Seal material, seal member for compressor, cup seal for reciprocation compressor, and chip seal for scroll type compressor

The PTFE resin composition with zinc-based powder and additives improves wear resistance and non-aggressiveness, addressing appearance and performance issues in compressors, ensuring stable sealing and extended equipment life.

JP2024137934APending Publication Date: 2024-10-07NTN CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024047374
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-12-20
Filing Date
2024-03-22
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

Conventional PTFE resin compositions used in compressors face issues with wear resistance and non-aggressiveness to mating materials, particularly under high surface pressure and non-lubricated conditions, with materials like copper and bronze causing appearance concerns and instability.

Method used

A PTFE resin composition containing zinc-based powder, copper-zinc alloy powder, molybdenum disulfide, and carbon fiber, with specific mass percentages and particle sizes, to enhance wear resistance and non-aggressiveness, forming a transfer film on the mating material surface.

Benefits of technology

The composition provides excellent wear resistance and non-aggressiveness, maintaining sealing performance and extending equipment life without lubrication, while avoiding color unevenness and reducing maintenance frequency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137934000001_ABST
    Figure 2024137934000001_ABST
Patent Text Reader

Abstract

To provide a seal material which is generally usable and is composed of a PTFE resin composition excellent in abrasion resistance and non-attack property to a counter part, a seal material for a compressor which is composed of the seal material, a cup seal for a reciprocation compressor which is composed of the seal material, and a chip seal for a scroll type compressor which is composed of the seal material.SOLUTION: A seal material composed of a polytetrafluoroethylene resin composition contains a polytetrafluoroethylene resin as a base resin, and contains zinc-based powder (metal zinc powder or copper zinc alloy powder), wherein a content of zinc to the total amount of the polytetrafluoroethylene resin composition is 1.0 mass% to 10 mass%, and an average particle diameter of the zinc-based powder is 5.0 μm to 80 μm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sealing material, a compressor sealing member, a cup seal for a reciprocating compressor, and a tip seal for a scroll-type compressor, each made of a polytetrafluoroethylene (PTFE) resin composition for use in a compressor that compresses and expands a gas such as air or a refrigerant. [Background technology]

[0002] For example, in a compressor, a seal member is used to seal a compression chamber in an unlubricated (dry) state without lubricating oil. Conventionally, as a material for such a seal member used in an unlubricated state, a PTFE resin composition has been used in which a PTFE resin having self-lubricating properties is used as a base resin and various fillers are mixed to impart abrasion resistance and the like.

[0003] For example, Patent Document 1 discloses a PTFE resin composition as a non-lubricant seal material, in which bronze powder (component Cu:Sn=9:1), carbon fiber, and molybdenum disulfide are simultaneously filled into a synthetic resin material containing PTFE resin. It is said that the use of this PTFE resin composition can suppress the self-wear and aggressiveness to mating materials in the non-lubricant seal material.

[0004] On the other hand, in Patent Document 2, the conventional sealing material containing bronze powder is exposed to high temperatures due to compression heat from the compression chamber and frictional heat, and the strength is reduced, accelerating wear, resulting in a shortened lifespan. The seal material is designed to have a thermal conductivity of 300 W m -1 ·K -1 The PTFE resin composition is disclosed, which contains the above powder material, carbon fiber, molybdenum disulfide, and PTFE resin. It also has a thermal conductivity of 300 W·m -1 ·K -1 It is disclosed that the powder material is one selected from the group consisting of copper, gold, and silver.

[0005] Furthermore, there are techniques described in Patent Document 3, Patent Document 4, etc., regarding materials for cup seals for conventional reciprocating compressors. Patent Document 3 describes that the seal is formed from a composite material in which CF (carbon fiber) and MoS2 (molybdenum disulfide) are appropriately mixed with a fluororesin material based on PTFE resin. Meanwhile, Patent Document 4 describes that the cup seal of Patent Document 3 has a problem in that when the rocking piston slides up and down along the inner peripheral surface of the cylinder and rocks left and right, the lip part is strongly pressed against the inner surface of the cylinder while repeating sliding displacement, and therefore the durability and life of the seal lip cannot necessarily be sufficiently ensured, and describes that the seal is formed from a composite material containing petroleum pitch-based graphitized carbon fiber, a powder material made of copper or copper alloy, molybdenum disulfide, and PTFE resin.

[0006] Furthermore, regarding materials for tip seals for conventional scroll compressors, there are techniques described in Patent Document 5, Patent Document 6, etc. Patent Document 5 describes a material that is mainly composed of PTFE resin or modified PTFE resin and is filled with at least 10 to 30 weight % of bronze, 5 to 20 weight % of carbon fiber or spherical carbon, and 1 to 10 weight % of molybdenum disulfide. Patent Document 6 describes a material that contains PTFE resin, 5 to 25 weight % of spherical copper powder, 5 to 20 weight % of pitch-based carbon fiber, and 1 to 10 weight % of molybdenum disulfide. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 6-109139 [Patent Document 2] JP 2005-264049 A [Patent Document 3] Japanese Patent Application Publication No. 10-148178 [Patent Document 4] JP 2006-283643 A [Patent Document 5] JP 2001-165072 A [Patent Document 6] JP 2004-210885 A Summary of the Invention [Problem to be solved by the invention]

[0008] As described above, abrasion resistance and non-aggression to mating materials are particularly required for sealing materials made of a PTFE resin composition used in, for example, compressors. -1 ·K -1 Although the above powder materials are used to improve wear resistance, gold and silver are expensive and difficult to use as a general-purpose sealing material. On the other hand, copper is easily discolored, and turns black when fired during compression molding, causing color unevenness in the appearance of the molded body, so there are concerns that it contains unstable elements in its commercial value and is difficult to use as a sealing material. In addition, the cup sealing material of Patent Document 4 and the chip sealing materials of Patent Documents 5 and 6 require a powder material made of copper or bronze (copper alloy) as an essential component, and there are similar concerns about appearance.

[0009] In recent years, scroll compressors have been developed to be more energy-efficient, more powerful, and more compact, and there is a demand for improved wear resistance in high-speed and high-load regions for tip seals used in the scroll orbiting parts of scroll compressors. The number of non-lubricated compressors produced is also increasing. The tip seal materials described in Patent Documents 5 and 6 may not have sufficient wear resistance and non-aggressiveness to mating materials under high surface pressure or non-lubricated conditions.

[0010] The present invention has been made in view of the above circumstances, and aims to provide a sealing material made of a PTFE resin composition that can be used for general purposes as a sealing material for compressors, etc., and that has excellent abrasion resistance and non-aggression toward mating materials even under non-lubricated conditions, and a compressor sealing material, a cup seal for a reciprocating compressor, and a tip seal for a scroll compressor made of the sealing material. In the present invention, "sealing material" means a part, and "sealing material" means a material. [Means for solving the problem]

[0011] The sealing material of the present invention is characterized in that it comprises a PTFE resin composition, has a PTFE resin as a base resin, contains zinc-based powder, has a zinc content of 1.0 mass% to 10 mass% relative to the total amount of the PTFE resin composition, and the zinc-based powder is metallic zinc powder or copper-zinc alloy powder.

[0012] The copper-zinc alloy powder is characterized in that the zinc content is 10% by mass to 50% by mass.

[0013] The PTFE resin composition is characterized in that it contains 2.0% by mass to 10% by mass of molybdenum disulfide and 2.0% by mass to 15% by mass of carbon fiber based on the total amount of the PTFE resin composition.

[0014] The PTFE resin composition is characterized in that the content by mass of the zinc-based powder is greater than the contents of the molybdenum disulfide and the carbon fiber.

[0015] The PTFE resin composition is characterized in that it does not contain any inorganic filler other than the zinc-based powder, the molybdenum disulfide, and the carbon fibers.

[0016] The zinc-based powder is characterized in that its average particle size is 5.0 μm to 80 μm.

[0017] The copper-zinc alloy powder has a zinc content of 10% by mass to 50% by mass, and the PTFE resin composition contains, relative to the total amount of the PTFE resin composition, 10% by mass to 30% by mass of the copper-zinc alloy powder, 2.0% by mass to 5.0% by mass of molybdenum disulfide, and 2.0% by mass to 8.0% by mass of carbon fiber, and the copper-zinc alloy powder has an average particle size of 25 μm to 80 μm.

[0018] The compressor seal of the present invention is characterized in that it is made of the seal material of the present invention. The seal of the present invention is characterized in that it is a non-lubricated seal.

[0019] The cup seal for a reciprocating compressor of the present invention is used in a reciprocating compressor having a piston and a cylinder, which compresses gas by the reciprocating motion of the piston, and is a cup seal that is fixed to the piston and press-fitted into the inner diameter of the cylinder to provide an air-tight seal between the piston and the cylinder, and is characterized in that the cup seal is made of the sealing material of the present invention.

[0020] The tip seal for a scroll-type compressor of the present invention is a spiral-shaped tip seal for sealing a compression chamber formed between a fixed scroll and a movable scroll, which are scroll members in a scroll-type compressor, and is characterized in that the tip seal is made of the sealing material of the present invention. Effect of the Invention

[0021] The sealing material made of the PTFE resin composition of the present invention contains zinc-based powder, and the zinc content relative to the total amount of the PTFE resin composition is 1.0 mass% to 10 mass%, so that it is more excellent in abrasion resistance and non-aggression to the mating material, as shown in the examples described later. By using zinc-based powder, a transfer film of the zinc component is formed on the surface of the mating material, and the aggressiveness of damaging the surface of the mating material can be suppressed. In addition, zinc-based powder (for example, metal zinc powder or copper-zinc alloy powder) does not discolor when fired during compression molding of the PTFE resin composition, so that color unevenness does not occur in the appearance of the product and the commercial value is not impaired. Furthermore, it is cheaper than gold or silver, so that the product price does not become expensive and it can be used universally.

[0022] Since the zinc-based powder is a copper-zinc alloy powder, it has a better reinforcing effect for the sealing material and a better heat dissipation effect for heat generated by sliding than metallic zinc powder. Furthermore, the zinc content in the copper-zinc alloy powder is 10% by mass to 50% by mass, and the zinc content relative to the total amount of the PTFE resin composition is 1.0% by mass to 10% by mass, so that the reinforcing effect for the sealing material and the heat dissipation effect for heat generated by sliding are even better. Note that metallic zinc powder is a powder consisting of zinc with a purity of 98% or more, and is sometimes referred to as pure zinc powder in this specification.

[0023] The PTFE resin composition contains 2.0 mass % to 10 mass % of molybdenum disulfide and 2.0 mass % to 15 mass % of carbon fiber, based on the total amount of the PTFE resin composition, and therefore can suitably improve the lubricating properties and mechanical strength of the sealing material.

[0024] Since the zinc-based powder has an average particle size of 5.0 μm to 80 μm, it is easily dispersed uniformly in the compact, and the effect of the zinc-based powder can be stably exerted.

[0025] The sealing material and compressor seal member of the present invention are made of a specific PTFE resin composition, and therefore have excellent abrasion resistance and non-aggression to mating materials, even when used in an unlubricated state, leading to maintenance of sealing properties and improved life span of devices such as compressors that use the sealing material, and contributing to reduced maintenance frequency.

[0026] The cup seal for a reciprocating compressor of the present invention is made of the sealing material of the present invention, that is, the base resin is PTFE resin, and the zinc content relative to the total amount of the PTFE resin composition is 1.0 mass% to 10 mass%, so that a transfer film of the zinc component is formed on the sliding surface of the inner wall of the cylinder, which is the mating material, and the aggressiveness of damaging the surface of the mating material can be suppressed. In addition, the PTFE resin composition does not discolor when baked during compression molding, and color unevenness does not occur in the cup seal. In addition, the zinc component is present in zinc metal alone or a copper-zinc alloy, and is uniformly dispersed in the cup seal, so that a transfer film of the zinc component is easily formed on the inner wall of the cylinder during sliding. In addition, the strength of the cup seal can be improved by filling the base resin with carbon fiber, and the stability against wear of the cup seal can be imparted by filling the base resin with molybdenum disulfide.

[0027] The tip seal for scroll compressors of the present invention is made of the sealing material of the present invention, that is, the base resin is PTFE resin, and the zinc content relative to the total amount of the PTFE resin composition is 1.0 mass% to 10 mass%, so that a transfer film of the zinc component is formed on the sliding surface of the bottom surface (end plate) of the scroll wrap, which is the mating material, and the aggressiveness of damaging the surface of the mating material can be suppressed. In addition, the PTFE resin composition does not discolor when baked during compression molding, and color unevenness does not occur in the tip seal. In addition, the zinc component is present in zinc metal alone or a copper-zinc alloy, and is uniformly dispersed in the tip seal, so that a transfer film of the zinc component is easily formed on the bottom surface of the scroll wrap during sliding. In addition, the strength of the tip seal can be improved by filling the base resin with carbon fiber, and the stability against wear of the tip seal can be imparted by filling the base resin with molybdenum disulfide. [Brief description of the drawings]

[0028] [Figure 1] 1 is a partial cross-sectional view of a reciprocating compressor to which the cup seal for a reciprocating compressor of the present invention is applied. [Diagram 2] FIG. 2 is a cross-sectional view showing an example of a cup seal for a reciprocating compressor according to the present invention. [Diagram 3] FIG. 2 is a partial cross-sectional view of a compression mechanism of a scroll compressor. [Figure 4] 1 is a plan view showing an example of a tip seal for a scroll compressor according to the present invention. FIG. [Diagram 5] FIG. 1 is a schematic diagram of a ring-on-disc test machine (ring-on-disc test 1). [Figure 6] FIG. 1 is a schematic diagram of a ring-on-disc test machine (ring-on-disc test 2). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] As described above, in the past, a resin composition containing bronze (copper-tin alloy) powder, molybdenum disulfide, and carbon fiber was known as a sealing material made of a PTFE resin composition. In order to further improve performance, the present inventors conducted intensive research. As a result, it was surprisingly found that when a zinc-based powder that can be used for general purposes is mixed with a predetermined zinc content, the wear resistance and non-aggression to the mating material can be further improved compared to the case where a conventional bronze powder is mixed. In addition, it was found that a transfer film of the zinc component is formed on the sliding surface of the mating material by containing a predetermined amount of zinc. The present invention is based on such findings.

[0030] The sealing material of the present invention contains a PTFE resin as a base resin and a zinc-based powder as an essential component.

[0031] In the present invention, the PTFE resin used as the base resin can be a general PTFE resin represented by -(CF2-CF2)n-. In addition, a perfluoroalkyl ether group (-C p F 2p -O-) (p is an integer from 1 to 4) or polyfluoroalkyl group (H(CF2) q Modified PTFE resins into which q is an integer of 1 to 20 has been introduced can also be used.

[0032] These PTFE resins and modified PTFE resins may be obtained by either the suspension polymerization method for obtaining general molding powders or the emulsion polymerization method for obtaining fine powders. As the PTFE resin, powder obtained by heating and sintering the PTFE resin at or above its melting point, or powder obtained by irradiating the heated and sintered powder with gamma rays or electron beams, etc., may also be used.

[0033] The sealing material of the present invention has a PTFE resin content of, for example, 60% by mass to 95% by mass. The PTFE resin content is preferably 65% ​​by mass or more, more preferably 70% by mass or more, and is preferably 90% by mass or less, more preferably 80% by mass or less.

[0034] The sealing material of the present invention contains a zinc-based powder, and the zinc content relative to the total amount of the PTFE resin composition is 1.0% by mass to 10% by mass. By setting the zinc content within this range, the cost increase of the entire PTFE resin composition can be suppressed, while the self-wear property and the attacking property of the counterpart can be improved by forming a transfer film of the zinc component to the counterpart material. The zinc content relative to the total amount of the PTFE resin composition is preferably 2.0% by mass to 10% by mass, more preferably 3.0% by mass to 10% by mass, and may be 3.0% by mass to 8.0% by mass. The higher the zinc content, the easier it is to improve the wear resistance, etc., but if the zinc content is the same, the zinc alloy powder has a higher wear resistance effect than pure zinc powder.

[0035] As the zinc-based powder, a powder of metallic zinc (metallic zinc powder) or an alloy powder containing zinc as an ingredient (zinc alloy powder) can be used. The zinc-based powder can be used alone or in combination of two or more kinds. For example, a combination of metallic zinc powder and zinc alloy powder can be used. The zinc-based powder can be prepared by gas atomization or the like, or a commercially available product can be used.

[0036] As the zinc alloy powder, copper-zinc alloy powder, zinc-aluminum alloy powder, zinc-magnesium alloy powder, zinc-tin alloy powder, etc. can be used. These alloy powders may further contain a third compounding element. Among these, it is preferable to use copper-zinc alloy powder.

[0037] The content of zinc contained in the copper-zinc alloy powder is not particularly limited, but is, for example, 10% by mass to 50% by mass. From the viewpoint of efficiently increasing the zinc content in the PTFE resin composition while suppressing the blending amount of the copper-zinc alloy powder, the content of zinc contained in the copper-zinc alloy powder is preferably 20% by mass to 45% by mass, and may be 20% by mass to 40% by mass. The copper-zinc alloy powder may further contain a third blending element such as iron (Fe), tin (Sn), or nickel (Ni).

[0038] The zinc-based powder may be in various shapes, such as spherical or scaly. The spherical shape is preferred because it has good fluidity and can be easily dispersed uniformly in the PTFE resin composition. The average particle diameter (D 50 ) is not particularly limited, but may be, for example, 5.0 μm to 100 μm, or 5.0 μm to 80 μm. When a zinc metal powder is used as the zinc-based powder, the average particle diameter is, for example, 5.0 μm to 20 μm, and when a zinc alloy powder is used, the average particle diameter is, for example, 25 μm to 80 μm.

[0039] Average particle size of zinc-based powder (D 50 ) is the particle size at which the cumulative value reaches 50% when the particle size distribution is considered as a cumulative distribution, and can be measured using a particle size distribution measuring device that uses the laser light scattering method.

[0040] The zinc-based powder is blended with the PTFE resin composition so that the zinc content in the resin composition is 1.0% by mass to 10% by mass. If the content of the zinc-based powder is greater than a certain amount, the effect of wear resistance will plateau and begin to decline, so the content of the zinc-based powder is preferably 25% by mass or less with respect to the total amount of the PTFE resin composition. When a metal zinc powder is used as the zinc-based powder, the content is, for example, 1.0 to 10% by mass with respect to the total amount of the PTFE resin composition, and when a zinc alloy powder is used, the content is, for example, 5% by mass to 25% by mass with respect to the total amount of the PTFE resin composition. The zinc alloy powder is preferably 10% by mass to 25% by mass, more preferably 15% by mass to 25% by mass. The content of the zinc-based powder may be greater than the content of each of the other fillers (excluding the base resin).

[0041] The sealing material of the present invention is preferably blended with molybdenum disulfide together with zinc-based powder. Molybdenum disulfide has a layered lattice structure and can be easily sheared into thin layers by sliding motion, thereby reducing frictional resistance. As molybdenum disulfide, commercially available products can be used, and powdered products can be used.

[0042] The content of molybdenum disulfide relative to the total amount of the PTFE resin composition is, for example, 2.0 mass% to 20 mass%, preferably 2.0 mass% to 10 mass%, may be 2.0 mass% to 8.0 mass%, or may be 2.0 mass% to 5.0 mass%.

[0043] The sealing material of the present invention preferably further contains a fibrous filler, which can improve the mechanical strength of the molded article (sealing member).

[0044] As the fibrous filler, for example, glass fiber, carbon fiber, aramid fiber, potassium titanate whisker, etc. can be used. Among these, it is preferable to use carbon fiber. The carbon fiber may be either pitch-based or PAN-based, which are classified based on the raw material. The firing temperature is not limited, and may be either a graphitized product fired at a high temperature of 2000°C or higher, or a carbonized product fired at about 1000 to 1500°C. In addition, either chopped fiber or milled fiber may be used, but it is preferable to use milled fiber with a short fiber length from the viewpoint of friction and wear properties.

[0045] The average fiber length of the fibrous filler is not particularly limited, but is preferably short fiber of 20 μm to 200 μm. For example, if the average fiber length is less than 20 μm, it is difficult to obtain the effect of improving wear resistance, and if it exceeds 200 μm, carbon fibers broken during sliding tend to get into the sliding surface, causing damage and wear to the counter material. Note that the average fiber length in this specification is a number-average fiber length.

[0046] The content of the carbon fiber relative to the total amount of the PTFE resin composition is, for example, 2.0% by mass to 20% by mass, preferably 2.0% by mass to 15% by mass, may be 2.0% by mass to 10% by mass, or may be 2.0% by mass to 8.0% by mass. The content of the carbon fiber may be higher than the content of the molybdenum disulfide.

[0047] The sealing material of the present invention may be composed only of PTFE resin, zinc-based powder, molybdenum disulfide, and fibrous filler, or may further contain known fillers to the extent that the effect of the present invention is not impaired. Specifically, inorganic fillers such as other metal powders not containing zinc, graphite, tungsten disulfide, coke powder, and colorants (carbon black, iron oxide, titanium oxide, etc.), and organic fillers such as resin powders (polyphenylene sulfide resin, polyether ether ketone resin, polyimide resin, fluororesin other than PTFE resin, etc.) may be contained.

[0048] A more specific embodiment of the sealing material of the present invention is a form in which the base resin is PTFE resin, the zinc-based powder (metallic zinc powder or copper-zinc alloy powder), molybdenum disulfide, and carbon fiber are contained, the zinc content is 1.0% by mass to 10% by mass (preferably 2.0% by mass to 10% by mass) relative to the total amount of the PTFE resin composition, and the molybdenum disulfide is 2.0% by mass to 10% by mass and the carbon fiber is 2.0% by mass to 15% by mass relative to the total amount of the PTFE resin composition. In this embodiment, the content of the zinc-based powder may be greater than the respective contents of molybdenum disulfide and carbon fiber, and more specifically, the order of the molybdenum disulfide content may be greater than the carbon fiber content.

[0049] The PTFE resin composition according to the present invention can be produced by a known method, for example, by mixing a PTFE resin, a zinc-based powder, molybdenum disulfide, and other fillers, which are added as necessary, in a Henschel mixer, an axial mixer, a ball mixer, a ribbon blender, or the like.

[0050] The sealing material of the present invention can be prepared by forming the PTFE resin composition into a columnar, ring, cylindrical, tubular or other shape by compression molding, and then machining the same into the desired product shape.

[0051] The sealing material of the present invention can be used, for example, as a piston ring for compressors such as refrigerators, piston rings for expanders, gas seals, sealing members for compressors for air conditioners, cup seals for reciprocating compressors, and tip seals for scroll compressors. The sealing material is effective as an air seal in an atmospheric environment, but is also expected to be effective in nitrogen gas, hydrocarbon gas, and hydrogen gas environments. It is also effective under oil lubrication, but is more effective than conventional products under non-lubrication conditions.

[0052] Fig. 1 is a partial cross-sectional view of a reciprocating compressor to which the cup seal of the present invention is applied, in which the cup seal 1 is made of the sealing material of the present invention.

[0053] The reciprocating compressor 2 is a compressor that sucks, compresses, and discharges gas by reciprocating a piston 4. The reciprocating compressor 2 includes a substantially cylindrical cylinder 3 (made of aluminum, for example) having a hollow portion, a substantially columnar piston 4 that is provided in the cylinder 3 so as to be capable of reciprocating while swaying, a cup seal 1 fixed to the piston 4, a suction valve 5, and a discharge valve 6. A pressure chamber 7 is formed between a cylinder head 3a located at the upper end of the cylinder 3 and one end of the piston 4. The reciprocating compressor 2 includes a drive means (not shown) on the other end side of the piston 4 that reciprocates the piston 4 in the axial direction while swaying. The drive means is, for example, a crankshaft that performs eccentric rotational motion in association with the rotation of a rotating shaft. The drive means causes the piston 4 to reciprocate in the directions indicated by the arrows X and Y in FIG. 1.

[0054] The cup seal 1 is a dish-shaped annular member having a through hole in the central shaft portion, and is sandwiched in a piston groove formed by a connecting rod 8 and a retainer 9, and is fastened and fixed by a fastener 10. When the piston 4 reciprocates, the outer peripheral surface of the lip portion of the cup seal 1 slides against the inner peripheral surface of the cylinder 3. Even when the cup seal 1 is used in an unlubricated state, by using the sealing material of the present invention, it is possible to exhibit excellent wear resistance while maintaining self-lubricating properties with excellent sliding properties, and further reduce aggressiveness to the inner peripheral surface of the cylinder 3.

[0055] As shown in Fig. 2, the cup seal 1 has an annular flat portion 1a provided on the inner periphery and a lip portion 1b provided on the outer periphery and curved so as to protrude from the flat portion 1a to one side in the axial direction. When the cup seal 1 is attached to the reciprocating compressor 2 (see Fig. 1), the flat portion 1a is fixed to the piston groove, and the lip portion 1b is bent and abuts against the inner periphery of the cylinder.

[0056] For example, the cup seal 1 is formed by drawing a hollow disk-shaped washer obtained by machining a cylindrical material produced by compression molding or ram extrusion molding using the sealing material of the present invention. In the drawing process, the outer periphery of the washer is bent toward one side in the axial direction to form the lip portion 1b.

[0057] Next, the structure of the compression mechanism of the scroll compressor to which the chip seal for scroll compressor of the present invention is applied will be described with reference to FIG. 3. FIG. 3 is a partial cross-sectional view of the compression mechanism of the scroll compressor. As shown in FIG. 3, the scroll compressor includes a fixed scroll 14 having a base plate 14a and a spiral wall 14b standing upright on the surface thereof, and a movable scroll 15 having a base plate 15a and a spiral wall 15b standing upright on the surface thereof. The fixed scroll 14 and the movable scroll 15 are eccentrically engaged with each other at a spiral wall boundary 16, and a compression chamber 12 is formed therebetween. The movable scroll 15 revolves around the axis of the fixed scroll 14, and the compression chamber 12 moves toward the center of the spiral shape, thereby compressing gas or the like. A seal groove 13 is formed on the tooth tip surface of the spiral shape tip of the fixed scroll 14 and the movable scroll 15 along the extension direction of the spiral. The chip seal 11 is accommodated in the seal groove 13 and is in sliding contact with the opposing scroll base plate to ensure the hermeticity of the compression chamber 12.

[0058] An example of the tip seal for a scroll compressor of the present invention will be described with reference to FIG. 4. FIG. 4 is a plan view of the tip seal as viewed from the sliding surface side with the mating scroll member that serves as the sealing surface. The tip seal 11 is a seal member for sealing a compression chamber formed between the scroll members, a fixed scroll and a movable scroll, in a scroll compressor. As shown in FIG. 4, the tip seal 11 has a spiral shape in which a long member with a substantially rectangular cross section is wound into a spiral. This spiral shape has a gradually increasing radius of curvature from the start end 11a to the end end 11b. The sliding surface 11c is a sliding surface with the opposing scroll base plate, and serves as a seal surface that seals gas and the like in the compression chamber. The wrap bottom surface of the opposing scroll base plate is, for example, an aluminum alloy that has been anodized.

[0059] The sealing material of the present invention is also a method of sliding a molded body made of a PTFE resin composition having a PTFE resin as a base resin, containing zinc-based powder, and having a zinc content of 1.0 mass% to 10 mass% based on the total amount of the PTFE resin composition against a counter material to form a transfer film containing a zinc component on the sliding surface of the counter material. The formation of the transfer film containing a zinc component can be confirmed by SEM / EDX (energy dispersive X-ray spectroscopy) or the like. EXAMPLES

[0060] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the following examples.

[0061] Examples 1 to 7, Comparative Examples 1 to 6 The following raw materials were weighed out in the blending ratio shown in Table 1 and dry-mixed to obtain a PTFE resin composition. The obtained PTFE resin composition was used to produce a molded body A of φ30×100 mm by compression molding (free sintering, compression 50 MPa, baking 370°C×4 hours (in air)), and then a ring test piece A (φ17×φ21×t3 mm) to be subjected to ring-on-disc test 1 was prepared. Before processing into the ring test piece A, the appearance of the molded body A was visually observed to confirm the presence or absence of a change in hue. Separately, a molded body B of φ14×φ25×100 mm was produced by compression molding (free sintering, compression 50 MPa, firing 370°C × 4 hours (in air)), and then a ring test piece B (φ17×φ21×t4 mm) was prepared for ring-on-disk test 2. Before processing into ring test piece B, the appearance of molded body B was visually observed to confirm the presence or absence of a change in color. Separately, a φ40×φ76×100mm compact was produced by compression molding (free sintering, compression 50MPa, firing 370℃×4 hours (in air)), and then a hollow disk-shaped washer with a thickness of 1mm obtained by machining was drawn to produce a cup seal (φ44×φ61×t6.5mm) with the shape shown in Figure 2. The appearance of the cup seal was also visually observed to check for color unevenness, and the results are shown in Table 1.

[0062] (1)PTFE resin Mitsui Chemours Fluoroproducts Co., Ltd.: Teflon 7-J (2) Metallic zinc powder (Zn100%) Fujifilm Wako Pure Chemical Corporation: Average particle size 6μm~9μm (3) Copper-zinc alloy 1 (Zn20% + Cu80%): irregular shape (water atomized powder) Fukuda Metal Foil & Powder Co., Ltd.: Bra-At(Zn20)-100: average particle size 35μm~55μm (4) Copper-zinc alloy 2 (Zn30% + Cu70%): irregular shape (water atomized powder) Nippon Atomize Co., Ltd.: BRASSPOWER BS7030: Average particle size 45μm~63μm (5) Copper-zinc alloy 3 (Zn40% + Cu60%): Irregular shape (water atomized powder) Nippon Atomize Co., Ltd.: BRASSPOWER BS6040: Average particle size 45μm~63μm (6) Copper-tin alloy 1 (Sn9%+Cu91%): Irregular shape (water atomized powder) Nippon Atomization Co., Ltd.: BRONZEPOWER S91-120: Average particle size 35μm~55μm (7) Copper-tin alloy 2 (Sn10% + Cu90%): spherical (gas atomized powder) Fukuda Metal Foil & Powder Co., Ltd.: Bro-At-100: average particle size 35μm~55μm (8) Carbon fiber 1 (PAN type) Toray Industries, Inc.: Milled Fiber MLD-30 (9) Carbon fiber 2 (pitch-based) Kureha Corporation: M-101S (10) Molybdenum disulfide DuPont Toray Specialty Materials Co., Ltd.: MOLYKOTE® Z Powder

[0063] <Ring-on-disc test 1> The obtained ring test piece A was subjected to a ring-on-disk type wear test shown in Fig. 5. The ring test piece A21 was fixed unrotatably to the surface of the rotating disk A22 of the testing machine and pressed with a predetermined surface pressure, while the rotating disk A22 was rotated. The test conditions were as follows. An aluminum alloy disk on which an anodized aluminum coating 23 was formed was used as the rotating disk A22 (mating material). (Test conditions) Speed:112m / min Surface pressure: 1MPa Lubrication: No lubrication (dry) Temperature: 80℃ Time: 50 hours

[0064] After the test was completed, the height of ring test piece A was measured, and the difference from the initial dimension was recorded as the amount of wear. The damage depth on the sliding surface of rotating disk A was also measured using a contact type surface roughness measuring device. The sliding surface of rotating disk A was then inspected using SEM / EDX. The SEM used was manufactured by JEOL Ltd., and the EDX used was manufactured by Horiba Ltd. The focus was on the sliding surface, and the measurement magnification was 200x. The results are shown in Table 1.

[0065] <Actual machine testing> The obtained cup seal was attached to a reciprocating air compressor (actual test machine) as shown in Figure 1, and a wear test was performed. The actual test machine has two stages, a primary compression and a secondary compression, and the cup seal (test piece) was attached to the piston on the primary compression side, and normal operation was performed with the primary compression outlet open. This actual test machine has a pressure control range of about 2.5 MPa to about 4.4 MPa, an air tank capacity of 8 L, and is a commercially available air compressor for construction tools used for nailing at construction sites. The test conditions are as follows. The surface pressure was measured by inserting a pressure gauge into the pipe connecting the primary compression and the secondary compression. The mating material was an anodized cylinder, and the test was performed by replacing it with a new one along with each test piece. (Test conditions) Rotational speed: 2450 rpm Speed: 68.6m / min Stroke: ±14mm Surface pressure: 0.13MPa Lubrication: No lubrication Time: 336 hours (continuous operation)

[0066] After the test, the thickness of the lip of the cup seal was measured with a rod-and-spherical micrometer, and the difference from the initial dimension was recorded as the amount of wear. The depth of damage to the sliding surface of the cylinder was also measured with a contact type surface roughness tester. The results are shown in Table 1.

[0067] <Ring-on-disc test 2> The obtained ring test piece B was subjected to a ring-on-disk type wear test shown in FIG. 6. In order to simulate the actual movement of a scroll compressor, the ring test piece B24 was attached with its center intentionally offset from the center of a rotating disk B25 (mating material) made of an aluminum alloy on which an anodized aluminum coating 26 was formed. The ring test piece B24 was pressed rotatably against the surface of the rotating disk B25 with a predetermined surface pressure (1 MPa) without being fixed, and the rotating disk B25 was rotated at a speed of 2.6 m / sec. Other test conditions were as follows. (Test conditions) Lubrication: No lubrication (dry) Temperature: 120℃ Time: 50 hours

[0068] After the test, the height of the ring test piece B was measured, and the difference from the initial dimension was recorded as the amount of wear, in the same manner as in the ring-on-disk test 1. The damage depth of the sliding surface of the rotating disk B was also measured. The results are shown in Table 1.

[0069] [Table 1]

[0070] As shown in Table 1, no change in hue or color unevenness was observed in any of the molded articles (molded article A, molded article B, and cup seal) made of the PTFE resin composition containing zinc-based powder in Examples 1 to 7 and Comparative Example 1. The molded articles (molded article A, molded article B, and cup seal) in Comparative Examples 2 to 5 were discolored black due to the influence of the copper-tin alloy, had darker areas, and color unevenness (light and dark) was observed.

[0071] In the ring-on-disk test 1, the wear amount after 50 hours of the ring test piece A made of the PTFE resin composition of Examples 1 to 7 was 35 μm or less, and no damage was observed on the sliding surface of the rotating disk A in Examples 1 to 6. In Example 7, minor damage of 3 μm in depth was observed on the rotating disk A.

[0072] In contrast, the wear amount of the ring test piece A made of the PTFE resin composition of Comparative Examples 1, 2, 4, and 6 exceeded 60 μm, and a clear difference in wear amount from the Examples was observed. The rotating disk A of Comparative Example 1 had significant damage to the sliding surface. Similarly, the rotating disk A of Comparative Example 2 and Comparative Example 4 had significant damage to the sliding surface. Comparative Example 2 and Comparative Example 4 contained bronze powder, which has traditionally been used as a filler, but the self-wear amount was also inferior to that of the case where zinc-based powder was used.

[0073] When the sliding surface was examined by SEM / EDX, it was found that a zinc component coating was formed on the sliding surface of the rotating disk A of Examples 1 to 7. The amount of the zinc component coating in Example 7 was small compared to Examples 1 to 6. In Comparative Example 1, no zinc component coating was detected on the sliding surface. In Comparative Examples 2 and 4, no transfer of the bronze component to the surface of the rotating disk A was observed.

[0074] In the actual machine test, the wear amount of the cup seals made of the PTFE resin composition of Examples 1 to 7 was 0.1 mm or less, and no damage to the mating material was observed. On the other hand, the wear amount of the cup seals made of the PTFE resin composition of Comparative Examples 1, 2, 4, and 6 exceeded 0.1 mm, and a difference in wear amount from the Examples was observed. Damage to the sliding surface was observed in the cylinder of Comparative Example 1, and damage to the cylinder sliding surface was more significant in Comparative Examples 2 and 4 than in Comparative Example 1.

[0075] In addition, in the ring-on-disk test 2, the wear amount after 50 hours of the ring test piece B made of the PTFE resin composition in Examples 1 to 7 was 45 μm or less, and damage to the sliding surface of the rotating disk B was not observed in Examples 1 to 5. In Example 6, minor damage was observed to the rotating disk B with a depth of 3 μm, and in Example 7, minor damage was observed to the rotating disk B with a depth of 4 μm.

[0076] In contrast, the wear amount of the ring test piece B made of the PTFE resin composition in Comparative Examples 1 to 6 exceeded 80 μm, and a clear difference in the wear amount from the Examples was observed. In particular, in Comparative Examples 2 to 6, which did not contain a zinc component, the wear amount of the ring test piece B exceeded 90 μm, and the difference from the Examples was remarkable.

[0077] Damage to the sliding surface of the rotating disk B was not observed in Examples 1 to 5.

[0078] The damage to the sliding surface of the rotating disk B in Comparative Example 1 was greater than that of the Example. Similarly, in Comparative Examples 2 to 6, the damage to the sliding surface of the rotating disk B was significant.

[0079] From the above test results, it is presumed that the reason why the wear of the ring test pieces A, B and the cup seal in Examples 1 to 7 is minor is that the zinc component coating formed on the sliding surface of the mating material (rotating disks A, B and cylinder) serves as a protective film for the mating material, making the surface of the mating material less likely to be damaged and less likely to cause abrasive wear during sliding. The sliding surfaces of the mating materials in Comparative Examples 1 to 6 do not form transfer films of zinc components or bronze components, and are significantly damaged and the damage depth is also larger than in the Examples. Therefore, it is presumed that abrasive wear is promoted and the wear of the ring test pieces A, B and the cup seal becomes large. In addition, although the PTFE resin composition in Example 1 contains a large amount of zinc components, the wear amount is larger than that in Examples 2 to 5. This is presumed to be because the reinforcing effect of the metal zinc powder on the PTFE resin composition and the heat dissipation effect of the sliding heat generation are lower than those of the copper-zinc alloy powder. [Industrial Applicability]

[0080] The sealing material made of the PTFE resin composition of the present invention can be used for general-purpose sealing materials, etc., and is excellent in abrasion resistance and non-aggression to mating materials, so that it can be suitably and widely used as a non-lubricated sealing material for compressors that compress and expand gases, refrigerants, etc., for example. The cup seal for reciprocating compressors of the present invention can be used as a cup seal for use in, for example, compressors for construction machinery, compressors for supplying air to factories, and medical oxygen concentrators, leading to maintenance of sealing properties and improvement of the life of devices using the sealing material, and contributing to reduction in maintenance frequency. The tip seal for scroll-type compressors of the present invention is a tip seal for scroll-type compressors that has low abrasion resistance and non-aggression to mating materials and has no color unevenness even when the scroll rotation conditions are high-speed and high-load conditions. It is effective as an air seal in an atmospheric environment, but is also expected to be effective in nitrogen gas, hydrocarbon gas, and hydrogen gas environments. [Explanation of symbols]

[0081] 1 Cup seal (sealing material) 2 Reciprocating Compressor 3 Cylinder 4 Piston 5. Intake valve 6. Discharge valve 7 Compression Chamber 8 Connecting rod 9 Retainer 10 Connectors 11 Tip seal (sealing material) 11a Spiral start end 11b End of spiral 11c Sliding surface 12 Compression chamber 13 Seal groove 14 Fixed Scroll 15 Movable scroll 21 Ring test piece A 22 Rotating Disk A 23 Anodized coating 24 Ring test piece B 25 Rotating Disk B 26 Anodized coating

Claims

1. A sealing material made of a polytetrafluoroethylene resin composition, The polytetrafluoroethylene resin composition has a polytetrafluoroethylene resin as a base resin and contains zinc-based powder, the zinc content relative to the total amount of the polytetrafluoroethylene resin composition being 1.0 mass% to 10 mass%, and the zinc-based powder being metallic zinc powder or copper-zinc alloy powder.

2. 2. The sealing material according to claim 1, wherein the zinc content in the copper-zinc alloy powder is 10% by mass to 50% by mass.

3. The polytetrafluoroethylene resin composition contains 2.0 mass% to 10 mass% of molybdenum disulfide and 2.0 mass% to 15 mass% of carbon fiber, based on the total amount of the polytetrafluoroethylene resin composition. The sealing material according to claim 1 or 2.

4. 4. The sealing material according to claim 3, wherein the content by mass of the zinc-based powder in the polytetrafluoroethylene resin composition is greater than the contents of the molybdenum disulfide and the carbon fiber.

5. 4. The sealing material according to claim 3, wherein the polytetrafluoroethylene resin composition does not contain any inorganic filler other than the zinc-based powder, the molybdenum disulfide, and the carbon fibers.

6. 3. The sealing material according to claim 1, wherein the zinc-based powder has an average particle size of 5.0 μm to 80 μm.

7. The zinc content in the copper-zinc alloy powder is 10% by mass to 50% by mass, The polytetrafluoroethylene resin composition contains, relative to the total amount of the polytetrafluoroethylene resin composition, 10% by mass to 30% by mass of the copper-zinc alloy powder, 2.0% by mass to 5.0% by mass of molybdenum disulfide, and 2.0% by mass to 8.0% by mass of carbon fiber; 2. The sealing material according to claim 1, wherein the copper-zinc alloy powder has an average particle size of 25 μm to 80 μm.

8. A seal member for a compressor, comprising the seal material according to claim 1 or 2.

9. 9. The seal member for a compressor according to claim 8, which is a non-lubricated seal member.

10. A cup seal for a reciprocating compressor, which has a piston and a cylinder and is used in a reciprocating compressor that compresses gas by the reciprocating motion of the piston, the cup seal being fixed to the piston and press-fitted into an inner diameter of the cylinder to provide an air-tight seal between the piston and the cylinder, 3. A cup seal for a reciprocating compressor, comprising the sealing material according to claim 1 or 2.

11. A scroll-type compressor tip seal having a spiral shape for sealing a compression chamber formed between a fixed scroll and a movable scroll, which are scroll members in a scroll-type compressor, comprising:

3. A tip seal for a scroll compressor, comprising the sealing material according to claim 1 or 2.

Citation Information

Patent Citations

  • Non-lubricant seal material

    JP1994109139A

  • Reciprocating compressor

    JP1998148178A

  • Chip seal for compressor

    JP2001165072A

  • Sealing material and scroll fluid machine equipped with the same

    JP2004210885A

  • Sealing material and oscillating-type compressor provided with the same

    JP2005264049A