polyhydric alcohol having 1 to 4 carbon atoms. The alcohol is preferably selected from ethanol, isopropyl alcohol, ethylene glycol, diethylene glycol, triethylene glycol, glycerin, polyethylene glycol, polypropylene glycol, polyglycerin, diglycerin, and a silicone compound having a polyglycerin structure, and it is more preferable that the silicone compound having a polyglycerin structure is one represented by the above general formula (4)' to (5)'.
[0227] The pretreatment method using a water-soluble salt-containing aqueous solution can wet the bioelectrode membrane after hardening by spraying, dispensing water droplets, etc. It can also be wetted in a high-temperature, high-humidity state such as a sauna. After wetting, in order to prevent drying, a protective film can be further laminated on the permeation layer to cover it. Since the protective film needs to be peeled off just before applying it to the skin, it can be coated with a release agent or a peelable fluororesin film can be used. For long-term storage, the dry electrode covered with a release film is preferably sealed in a bag covered with aluminum or the like. In order to prevent drying in the aluminum-covered bag, it is preferable to seal moisture in it.
[0228] Before attaching the bioelectrode of the present invention to the skin, the skin side can be moistened with water, alcohol, etc., or the skin can be wiped with a cloth or absorbent cotton containing water, alcohol, etc. The above-mentioned salt can also be contained in the water or alcohol.
[0229] As described above, the manufacturing method of the bioelectrode of the present invention makes it possible to easily manufacture, at low cost, the bioelectrode of the present invention which has excellent conductivity and biocompatibility, is lightweight, and whose conductivity does not decrease significantly whether it is wetted with water or dried. EXAMPLES
[0230] The present invention will be specifically described below using examples and comparative examples, but the present invention is not limited to these.
[0231] Ionic urethane resins 1 to 28 were synthesized by mixing the following dihydroxy group-containing sulfonamide compounds 1 to 20 with an isocyanate compound, a dihydroxy compound for chain extension in some cases, a monohydroxy compound or a monoisocyanate compound for terminal blocking, a solvent propylene glycol monomethyl ether acetate in an amount twice the mass of the raw material compounds, and 0.02 mass% of catalyst XK-640 (manufactured by KING INDUSTRIES) per 100 mass parts of the raw material compounds, and reacting them at 90°C for 9 hours.
[0232] The composition of the obtained polymer was the ratio of the charged raw materials, and the molecular weight (Mw) and dispersity (Mw / Mn) were confirmed by gel permeation chromatography (GPC) using tetrahydrofuran (THF) as a solvent.
[0233] [ka]
[0234] [ka]
[0235] [ka]
[0236] Ionic urethane resin 1 (derived from dihydroxy group-containing sulfonamide compound 4) [ka]
[0237] Ionic urethane resin 2 (derived from dihydroxy group-containing sulfonamide compound 1) Mw=7,700 Mw / Mn=2.01 [ka]
[0238] Ionic urethane resin 3 (derived from dihydroxy group-containing sulfonamide compound 2) Mw=17,600 Mw / Mn=2.11 [ka]
[0239] Ionic urethane resin 4 (derived from dihydroxy group-containing sulfonamide compound 7) Mw=16,600 Mw / Mn=2.09 [ka]
[0240] Ionic urethane resin 5 (derived from dihydroxy group-containing sulfonamide compound 1) Mw=7,600 Mw / Mn=2.00 [ka]
[0241] Ionic urethane resin 6 (derived from dihydroxy group-containing sulfonamide compound 1) Mw=8,800 Mw / Mn=2.11 [ka]
[0242] Ionic urethane resin 7 (derived from dihydroxy group-containing sulfonamide compound 1) Mw=9,500 Mw / Mn=2.30 [ka]
[0243] Ionic urethane resin 8 (derived from dihydroxy group-containing sulfonamide compound 5) Mw=48,000 Mw / Mn=3.30 [ka]
[0244] Ionic urethane resin 9 (derived from dihydroxy group-containing sulfonamide compound 3) Mw=12,000 Mw / Mn=2.80 [ka]
[0245] Ionic urethane resin 10 (derived from dihydroxy group-containing sulfonamide compound 5) Mw=22,600 Mw / Mn=2.70 [ka] In the formula, * represents a bond.
[0246] Ionic urethane resin 11 (derived from dihydroxy group-containing sulfonamide compound 5) Mw=38,000 Mw / Mn=3.10 [ka] In the formula, * represents a bond.
[0247] Ionic urethane resin 12 (derived from dihydroxy group-containing sulfonamide compound 6) Mw=12,000 Mw / Mn=2.90 [ka]
[0248] Ionic urethane resin 13 (derived from dihydroxy group-containing sulfonamide compound 7) Mw=30,000 Mw / Mn=2.91 [ka] In the formula, * represents a bond.
[0249] Ionic urethane resin 14 (derived from dihydroxy group-containing sulfonamide compound 7) Mw=50,500 Mw / Mn=2.97 [ka]
[0250] Ionic urethane resin 15 (derived from dihydroxy group-containing sulfonamide compound 8) Mw=53,000 Mw / Mn=3.02 [ka]
[0251] Ionic urethane resin 16 (derived from dihydroxy group-containing sulfonamide compound 9) Mw=23,000 Mw / Mn=2.80 [ka] In the formula, * represents a bond.
[0252] Ionic urethane resin 17 (derived from dihydroxy group-containing sulfonamide compound 10) Mw=23,600 Mw / Mn=2.88 [ka] In the formula, * represents a bond.
[0253] Ionic urethane resin 18 (derived from dihydroxy group-containing sulfonamide compound 11) Mw=24,000 Mw / Mn=2.82 [ka] In the formula, * represents a bond.
[0254] Ionic urethane resin 19 (derived from dihydroxy group-containing sulfonamide compound 12) Mw=24,400 Mw / Mn=2.89 [ka] In the formula, * represents a bond.
[0255] Ionic urethane resin 20 (derived from dihydroxy group-containing sulfonamide compound 9) Mw=9,900 Mw / Mn=2.08 [ka] In the formula, * represents a bond.
[0256] Ionic urethane resin 21 (derived from dihydroxy group-containing sulfonamide compound 13) Mw=22,900 Mw / Mn=2.78 [ka] In the formula, * represents a bond.
[0257] Ionic urethane resin 22 (derived from dihydroxy group-containing sulfonamide compound 14) Mw=23,000 Mw / Mn=2.81 [ka] In the formula, * represents a bond.
[0258] Ionic urethane resin 23 (derived from dihydroxy group-containing sulfonamide compound 15) Mw=23,200 Mw / Mn=2.83 [ka] In the formula, * represents a bond.
[0259] Ionic urethane resin 24 (derived from dihydroxy group-containing sulfonamide compound 16) Mw=24,000 Mw / Mn=2.87 [ka] In the formula, * represents a bond.
[0260] Ionic urethane resin 25 (derived from dihydroxy group-containing sulfonamide compound 17) Mw=23,200 Mw / Mn=2.80 [ka] In the formula, * represents a bond.
[0261] Ionic urethane resin 26 (derived from dihydroxy group-containing sulfonamide compound 18) Mw=23,000 Mw / Mn=2.79 [ka] In the formula, * represents a bond.
[0262] Ionic urethane resin 27 (derived from dihydroxy group-containing sulfonamide compound 19) Mw=24,000 Mw / Mn=2.81 [ka] In the formula, * represents a bond.
[0263] Ionic urethane resin 28 (derived from dihydroxy group-containing sulfonamide compound 20) Mw=23,300 Mw / Mn=2.63 [ka] In the formula, * represents a bond.
[0264] The silicone pendant urethane (meth)acrylate 1 incorporated in the bioelectrode solution is shown below. Silicone pendant urethane (meth)acrylate 1 Mw=24,800 Mw / Mn=2.65 [ka] (The number of repetitions in the formula indicates the average value.)
[0265] The acrylic resin 1 blended as an acrylic resin in the bioelectrode solution and the urethane resins 1 and 2 blended as urethane resins in the bioelectrode solution are shown below. Acrylic Resin 1 Mw=337,000 Mw / Mn=3.65 [ka]
[0266] Urethane resin 1 Mw=83,000 Mw / Mn=4.02 [ka]
[0267] Urethane Resin 2 Mw=84,000 Mw / Mn=4.22 [ka] In the formula, * represents a bond.
[0268] Polyglycerin silicones 1 and 2 are shown below.
[0269] Polyglycerin Silicone 1 [ka]
[0270] Polyglycerin Silicone 2 [ka]
[0271] The organic solvents added to the bioelectrode solution are shown below. EDE: Diethylene glycol diethyl ether PGMEA: Propylene glycol monomethyl ether acetate
[0272] The lithium titanate powder, radical generator, and conductivity enhancer (carbon black, multi-walled carbon nanotubes, graphite, and silver flakes) that were added to the bioelectrode solution as additives are shown below. Lithium titanate powder: Sigma-Aldrich, size 200 nm or less Radical generator: BASF Irgacure TPO Carbon black: Denka Black Li-400 manufactured by Denka Multi-walled carbon nanotubes: Sigma-Aldrich, diameter 110-170 nm, length 5-9 μm Graphite: Sigma-Aldrich, diameter 20 μm or less Silver flakes: Sigma-Aldrich, average size 10 μm
[0273] [Examples 1 to 27, Comparative Example 1] Ionic urethane resin, resin, organic solvent, and additives (radical generator, conductivity enhancer) were blended in the compositions shown in Tables 1 to 3 to prepare bioelectrode solutions (bioelectrode solutions 1 to 27, comparative bioelectrode solution 1).
[0274] [Table 1]
[0275] [Table 2]
[0276] [Table 3]
[0277] (Preparation of bioelectrodes) As shown in FIG. 3, a conductive paste manufactured by Fujikura Kasei, Dotite FA-333, was coated on ST-604 of a thermoplastic urethane (TPU) film 20 manufactured by Bemis by screen printing, and baked in an oven at 120°C for 10 minutes to print a keyhole-shaped conductive pattern with a circle diameter of 2 cm. The bioelectrode solutions listed in Tables 1 to 3 were applied by stencil printing on the circular part on top of the film, air-dried at room temperature for 10 minutes, and then baked in an oven at 120°C for 10 minutes to evaporate the solvent and harden the film, thereby producing a bioelectrode 1. Each bioelectrode 1 included a conductive base material 2 and a biocontact layer 3 formed on the circular part of the conductive base material 2. The bioelectrodes to which the bioelectrode solutions 1 to 6 were applied were exposed to 500 mJ / cm 2 of a 1,000 W xenon lamp under a nitrogen atmosphere. 2 The composition coating film was cured by irradiating it with light of 1000 nm.
[0278] (Measurement of the thickness of the biological contact layer) The thickness of the biocontact layer of the bioelectrode thus prepared was measured using a micrometer. The results are shown in Table 4.
[0279] As shown in FIG. 4, a thermoplastic urethane film 20 on which a bioelectrode was printed was cut out, and a double-sided tape 21 was attached to it to prepare three bioelectrode samples 10 for each bioelectrode solution.
[0280] (Measurement of biological signals) The conductive wiring pattern made of conductive paste of the bioelectrode was connected to a portable electrocardiograph HCG-901 manufactured by Omron Healthcare Co., Ltd. with a conductive wire, and the positive electrode of the electrocardiograph was attached to the LA position of the human body in Fig. 5, the negative electrode to the LL position, and the earth to the RA position. Immediately after attachment, the electrocardiogram measurement was started, and the time until the electrocardiogram waveform consisting of P, Q, R, S, and T waves shown in Fig. 6 appeared was measured. The results are shown in Table 4.
[0281] [Table 4]
[0282] As shown in Table 4, in Examples 1 to 27 in which a biocontact layer was formed using bioelectrode solutions 1 to 27, which are bioelectrode compositions of the present invention containing a resin having a urethane bond in the main chain and one or more salts selected from ammonium salts, sodium salts, potassium salts, and silver salts of sulfonamide in the side chain, a biosignal could be obtained in a short time after application to the body. On the other hand, in Comparative Example 1 in which comparative bioelectrode solution 1 not containing an ionic component with a specific structure was used, a biosignal could not be obtained.
[0283] The present specification includes the following aspects. [1]: A bioelectrode composition, comprising, as component (A), a resin having a urethane bond in its main chain and one or more salts selected from ammonium salts, sodium salts, potassium salts, and silver salts of sulfonamide in its side chains. [2]: The bioelectrode composition according to the above [1], characterized in that the component (A) is represented by the following general formula (1): [ka] (In general formula (1), R 1 , R 3 R is a single bond or a linear or branched alkylene group having 1 to 6 carbon atoms, which may have an ether bond or a bromine atom. 2R is a hydrogen atom, a hydroxyl group, a linear or branched alkyl group having 1 to 6 carbon atoms, or an alkoxy group. 4 represents a single bond or a linear, branched or cyclic hydrocarbylene group having 1 to 20 carbon atoms, which may have a carbonyl group, an ether group or an ester group; R 1 R may be bonded to form a ring. 5 is a linear, branched, or cyclic alkyl group having 1 to 10 carbon atoms, which may be substituted with a fluorine atom, or an alkenyl group having 2 to 6 carbon atoms, an alkynyl group having 2 to 6 carbon atoms, or an aryl group having 6 to 10 carbon atoms, which may have a fluorine atom, a trifluoromethyl group, a cyano group, a nitro group, a hydroxy group, an alkoxy group having 1 to 6 carbon atoms, or an alkyl group having 1 to 6 carbon atoms. M + is an ammonium ion, a sodium ion, a potassium ion, or a silver ion. [3]: The bioelectrode composition according to [1] or [2], characterized in that the component (A) contains an ammonium ion represented by the following general formula (2) as an ammonium ion constituting the ammonium salt: [ka] (In general formula (2), R 101d , R 101e , R 101f , and R 101g R is a hydrogen atom, a linear, branched, or cyclic alkyl group having 1 to 15 carbon atoms, a linear, branched, or cyclic alkenyl or alkynyl group having 2 to 12 carbon atoms, or an aromatic group having 4 to 20 carbon atoms, and may have one or more groups selected from an ether group, a carbonyl group, an ester group, a hydroxy group, an amino group, a nitro group, a sulfonyl group, a sulfinyl group, a halogen atom, and a sulfur atom. 101d and R 101e , or R 101d , R 101e and R 101f may form a ring together with the nitrogen atom to which they are attached, and when they form a ring, R 101d and R 101e , or R 101d , R101e and R 101f is an alkylene group having 3 to 10 carbon atoms, or forms a heteroaromatic ring having the nitrogen atom in the general formula (2) in the ring. [4]: The bioelectrode composition according to any one of [1] to [3] above, characterized in that the bioelectrode composition further contains, as component (B), a resin other than the component (A). [5]: The bioelectrode composition according to the above [4], wherein the component (B) is at least one selected from the group consisting of silicone resins, (meth)acrylate resins, and urethane resins. [6]: The bioelectrode composition according to any one of [1] to [5] above, further comprising, as component (C), either or both of a carbon material and a metal powder. [7]: The bioelectrode composition according to [6] above, characterized in that the carbon material is either or both of carbon black and carbon nanotubes. [8]: The bioelectrode composition according to [6] or [7], characterized in that the metal powder is a metal powder selected from the group consisting of gold, silver, platinum, copper, tin, titanium, nickel, aluminum, tungsten, molybdenum, ruthenium, chromium, and indium. [9]: The bioelectrode composition according to [8] above, characterized in that the metal powder is silver powder.
[10] : The bioelectrode composition according to any one of [1] to [9] above, further comprising an organic solvent as component (D).
[11] : A bioelectrode having a conductive substrate and a biocontact layer formed on the conductive substrate, characterized in that the biocontact layer is a cured product of the bioelectrode composition according to any one of [1] to
[10] above.
[12] : The bioelectrode according to
[11] above, characterized in that the conductive base material contains one or more selected from gold, silver, silver chloride, platinum, aluminum, magnesium, tin, tungsten, iron, copper, nickel, stainless steel, chromium, titanium, carbon, and conductive polymers.
[13] : A method for manufacturing a bioelectrode having a conductive substrate and a biocontact layer formed on the conductive substrate, comprising applying any one of the bioelectrode compositions [1] to
[10] above onto the conductive substrate and curing the composition to form the biocontact layer.
[14] : A method for producing a bioelectrode according to
[13] above, characterized in that the conductive base material contains one or more metals selected from gold, silver, silver chloride, platinum, aluminum, magnesium, tin, tungsten, iron, copper, nickel, stainless steel, chromium, titanium, carbon, and conductive polymers.
[0284] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. [Explanation of symbols]
[0285] 1...bioelectrode, 2...conductive substrate, 3...biocontact layer, 4...conductive powder, 5...ionic urethane resin, 6...resin, 7...Body, 10...Bioelectrode sample, 20...Thermoplastic urethane film, 21...Double-sided tape.
Claims
1. A bioelectrode composition, comprising, as component (A), a resin having a urethane bond in its main chain and one or more salts selected from ammonium salts, sodium salts, potassium salts, and silver salts of sulfonamide in its side chains.
2. 2. The bioelectrode composition according to claim 1, wherein the component (A) is represented by the following general formula (1): [Formula 1] (In general formula (1), R 1 , R 3 R is a single bond or a linear or branched alkylene group having 1 to 6 carbon atoms, which may have an ether bond or a bromine atom. 2 R is a hydrogen atom, a hydroxyl group, a linear or branched alkyl group having 1 to 6 carbon atoms, or an alkoxy group. 4 represents a single bond or a linear, branched or cyclic hydrocarbylene group having 1 to 20 carbon atoms, which may have a carbonyl group, an ether group or an ester group; R 1 may be bonded to form a ring. 5 is a linear, branched, or cyclic alkyl group having 1 to 10 carbon atoms, which may be substituted with a fluorine atom, or an alkenyl group having 2 to 6 carbon atoms, an alkynyl group having 2 to 6 carbon atoms, or an aryl group having 6 to 10 carbon atoms, which may have a fluorine atom, a trifluoromethyl group, a cyano group, a nitro group, a hydroxy group, an alkoxy group having 1 to 6 carbon atoms, or an alkyl group having 1 to 6 carbon atoms. M + is an ammonium ion, a sodium ion, a potassium ion, or a silver ion.
3. The bioelectrode composition according to claim 1, characterized in that the component (A) contains an ammonium ion represented by the following general formula (2) as an ammonium ion constituting the ammonium salt: [Case 2] (In general formula (2), R 101d , R 101e , R 101f , and R 101g R each represents a hydrogen atom, a linear, branched, or cyclic alkyl group having 1 to 15 carbon atoms, a linear, branched, or cyclic alkenyl or alkynyl group having 2 to 12 carbon atoms, or an aromatic group having 4 to 20 carbon atoms, and may have one or more groups selected from an ether group, a carbonyl group, an ester group, a hydroxy group, an amino group, a nitro group, a sulfonyl group, a sulfinyl group, a halogen atom, and a sulfur atom. 101d and R 101e , or R 101d , R 101e and R 101f may form a ring together with the nitrogen atom to which they are attached, and when they form a ring, R 101d and R 101e , or R 101d , R 101e and R 101f is an alkylene group having 3 to 10 carbon atoms, or forms a heteroaromatic ring having the nitrogen atom in the general formula (2) in the ring.
4. 2. The bioelectrode composition according to claim 1, further comprising a resin other than the component (A) as a component (B).
5. 5. The bioelectrode composition according to claim 4, wherein the component (B) is at least one selected from the group consisting of silicone resins, (meth)acrylate resins, and urethane resins.
6. 2. The bioelectrode composition according to claim 1, further comprising, as component (C), either or both of a carbon material and a metal powder.
7. 7. The bioelectrode composition according to claim 6, wherein the carbon material is either or both of carbon black and carbon nanotubes.
8. 7. The bioelectrode composition according to claim 6, wherein the metal powder is selected from the group consisting of gold, silver, platinum, copper, tin, titanium, nickel, aluminum, tungsten, molybdenum, ruthenium, chromium, and indium.
9. 9. The bioelectrode composition according to claim 8, wherein the metal powder is silver powder.
10. 2. The bioelectrode composition according to claim 1, further comprising an organic solvent as component (D).
11. A bioelectrode having a conductive substrate and a biocontact layer formed on the conductive substrate, the bioelectrode being characterized in that the biocontact layer is a cured product of the bioelectrode composition according to any one of claims 1 to 10.
12. The bioelectrode according to claim 11, characterized in that the conductive base material contains one or more selected from gold, silver, silver chloride, platinum, aluminum, magnesium, tin, tungsten, iron, copper, nickel, stainless steel, chromium, titanium, carbon, and conductive polymers.
13. A method for manufacturing a bioelectrode having a conductive substrate and a biocontact layer formed on the conductive substrate, comprising applying a bioelectrode composition according to any one of claims 1 to 10 onto the conductive substrate and curing the composition to form the biocontact layer.
14. The method for manufacturing a bioelectrode according to claim 13, characterized in that the conductive base material contains one or more selected from gold, silver, silver chloride, platinum, aluminum, magnesium, tin, tungsten, iron, copper, nickel, stainless steel, chromium, titanium, carbon, and conductive polymers.
Citation Information
Patent Citations
New diol sulfonic acid quaternary ammonium salt and polyurethane resin containing the same compound as diol component
JP2001048858A
Hydrophilic polymer composition
JP2001348496A
Biomedical electrode composition, biomedical electrode, and manufacturing method of biomedical electrode
JP2019076696A
Bio-electrode composition, bio-electrode, and method for manufacturing bio-electrode
JP2020000851A
Bioelectrode composition, bioelectrode, manufacturing method of bioelectrode, and silicon material particles
JP2022048991A