Substrate structuring method

The method of bonding substrates to carrier plates, patterning with electromagnetic radiation, and microblasting to form structured patterns addresses the high cost and complexity of traditional structuring methods, enabling efficient and cost-effective formation of high aspect ratio features on semiconductor substrates for advanced packaging.

JP2024137943AInactive Publication Date: 2024-10-07APPLIED MATERIALS INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024078724
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-11-18
Filing Date
2024-05-14
Publication Date
2024-10-07
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The traditional methods for structuring semiconductor substrates, particularly for advanced packaging applications, face challenges in forming high aspect ratio features like through-silicon vias due to high costs associated with silicon via etching and chemical mechanical planarization, which are impractical for miniaturized and complex integrated circuits.

Method used

A method involving bonding a substrate to a carrier plate with adhesive layers, applying a resist layer, patterning using electromagnetic radiation, and microblasting with powder particles to form patterns, followed by etching to remove debris and smooth the surface, thereby forming structured patterns efficiently.

Benefits of technology

This method enables the cost-effective formation of high aspect ratio features on glass and silicon substrates, reducing manufacturing costs and providing a viable alternative to silicon interposers for advanced integrated circuit packaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137943000001_ABST
    Figure 2024137943000001_ABST
Patent Text Reader

Abstract

To provide a method and apparatus for structuring a semiconductor substrate.SOLUTION: A substrate structuring method optionally applies a resist layer to a substrate placed on a carrier, involves patterning the resist layer using UV radiation or laser ablation, transfers and forms a desired features on the substrate by microblasting onto the patterned areas of the resist layer, shields the rest of the substrate with a non-exposed or non-ablated portion of the resist layer, exposes the substrate to etching and stripping processes to remove the resist layer and releases the carrier.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] FIELD OF THE DISCLOSURE

[0001] Embodiments of the present disclosure generally relate to methods and apparatus for structuring semiconductor substrates. More particularly, embodiments described herein relate to methods and apparatus for structuring semiconductor substrates using microblasting and laser ablation techniques. [Background technology]

[0002]

[0002] Due to the ever-increasing demand for miniaturized electronic devices and components, integrated circuits have evolved into complex 2.5D and 3D devices that can contain millions of transistors, capacitors, and resistors on a single chip. Evolution in chip design has increased circuit density and improved the processing power and speed of integrated circuits. The demand for faster processing power at higher circuit densities imposes corresponding demands on the materials, structures, and processes used in the manufacture of such integrated circuit chips. However, alongside these trends toward increased integration and performance, there is a constant pursuit of reducing manufacturing costs.

[0003]

[0003] Traditionally, integrated circuit chips have been fabricated on organic packaging substrates due to the ease of forming features and interconnections therethrough and the relatively low package manufacturing costs associated with organic composite materials. However, as circuit density increases and electronic devices become smaller, the use of organic packaging substrates becomes impractical due to limitations in the resolution of material structuring required to maintain device scaling and associated performance requirements. Recently, to compensate for some of the limitations associated with organic packaging substrates, 2.5D and 3D integrated circuits have been fabricated using passive silicon interposers disposed on organic packaging substrates as redistribution layers. The use of silicon interposers is driven by their potential for high-bandwidth density, low-power chip-to-chip communication, and heterogeneous integration requirements in advanced packaging applications. Nevertheless, the formation of features on silicon interposers, such as through-silicon vias (TSVs), remains challenging and costly. In particular, high costs are imposed by high-aspect-ratio silicon via etching, chemical-mechanical planarization, and semiconductor back-end-of-line (BEOL) interconnects.

[0004]

[0004] Therefore, what is needed in the art is an improved method of substrate structuring for advanced packaging applications. Summary of the Invention

[0005] In one embodiment, a method for substrate structuring is provided. The method includes bonding a substrate to a carrier plate using a first adhesive layer, bonding a resist layer on the substrate using a second adhesive layer, and patterning the resist layer using electromagnetic radiation. The method further includes propelling powder particles against the patterned resist layer to form a structured pattern on the substrate, and exposing the substrate to an etching process to remove debris from the structured pattern and smooth one or more surfaces thereof. Releasing the second adhesive layer peels the resist layer from the substrate, and releasing the first adhesive layer peels the substrate from the carrier plate.

[0006] In one embodiment, a method for substrate structuring is provided that includes forming a resist layer on a silicon solar substrate, patterning the resist layer by exposing the resist layer to electromagnetic radiation, propelling a stream of powder particles under high pressure toward the substrate to dislodge and remove material from the substrate and form a structured pattern therein, and exposing the substrate to an etching process to remove debris from the structured pattern and smooth one or more surfaces of the substrate.

[0007] In one embodiment, a method for substrate structuring is provided. The method includes bonding a first resist layer onto a first surface of a substrate using a first adhesive layer, bonding a second resist layer onto a second surface of the substrate using a second adhesive layer, and patterning the first resist layer and the second resist layer. The method further includes propelling powder particles toward the first surface of the substrate to form one or more patterned structures therein, propelling the powder particles toward the second surface of the substrate to extend the one or more patterned structures across a thickness of the substrate between the first and second surfaces, and exposing the substrate to an etching process to remove debris from the substrate and smooth one or more surfaces thereof.

[0008]

[0008] So that the above-mentioned features of the present disclosure may be understood in detail, a more particular description of the present disclosure briefly summarized above may be had by reference to embodiments, some of which are illustrated in the accompanying drawings. It should be noted, however, that the accompanying drawings illustrate only exemplary embodiments and therefore should not be considered as limiting its scope, as other equally effective embodiments may be recognized. [Brief explanation of the drawings]

[0009] [Figure 1] 1 shows a flow diagram of a substrate structuring process according to embodiments described herein. [Figures 2A-2F] 1A-1D schematically illustrate cross-sectional views of a substrate at various stages of a substrate structuring process according to embodiments described herein. [Figures 3A-3F] 1A-1D schematically illustrate cross-sectional views of a substrate at various stages of a substrate structuring process according to embodiments described herein. [Figures 4A-4E] 1A-1D schematically illustrate cross-sectional views of a substrate at various stages of a substrate structuring process according to embodiments described herein. [Figure 5] 1 shows a flow diagram of a substrate structuring process according to embodiments described herein. [Figures 6A-6D] 1A-1D schematically illustrate cross-sectional views of a substrate at various stages of a substrate structuring process according to embodiments described herein. DETAILED DESCRIPTION OF THE INVENTION

[0010]

[0015] For ease of understanding, wherever possible, identical reference numerals have been used to designate identical elements common to the figures. It is contemplated that elements and features of one embodiment may be beneficially incorporated in other embodiments without further recitation.

[0011]

[0016] The present disclosure relates to a method and apparatus for structuring a semiconductor substrate. In one embodiment, a method of substrate structuring includes applying a resist layer to a substrate, optionally disposed on a carrier plate. The resist layer is patterned using ultraviolet radiation or laser ablation. The patterned portions of the resist layer are then transferred onto the substrate by microblasting, while the unexposed or unablated portions of the resist layer shield the remainder of the substrate. The substrate is then exposed to an etching process and a stripping process to remove the resist layer and release the carrier. In another embodiment, desired features are formed in the substrate by laser ablation.

[0012]

[0017] FIG. 1 shows a flow chart of an exemplary method 100 for structuring a substrate 102. FIGS. 2A-2F and 3A-3F show schematic cross-sectional views of the substrate 102 at various stages of the structuring process of FIG. 1. Accordingly, references to FIGS. 2A-2F and 3A-3F are included in the description of FIG. 1 and method 100 as necessary. Furthermore, method 100 for structuring a substrate 102 has multiple steps. The steps can be performed in any order or simultaneously (unless the context precludes such a possibility), and the method can include one or more other steps that are performed before any of the defined steps, between two defined steps, or after all of the defined steps (unless the context precludes such a possibility).

[0013]

[0018] Generally, method 100 includes applying a resist film to substrate 102 in step 110. In some embodiments, substrate 102 is optionally coupled to a carrier plate before applying the resist film. In step 120, method 100 includes exposing substrate 102 to electromagnetic or laser radiation to pattern the resist film. In step 130, substrate 102 is microblasted to form structures, such as blind vias, through vias, or cavities, within substrate 102. The method further includes etching substrate 102 in step 140 to remove debris and surface microcracks formed during the microblasting process, while leaving the patterned resist film intact. The patterned resist layer is then removed in step 150, after which the substrate may be further exposed to a carrier plate stripping process in step 160.

[0014]

[0019] The substrate 102 may be a III-V compound semiconductor material, silicon, crystalline silicon (e.g., Si <100> or Si <111> The substrate 102 may be formed of any suitable substrate material, including, but not limited to, silicon dioxide, silicon germanium, doped or undoped silicon, doped or undoped polysilicon, silicon nitride, quartz, borosilicate glass, glass, sapphire, alumina, and ceramic. In one embodiment, the substrate 102 is a packaging substrate. In one embodiment, the substrate 102 is a monocrystalline p-type or n-type silicon substrate. In one embodiment, the substrate 102 is a polycrystalline p-type or n-type silicon substrate. In another embodiment, the substrate 102 is a p-type or n-type silicon solar substrate. Unless otherwise noted, the embodiments and examples described herein are practiced using a substrate having a thickness between about 50 μm and about 1000 μm, e.g., between about 90 μm and about 780 μm. For example, the substrate 102 has a thickness between about 100 μm and about 300 μm, e.g., between about 110 μm and about 200 μm.

[0015]

[0020] In embodiments in which the substrate 102 has a thickness of less than about 200 μm, e.g., about 50 μm, the substrate 102 is coupled to a carrier plate 106 during the substrate structuring process 100. The carrier plate 106 provides mechanical support to the substrate 102 during the substrate structuring process 100 and prevents the substrate 102 from breaking. The carrier plate 106 is formed of any suitable chemically and thermally stable, rigid material, including, but not limited to, glass, ceramic, metal, etc. The carrier plate 106 has a thickness of between about 1 mm and about 10 mm, e.g., between about 2 mm and about 5 mm. In one embodiment, the carrier plate 106 has a textured surface onto which the substrate 102 is coupled. In another embodiment, the carrier plate 106 has a polished surface onto which the substrate 102 is coupled.

[0016]

[0021] In one embodiment, the substrate 102 is coupled to the carrier plate 106 via an adhesive layer 108. The adhesive layer 108 is formed of any suitable temporary adhesive material, including, but not limited to, wax, glue, and similar adhesives. The adhesive layer 108 can be applied to the carrier plate 106 by mechanical rolling, pressing, lamination, spin coating, doctor blading, or the like. In one embodiment, the adhesive layer 108 is a water-soluble or solvent-soluble adhesive layer. In another embodiment, the adhesive layer 108 is a UV-release adhesive layer. In yet another embodiment, the adhesive layer 108 is a heat-release adhesive layer. In such embodiments, the adhesive properties of the adhesive layer 108 deteriorate upon exposure to high temperatures, such as temperatures above 110° C., e.g., above 150° C. The adhesive layer 108 may further include one or more layers of films (not shown), such as liners, heat-release adhesive films, base films, pressure-sensitive films, and other suitable layers.

[0017]

[0022] 2A and 3A, a resist film is applied to substrate 102 to form resist layer 104. Resist layer 104 is used to transfer a desired pattern into substrate 102 during subsequent processing steps. After being patterned in step 120, resist layer 104 protects selected areas of the underlying substrate 102 during a microblasting process in step 130.

[0018]

[0023] The substrate 102 has one or more substantially planar surfaces upon which a resist layer 104 can be formed. In one embodiment, such as the embodiment shown in FIG. 3A, the resist layer 104 is bonded to the substrate 102 via a resist adhesive layer 109. The resist adhesive layer 109 is formed from any suitable temporary adhesive material, including, but not limited to, polyvinyl alcohol, triesters including 2-ethyl-2-(hydroxymethyl)-1,3-propanediol, and other water-soluble or solvent-soluble materials. In one embodiment, the resist adhesive layer 109 is formed from a different material than the adhesive layer 108. In one embodiment, the resist adhesive layer 109 is substantially similar in composition to the adhesive layer 108. The resist adhesive layer 109 can be applied onto the substrate 102 by mechanical rolling, pressing, lamination, spin coating, doctor blading, or a similar process. In another embodiment, such as the one shown in FIG. 2A, the resist layer 104 is formed from a temporary adhesive material such as polyvinyl alcohol, and thus the resist layer 104 can be applied and bonded directly to the surface of the substrate 102. Furthermore, the resist layer 104 may include one or more layers, for example, a first resist layer and a second resist layer (not shown).

[0019]

[0024] In one embodiment, such as the embodiment shown in FIG. 2A, the resist layer 104 is a photoresist. The resist layer 104 may include a solvent, a photoresist resin, and a photoacid generator. The photoresist resin may be any positive-tone or negative-tone photoresist resin. Exemplary photoresist resins include acrylates, novolac resins, poly(methyl methacrylate), and poly(olefin sulfone). Other photoresist resins may also be used. Upon exposure to electromagnetic radiation, the photoacid generator generates charged species, such as acidic cations and anions. The photoacid generator may also generate polarized species. The photoacid generator sensitizes the resin to electromagnetic radiation. Exemplary photoacid generators include sulfonate compounds, such as sulfonate salts, sulfonate esters, and sulfonyloxyketones. Other suitable photoacid generators include onium salts, such as aryl diazonium salts, halonium salts, aromatic sulfonium salts, and sulfoxonium salts or selenium salts. Other representative photoacid generators include nitrobenzyl esters, s-triazine derivatives, ionic iodonium sulfonates, perfluoroalkane sulfonates, aryl triflates and their derivatives and analogs, pyrogallol derivatives, and alkyl disulfones. Other photoacid generators may also be used.

[0020]

[0025] In one embodiment, such as the embodiment shown in FIG. 3A, the resist layer 104 is a laser-sensitive resist. The resist layer 104 can be formed of any material having a hardness suitable for laser ablation. For example, the resist layer 104 is formed of a material having a Shore A hardness value of between about 40 and about 90, e.g., between about 60 and about 70. In one embodiment, the resist layer 104 is formed of a material having a Shore A hardness value of about 65. In further embodiments, the resist layer 404 is formed of a material having a tensile strength of between about 0.5 MPa and about 10 MPa, e.g., between about 1 MPa and about 8 MPa. For example, the resist layer 104 is formed of a material having a tensile strength of about 7 MPa. In some embodiments, the resist layer 104 is formed of a polydimethylsiloxane material. In other embodiments, the laser-sensitive resist layer 104 is formed of polyvinyl alcohol, a triester including 2-ethyl-2-(hydroxymethyl)-1,3-propanediol, or the like.

[0021]

[0026] In step 120, corresponding to FIGS. 2B and 3B, the substrate 102 having the resist layer 104 formed thereon is exposed to electromagnetic radiation to pattern the resist layer 104. In the embodiment illustrated by FIG. 2B, the substrate 102 having the resist layer 104 formed thereon is exposed to electromagnetic radiation in the ultraviolet (UV) range. Portions of the resist layer 104 are selectively exposed, and portions of the resist layer 104 are selectively not exposed to UV radiation. As illustrated in FIG. 2B, upon exposure to UV radiation, the selectively exposed portions of the resist layer 104 become structurally weakened, while the non-selectively exposed portions maintain their structural integrity. In one embodiment, a mask 112 having a desired pattern is formed on or adjacent to the resist layer 104 prior to UV radiation exposure. In some embodiments, the mask 112 is a reticle positioned between the resist layer 104 and a UV radiation source. Mask 112 is configured to transfer a desired pattern of UV radiation into resist layer 104 and is formed from any suitable polymeric material, including but not limited to PTFE, PVDF, FEP, polyimide, and the like.

[0022]

[0027] In the embodiment shown in FIG. 3B , the substrate 102 having the resist layer 104 formed thereon is exposed to electromagnetic radiation generated by a laser source 303 instead of a UV radiation source. In this manner, patterning is achieved by targeted laser ablation without the use of a mask. The laser source 303 can be any type of laser source suitable for patterning the laser-sensitive resist layer 104. In some examples, the laser source 303 is a femtosecond green laser. In other examples, the laser source 303 is a femtosecond UV laser. The laser source 303 generates a continuous or pulsed laser beam for patterning the resist layer 104. For example, the laser source 303 can generate a pulsed laser beam having a frequency between about 100 kHz and about 1200 kHz, e.g., between about 200 kHz and about 1000 kHz. It is further contemplated that in some embodiments, the electromagnetic radiation in step 120 can alternatively or additionally include an electron beam or an ion beam.

[0023]

[0028] In step 130, corresponding to FIGS. 2C and 3C , the substrate 102 having the resist layer 104 formed thereon is microblasted to form a desired pattern in the substrate 102. During the microblasting process, a stream of powder particles 205 is propelled under high pressure toward the substrate 102 to remove exposed portions of the substrate 102 and / or layers formed thereon. The microblasting process can be performed using any suitable substrate polishing system. In one embodiment, the powder particles 205 are propelled using a fluid flow of an inert gas, including, but not limited to, helium, argon, and nitrogen. In another embodiment, the powder particles 205 are propelled using a fluid flow of air.

[0024]

[0029] The microblasting process is determined by the material properties of the powder particles 205, the momentum of the powder particles 205 impacting the exposed surface of the substrate 102, and, if applicable, the material properties of the substrate 102 along with the selectively exposed portions of the resist layer 104. To achieve the desired substrate patterning characteristics, adjustments are made to the type and size of the powder particles 205, the size of the polishing system's applicator nozzle and its distance to the substrate 102, the pressure utilized to propel the powder particles 205, and the density of the powder particles 205 in the fluid stream. For example, for a given desired microblasting device nozzle orifice size, the desired fluid pressure of the carrier gas used to propel the powder particles 205 toward the substrate 102 can be determined based on the materials of the substrate 102 and the powder particles 205. In one embodiment, the fluid pressure utilized to microblast the substrate 102 generally ranges between about 50 psi and about 150 psi, e.g., between about 75 psi and about 125 psi, with carrier gas and particle velocities between about 300 meters per second (m / s) and about 1000 m / s and / or about 0.001 cubic meters per second (m 3 / s) to approximately 0.002 m 3 A flow rate of between about 1000 m / s and about 2350 m / s is achieved. For example, the fluid pressure of the inert gas (e.g., nitrogen (N), CDA, argon) utilized to propel the powder particles 205 during microblasting is about 95 psi, achieving a carrier gas and particle velocity of about 2350 m / s. In one embodiment, the applicator nozzle utilized to microblast the substrate 102 has an inner diameter of about 0.1 millimeters (mm) to about 2.5 mm, positioned at a distance of about 1 mm to about 5 mm (e.g., about 2 mm to about 4 mm) from the substrate 102. For example, the applicator nozzle is positioned at a distance of about 3 mm from the substrate 102 during microblasting.

[0025]

[0030] Generally, the microblasting process is performed using powder particles 205 having sufficient hardness and a high melting point to prevent adhesion of the particles upon contact with the substrate 102 and / or any layers formed thereon. For example, the microblasting process is performed utilizing powder particles 205 formed from a ceramic material. In one embodiment, the powder particles 205 utilized in the microblasting process are formed from aluminum oxide (Al2O3). In another embodiment, the powder particles 205 are formed from silicon carbide (SiC). Other suitable materials for the powder particles 205 are also contemplated. The powder particles 205 generally range in size from about 15 μm to about 60 μm in diameter, e.g., from about 20 μm to about 40 μm in diameter. For example, the powder particles 205 have an average particle size of about 27.5 μm in diameter. In another example, the powder particles 205 have an average particle size of about 23 μm in diameter.

[0026]

[0031] The effectiveness of the microblasting process in step 120 further depends on the material properties of the resist layer 104. Utilizing a material with too high a Shore A hardness can cause the powder particles 205 to undesirably bounce between the sidewalls of the resist layer 104, thus reducing the rate at which the powder particles 205 impact the substrate 102 and ultimately reducing the effectiveness of the powder particles 205 in eroding or removing exposed areas of the substrate 102. Conversely, utilizing a material with too low a Shore A hardness can cause undesirable adhesion of the powder particles 205 to the resist layer 104. As noted above, Shore A hardness values ​​of between about 40 and about 90 are contemplated for use in resist layer 104 materials.

[0027]

[0032] In embodiments in which the resist layer 104 is a photoresist, as shown in FIG. 2C , the substrate 102 remains unexposed at the start of step 130. Thus, the powder particles 205 first impact the surface of the resist layer 104, dislodging and removing material from portions of the photoresist that have been exposed to UV and structurally weakened. The powder particles 205 eventually penetrate and remove the weakened UV-exposed portions, creating voids in the resist layer 104, thus exposing desired areas of the substrate 102, while other areas remain shielded by the UV-unexposed portions of the photoresist. Microblasting is then continued until the powder particles 205 dislodge and remove a desired amount or depth of material from the exposed areas of the substrate 102, thus forming the desired pattern on the substrate 102.

[0028]

[0033] 3C, in embodiments in which the resist layer 104 is patterned by laser ablation, the desired areas of the substrate 102 are already exposed through voids in the resist layer 104 prior to microblasting in step 130. Therefore, it is believed that minimal or no removal of the resist layer 104 occurs during the microblasting process in step 130. In one embodiment, the microblasting process is optional, and the substrate 102 may be patterned using only laser ablation.

[0029]

[0034] After the desired pattern has been microblasted onto the substrate 102, the substrate 102 is exposed to an etching process in step 140, which corresponds to Figures 2D and 3D. The etching process in step 140 is utilized to smooth the surface of the substrate 102 and remove any undesired mechanical defects thereon. The etching process proceeds for a predetermined time to planarize the surface of the substrate 102, particularly the surface exposed to the microblasting process in step 130. In one embodiment, the etching process in step 140 is utilized to remove any undesired debris remaining from the microblasting process in step 130. Any remaining powder particles 205 adhering to the substrate 102 may be removed during the etching process in step 140.

[0030]

[0035] In one embodiment, the etching process in step 140 is a wet etching process that utilizes a buffered etching process that preferentially etches the substrate surface over the material of the resist layer 104. For example, the buffered etching process can be selective to polyvinyl alcohol. In one embodiment, the etching process is a wet etching process that utilizes an aqueous etching process. Any suitable wet etchant or combination of wet etchants can be used in the wet etching process. In one embodiment, the substrate 102 is immersed in an aqueous HF etching solution for etching. In another embodiment, the substrate 102 is immersed in an aqueous KOH etching solution for etching. In one embodiment, the etching solution is heated to a temperature between about 40° C. and about 80° C., e.g., between about 50° C. and about 70° C., during the etching process. For example, the etching solution is heated to a temperature of about 60° C. The etching process can also be isotropic or anisotropic. In one embodiment, the etching process in step 140 is a dry etching process. Examples of dry etching processes include plasma-based dry etching processes.

[0031]

[0036] 2E and 3E , the substrate 102 is exposed to a resist stripping process. The stripping process in step 150 is utilized to strip the resist layer 104 from the substrate 102. In one embodiment, a wet process is used to strip the resist layer 104 from the substrate 102 by dissolving / solubilizing the resist adhesive layer 109 and / or the resist layer 104. Other types of etching processes are also contemplated to release the resist adhesive layer 109 and / or the resist layer 104. In one embodiment, a mechanical rolling process is used to physically peel the resist layer 104 or the resist adhesive layer 109, thereby stripping the resist layer 104 from the substrate 102. In one embodiment, an ashing process is used to remove the resist layer 104 from the substrate 102, for example, by using an oxygen plasma-assisted process.

[0032]

[0037] At step 160, corresponding to Figures 2F and 3F, the substrate 102 is exposed to an optional carrier release process. Utilization of the carrier release process depends on whether the substrate 102 is coupled to a carrier plate 106 and the type of adhesive material utilized to couple the substrate 102 thereto. As noted above, in embodiments in which the substrate 102 has a thickness of less than about 200 μm, as shown in Figures 2A-2F and 3A-3F, the substrate is coupled to the carrier plate 106 for mechanical support during the substrate structuring process 100. In some embodiments, the substrate 102 is coupled to the carrier plate 106 via an adhesive layer 108. Thus, the substrate 102 coupled to the carrier plate 106 is exposed to the carrier release process at step 160 to release the adhesive layer 108 and thereby peel the substrate 102 from the carrier plate 106.

[0033]

[0038] In one embodiment, the adhesive layer 108 is released by exposing the substrate 102 to a bake process. In one embodiment, the substrate 102 is exposed to a temperature between about 50° C. and about 300° C., such as between about 100° C. and about 250° C. For example, the substrate 102 is exposed to a temperature between about 150° C. and about 200° C., such as about 160° C., for a desired time to release the adhesive layer 108. In another embodiment, the adhesive layer 108 is released by exposing the substrate 102 to UV radiation.

[0034]

[0039] 2F and 3F illustrate the structured substrate 102 after completion of the method 100. The substrate 102 shown in FIGS. 2F and 3F has three structures 220 formed therethrough. The method 100 is utilized to form patterned structures 220 in the substrate 102 having various desired depths, dimensions, and shapes. In one embodiment, the structures 220 have a depth equal to the thickness of the substrate 102, thus forming holes through two opposing surfaces of the substrate 102. In one embodiment, the structures 220 have a depth less than the thickness of the substrate 102, thus forming holes in only one surface of the substrate 102. For example, the structures 220 formed in the substrate 102 may have a depth between about 10 μm and about 600 μm, e.g., between about 25 μm and about 200 μm, depending on the thickness of the substrate 102. In one embodiment, structures 220 have lateral dimensions ranging from about 20 μm to about 15 mm (e.g., about 50 μm to about 5 mm), depending on the dimensions of substrate 102. In one embodiment, structures 220 formed on substrate 102 have a spheroid or conical shape. In another embodiment, structures 220 formed on substrate 102 have a rectangular parallelepiped shape. It is contemplated that structures 220 formed by method 100 may have any desired shape, size, and depth as permitted by substrate 102.

[0035]

[0040] 4A-4E show schematic cross-sectional views of substrate 102 during an alternative structuring sequence similar to the above embodiment. The alternative sequence shown in FIGS. 4A-4E involves patterning substrate 102 on two major opposing surfaces, as opposed to only one surface, thus enabling increased efficiency during structuring of substrate 102. The substrate structuring sequence shown in FIGS. 4A-4E includes substantially all of the features and steps as described with reference to FIGS. 1, 2A-2F, and 3A-3F. For example, FIG. 4A corresponds to step 110 and FIGS. 2A and 3A; FIG. 4B corresponds to step 120 and FIGS. 2B and 3B; FIG. 4C corresponds to step 130 and FIGS. 2C and 3C; FIG. 4D corresponds to step 140 and FIGS. 2D and 3D; and FIG. 4E corresponds to step 150 and FIGS. 2F and 3F. However, unlike the previous embodiment, the embodiment shown in Figures 4A-4E includes a substrate 102 with two resist layers 104 formed on opposing surfaces 405, 407, allowing the structuring process to be performed on both surfaces 405, 407.

[0036]

[0041] For example, after exposing the resist layer 104 formed on the surface 405 of the substrate 102 to electromagnetic radiation for patterning in step 120, the substrate 102 is optionally inverted (e.g., flipped over) so that the resist layer 104 on the opposite surface 407 of the substrate 102 can be exposed to electromagnetic radiation for patterning, as shown in Figure 4B. Similarly, after performing the microblasting process of step 130 on the surface 405 of the substrate 102, the substrate 102 can optionally be inverted again so that microblasting can be performed on the opposite surface 407 of the substrate 102, as shown in Figure 4C. By utilizing two resist layers 104 on opposing surfaces 405, 407 of the substrate 102 and performing the microblasting process on both surfaces, tapering of the structures formed through the entire thickness of the substrate 102 during microblasting can also be reduced or eliminated.

[0037]

[0042] FIG. 5 shows a flow chart of another exemplary method 500 for structuring a substrate 102. FIGS. 6A-6D show schematic cross-sectional views of the substrate 102 at various stages of the structuring process of FIG. 5. Accordingly, reference to FIGS. 6A-6D is included in the description of FIG. 5 and method 500, as appropriate. Similar to the methods described above, method 500 for structuring a substrate 102 has multiple steps. The steps can be performed in any order or simultaneously (unless the context precludes such a possibility), and the method can include one or more other steps that are performed before any of the defined steps, between two defined steps, or after all of the defined steps (unless the context precludes such a possibility).

[0038]

[0043] Generally, method 500 includes placing substrate 102 on stand 606 of a laser ablation system at step 510. In some embodiments, substrate 102 is optionally coupled to a carrier plate prior to placement on stand 606. At step 520, substrate 102 is exposed to laser radiation to pattern substrate 102 and form desired features therein. At step 530, substrate 102 is exposed to an etching process to remove debris and surface microcracks caused by laser patterning. In embodiments in which substrate 102 is coupled to a carrier plate, substrate 102 is further delaminated from the carrier plate once the etching process has been performed.

[0039]

[0044] 6A and corresponding to step 510, a substrate 102, such as a solar substrate, is placed on a stand 606 of a laser ablation system (not shown). The stand 606 can be any suitable rigid, planar surface for providing mechanical support to the substrate 102 during laser ablation. In some embodiments, the stand 606 includes an electrostatic chuck for electrostatically chucking the substrate 102 to the stand 606. In some embodiments, the stand 606 includes a vacuum chuck for vacuum-chucking the substrate 102 to the stand 606.

[0040]

[0045] After placing the substrate 102 on the stand 606, a desired pattern is formed in the substrate 102 by laser ablation, as shown in FIG. 6B and corresponding to step 520. The laser ablation system may include any suitable type of laser source 603 for patterning the substrate 102. In some examples, the laser source 603 is an infrared (IR) laser. In some examples, the laser source 603 is a picosecond UV laser. In other examples, the laser source 603 is a femtosecond UV laser. In yet other examples, the laser source 603 is a femtosecond green laser. The laser source 603 generates a continuous or pulsed laser beam 607 for patterning the substrate 102. For example, the laser source 603 can generate a pulsed laser beam 607 having a frequency between 100 kHz and 1200 kHz, e.g., between 200 kHz and about 1000 kHz. The laser source 603 is configured to form any desired patterns and features in the substrate 102, including cavities and vias.

[0041]

[0046] Similar to microblasting, the process of direct laser patterning of substrate 102 can cause undesirable mechanical defects, including chipping and cracking, in the surface of substrate 102. Therefore, after forming the desired features in substrate 102 by direct laser patterning, in step 530, substrate 102 is exposed to an etching process substantially similar to the etching process described with reference to step 140 to remove any remaining debris and smooth the surface of substrate 102. Figures 6C-6D show substrate 102 before and after performing the etching process, which ends with a structured substrate 102 having three features 620 (e.g., vias) formed therein.

[0042]

[0047] The embodiments described herein advantageously provide improved methods of substrate structuring for advanced integrated circuit packaging. Utilizing such methods, high aspect ratio features can be formed on glass and / or silicon substrates at significantly reduced manufacturing costs, which can serve as a low-cost alternative to silicon interposers.

[0043]

[0048] While the forgoing is directed to embodiments of the present disclosure, other and further embodiments of the present disclosure may be devised without departing from the basic scope thereof, which scope is determined by the following claims.

Claims

1. A method for substrate structuring, comprising: bonding the substrate to a carrier plate via a first adhesive layer; forming a resist layer on the substrate, the resist layer being bonded to the substrate via a second adhesive layer; patterning the resist layer via electromagnetic radiation; patterning the substrate by propelling a stream of powder particles against the patterned resist layer to form a structured pattern therein; exposing the substrate to an etching process to remove debris from the structured pattern in the substrate and to smooth one or more surfaces of the substrate; peeling the resist layer from the substrate by releasing the second adhesive layer; peeling the substrate from the carrier plate by releasing the first adhesive layer; The method includes:

2. The method of claim 1 , wherein the substrate is a single crystal p-type silicon substrate.

3. The method of claim 1 , wherein the substrate is a silicon solar substrate.

4. The method of claim 3 , wherein the substrate has a thickness of less than about 200 μm.

5. The method of claim 1 , wherein the resist layer is patterned by laser ablation.

6. The method of claim 1 , wherein the powder particles comprise a ceramic material.

7. The method of claim 6 , wherein the powder particles comprise aluminum oxide.

8. The method of claim 6 , wherein the powder particles comprise silicon carbide.

9. The method of claim 6 , wherein the powder particles have a diameter between about 15 μm and about 40 μm.

10. 7. The method of claim 6, wherein the fluid pressure utilized to impel the stream of powder particles is between about 50 psi and about 150 psi.

11. A method for substrate structuring, comprising: forming a resist layer on a silicon solar substrate; patterning the resist layer by exposing the resist layer to electromagnetic radiation; propelling a stream of powder particles under high pressure towards the substrate to dislodge and remove material from the substrate and form a structured pattern in the substrate; exposing the substrate to an etching process to remove debris from the structured pattern in the substrate and to smooth one or more surfaces of the substrate; The method includes:

12. The method of claim 11 , wherein the substrate is a single crystal silicon solar substrate.

13. The method of claim 11 , wherein the powder particles have a diameter between about 20 μm and about 35 μm.

14. A method for substrate structuring, comprising: forming a first resist layer on a first surface of a substrate, the first resist layer being bonded to the substrate via a first adhesive layer; forming a second resist layer on a second surface of the substrate, the substrate having a thickness extending between the first surface and the second surface, the second resist layer being bonded to the substrate via a second adhesive layer; patterning the first resist layer; patterning the second resist layer; propelling powder particles against the first surface of the substrate to form one or more patterned structures within the first surface of the substrate; propelling powder particles against the second surface of the substrate to extend the one or more patterned structures across the thickness of the substrate; exposing the substrate to an etching process to remove debris from the substrate and further smooth one or more surfaces of the substrate; The method includes:

15. The method of claim 14 , wherein the first resist layer and the second resist layer are patterned by laser ablation.

Citation Information

Patent Citations

  • Method of forming semiconductor integrated circuit

    JP1994216099A

  • Laser beam machining method

    JP2004042082A

  • Ultraviolet laser ablation patterning method for microstructures in semiconductors

    JP2004526575A

  • Manufacturing equipment for producing layered structures

    JP2014519203A

  • Manufacturing method for element chip

    JP2018006677A