Electrode material
By enhancing the crystallinity and reducing impurity concentrations in lithium phosphate compounds and supporting carbon on the surface, the electrode materials achieve higher capacity and faster charging/discharging speeds in power storage devices, addressing the capacity limitations of existing lithium phosphate compounds.
Patent Information
- Application Number
- JP2024113398
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2010-10-08
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-07
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Lithium phosphate compounds used as positive electrode active materials in power storage devices exhibit a smaller capacity than their theoretical capacity due to challenges in lithium ion diffusion paths and crystal structure stability during charging and discharging.
Improving the crystallinity of lithium iron phosphate and lithium manganese phosphate by using a cleaning process and controlling impurity concentrations, and supporting carbon on the surface of the crystal particles to enhance conductivity and stability.
The improved electrode materials result in power storage devices with increased capacity and faster charging/discharging speeds, suitable for applications in portable electronic devices and electric vehicles.
Smart Images

Figure 2024137973000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrode material, an electricity storage device using the same, and a method for manufacturing the same. [Background technology]
[0002] There has been remarkable progress in the field of portable electronic devices such as personal computers and mobile phones. In portable electronic devices, it is necessary to develop a battery that is small, lightweight, reliable, has a high energy density and is rechargeable. There is a need for a storage device that can be charged. In addition, due to the growing awareness of environmental and energy issues, lithium secondary batteries are becoming more widely used. The development of electric propulsion vehicles equipped with lithium-ion secondary batteries is also progressing rapidly.
[0003] In lithium-ion secondary batteries, lithium iron phosphate (LiFeP O4), lithium manganese phosphate (LiMnPO4), etc. Lithium phosphate compounds with an olivine structure containing Fe or Mn (See Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 11-25983 Summary of the Invention [Problem to be solved by the invention]
[0005] Lithium phosphate compounds are capable of inserting and extracting lithium ions. Since the change in crystal structure caused by the insertion and removal of ions is unlikely to occur, it is suitable as a positive electrode active material for energy storage devices. It is considered promising.
[0006] However, the lithium phosphate compound is not a positive electrode active material. The capacity obtained was smaller than the theoretical capacity calculated from the crystal structure of the lithium compound. Not yet.
[0007] In view of the above problems, one aspect of the disclosed invention is to provide a material for an electrode having a large capacity. Another object of the present invention is to provide a power storage device using a large-capacity electrode material. This is one of the challenges. [Means for solving the problem]
[0008] In lithium-ion secondary batteries, the lithium contained in the positive electrode active material is converted into lithium ions during charging. When the volume of the positive electrode active material layer is the same, the intercalation and The more carrier ions (here, lithium ions) that can be released and removed, the better the battery performance. The capacity can be increased.
[0009] Lithium iron phosphate or lithium manganese phosphate, etc., used as the positive electrode active material Lithium phosphate compounds have an olivine structure in which lithium atoms are arranged one-dimensionally. Therefore, the diffusion path of the lithium ions, which are carrier ions, is one-dimensional, i.e., in only one direction. Here, if there is a crystal distortion in the crystal structure of the lithium phosphate compound, This is likely to cause problems, and the amount of lithium ions inserted and removed is reduced. Therefore, by improving the crystallinity of lithium iron phosphate, the amount of lithium ions inserted and removed can be reduced. It is believed that the amount of charge stored in the battery will increase, resulting in an increase in the capacity of the power storage device.
[0010] In one embodiment of the present invention, a cleaning step is performed in a manufacturing process of a power storage device, The capacity of a material and a power storage device using the material is increased.
[0011] One aspect of the present invention is a method for producing a lithium-containing compound having a manganese, iron, cobalt, or nickel-containing compound. A mixture of a compound containing a metal element selected from the group consisting of ruthenium and a compound containing phosphorus is added to the first mixture. A heat treatment is performed, and the mixture that has been subjected to the first heat treatment is subjected to a washing step. A lithium phosphate compound is formed by subjecting the lithium phosphate compound to a second heat treatment. The present invention relates to a method for manufacturing an electricity storage device in which electrodes are formed by using a metal film.
[0012] One aspect of the present invention is a method for producing a lithium-containing compound having a manganese, iron, cobalt, or nickel-containing compound. A mixture of a compound containing a metal element selected from the group consisting of ruthenium and a compound containing phosphorus is added to the first mixture. A heat treatment is performed, and the mixture that has been subjected to the first heat treatment is subjected to a washing step. An organic compound is added to the mixture, and the mixture to which the organic compound is added is subjected to a second heat treatment to obtain phosphorus. A lithium phosphate compound is used to form an electrode, and a lithium phosphate compound is used to form an electrode. It is a manufacturing method.
[0013] In the above configuration, the cleaning liquid used in the cleaning step is a neutral or alkaline cleaning liquid. It can be used.
[0014] The inventors also investigated the effects of sulfur, manganese, nickel, and copper contained in lithium iron phosphate. The total content of zinc, boron, chromium, molybdenum and zinc is less than the weight of lithium iron phosphate. When lithium iron phosphate, which has a concentration of 10 ppm or less relative to the electrolyte, is used as the positive electrode active material, It has been found that it is possible to obtain a large capacity power storage device.
[0015] That is, one aspect of the present invention is to provide a method for producing lithium iron phosphate by using sulfur, manganese, nickel, and the like contained in the lithium iron phosphate. The total content of zinc, cobalt, boron, chromium, molybdenum and zinc is lithium iron phosphate. This is an electrode material with a content of 10 ppm or less based on the weight of the material.
[0016] In one embodiment of the present invention, the concentration of sulfur contained in lithium iron phosphate is 5.1 ppm or less. Below, manganese concentration is 0.55 ppm or less, nickel concentration is 0.1 ppm or less, cobalt concentration is 0.5 ppm or less, The concentration of cadmium is 0.1 ppm or less, the concentration of boron is 1.7 ppm or less, and the concentration of chromium is 0.3 ppm or less. 8 ppm or less, molybdenum concentration is 0.1 ppm or less, and zinc concentration is 0.59 ppm or less The electrode material has lithium iron phosphate, which is:
[0017] The lithium iron phosphate is a carbon-supported electrode material.
[0018] Another embodiment of the present invention is a power storage device using any of the above-described electrode materials as a positive electrode active material. It is. Effect of the Invention
[0019] According to one embodiment of the disclosed invention, a material for an electrode having a large capacity can be obtained. According to one embodiment of the disclosed invention, a power storage device with large capacity can be obtained. [Brief description of the drawings]
[0020] [Figure 1] FIG. 1 illustrates one embodiment of a power storage device. [Diagram 2] 13A to 13C are diagrams illustrating application examples of a power storage device. [Diagram 3] 13A to 13C are diagrams illustrating application examples of a power storage device. [Figure 4] 4A and 4B show characteristics of a power storage device manufactured in an example. [Diagram 5] 4A and 4B show characteristics of a power storage device manufactured in an example. [Figure 6] 4A and 4B show characteristics of a power storage device manufactured in an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The present invention will be described below with reference to the drawings. The present invention is not limited to the above description without departing from the spirit and scope of the present invention. It will be readily understood by those skilled in the art that the form and details of the present invention may be modified in various ways. Therefore, the present invention is not limited to the following embodiments and examples. In addition, when explaining the configuration of the present invention using the drawings, The reference numerals denoting the above are commonly used among different drawings.
[0022] The size, layer thickness, and area of each component shown in the drawings of each embodiment are For clarity, the figures may be exaggerated. Not limited.
[0023] In this specification, terms using ordinal numbers such as first, second, and third refer to components. These are added for convenience in order to distinguish between the steps, and are not intended to limit the number, order of steps, etc.
[0024] (Embodiment 1) In this embodiment, an example of a method for producing an electrode material will be described. In this case, a lithium phosphate compound represented by the general formula LiMePO4 is used as the electrode material. More specifically, for example, iron phosphate using manganese (Mn) or iron (Fe) as Me An example of a method for producing an electrode material containing lithium or lithium manganese phosphate is described. In the following, a method for producing an electrode material by a solid phase method will be described. However, the present invention is not limited to this, and the electrode material may be produced by a liquid phase method.
[0025] First, the general formula is LiMePO4 (where Me represents manganese (Mn) or iron (Fe) In the ion exchange reaction, the lithium-containing compound that supplies Li and the phosphorus-containing compound that supplies P are and a compound containing iron or a compound containing manganese, which is a source of Me, are mixed in a predetermined combination. The ingredients are mixed in the appropriate ratio to form a mixed material.
[0026] Examples of compounds containing lithium include lithium carbonate (Li2CO3), lithium oxide (Li2CO3), and Lithium (Li2O), lithium sulfide (Li2S), lithium peroxide (Li2O2), lithium sulfate Lithium (Li2SO4), Lithium sulfite (Li2SO3), Lithium thiosulfate (Li2S 2O3), lithium chromate (Li2CrO4), and lithium dichromate (Li2Cr Lithium salts such as 2O7) can be used.
[0027] Examples of manganese-containing compounds include manganese oxide and manganese(II) oxalate. Manganese(II) hydrate, manganese(II) carbonate, etc. can be used. When a compound containing the compound is applied to the mixed material, an electrode material containing lithium manganese phosphate is produced. Examples of compounds containing iron include iron oxide and iron oxalate (I Iron(II) dihydrate, or iron(II) carbonate, etc. can be used. When the compound is applied to a mixed material, it is possible to produce an electrode material containing lithium iron phosphate. can.
[0028] In the lithium phosphate compound represented by the general formula LiMePO4, Me is Co. Baltic (Co) and nickel (Ni) may also be used. Compounds containing cobalt or nickel The substances include oxides of cobalt or nickel (cobalt oxide, nickel oxide), oxalate, salts (cobalt oxalate, nickel oxalate) or carbonates (cobalt carbonate, nickel carbonate) (ru), etc. can be used.
[0029] Examples of compounds containing phosphorus include ammonium dihydrogen phosphate (NH4H2P Phosphates such as diphosphorus pentoxide (P2O5) and phosphorus pentoxide (P2O5) can be used.
[0030] The above-mentioned compounds can be mixed, for example, by ball milling. For example, a highly volatile solvent such as acetone is added to each weighed compound, and the compound is then mixed with a metal or The ball is made of ceramic (ball diameter φ1mm to 10mm) and the rotation speed is 50r. The ball mill is rotated at a speed of 500 rpm or more and 500 rpm or less for a rotation time of 30 minutes or more and 5 hours or less. By performing the mixing process, it is possible to mix the compounds and simultaneously break them into fine particles. This makes it possible to finely pulverize the electrode material after preparation. By carrying out this process, the raw material compounds can be mixed uniformly, and the electrode material after production can be It is possible to increase the crystallinity. In addition to acetone, other solvents such as ethanol and meth A solvent in which the raw material is not dissolved, such as alcohol, can be used.
[0031] The mixed material is then heated to evaporate the solvent and then pressed into pellets in a pellet press. The pellets are then molded and subjected to a first heat treatment (calcination). At a temperature of 300° C. to 400° C., for 1 hour to 20 hours, preferably 10 hours If the temperature of the first heat treatment (calcination) is too high, the particle size of the positive electrode active material becomes large. However, the first heat treatment is performed at low temperatures between 300℃ and 400℃. By carrying out the treatment (calcination), it is possible to form crystal nuclei while suppressing crystal growth. This allows the electrode material to be made into fine particles.
[0032] The first heat treatment is performed in a hydrogen atmosphere or in a rare gas atmosphere (helium, neon, argon, etc.). It is preferable to carry out the reaction in an atmosphere of an inert gas such as benzene, xenon, or nitrogen.
[0033] After the first heat treatment, the fired product is washed. A potash-based cleaning solution can be used, for example pure water or a weak alkaline aqueous solution (e.g., p For example, a sodium hydroxide solution of about H9.0 can be used. After washing for a while, the solution is filtered to recover the fired product.
[0034] Washing the fired product reduces impurities contained in the fired product, and the lithium phosphate produced The compound can be highly purified. The lithium compound also has improved crystallinity, so the carrier ions that are inserted and removed during charging and discharging are It is possible to increase the amount of ON.
[0035] Also, after the first heat treatment, or after the first heat treatment and the subsequent cleaning step, After that, an organic compound such as glucose may be added. When this is done, the carbon supplied from glucose adheres to the surface of the crystal particles of the lithium phosphate compound. In this specification, the carbon material is supported on the surface of the crystal particles of the lithium phosphate compound. The term "supported" is also used to mean that the crystal particles of the lithium phosphate compound are carbon-coated.
[0036] By supporting carbon on the surface of the lithium phosphate compound crystal particles, The electrical conductivity of the crystal grain surface of the lithium phosphate compound can be increased. When the crystal particles come into contact with each other through the carbon supported on their surfaces, the crystals of the lithium phosphate compound The particles are electrically connected to each other, which increases the conductivity of the active material layer. The thickness of the film is preferably greater than 0 nm and less than 100 nm, more preferably greater than 5 nm and less than 10 nm. It is nice.
[0037] Glucose is suitable as a carbon source because it reacts easily with phosphate groups. In addition, instead of glucose, cyclic monosaccharides, linear monosaccharides, or Polysaccharides may also be used.
[0038] Next, the washed material is crushed in a mortar or the like, and mixed by the same ball mill treatment as above. The mixed material is then heated to evaporate the solvent and then compressed in a pellet press. Pellets are molded and the molded pellets are subjected to a second heat treatment (main firing).
[0039] The second heat treatment is performed at a temperature of 500° C. to 800° C. (preferably about 600° C.) for 1 The second heat treatment temperature is from 100 to 2000 hours (preferably 10 hours or less). is preferably higher than the temperature of the first heat treatment.
[0040] Through the above steps, a lithium phosphate compound that can be used as an electrode material can be produced. can.
[0041] The electrode material of the present embodiment manufactured using the above-mentioned cleaning process is In addition, the capacity of the power storage device can be improved.
[0042] The configurations, methods, etc. described in this embodiment may be different from the configurations, methods, etc. described in other embodiments. They can be used in appropriate combination.
[0043] (Embodiment 2) In this embodiment, another example of a method for producing an electrode material will be described. More specifically, In this embodiment, the present invention relates to an electrode material containing lithium iron phosphate represented by LiFePO4. An example of the manufacturing method will be described. In the following, the manufacturing method of the electrode material by the solid phase method will be described. However, the present embodiment is not limited to this, and the electrode material may be produced by a liquid phase method. You can also create it.
[0044] The electrode material according to one aspect of the present invention has improved crystallinity, which facilitates the diffusion of carrier ions. The cause of the crystal distortion is the deficiency of the constituent elements and impurities. In this embodiment, the raw material of lithium iron phosphate is By using compounds with reduced impurities as raw materials, the iron phosphate The aim is to improve the crystallinity by purifying the lithium. One of the indicators of crystallinity is the lattice constant. The lattice constants of the crystal structures of inorganic compounds are calculated using the Inorganic Crystal Structure Database (ICSD). Organic Crystal Structure Database) is.
[0045] The following describes the specific raw materials.
[0046] First, a compound containing lithium as a source of Li and a compound containing P as a source of P in LiFePO4 are A compound containing phosphorus which serves as a source of Fe and a compound containing iron which serves as a source of Fe are mixed in a predetermined composition ratio. 2. Mix thoroughly to form a mixed material.
[0047] Examples of compounds containing lithium include lithium carbonate (Li2CO3), lithium oxide (Li2CO3), and Lithium salts such as lithium hydride (Li2O) and lithium peroxide (Li2O2) can be used.
[0048] The impurity element concentrations of the lithium-containing compound are preferably the values shown below. For example, In the case of lithium carbonate (Li2CO3), the sulfur concentration is less than 1 ppm, and the manganese concentration is 0.02ppm or less, nickel concentration is 0.05ppm or less, cobalt concentration is 0.00 5ppm or less, boron concentration is 0.01ppm or less, and chromium concentration is 0.51ppm or less The molybdenum concentration is less than 0.05 ppm, and the zinc concentration is less than 0.17 ppm. is preferred.
[0049] The concentrations of these elements were measured using glow discharge mass spectrometry (GDMS). It can be measured by mass spectrometry (MS) etc.
[0050] Examples of compounds containing iron include iron oxide, iron(II) oxalate dihydrate, and iron carbonate. Iron(II) and the like can be used.
[0051] The impurity element concentrations of the iron-containing compound are preferably as follows: In the case of iron(II) phosphate dihydrate (FeC2O4·2H2O), the sulfur concentration is 1.6 ppm. The manganese concentration is 0.1 ppm or less, the nickel concentration is 0.1 ppm or less, and the cobalt concentration is 0.1 ppm or less. The concentration of cadmium is less than 0.1 ppm, the concentration of boron is less than 0.25 ppm, and the concentration of chromium is less than 0. 1 ppm or less, molybdenum concentration is 0.8 ppm or less, zinc concentration is 0.1 ppm or less, It is preferable that the concentration of these impurity elements is as low as possible.
[0052] Examples of compounds containing phosphorus include ammonium dihydrogen phosphate (NH4H2P Phosphates such as diphosphorus pentoxide (P2O5) and phosphorus pentoxide (P2O5) can be used.
[0053] The impurity element concentration of the phosphorus-containing compound is preferably the value shown below. For example, In the case of ammonium dihydrogen phosphate (NH4H2PO4), the sulfur concentration is 5 ppm or less, Cancer concentration is less than 0.1 ppm, nickel concentration is less than 0.1 ppm, and cobalt concentration is 0.05 ppm or less, boron concentration is 1.3 ppm or less, chromium concentration is 0.5 ppm or less The molybdenum concentration must be less than 0.1 ppm, and the zinc concentration must be less than 0.5 ppm. In addition, the lower the concentration of these impurity elements, the more preferable.
[0054] The above-mentioned compounds can be mixed, for example, by ball milling. For example, a highly volatile solvent such as acetone is added to each weighed compound, and the compound is then mixed with a metal or The ball is made of ceramic (ball diameter φ1mm to 10mm) and the rotation speed is 50r. The ball mill is rotated at a speed of 500 rpm or more and 500 rpm or less for a rotation time of 30 minutes or more and 5 hours or less. By performing the mixing process, it is possible to mix the compounds and simultaneously break them into fine particles. This makes it possible to finely pulverize the electrode material after preparation. By carrying out this process, the raw material compounds can be mixed uniformly, and the electrode material after production can be It is possible to increase the crystallinity. In addition to acetone, other solvents such as ethanol and meth A solvent in which the raw material is not dissolved, such as alcohol, can be used.
[0055] The mixed material is then heated to evaporate the solvent and then pressed into pellets in a pellet press. The pellets are then molded and subjected to a first heat treatment (calcination). At a temperature of 300° C. to 400° C., for 1 hour to 20 hours, preferably 10 hours If the temperature of the pre-baking is too high, the particle size of the positive electrode active material becomes too large, which deteriorates the battery characteristics. However, the first heat treatment (pre-baking) is performed at a low temperature of 300°C to 400°C. By carrying out the above process, it is possible to form crystal nuclei while suppressing crystal growth. It is possible to reduce the size of the materials used.
[0056] The first heat treatment is performed in a hydrogen atmosphere or in a rare gas atmosphere (helium, neon, argon, etc.). It is preferable to carry out the reaction in an atmosphere of an inert gas such as benzene, xenon, or nitrogen.
[0057] After that, the mixed material that has been subjected to the first heat treatment is crushed in a mortar or the like. After crushing, it is washed with pure water or The fired product is placed in a weak alkaline solution (e.g., a sodium hydroxide solution with a pH of about 9.0). The fired product may be washed. By washing the fired product, impurities contained therein can be further reduced. This makes it possible to further improve the crystallinity of the lithium iron phosphate produced. For example, after washing at room temperature for 1 hour, the solution can be filtered to recover the fired product.
[0058] In addition, after the first heat treatment and crushing are completed, or after the subsequent washing step is completed, Organic compounds such as glucose may be added. Glucose is added before the subsequent steps. The carbon supplied from glucose is supported on the surface of the lithium iron phosphate crystal particles. In this specification, the carbon material is supported on the surface of the lithium iron phosphate crystal particles. This is also referred to as the lithium iron phosphate crystal particles being carbon coated.
[0059] By supporting carbon on the surface of lithium iron phosphate crystal particles, The electrical conductivity of the surface of the lithium iron phosphate crystal particles can be increased. However, when the lithium iron phosphate crystal particles come into contact with each other through the carbon supported on the surface, they become conductive to each other. The thickness of the supported carbon (carbon layer) is 0.5 to 1.0 mm. It is preferable that the thickness is larger than m and not larger than 100 nm, and more preferably, is 5 nm or more and not larger than 10 nm.
[0060] Glucose is suitable as a carbon source because it reacts easily with phosphate groups. In addition, instead of glucose, cyclic monosaccharides, linear monosaccharides, or Polysaccharides may also be used.
[0061] Next, mixing is performed by the same ball mill treatment as above. After that, the mixed materials are heated. After the solvent was evaporated, the mixture was pressed in a pellet press to form pellets. The pellet is subjected to a second heat treatment (main firing).
[0062] The second heat treatment is performed at a temperature of 500° C. to 800° C. (preferably about 600° C.) for 1 The second heat treatment temperature is from 100 to 2000 hours (preferably 10 hours or less). is preferably higher than the temperature of the first heat treatment.
[0063] Through the above steps, lithium iron phosphate that can be used as an electrode material can be produced. do.
[0064] The impurity element concentration of the lithium iron phosphate used as the electrode material is 122 ppm or less. The content is preferably 70 ppm or less, and more preferably 10 ppm or less. Impurity elements include, for example, sulfur, manganese, nickel, cobalt, boron, chromium, molybdenum, and The total content of bismuth, zinc and zinc is 100% by weight of the lithium iron phosphate. The concentration is preferably 70 ppm or less, more preferably 10 ppm or less. The sulfur concentration is less than 5.1 ppm, the manganese concentration is less than 0.55 ppm, and the nickel concentration is is less than 0.1 ppm, cobalt concentration is less than 0.1 ppm, and boron concentration is 1.7 ppm. The concentration of chromium is 0.38 ppm or less, the concentration of molybdenum is 0.1 ppm or less, and zinc is The concentration of these impurity elements is preferably 0.59 ppm or less. , the lower the better.
[0065] In addition, by reducing the impurity elements contained in lithium iron phosphate, The crystallinity of the lithium iron phosphate with improved crystallinity is The child constant is 10.3254 x 10 -10 (m) or more 10.3258×10 -10 (m) or less and the lattice constant of the b axis is 6.0035×10 -10 (m) or more 6.0052×10 -1 0 (m) or less, and the c-axis lattice constant is 4.6879×10 -10 (m) or more 4.690 2×10 -10 It is preferable that the thickness is equal to or less than (m).
[0066] The electrode material of the present embodiment produced as described above is highly purified and has improved crystallinity. This makes it possible to increase the amount of carrier ions inserted and removed during charging and discharging. Therefore, by using this electrode material in a power storage device, the capacity of the power storage device can be improved. It can be done.
[0067] The configurations, methods, etc. described in this embodiment may be different from the configurations, methods, etc. described in other embodiments. They can be used in appropriate combination.
[0068] (Embodiment 3) In this embodiment, an electrode material obtained by the manufacturing process shown in the above embodiment 1 or 2 is A lithium-ion secondary battery using the lithium-ion battery as a positive electrode active material will be described. An overview of a secondary battery is shown in Figure 1.
[0069] The lithium ion secondary battery shown in FIG. 1 includes a positive electrode 102, a negative electrode 107, and a separator 11. The battery 10 is placed in a housing 120 that is isolated from the outside, and the housing 120 is filled with an electrolyte 111. A positive electrode active material layer 101 is formed on a positive electrode current collector 100. The electrode material prepared in the first embodiment is included in the negative electrode current collector 105. In this specification, the positive electrode active material layer 101 and the negative electrode active material layer 106 are formed on the positive electrode active material layer 101. The positive electrode current collector 100 on which the negative electrode active material layer 106 is formed is collectively referred to as a positive electrode 102. The negative electrode current collector 105 on which it is formed is collectively referred to as a negative electrode 107.
[0070] In addition, a separator 110 is provided between the positive electrode 102 and the negative electrode 107. A first electrode 121 is connected to the negative electrode current collector 100, and a second electrode 122 is connected to the negative electrode current collector 105. Charging and discharging are performed through the first electrode 121 and the second electrode 122. Between the layer 101 and the separator 110 and between the negative electrode active material layer 106 and the separator 110 are shown at regular intervals, but are not limited to this. The separator 110 and the negative electrode active material layer 106 are in contact with each other. In addition, the positive electrode 102 and the negative electrode 107 are packed in a cylindrical container with a separator 110 disposed therebetween. It is okay to roll it into a shape.
[0071] The active material refers to a material involved in the insertion and removal of ions, which act as carriers. Lithium compounds or carbon supported lithium phosphate compounds. In this specification, the positive electrode active material layer refers to a thin film containing an active material, a binder, and a conductive assistant.
[0072] The positive electrode current collector 100 is made of a highly conductive material such as aluminum or stainless steel. The positive electrode current collector 100 may be in a suitable shape such as a foil, a plate, or a mesh. do.
[0073] As the positive electrode active material, the lithium phosphate compound shown in the first embodiment is used.
[0074] After the second heat treatment (main calcination), the obtained lithium phosphate compound was again crushed in a ball mill. The material is pulverized to obtain a fine powder. The fine powder is then mixed with a conductive agent, binder, and solvent to form a paste. Mix in a foam shape.
[0075] The conductive additive is an electronic conductor itself and undergoes chemical reactions with other substances in the battery device. For example, graphite, carbon fiber, carbon black, acetylene Racks, carbon-based materials such as VGCF (trademark), copper, nickel, aluminum, or These include powders or fibers of metallic materials such as silver or mixtures of these. It is a material that helps the electrical conductivity between active materials. It is filled between the active materials that are separated, and it connects the active materials. It is a material that provides electrical conductivity.
[0076] Binders include starch, carboxymethyl cellulose, and hydroxypropyl cellulose. Polysaccharides such as cellulose, regenerated cellulose, and diacetyl cellulose, as well as polyvinyl chloride, poly Ethylene, polypropylene, polyvinyl alcohol, polyvinylpyrrolidone, polytetrafluoroethylene Fluoroethylene, polyvinylidene fluoride, EPDM (Ethylene Propyl ene-diene monomer) rubber, sulfonated EPDM rubber, styrene butadiene Vinyl polymers such as ethylene rubber, butadiene rubber, and fluororubber, polyethylene oxide, etc. Which polyethers etc.
[0077] The lithium phosphate compound, conductive agent, and binder used as the electrode material are The ratios are 80-96% by weight, 2-10% by weight, and 2-10% by weight, respectively, and the total weight is 100%. % by volume. Then, the mixture of the electrode material, the conductive additive, and the binder is mixed. The electrode material, conductive additive, and biomaterial are mixed with the organic solvent in an amount of about 1000g / g to form a slurry. The substance obtained by processing the solvent and organic solvent into a slurry is called a slurry. Examples of the active material and the conductive material are N-methyl-2-pyrrolidone and lactate ester. When the adhesion of the conductive additive is weak, the amount of binder should be increased, and when the resistance of the active material is high, the amount of conductive additive should be increased. It is advisable to adjust the proportions of the active material, conductive additive, and binder appropriately by, for example, decreasing the amount of the active material, conductive additive, and binder.
[0078] Here, aluminum foil is used as the positive electrode current collector 100, and the slurry is dropped onto the aluminum foil to form a cathode current collector. After spreading it thinly using the stretching method, it is further stretched using a roll press machine to make the thickness uniform, and then vacuum dried. The positive electrode active material is then dried (10 Pa or less) or heated and dried (150 to 280° C.) to form a positive electrode active material on the positive electrode current collector 100. The material layer 101 is formed. The thickness of the positive electrode active material layer 101 is set to a desired value between 20 and 150 μm. The thickness of the positive electrode active material layer 101 is appropriately adjusted so that cracks and peeling do not occur. Furthermore, depending on the shape of the battery, it is preferable to arrange the battery in a cylindrical or round shape, in addition to a flat shape. It is preferable to prevent cracks or peeling from occurring in the positive electrode active material layer 101 when the positive electrode active material layer 101 is heated.
[0079] The negative electrode current collector 105 is made of a highly conductive material such as copper, stainless steel, iron, or nickel. There can be.
[0080] The negative electrode active material layer 106 may be made of lithium, aluminum, graphite, silicon, germanium, or the like. A negative electrode is formed on the negative electrode current collector 105 by coating, sputtering, vapor deposition, or the like. Alternatively, each material may be used alone as the negative electrode active material layer 106. In comparison with graphite, germanium, silicon, lithium, aluminum The theoretical lithium storage capacity is large. If the storage capacity is large, charging and discharging can be performed sufficiently even with a small area. This leads to cost reduction and miniaturization of secondary batteries. However, silicon and other materials are not lithium-ion batteries. The volume of the material increases by about four times due to absorption, making the material itself brittle and increasing the risk of explosion. You need to be very careful about everything.
[0081] The electrolyte may be a liquid electrolyte or a solid electrolyte. The electrolyte contains alkali metal ions or alkaline earth metal ions, which are carrier ions. The alkali metal ions are: For example, lithium ions, sodium ions, or potassium ions. Examples of earth metal ions include calcium ions, strontium ions, and Barium ions are also used as carrier ions. Beryllium ions and magnesium ions are also used as carrier ions. There is an ion.
[0082] The electrolyte solution 111 is, for example, a mixture of a solvent and a lithium salt or a sodium salt that dissolves in the solvent. The lithium salt is, for example, lithium chloride (LiCl), lithium fluoride (LiCl), Lithium (LiF), lithium perchlorate (LiClO4), lithium borofluoride (LiBF4 ), LiAsF6, LiPF6, Li(C2F5SO2)2N, etc. Sodium salts and Examples of such substances include sodium chloride (NaCl), sodium fluoride (NaF), and perchloric acid. Examples include sodium (NaClO4), sodium borofluoride (NaBF4), etc.
[0083] As a solvent for the electrolytic solution 111, a cyclic carbonate (for example, ethylene carbonate (hereinafter (hereinafter abbreviated as EC), propylene carbonate (PC), butylene carbonate (BC), and vinylene carbonate (VC), acyclic carbonates (dimethyl carbonate, etc.) diethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC ), methyl propyl carbonate (MPC), isobutyl methyl carbonate, and di propyl carbonate (DPC), etc.), aliphatic carboxylic acid esters (methyl formate, acetic acid methyl propionate, methyl propionate, and ethyl propionate), acyclic ethers ( γ-lactones such as γ-butyrolactone, 1,2-dimethoxyethane (DME), 1,2 -Diethoxyethane (DEE), ethoxymethoxyethane (EME), etc.), cyclic ethane ethers (tetrahydrofuran, 2-methyltetrahydrofuran, etc.), cyclic sulfones (sulfones (e.g., 1,3-dioxola), alkyl phosphate esters (dimethyl sulfoxide, trimethyl phosphate, triethyl phosphate, and trioctyl phosphate) and their derivatives There are various types of fluorides, and one or more of these can be used in combination.
[0084] The separator 110 is made of paper, nonwoven fabric, glass fiber, or nylon (polyamide). ), Vinylon (also called Vinalon) (polyvinyl alcohol fiber), polyester, a Synthetic fibers such as acrylic, polyolefin, and polyurethane can be used. It is necessary to select a material that is not dissolved in the electrolyte solution 111 described above.
[0085] More specifically, the separator 110 may be made of a material such as a fluorine-based polymer or a polyethylene. Polyethers such as ethylene oxide and polypropylene oxide, polyethylene, polypropylene Polyolefins such as ethylene, polyacrylonitrile, polyvinylidene chloride, polymethylmethacrylate Acrylate, polymethyl acrylate, polyvinyl alcohol, polymethacrylonitrile , polyvinyl acetate, polyvinylpyrrolidone, polyethyleneimine, polybutadiene , polystyrene, polyisoprene, polyurethane polymers and their derivatives, cellulosic One material selected from the group consisting of paper, spunbond, and nonwoven fabric can be used alone or in combination of two or more materials. can.
[0086] When charging the lithium ion secondary battery described above, a positive terminal is connected to the first electrode 121, A negative electrode terminal is connected to the second electrode 122. Electrons flow from the positive electrode 102 through the first electrode 121. The lithium ions are then transported to the negative electrode 107 through the second electrode 122. The ions are dissolved from the active material in the positive electrode active material layer 101 and pass through the separator 110 to become the negative electrode. The lithium ions reach the negative electrode 107 and are incorporated into the active material in the negative electrode active material layer 106. The ions and electrons combine and are absorbed in the negative electrode active material layer 106. At the same time, the positive electrode active material layer 101 In this case, electrons are released from the active material, causing an oxidation reaction of the iron contained in the active material.
[0087] When discharging, the negative electrode active material layer 106 in the negative electrode 107 releases lithium as ions. The electrons are transferred to the second electrode 122. The lithium ions pass through the separator 110. Then, the positive electrode active material layer 101 is reached and is taken up into the active material in the positive electrode active material layer 101. Occasionally, electrons from the negative electrode 107 also reach the positive electrode 102, causing a reduction reaction of iron.
[0088] The lithium ion secondary battery produced as described above was manufactured using a cleaning process. The positive electrode active material is a lithium phosphate compound having a liber structure. The lithium ion secondary battery obtained in the embodiment has a large discharge capacity and a high charge / discharge rate. The battery may be a large lithium ion secondary battery.
[0089] In addition, lithium phosphate compounds are highly purified and have improved crystallinity, making them ideal for charging and discharging. It is possible to increase the amount of carrier ions inserted and removed during the process. The lithium ion secondary battery obtained in this embodiment has a large discharge capacity and a high charge / discharge rate. It can be a large lithium ion secondary battery.
[0090] The configurations, methods, etc. described in this embodiment may be different from the configurations, methods, etc. described in other embodiments. They can be used in appropriate combination.
[0091] (Embodiment 4) In this embodiment, an application of a power storage device according to one embodiment of the present invention will be described.
[0092] The power storage device can be installed in various electronic devices. For example, digital cameras Cameras such as video cameras, mobile phones, personal digital assistants, e-book terminals, portable games The battery can be mounted on a computer, a digital photo frame, an audio player, etc. is an electric vehicle, a hybrid vehicle, a railroad electric vehicle, a work vehicle, a cart, a wheelchair, or It can be mounted on electric propulsion vehicles such as bicycles.
[0093] A power storage device according to one embodiment of the present invention has improved characteristics, such as a higher capacity and an improved charge / discharge rate. Improving the characteristics of the power storage device will also lead to making the device smaller and lighter. By installing such a power storage device, it is possible to charge electronic devices, electric propulsion vehicles, etc. It is possible to reduce operating time, extend usage time, and reduce size and weight, improving convenience and design. This can also be achieved.
[0094] 2A shows an example of a mobile phone. The mobile phone 3010 has a housing 3011. The housing 3011 further includes an operation button 3013, an operation An operation button 3017, an external connection port 3014, a speaker 3015, and a microphone 3016 By mounting a power storage device according to one embodiment of the present invention on such a mobile phone, This can improve convenience and design.
[0095] FIG. 2B shows an example of an e-book terminal. The e-book terminal 3030 is a first The housing is made up of two housings, a first housing 3031 and a second housing 3033, and the two housings are connected to the shaft portion 3 The first housing 3031 and the second housing 3033 are integrated by a shaft portion 3032. The first housing 3031 has a first display unit 3 035 is incorporated in the second housing 3033, and a second display unit 3037 is incorporated in the second housing 3033. In addition, the second housing 3033 includes an operation button 3039, a power supply 3043, and a speaker. In such an e-book terminal, a power storage device according to one embodiment of the present invention is provided. By incorporating this, convenience and design can be improved.
[0096] FIG. 3A shows an example of an electric vehicle. The electric vehicle 3050 includes a power storage device 3 The power output of the power storage device 3051 is adjusted by a control circuit 3053. The control circuit 3053 is connected to a computer 3055. is controlled by.
[0097] The drive unit 3057 is a DC motor or an AC motor alone, or a motor and an internal combustion engine, The computer 3055 controls the operation of the driver of the electric vehicle 3050. Operation information (acceleration, deceleration, stopping, etc.) and driving information (uphill and downhill slopes, etc., Based on the input information (such as load information), a control signal is output to the control circuit 3053. The circuit 3053 is supplied with power from the power storage device 3051 by a control signal from the computer 3055. The output of the drive unit 3057 is controlled by adjusting the electrical energy supplied. If the power supply is connected to a power source, an inverter that converts direct current to alternating current is also built in.
[0098] The power storage device 3051 can be charged by an external power supply using plug-in technology. By installing a power storage device according to one embodiment of the present invention as the power storage device 3051, This can contribute to shortening the charging time, improving convenience. Improving the discharge speed can contribute to improving the acceleration of electric vehicles, and thus improve the performance of electric vehicles. In addition, the improvement of the characteristics of the power storage device 3051 can contribute to the improvement of the performance of the power storage device 3052. If the 051 itself could be made smaller and lighter, it would contribute to reducing the weight of the vehicle, which would also lead to improved fuel efficiency. It can be attached.
[0099] FIG. 3B shows an example of an electric wheelchair. The wheelchair 3070 includes a power storage device, The controller 3073 includes a force controller, a control unit, and the like. The power of the power storage device, whose power has been adjusted, is supplied to the drive unit 3075. In addition, the control unit 3073 , and is connected to a controller 3077. By operating the controller 3077, The drive unit 3075 can be driven via the drive unit 3073, and the wheelchair 3070 can move forward and backward. , turning, and other movements and speed can be controlled.
[0100] The Wheelchair 3070's power storage device also uses plug-in technology to supply power from an external source. The power storage device 3051 can be charged by using a power storage device according to one embodiment of the present invention. By incorporating this technology, it will contribute to shortening charging times and improving convenience. In addition, if the characteristics of the power storage device can be improved to make the power storage device itself smaller and lighter, it will be possible to use it in wheelchairs. This makes the 3070 easier to use for users and caregivers.
[0101] In addition, when installing a power storage device on an electric railcar as an electrically propelled vehicle, overhead lines and conductive rails are required. It is also possible to charge the battery using power supplied from a power grid.
[0102] The configurations, methods, etc. described in this embodiment may be different from the configurations, methods, etc. described in other embodiments. They can be used in appropriate combination. EXAMPLES
[0103] In this embodiment, when a carbon material is supported on lithium manganese phosphate, the washing step is performed after the battery is charged. The results of an investigation into the effect on the battery characteristics of the device will be described below.
[0104] A method for manufacturing the electricity storage device used in this embodiment will be described. Sample 1 was made by washing with a neutral washing solution, and sample 2 was made by washing with an alkaline washing solution. Sample 2 was prepared by subjecting the sample to a cleaning process, and sample 3 was prepared without performing the cleaning process.
[0105] The materials for lithium manganese phosphate are lithium carbonate (Li2CO3) and manganese carbonate. (II) (MnCO3) and ammonium dihydrogen phosphate (NH4H2PO4) were mixed in L The mixture was weighed so that the molar ratio of i:Mn:P was 1:1:1, and then subjected to a first ball mill treatment. Lithium carbonate is a raw material for introducing lithium, and manganese carbonate is a raw material for introducing manganese. The raw material for the introduction of ammonium dihydrogen phosphate is the raw material for the introduction of phosphoric acid. In samples 1 to 3, lithium carbonate and manganese carbonate were used as raw materials for lithium manganese phosphate. Ammonium dihydrogen phosphate and ammonium dihydrogen phosphate were used.
[0106] The first ball mill treatment was carried out with acetone added as a solvent at a rotation speed of 400 rpm. The ball mill pot (cylindrical container) and The balls used were made of zirconia.
[0107] After the first ball milling, the mixture of raw materials was mixed to obtain a 1.47×10 2 N(150kgf) force The pellets were molded.
[0108] Next, the pellets were subjected to a first heat treatment (calcination). In the first heat treatment, the mixture was heated in a nitrogen atmosphere. The heating was carried out in an atmosphere at 350° C. for 10 hours.
[0109] After the first heat treatment, the fired product was crushed in a mortar. The crushed fired product was placed in an Erlenmeyer flask and washed. Sample 1 (when the cleaning solution is neutral) was cleaned by putting 500 ml of pure water into an Erlenmeyer flask. The washing of sample 2 (when the washing solution was alkaline) was performed by stirring at room temperature for 1 hour. To purify the solution, add NaOH to 500 ml of pure water, adjust the pH to 9.0, and then use a triangular flask. The mixture was placed in a scoop and stirred at room temperature for 1 hour. After stirring, the desired product was extracted by suction filtration. The product (mixture) was recovered.
[0110] Next, glucose was added to the washed material in an amount of 10 wt %.
[0111] The mixture with added glucose was subjected to a second ball milling treatment. The treatment was carried out with acetone added as a solvent, the rotation speed was 400 rpm, the rotation time was 2 hours, and the ball diameter was φ The experiment was carried out under the condition of 3 mm.
[0112] After the second ball milling, the mixture was mixed at 1.47 x 10 2 Pele with a force of N (150kgf) The molded product was then molded.
[0113] Next, the pellets were subjected to a second heat treatment (main sintering). In the second heat treatment, the mixture was heated in a nitrogen atmosphere. The process was carried out in an atmosphere at 600°C for 10 hours. Surface-supported lithium manganese phosphate was obtained.
[0114] After the second heat treatment, the fired product was ground in a mortar.
[0115] Lithium manganese phosphate (LiMnPO4), which is a crushed and fired material, and a conductive additive Acetylene black (AB) and polytetrafluoroethylene (PTFE) as binder were weighed out so as to give a ratio of 80:15:5 (wt %).
[0116] Next, the lithium manganese phosphate and acetylene black were mixed in a mortar, and the mixture was Polytetrafluoroethylene was added thereto and kneaded to disperse the mixture.
[0117] The mixture was rolled four times using a roll press to produce a sheet with a thickness of 114 μm. An aluminum mesh current collector was pressed onto the electrode layer to form a circular electrode with a diameter of 12 mm. By punching out the positive electrode of the electricity storage device, a positive electrode for the electricity storage device was obtained.
[0118] The negative electrode was made of lithium foil, and the separator was made of polypropylene (PP). The electrolyte is made of lithium hexafluorophosphate (LiPF6) as the solute and ethylene as the solvent. Carbonate (EC) and dimethyl carbonate (DMC) were used. The positive electrode was impregnated with the electrolyte.
[0119] In the manner described above, a coin-type electricity storage device having a positive electrode, a negative electrode, a separator, and an electrolyte solution is obtained. The positive electrode, negative electrode, separator, and electrolyte were assembled in an argon atmosphere. It was done in the glove box.
[0120] Next, a manufacturing method of an electricity storage device (sample 3) used as a comparative example will be described.
[0121] Sample 3 was manufactured in the same manner as Samples 1 and 2, except that the cleaning step was not performed. The electricity storage device was manufactured by this method.
[0122] Charge / discharge tests were performed using samples 1 to 3 (Toyo System Co., Ltd. charge / discharge test equipment TOS The results of the test using the CAT-3100 are explained below. The measurement voltage was 2.0V to 4. Set the range to 8V, and measure constant current constant voltage (CCCV) when charging, and constant current (C C) Measurements were performed. The constant current rate was 0.2C, and the constant voltage cutoff current was 0.016C. The charge and discharge rest periods were set to 2 hours.
[0123] FIG. 4 shows the results of the discharge characteristics of the power storage devices of Samples 1 to 3. In FIG. The vertical axis represents the discharge capacity (mAh / g) and the vertical axis represents the voltage (V). The discharge characteristics are shown in Fig. 4. The thin solid line shows the discharge characteristics of sample 2, and the dotted line shows the discharge characteristics of sample 3. As shown, Samples 1 and 2, which were subjected to the cleaning process, were different from Sample 3, which was not subjected to the cleaning process. The discharge density was comparatively high.
[0124] From the above results, by carrying out a cleaning process in the manufacturing process of the electricity storage device, the discharge It was confirmed that the capacity can be improved. A power storage device with a large discharge capacity can be obtained. EXAMPLES
[0125] In this embodiment, lithium iron phosphate with reduced impurity concentration and improved crystallinity was used as the positive electrode active material. The battery characteristics of the energy storage device using the material are shown.
[0126] A method for manufacturing the electricity storage device (sample 4) used in this example will be described.
[0127] First, lithium carbonate (Li2CO3) and iron oxalate ( II) dihydrate (FeC2O4·2H2O), and ammonium dihydrogen phosphate (NH4H 2PO4) was weighed out so that the molar ratio of Li:Fe:P was 1:1:1. The mixture was mixed by ball milling. Lithium carbonate is a raw material for lithium doping. Iron(II) oxalate dihydrate is a source for iron introduction, and ammonium dihydrogen phosphate is a source for phosphate introduction. In sample 4, the raw materials for lithium iron phosphate were Lithium carbonate, iron(II) oxalate dihydrate, and iron(II) dihydrogen phosphate with reduced concentrations of metal elements Ammonium was used.
[0128] The first ball mill treatment was carried out with acetone added as a solvent at a rotation speed of 400 rpm. The ball mill pot (cylindrical container) and The balls used were made of zirconia.
[0129] After the first ball milling, the mixture of raw materials was mixed to obtain a 1.47×102 N(150kgf) force The pellets were molded.
[0130] Next, the pellets were subjected to a first heat treatment (calcination). In the first heat treatment, the mixture was heated in a nitrogen atmosphere. The sample was subjected to a heat treatment at 350° C. for 10 hours in an atmospheric environment.
[0131] After the first heat treatment, the fired product was crushed in a mortar. The crushed fired product was then placed in a second ball mill. The mixture was further pulverized by grinding.
[0132] The second ball mill treatment was carried out with acetone added as a solvent at a rotation speed of 400 rpm. The test was performed for 2 hours with a ball diameter of φ3 mm.
[0133] After the second ball milling process, the crushed material was mixed with 1.47 × 10 2 With a force of N (150 kgf) Pellets were molded.
[0134] Next, the pellets were subjected to a second heat treatment (main sintering). The resulting product was heat-treated at 600°C for 1 hour in a nitrogen atmosphere. Lithium iron phosphate was obtained.
[0135] After the second heat treatment, the fired product was ground in a mortar.
[0136] Here, the fired product after the second heat treatment was subjected to X-ray diffraction (XRD). The calcined material was determined to have a L structure in the space group Pnma(62) by X-ray diffraction. It was confirmed that it was a single phase iFePO4.
[0137] Next, the obtained fired material (lithium iron phosphate (LiFePO4)) and the conductive additive (acetylene black (AB)) and binder (polytetrafluoroethylene (PTFE)) at 80 The ratio was weighed out to give a ratio of 15:5 (wt%).
[0138] Next, lithium iron phosphate and acetylene black were mixed in a mortar, and the mixture was added with polystyrene. Tetrafluoroethylene was added and dispersed by kneading.
[0139] The mixture was rolled four times using a roll press to produce a sheet with a thickness of 114 μm. An aluminum mesh current collector was pressed onto the electrode layer to form a circular electrode with a diameter of 12 mm. By punching out the positive electrode of the electricity storage device, a positive electrode for the electricity storage device was obtained.
[0140] The negative electrode was made of lithium foil, and the separator was made of polypropylene (PP). The electrolyte is made of lithium hexafluorophosphate (LiPF6) as the solute and ethylene as the solvent. Carbonate (EC) and dimethyl carbonate (DMC) were used. The positive electrode was impregnated with the electrolyte.
[0141] In the manner described above, a coin-type electricity storage device having a positive electrode, a negative electrode, a separator, and an electrolyte solution is obtained. The positive electrode, negative electrode, separator, and electrolyte were assembled in an argon atmosphere. It was done in the glove box.
[0142] Next, a manufacturing method of a power storage device (sample 5) used as a comparative example will be described.
[0143] In sample 5, as a raw material for lithium iron phosphate, compared with the raw material used in sample 4, Lithium carbonate, iron(II) oxalate dihydrate, and phosphoric acid dihydrate have high concentrations of impurities, respectively. The raw materials for the lithium iron phosphate were the same as those for sample 4. An electrical device was fabricated.
[0144] In Samples 4 and 5, the lithium carbonate (Li CO3), iron(II) oxalate dihydrate (FeC2O4·2H2O) and dihydrogen phosphate ammonium (NH4H2PO4) and lithium iron phosphate (L The concentrations of impurity elements contained in iFePO4) and iFePO4) are shown in Table 1. The impurity concentrations were measured by glow discharge mass spectrometry. The VG-9000 manufactured by Elemental was used. The values shown are below the detection limit and indicate that the substance was not detected.
[0145] [Table 1]
[0146] As shown in Table 1, the sulfur (S The concentration of manganese (Mn) is 0.02 ppm, and the concentration of nickel (Ni) is 1 ppm. The concentration of zinc is 0.05 ppm, and the concentration of cobalt (Co) is 0.005 ppm or less (below the detection limit). The concentration of boron (B) is less than 0.01 ppm (below the detection limit), and the concentration of chromium (Cr) is 0.51 ppm, molybdenum (Mo) concentration is 0.05 ppm or less (below the detection limit), The lead (Zn) concentration is 0.17 ppm.
[0147] On the other hand, the lithium carbonate (Li2CO3) used as the raw material for Sample 5, which was prepared as a comparative example, The concentration of sulfur (S) is 6.6 ppm, the concentration of manganese (Mn) is 0.08 ppm, and the concentration of nickel The concentration of (Ni) is 0.02 ppm, the concentration of cobalt (Co) is 0.02 ppm, and the concentration of boron ( B) concentration was below 0.01 ppm (below the detection limit), and the chromium (Cr) concentration was 0.46 ppm. pm, Molybdenum (Mo) concentration is below 0.05 ppm (below the detection limit), Zinc (Zn) The concentration is 0.56 ppm.
[0148] In addition, iron (II) oxalate dihydrate (FeC2O4·2H2O) used as the raw material for sample 4 The sulfur (S) concentration is 1.6 ppm, and the manganese (Mn) concentration is less than 0.1 ppm (detectable). Nickel (Ni) concentration is 0.1 ppm or less (below the detection limit), Cobalt ( The concentration of Co was 0.1 ppm or less (below the detection limit), and the concentration of boron (B) was 0.25 ppm. m, chromium (Cr) concentration is 0.1 ppm or less (below the detection limit), molybdenum (Mo) The concentration is 0.8 ppm, and the zinc (Zn) concentration is less than 0.1 ppm (below the detection limit).
[0149] On the other hand, iron(II) oxalate dihydrate (FeC2O4·2H2O) used as the raw material for sample 5 The sulfur (S) concentration is 1100 ppm, the manganese (Mn) concentration is 300 ppm, and the nickel concentration is The concentration of nickel (Ni) is 110 ppm, the concentration of cobalt (Co) is 53 ppm, and the concentration of boron (B) is 100 ppm. The concentration of Cr is 4.2 ppm, the concentration of Cr is 17 ppm, and the concentration of Mo is The concentration of zinc (Zn) is 4.6 ppm.
[0150] In addition, the sulfur ( The concentration of manganese (Mn) was less than 0.1 ppm. Nickel (Ni) concentration is 0.1 ppm or less (below the detection limit), The concentration of ballast (Co) was less than 0.05 ppm (below the detection limit), and the concentration of boron (B) was 1 .3 ppm, chromium (Cr) concentration is less than 0.5 ppm (below the detection limit), molybdenum ( The concentration of Mo was 0.1 ppm or less (below the detection limit), and the concentration of zinc (Zn) was 0.5 ppm. below the detection limit.
[0151] On the other hand, the sulfur ( The concentration of manganese (Mn) was 1.2 ppm, The nickel (Ni) concentration is 0.15 ppm, and the cobalt (Co) concentration is 0.05 ppm or less. Below the detection limit, the concentration of boron (B) is 16 ppm and the concentration of chromium (Cr) is 0.5 ppm or less (below the detection limit), and the concentration of molybdenum (Mo) is 0.1 ppm or less (below the detection limit or less), and the zinc (Zn) concentration is 0.5 ppm or less (below the detection limit).
[0152] From Table 1, lithium carbonate, iron(II) oxalate dihydrate (FeC2O4·2H2O), For each of the ammonium dihydrogen phosphates, the raw materials used for sample 4 were the same as those used for sample 5. It can be seen that the impurity concentration is reduced compared to the raw material. In particular, iron (II) oxalate dihydrate The total concentration of impurity elements shown in Table 1 was 1697 ppm for sample 5. In contrast, in sample 4, the concentration was significantly reduced to 66.04 ppm.
[0153] In the case of sample 5, the iron (II) oxalate dihydrate contained 1100p of sulfur, an impurity element. pm, which is the impurity element concentration of iron(II) oxalate dihydrate. In addition, the raw materials used are not subject to reduction of impurity element concentrations. It was found that the lithium iron phosphate produced by this method contained 300 ppm of sulfur. This accounts for approximately 46% of the impurity element concentration in lithium iron phosphate.
[0154] In contrast, in the case of sample 4, the sulfur content of iron(II) oxalate dihydrate was 1.6 It was found that the impurity element concentration was reduced to ppm. The sulfur content in lithium iron phosphate made using this material was reduced to 5.1 ppm. This allowed us to determine the concentration of sulfur in iron(II) oxalate dihydrate. It has been found that reducing the concentration of impurity elements in lithium iron phosphate greatly contributes to reducing the concentration of impurity elements in lithium iron phosphate. It was.
[0155] In the case of sample 5, the iron (II) oxalate dihydrate contained manganese, an impurity element. It was found to contain 300 ppm of iron(II) oxalate dihydrate. In addition, the impurity element concentration of raw materials that have not been reduced is approximately 18%. The lithium iron phosphate prepared using this material contains 150 ppm of manganese. This accounts for approximately 23% of the impurity element concentration in lithium iron phosphate.
[0156] In contrast, in the case of sample 4, the manganese contained in iron (II) oxalate dihydrate was 0 It was found that the concentration of impurities was reduced to .1 ppm. In lithium iron phosphate made from these raw materials, manganese was reduced to 0.55 ppm. This revealed that the concentration of manganese in iron (II) oxalate dihydrate was Reducing the concentration of impurities in lithium iron phosphate is expected to contribute greatly to the reduction of the concentration of impurities in lithium iron phosphate. Understood.
[0157] In addition, from Table 1, the impurity element concentration of the lithium iron phosphate used as the positive electrode active material of sample 4 The impurity concentration of the lithium iron phosphate used as the positive electrode active material of Sample 5 was 122 ppm or less. This is a reduction compared to the 650.27 ppm of the total element concentration used in sample 4. The sulfur (S) concentration of the lithium iron phosphate was 5.1 ppm and the manganese (Mn) concentration was 0. 55ppm, nickel (Ni) concentration is less than 0.1ppm, and cobalt (Co) concentration is 0 .1 ppm or less, boron (B) concentration is 1.7 ppm, and chromium (Cr) concentration is 0.38 ppm, molybdenum (Mo) concentration is less than 0.1 ppm, zinc (Zn) concentration is 0.59 The total content of the above elements was 8.62 ppm or less. The sulfur (S) concentration of the lithium iron phosphate used in sample 5 was 300 ppm, and manganese (Mn) The concentration of nickel (Ni) is 150 ppm, the concentration of cobalt (Co) is 71 ppm, The concentration of boron (B) is 9.5 ppm, and the concentration of chromium (Cr) is 4.1 ppm. m, the concentration of molybdenum (Mo) was 3.9 ppm, and the concentration of zinc (Zn) was 2.6 ppm. The total content of the above elements was 578.1 ppm or less.
[0158] The lattice constant of the lithium iron phosphate used as the positive electrode active material in Samples 4 and 5 was measured using X-ray diffraction. The results of the diffraction measurements are shown in Table 2. The measurement results for sample number n=1 are shown, and for sample 5, the average of the measurement results for sample number n=9 is shown. In Table 2, the database value is the inorganic compound crystal structure data. The lattice constants of lithium iron phosphate are disclosed in the International Chemical Society of Japan (ICSD).
[0159] [Table 2]
[0160] As shown in Table 2, in the lithium iron phosphate sample 4 in which the impurity element concentration was reduced, , the lattice constant of the a-axis is 10.3258×10 -10 (m), and the b-axis lattice constant is 6.0 052×10 -10 (m), and the c-axis lattice constant is 4.6902×10 -10 (m) The lithium iron phosphate used in sample 4 has a smaller a-axis value in the database than sample 5. Lattice constant: 10.3254×10 -10 (m), b-axis lattice constant 6.0035×10 -10 (m), c-axis lattice constant 4.6879×10 -10 The value is closer to (m).
[0161] This is because in sample 5, in which the impurity element concentration is not reduced, the crystallization of lithium iron phosphate In the crystal structure, the substitution of foreign elements by impurity elements causes crystal distortion. This is thought to be because the lithium iron phosphate used in sample 4 is In other words, the crystallinity is improved compared to that of the conventional quartz crystal.
[0162] Next, a charge-discharge test was conducted using Sample 4 and Sample 5 (Toyo System Co., Ltd. charge-discharge test equipment). The results of the measurement using TOSCAT-3100 are explained below. The measurement voltage was 2.0V. Set the voltage to within 4.2V, and measure constant current and constant voltage (CCCV) during charging and constant voltage during discharging. Current (CC) measurements were performed. The constant current rate was 0.2C, and the cutoff current for the constant voltage was 0.0 A current value equivalent to 16 C was used, and the rest time between charging and discharging was set to 2 hours.
[0163] FIG. 5 shows the results of the discharge characteristics of the power storage devices of Samples 4 and 5. In FIG. 5, the horizontal axis indicates the discharge The vertical axis represents the capacity (mAh / g) and the vertical axis represents the voltage (V). The thin solid line shows the charge characteristics of sample 1, and the thin solid line shows the discharge characteristics of sample 5.
[0164] As shown in FIG. 5, the lithium iron phosphate of Sample 4 with improved crystallinity can be applied to an energy storage device. It was shown that the discharge capacity of the electricity storage device can be improved by this.
[0165] From the above results, the following can be considered. The diffusion path of lithium is one-dimensional. Therefore, in the crystal structure of lithium iron phosphate, When crystal distortion exists, it is easy for the diffusion path of lithium to be adversely affected. The causes of distortion are thought to be low crystallinity and deficiencies of constituent elements. In the structure, the substitution of different elements such as impurities is also a major factor in the occurrence of crystal distortion. .
[0166] As shown in this embodiment, in sample 5 in which the impurity element concentration is not reduced, phosphorus In the crystal structure of lithium iron oxide, the substitution of foreign elements with impurity elements occurs, It is believed that crystal distortion has occurred, which has caused problems in the diffusion path of lithium ions. Therefore, it is considered that the discharge capacity was lower than the theoretical capacity.
[0167] In contrast, in sample 4, in which the impurity element concentration was reduced, the crystals of lithium iron phosphate In the structure, the occurrence of crystal distortion is suppressed by reducing the substitution of foreign elements with impurity elements. It is believed that the crystallinity has been improved, and this allows the lithium ions to diffuse well. It is considered that the discharge capacity approached the theoretical capacity.
[0168] As described above, by improving the crystallinity of lithium iron phosphate, the battery characteristics of the power storage device can be improved. It has been shown that improvements can be made. EXAMPLES
[0169] In this embodiment, when a carbon material is supported on lithium iron phosphate, the raw material of lithium iron phosphate How does the concentration of impurity elements in the battery affect the battery characteristics of the power storage device? The results of the investigation will be explained.
[0170] A manufacturing method of the power storage device (Sample 6) used in this embodiment will be described.
[0171] The materials for lithium iron phosphate are lithium carbonate (Li2CO3) and iron (II) oxalate. Dihydrate (FeC2O4·2H2O) and ammonium dihydrogen phosphate (NH4H2PO 4) were mixed by the first ball mill treatment. The above raw materials were low in impurity elements. Reduced material was used.
[0172] The first ball mill treatment was carried out with acetone added as a solvent at a rotation speed of 400 rpm. The ball mill pot (cylindrical container) and The balls used were made of zirconia.
[0173] After the first ball milling, the mixture of raw materials was mixed to obtain a 1.47×10 2 N(150kgf) force The pellets were molded.
[0174] Next, the pellets were subjected to a first heat treatment (calcination). In the first heat treatment, the mixture was heated in a nitrogen atmosphere. The heating was carried out in an atmosphere at 350° C. for 10 hours.
[0175] After the first heat treatment, the fired product was ground in a mortar.
[0176] Next, glucose was added to the ground baked product. The amount of glucose was 10 wt%. .
[0177] The mixture with added glucose was subjected to a second ball milling treatment. The treatment was carried out with acetone added as a solvent, the rotation speed was 400 rpm, the rotation time was 2 hours, and the ball diameter was φ The experiment was carried out under the condition of 3 mm.
[0178] After the second ball milling, the mixture was mixed at 1.47 x 10 2 Pele with a force of N (150kgf) The molded product was then molded.
[0179] Next, the pellets were subjected to a second heat treatment (main sintering). In the second heat treatment, the mixture was heated in a nitrogen atmosphere. The process was carried out at 600°C for 10 hours in an atmospheric environment. The lithium iron phosphate was obtained.
[0180] After the second heat treatment, the fired product was ground in a mortar.
[0181] Next, the obtained fired material (lithium iron phosphate (LiFePO4)) and the conductive additive (acetylene black (AB)) and binder (polytetrafluoroethylene (PTFE)) at 80 The ratio was weighed out to give a ratio of 15:5 (wt%).
[0182] Next, lithium iron phosphate and acetylene black were mixed in a mortar, and the mixture was added with polystyrene. Tetrafluoroethylene was added and dispersed by kneading.
[0183] The mixture was rolled four times using a roll press to produce a sheet with a thickness of 114 μm. An aluminum mesh current collector was pressed onto the electrode layer to form a circular electrode with a diameter of 12 mm. By punching out the positive electrode of the electricity storage device, a positive electrode for the electricity storage device was obtained.
[0184] The negative electrode was made of lithium foil, and the separator was made of polypropylene (PP). The electrolyte is made of lithium hexafluorophosphate (LiPF6) as the solute and ethylene as the solvent. Carbonate (EC) and dimethyl carbonate (DMC) were used. The positive electrode was impregnated with the electrolyte.
[0185] In the manner described above, a coin-type electricity storage device having a positive electrode, a negative electrode, a separator, and an electrolyte solution is obtained. The positive electrode, negative electrode, separator, and electrolyte were assembled in an argon atmosphere. It was done in the glove box.
[0186] Next, a manufacturing method of a power storage device (sample 7) used as a comparative example will be described.
[0187] In sample 7, the impurity element concentration was not reduced as a raw material for lithium iron phosphate. Other than using lithium carbonate, iron(II) oxalate dihydrate, and ammonium dihydrogen phosphate, A power storage device was manufactured by a method similar to that of Sample 6.
[0188] The impurity element concentrations of the lithium iron phosphate, which is the positive electrode active material of Samples 6 and 7, were measured. The samples are similar to Samples 4 and 5 shown in Table 1 of Example 2.
[0189] Next, a charge-discharge test was performed using samples 6 and 7 (Toyo System Co., Ltd. charge-discharge test equipment). The results of the measurement using TOSCAT-3100 are explained below. The measurement voltage was 2.0V. Set the voltage to within 4.2V, and measure constant current and constant voltage (CCCV) during charging and constant voltage during discharging. Current (CC) measurements were performed. The constant current rate was 0.2C, and the cutoff current for the constant voltage was 0.0 A current value equivalent to 16 C was used, and the rest time between charging and discharging was set to 2 hours.
[0190] FIG. 6 shows the results of the discharge characteristics of the energy storage devices of Samples 6 and 7. In FIG. The vertical axis represents the discharge capacity (mAh / g) and the vertical axis represents the voltage (V). The thin solid line shows the discharge characteristics of sample 7.
[0191] As shown in Figure 6, the energy density can be improved by reducing the impurity element concentration of the raw materials. It was confirmed that this is possible. [Explanation of symbols]
[0192] 100 Positive electrode current collector 101 Cathode active material layer 102 Positive electrode 105 Negative electrode current collector 106 Negative electrode active material layer 107 Negative electrode 110 Separator 111 Electrolyte 120 Case 121 Electrode 122 electrodes 3010 Mobile phone 3011 Case 3012 Display section 3013 Operation button 3014 External connection port 3015 Speaker 3016 Mike 3017 Operation button 3030 E-book terminal 3031 Case 3032 Shaft 3033 Case 3035 Display section 3037 Display section 3039 Operation button 3041 Speaker 3043 Power supply 3050 Electric Vehicle 3051 Electricity storage device 3053 Control circuit 3055 Computer 3057 Drive unit 3070 Wheelchair 3073 Control Unit 3075 Drive unit 3077 Controller
Claims
1. a total content of impurity elements contained in the lithium iron phosphate is 122 ppm or less based on the weight of the lithium iron phosphate; The lattice constant of the a-axis is 10.3254 × 10 -10 (m) or more 10.3258×10 -10 (m) or less; The lattice constant of the b axis is 6.0035 × 10 -10 (m) or more 6.0052×10 -10 (m) or less; The c-axis lattice constant is 4.6879 × 10 -10 (m) or more 4.6902×10 -10 (m) An electrode material comprising the lithium iron phosphate having the following structure:
2. In claim 1, The lithium iron phosphate is a carbon-supported electrode material.
Citation Information
Patent Citations
Manufacturing method of positive electrode material for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery equipped with the same
JP2007109533A
Compound having olivine-type structure, positive electrode for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery
WO2008105490A1