Neutral solidifying material and soil treatment method
A neutral solidification material with magnesium oxide, sulfates, and a polymer flocculant with a specific acrylamide ratio stabilizes soil strength and pH, enabling effective reuse in construction projects.
Patent Information
- Application Number
- JP2024124400
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2040-02-28
AI Technical Summary
Existing gypsum-based soil solidification materials lack sufficient strength and are prone to strength loss during excavation and transportation, limiting their reuse in construction applications.
A neutral solidification material composed of magnesium oxide, sulfates (aluminum sulfate and ferrous sulfate), and a polymer flocculant with a specific acrylamide unit ratio is used to maintain pH neutrality and enhance soil strength, incorporating a foaming agent for improved handling.
The material achieves high strength soil that maintains pH neutrality, allowing for effective reuse in various construction applications without significant strength loss during transportation or excavation.
Smart Images

Figure 2024138190000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a neutral solidification material and a soil treatment method. [Background technology]
[0002] Soil solidification materials that improve soil strength are used to facilitate the removal and reuse of soft soil and construction waste soil. Soil solidification materials are classified into cement-based, lime-based, gypsum-based, etc. according to the components they contain, and typically, gypsum-based soil solidification materials are used that can maintain the pH of soil after soil improvement near neutral, taking into consideration the conservation of the surrounding environment such as water quality and vegetation. However, gypsum-based soil solidification materials sometimes do not exhibit sufficient strength compared to cement-based materials, and there is room for improvement in this regard.
[0003] For the purpose of improving the strength of improved soil when a soil solidification material is used, Patent Document 1 discloses a soil solidification material consisting of magnesium oxide, aluminum sulfate and / or ferrous sulfate, with the remainder being gypsum. Patent Document 2 discloses a soil improvement material that contains auxiliary materials such as hemihydrate gypsum in addition to metal salts such as metal sulfates, magnesium-containing substances, and polymer-based thickening materials. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2000-109829 A [Patent Document 2] JP 2008-100313 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, although the soil improvement materials described in Patent Documents 1 and 2 were able to maintain the pH of the improved soil near neutral, they did not have sufficient strength development and sometimes could not improve the soil to the desired strength.
[0006] The improved soil obtained by performing a solidification treatment on construction waste soil may be reused either at the site where the construction waste soil was generated or at another site. In the latter case, the improved soil is typically cured for a certain period of time at the site where the construction waste soil was generated and then transported to the site where it will be reused. At this time, the strength of the improved soil may decrease due to the steps of excavation and loosening. As a result, the soil may not be able to achieve sufficient strength at the site where it is to be reused. The soil improvement materials described in Patent Documents 1 and 2 do not consider any improvement in such respects.
[0007] Therefore, an object of the present invention is to provide a neutral solidification material that can obtain improved soil that maintains a pH level close to neutral and is resistant to loss of strength due to excavation and loosening. [Means for solving the problem]
[0008] As a result of intensive research into solving the above problems, the inventors discovered that by using a polymer flocculant having a specific composition, it is possible to maintain the pH of the improved soil while also achieving high strength, thereby completing the present invention.
[0009] That is, the present invention relates to a composition comprising magnesium oxide and At least one sulfate selected from aluminum sulfate, ferrous sulfate, and gypsum; A polymer flocculant having an acrylamide unit and a sodium acrylate unit, The present invention provides a neutral solidification material, in which the composition ratio of the acrylamide units constituting the polymer flocculant is 55 to 90 mol %.
[0010] In a further preferred embodiment of the present invention, there is provided a neutral solidification material containing 1 to 8 mass % of the polymer flocculant.
[0011] In a preferred embodiment of the present invention, there is provided a neutral solidification material containing 10 to 50 mass % of the magnesium oxide.
[0012] Furthermore, the present invention provides a method for treating a mixture of soil and neutral solidification material with a cone index of 800 kN / m2 or more, as measured in accordance with JIS A1228. 2 A process of curing the product until it reaches the above condition is provided. The neutral solidification material includes magnesium oxide, at least one sulfate selected from aluminum sulfate, ferrous sulfate, and gypsum, and a polymer flocculant having polyacrylamide and sodium acrylate as main components, and the composition ratio of the acrylamide units constituting the polymer flocculant is 55 to 90 mol %.
[0013] A further preferred embodiment of the present invention provides a method for treating soil, the method comprising the step of treating the soil containing an aerating agent. Effect of the Invention
[0014] According to the present invention, soil can be improved to have high strength while maintaining the pH close to neutral, so that the improved soil can be reused for a wide range of applications, leading to effective use of resources. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of a method for treating soil using a neutral solidification material, together with an example of a shield machine used in the air bubble shield method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] A preferred embodiment of the present invention will be described below. Note that the present invention is not limited to the following embodiment. In the following description, when it is written "X to Y[Z]" (X and Y are arbitrary numbers, and [Z] is a unit), it means "X[Z] or more and Y[Z] or less" unless otherwise specified.
[0017] The neutral solidification material of the present invention is a material used to obtain soil that maintains a neutral pH and exhibits high strength by mixing with the soil to be improved. Examples of soil to be improved include water-containing soil such as soft soil containing water, and construction waste soil and construction sludge, which are generated secondarily from various construction works such as road construction, tunnel construction using the shield tunneling method, and building construction work. In other words, the neutral solidification material of the present invention is suitably used to solidify at least one of water-containing soil, construction waste soil, and construction sludge. In the following description, "improved soil" refers to soil that has been improved by adding the neutral solidification material of the present invention to the soil to be improved.
[0018] In the present invention, "neutral" refers to "the pH of the improved soil is 5.8 or more and 8.6 or less." This is the value shown in the section on "discharge into public water areas other than sea areas" in the effluent pH standard stipulated in the Water Pollution Control Act. Therefore, improved soil containing the neutral solidification material of the present invention complies with the effluent standard even if, for example, rainwater that has permeated the improved soil flows into groundwater or a river, and the improved soil can be reused with reduced environmental impact without being limited by its application or place of use.
[0019] The neutral solidification material of the present invention contains the following components (1) to (3). (1) Magnesium oxide (2) At least one sulfate selected from the group consisting of aluminum sulfate, ferrous sulfate, and gypsum. (3) Polymer flocculant having an acrylamide unit and a sodium acrylate unit
[0020] The neutral solidification material of the present invention contains magnesium oxide, which is a component that is mainly mixed to solidify the soil to be improved. Examples of magnesium oxide include lightly burned magnesium oxide obtained by burning magnesium hydroxide or magnesium carbonate at 600 to 900°C.
[0021] The content of magnesium oxide in the neutral solidification material is preferably 10 to 50 mass %, more preferably 10 to 47 mass %, and even more preferably 10 to 45 mass %, calculated as anhydrous. By setting the magnesium oxide content as described above, it is possible to achieve a high level of strength development of the soil to be improved and to maintain the pH at neutral. In addition, when the soil to be improved is contaminated with heavy metals or the like, it is possible to insolubilize the heavy metals and suppress the elution of the heavy metals from the improved soil. As a result, there is also an advantage that the environment around the improved soil can be preserved.
[0022] The neutral solidification material of the present invention contains at least one sulfate selected from the group consisting of aluminum sulfate, ferrous sulfate, and gypsum. The sulfate is a component that is mainly blended to maintain the pH of the soil to be improved at neutral.
[0023] The sulfate contained in the neutral solidification material may be any one of aluminum sulfate, ferrous sulfate, or gypsum, or may contain two of aluminum sulfate, ferrous sulfate, and gypsum, or may contain all of aluminum sulfate, ferrous sulfate, and gypsum. From the viewpoint of achieving a high level of strength development of the soil to be improved while maintaining a neutral pH, it is preferable that the sulfates contained in the neutral solidification material contain at least two or more of aluminum sulfate, ferrous sulfate, and gypsum, more preferably contain at least aluminum sulfate and ferrous sulfate, and even more preferably contain all of aluminum sulfate, ferrous sulfate, and gypsum.
[0024] The total content of sulfates in the neutral solidification material is preferably 42 to 89 mass %, more preferably 44 to 87 mass %, and even more preferably 46 to 84 mass %, calculated on an anhydride basis. By adjusting the sulfate content within the above range, it is possible to develop strength in the soil to be improved while maintaining the pH at a neutral and stable level.
[0025] When aluminum sulfate is contained as a sulfate, the content of aluminum sulfate in the neutral solidification material is preferably 0 to 65 mass%, more preferably 0 to 60 mass%, and even more preferably 0 to 55 mass% in terms of anhydride. In other words, as long as the total content of sulfates satisfies the above range, aluminum sulfate may not be contained. By adjusting the aluminum sulfate content within the above range, it is possible to develop the strength of the soil to be improved while maintaining the pH at a neutral and stable level.
[0026] When ferrous sulfate is contained as sulfate, the content of ferrous sulfate in the neutral solidification material is preferably 0 to 30 mass%, more preferably 0 to 25 mass%, and even more preferably 0 to 20 mass% in terms of anhydrous. In other words, as long as the total content of sulfates satisfies the above range, ferrous sulfate may not be contained. By setting the ferrous sulfate content as described above, the pH of the soil to be improved can be maintained neutral while the soil exhibits higher strength. In addition, when improving soil contaminated with heavy metals, the heavy metals can be reduced and insolubilized, thereby suppressing the elution of the heavy metals from the improved soil.
[0027] When gypsum is contained as the sulfate, at least one of anhydrous gypsum, hemihydrate gypsum, dihydrate gypsum, etc. can be used as the gypsum. Gypsum specified in JIS R9151 can also be used. Among these, it is preferable to use hemihydrate gypsum as the gypsum from the viewpoint of achieving a reduction in production costs in addition to improving the strength and maintaining the pH of the soil to be improved. When gypsum is contained as a sulfate, the content of gypsum in the neutral solidification material is preferably 0 to 75 mass%, more preferably 0 to 70 mass%, and further preferably 0 to 65 mass% in terms of anhydride. In other words, as long as the total content of sulfates satisfies the above-mentioned range, gypsum may not be contained. By adjusting the content of gypsum within the above range, the hydraulic properties of the gypsum itself can be utilized to further increase the strength of the improved soil.
[0028] The neutral solidification material of the present invention contains a polymer flocculant having an acrylamide unit and a sodium acrylate unit. The polymer flocculant is a component that is mainly mixed to flocculate the soil particles to be improved and increase the strength of the improved soil, and is preferably a single component or a mixture of organic polymers. The total content of the polymer flocculant in the neutral solidification material is preferably 1 to 8 mass%, more preferably 1 to 7 mass%, and even more preferably 1 to 6 mass%. In the present invention, the term "unit" refers to a monomer unit constituting a polymer.
[0029] A specific embodiment of the polymer flocculant contained in the neutral solidification material is, for example, a copolymer formed by polymerization of acrylamide as a first monomer and sodium acrylate as a second monomer, and the polymer flocculant has an acrylamide unit and a sodium acrylate unit. The copolymer may be in at least one of the following forms: an alternating copolymer in which each monomer is polymerized alternately; a random copolymer in which the arrangement of each monomer is random; a block copolymer having structural units in which the same type of monomers are polymerized successively; and a graft copolymer in which a polymer made of one monomer is branched and bonded to a polymer made of the other monomer.
[0030] One of the characteristics of the polymer flocculant contained in the neutral solidification material is that the acrylamide units constituting the polymer flocculant have a specific composition ratio. In detail, the composition ratio of the acrylamide unit contained in the polymer flocculant is preferably 55 to 90 mol%, more preferably 60 to 85 mol%, and even more preferably 60 to 80 mol%. By using a polymer flocculant in which the acrylamide unit is composed in such a ratio, it is possible to achieve a high level of both strength development of the soil to be improved and maintenance of neutral pH.
[0031] The reason why the use of a polymer flocculant having the above-mentioned ratio of acrylamide units can be modified to improve strength is not clear, but the present inventors speculate as follows. Generally, in the neutral to alkaline pH range (i.e., pH range of 5.8 or higher), the mineral particles that make up the soil particles have a low isoelectric point, so the particles are negatively charged and electrostatic repulsion is likely to occur between the water and the soil particles. Therefore, the soil particles are less likely to form aggregates such as coagulation, and as a result, the strength of the soil as a whole tends to be low. When the above-mentioned polymer flocculant is added, first, the amide group derived from the acrylamide unit is adsorbed on the soil particle surface, and then the carboxyl group derived from the sodium acrylate unit repels each other, spreading the molecular chain of the polymer flocculant, which embraces (takes in) the soil particles and water, effectively agglomerating the soil particles and retaining water between the soil particles, which is thought to improve the strength of the improved soil. In particular, the strength development process by adding the above-mentioned polymer flocculant is thought to proceed in the following order: (i) adsorption of the flocculant to the surface of the soil particles, (ii) cross-linking between the soil particles, and (iii) agglomeration of the soil particles. It is thought that by setting the composition ratio of the acrylamide unit contained in the polymer flocculant to preferably 55 to 90 mol%, the above-mentioned processes (i) and (ii), which are important for strength development, can be progressed in a balanced manner.
[0032] Carbon, hydrogen and nitrogen contained in the polymer flocculant can be measured, for example, by the following method. In detail, about 2 mg of the polymer flocculant to be measured is precisely weighed and introduced into an elemental analyzer (for example, Microcorder JM10, manufactured by J Science Labs) to quantitatively measure the mass of each element. For example, antipyrine (carbon element: 70.2 mass%, hydrogen element: 6.4 mass%, nitrogen element: 14.9 mass%) can be used as the standard.
[0033] The mass ratio (mass%) of carbon element measured by the above-mentioned method is designated as C1, and the mass ratio (mass%) of nitrogen element is designated as N1. From these values, the composition ratios of acrylamide units and sodium acrylate units are calculated by the following method. First, the acrylamide unit has the chemical formula "-CH2-CH(CO-NH2)-", and the unit has 3 carbon atoms and 1 nitrogen atom. In addition, the sodium acrylate unit has the chemical formula "-CH2-CH(COONa)-", and the number of carbon atoms in the unit is 3 and the number of nitrogen atoms in the unit is zero.
[0034] The composition ratio (mol%) of the acrylamide unit in the polymer flocculant is "A", the composition ratio (mol%) of the sodium acrylate unit in the polymer flocculant is "100-A", and based on the number of carbon and nitrogen in each unit, the composition ratio (mol%) of the carbon in the acrylamide unit is expressed as "3×A", and the composition ratio (mol%) of the nitrogen in the acrylamide unit is expressed as "A". The composition ratio (mol%) of the carbon in the sodium acrylate unit is expressed as "3×(100-A)".
[0035] Based on the above-mentioned proportions, the ratio (C5 / N5) of the carbon element composition ratio (C5) to the nitrogen element composition ratio (N5) in the polymer flocculant is calculated by the following formula (a). (C5 / N5)={(3×A)+3×(100-A)} / A=300 / A ···(a)
[0036] Here, C5 / N5 is expressed as "{(C1) / (carbon atom amount)} / {(N1) / (nitrogen atom amount)}" (carbon atom amount = 12, nitrogen atom amount = 14), so the composition ratio A of the acrylamide unit is calculated by the following formula (b). Acrylamide unit composition ratio A (mol%) =300 / {(C1) / (atomic mass of carbon)} / {(N1) / (atomic mass of nitrogen)} ··(b)
[0037] The composition ratio of the sodium acrylate unit is calculated by the following formula (c). Composition ratio of sodium acrylate unit (mol%) = 100-A (c)
[0038] The composition ratio of the sodium acrylate unit contained in the polymer flocculant is preferably 10 to 45 mol %, more preferably 15 to 40 mol %, and further preferably 20 to 35 mol %.
[0039] The magnesium oxide, sulfate and polymer flocculant may each independently be in the form of a powder, or in the form of a liquid or slurry dissolved or dispersed in a solvent such as water. The magnesium oxide and sulfate may each independently be in the form of anhydride or hydrate. From the viewpoint of improving the ease of handling during transportation and use of the neutral solidification material, it is preferable that the magnesium oxide, sulfate and polymer flocculant are all in a powder form. From the same viewpoint, the neutral solidification material of the present invention is preferably in powder form.
[0040] The Blaine specific surface area of magnesium oxide is preferably 6000 to 20000 cm 2 / g, and more preferably 7000 to 20000 cm 2 / g, and more preferably 8000 to 20000 cm 2 / g. By setting the Blaine specific surface area in this range, the workability of the neutral solidification material can be improved, and the strength of the improved soil can be improved by increasing the solidification property of the soil to be improved due to its high hydration activity. In addition, it is preferable that the above-mentioned range of Blaine specific surface area is satisfied when light-burned magnesium oxide is used as the magnesium oxide, since this allows both improvement of workability and improvement of the strength of the improved soil to be achieved at a high level. The Blaine specific surface area of magnesium oxide can be measured, for example, according to JIS R5201:1997 "Physical testing methods for cement" using a Blaine air permeability device.
[0041] The BET specific surface area of magnesium oxide is preferably 5 to 30 m 2 / g, more preferably 7 to 30m 2 / g, more preferably 8 to 30m 2 / g. By setting the range in this way, the workability of the neutral solidification material can be improved, and the strength of the improved soil can be improved by increasing the solidification property of the soil to be improved due to its high hydration activity. In addition, it is preferable that the above-mentioned range of Blaine's specific surface area is satisfied when light-burned magnesium oxide is used as the magnesium oxide, since this allows both improvement of workability and improvement of the strength of the improved soil to be achieved at a high level. The BET specific surface area of magnesium oxide can be measured by a constant volume gas adsorption method using, for example, a high-precision gas adsorption apparatus (BELSORP-mini, manufactured by BEL Japan Co., Ltd.).
[0042] The MgO content in the magnesium oxide is preferably 80% by mass or more, more preferably 85% by mass or more, and even more preferably 90% by mass or more. This content makes it difficult for the pH buffering ability of the surrounding environment of the improved soil to decrease, and can improve the strength of the improved soil.
[0043] The CaO content in magnesium oxide is preferably 3 mass % or less, more preferably 2 mass % or less, and even more preferably 1 mass % or less. This content makes it easier to maintain the pH of the environment surrounding the improved soil neutral, and also improves the strength of the improved soil.
[0044] The MgO content and CaO content in the above-mentioned magnesium oxide can be measured in accordance with JIS M 8853:1998 "Method of chemical analysis of aluminosilicate raw materials for ceramics".
[0045] As long as the effects of the present invention are achieved, the neutral solidification material may further contain additives depending on the properties of the soil to be improved. Examples of additives that can be used include at least one of calcium aluminate minerals such as hydrotalcite and hydrocalumite, silicon-containing minerals such as silica stone, carbonates such as magnesium carbonate and limestone, porous materials such as sepiolite, perlite, zeolite, and silica, and chelating agents. The various additives may each independently be in the form of a powder, or in the form of a liquid or slurry in which they are dissolved or dispersed in a solvent such as water. Furthermore, each of the various additives may be independently in the form of anhydride or hydrate. It is preferable to carry out a blending test in advance and determine whether or not various additives are added and the mixing amounts based on the results.
[0046] The neutral solidification material of the present invention can be used in a solidification treatment method in which the neutral solidification material is mixed with the soil to be improved and solidification treatment is performed. The neutral solidification material when mixed with the soil to be improved may be in the form of a powder or a slurry. In addition, when mixing the neutral solidification material with the soil to be improved, the neutral solidification material and the soil to be improved may be mixed simultaneously, or one of the neutral solidification material and the soil to be improved may be added to the other.
[0047] 1m of soil to be improved 3 The amount of neutral solidification material added per unit area can be changed as appropriate depending on the type and properties of the soil to be improved and the desired developed strength. From the viewpoints of achieving uniform mixing, improved developed strength, and reduced processing costs, the amount is preferably 20 to 200 kg / m. 3 More preferably, it is 20 to 150 kg / m 3 and more preferably 20 to 75 kg / m 3 It is.
[0048] The equipment used to mix the neutral solidification material with the soil to be improved may be any equipment commonly used in the art, such as a backhoe, a backhoe equipped with a mixing bucket, a stabilizer, a self-propelled soil improvement machine, a stationary mixer, a trencher-type agitation mixer, a deep layer mixing machine, a power blender, and a plant mixer.
[0049] An example of a method for treating soil using the neutral solidification material of the present invention will be described below with reference to Fig. 1. The neutral solidification material of the present invention can be used for excavated soil such as mud discharged by shield methods such as the mud pressure shield method and the air bubble shield method as the soil to be treated for improvement. The shield machine 1 shown in Fig. 1 is typically used in the air bubble shield method. The shield machine 1 includes a disk-shaped cutter 11 with multiple holes penetrating in the excavation direction, and a motor 12 connected to the cutter 11 for rotating the cutter 11. The direction in which the drive shaft of the motor 12 extends coincides with the excavation direction. The shield machine 1 shown in the figure also includes a screw conveyor 3 located behind the cutter 11 in the excavation direction, for transporting the excavated soil excavated by the cutter 11 backward in the excavation direction.
[0050] First, the ground is excavated by the shield machine 1. In this embodiment, an air bubble injection pipe 15 is provided for injecting air bubbles into the soil to be excavated in order to increase the fluidity of the excavated soil when excavating the ground. One end of the air bubble injection pipe 15 is connected to an air bubble supplying device (not shown) such as a pump, and the other end opens to the cutter 11 side. The air bubble supplying device may supply air bubbles together with an air foaming agent, for example.
[0051] The excavated soil generated by excavating the ground is transported in the opposite direction to the excavation direction by the chamber 2 and the screw conveyor 3 in the shield machine 1 through holes provided in the cutter 11. The excavated soil containing the air foaming agent has high fluidity and is easy to transport. During transportation by the screw conveyor 3, in order to prevent eruptions caused by pressure changes when the excavated soil is discharged from the screw conveyor 3, an anti-eruption material may be added inside the screw conveyor 3 using a dosing device 4 provided on the front side of the screw conveyor 3 in the excavation direction, and the material may be mixed with the excavated soil 10 while being transported. Next, the excavated soil 10 transported rearward in the excavation direction by the screw conveyor 3 is discharged onto the belt conveyor 5 through a gate 31 located on the rear side of the screw conveyor 3 in the excavation direction, and is transported there.
[0052] The excavated soil 10 transported by the belt conveyor is then placed in a bucket 6, the neutral solidification material of the present invention is added to the excavated soil 10 from a solidification material adding device 20, the soil is mixed by a mixer 30, and the soil is preferably cured for a certain period of time. These operations may be carried out after the excavated soil 10 is transported to the ground through a dump or a vertical shaft, or may be carried out at the tunnel construction site. The curing period can be changed as appropriate depending on the desired strength and the acceptance conditions of the destination, but is preferably about 1 to 14 days, more preferably about 1 to 7 days.
[0053] Through the above steps, improved soil that has developed strength can be obtained. The cured soil is then transported to the desired location, such as a treatment plant or a reuse site, using transport equipment such as a dutch or truck, and is reused or disposed of as necessary. Since the improved soil has a strength that is improved to a level that allows it to be reused, it can be transported as construction material and can be used effectively.
[0054] In this way, by using the neutral solidification material of the present invention, construction waste soil, which in conventional technology would have been treated as industrial waste or soil with limited uses due to its insufficient strength, can be solidified before being transported outside the site where the construction waste soil was generated, and the improved soil can be reused as construction material at the same or a different construction site.
[0055] In particular, when improved soil is used at a construction site different from the one where the construction generated soil was generated, the improved soil is cured for a certain period of time before being transported to the other construction site, but improved soil solidified using the neutral solidification material of the present invention can be transported with its strength adequately maintained even if it is excavated or loosened when it is transported. Furthermore, the improved soil can be reused as it is at the other construction site to which it was transported, without going through any special process.
[0056] In addition, since the soil improved by the neutral solidification material of the present invention has high strength, it can be suitably used, for example, as "Class 2 construction generated soil" as specified in the soil classification standard of the notification "Standards for Utilization of Generated Soil" by the Ministry of Land, Infrastructure, Transport and Tourism, or as "Class 2 treated soil" as specified in the quality standard of the notification "Technical Standards for Utilization of Construction Sludge Treatment Level" by the Ministry of Land, Infrastructure, Transport and Tourism. In detail, the soil improved by the neutral solidification material of the present invention can be suitably used in a wide range of applications, such as backfilling of structures, backfilling of buildings, backfilling of civil engineering structures, embankments for roads, embankments, land development, railway embankments, airport embankments, and water surface reclamation, and for civil engineering or construction work. EXAMPLES
[0057] The present invention will be described in more detail below with reference to examples. The scope of the present invention is not limited to such examples. In the following description, "%" means "mass %" unless otherwise specified.
[0058] [Examples 1 to 6 and Comparative Examples 1 to 5] <1. Preparation of construction waste soil samples> Powdered mudstone was used as the raw soil. The water content of this mudstone measured according to JIS A1203 (hereinafter simply referred to as "water content") was 29.9%, and the wet density measured according to JIS A1210 was 1.75 g / cm. 3 and the pH measured according to JGS 0211-2000 was 8.4. Next, water, an aeration agent (OK-1, manufactured by Pacific Shield Mechanics Co., Ltd.) and an eruption prevention material (SP-α, manufactured by Pacific Shield Mechanics Co., Ltd.) were added to the mudstone in the ratios shown in Table 1 below to obtain two types of construction generated soil replica samples (mud-like samples) with different water contents. Hereinafter, these construction generated soil replica samples will also be referred to as "generated soil sample 1" and "generated soil sample 2".
[0059] [Table 1]
[0060] <2. Preparation of neutral solidification material> As raw materials, magnesium oxide, aluminum sulfate, and ferrous sulfate shown below were mixed with polymer flocculants containing different mol% of acrylamide units and sodium acrylate units in the ratios shown in Table 2 below to prepare a total of 10 types of powdered neutral solidification materials. Magnesium oxide: Light-burned magnesium oxide manufactured by Ube Material Industries, Ltd. Aluminum sulfate: Made in China, aluminum sulfate 14-hydrate Ferrous sulfate: Made in China, ferrous sulfate monohydrate Polymeric flocculants: (1) Neutral solidification materials B and H: Acofloc A-150UH, manufactured by MT Aquapolymer Co., Ltd. (2) Neutral solidification material C: Sanflock AH-9S, manufactured by Sanyo Chemical Industries, Ltd. (3) Neutral solidification materials D and I: Sanfloc AH-4SFA, manufactured by Sanyo Chemical Industries, Ltd. (4) Neutral solidification materials E and J: Acofloc A-125, manufactured by MT Aquapolymer Co., Ltd. (5) Neutral solidification material F: Waterflock PA-041, manufactured by Technica Co., Ltd. (6) Neutral solidification material G: MT Aquapolymer Co., Ltd., Acofloc A-220
[0061] [Table 2]
[0062] <3. Preparation of improved soil> Powdered neutral solidification material was applied to the excavated soil sample 1 at a rate of 30 kg / m 3 The amount of added soil was 40 kg / m 3 The pH of each improved soil was maintained at neutral.
[0063] [Soil strength evaluation] The cone index was measured for the generated soil samples and improved soil according to JIS A1228. For the excavated soil samples, test specimens for measuring the cone index were prepared immediately after mixing of each material, and the cone index of each was measured. In order to confirm the effect of re-kneading, the same improved soil was repeatedly used after 1 day of curing and after 7 days of curing, and specimens for measuring the cone index were prepared for each curing period immediately before the test, and the cone index was measured for each period. The soil strength was estimated by multiplying the cone index measured after the above-mentioned period of indoor curing by 0.9, taking into consideration the effect of strength reduction during excavation and loosening of the improved soil, and differences in the surrounding environment, and this estimated value was 800 kN / m 2 Those with an estimated value of 800 kN / m or more (Class 2 construction generated soil or more) are rated as good (shown as "〇" in Table 3). 2 The results are shown in Tables 1 and 3.
[0064] [Table 3]
[0065] As shown in Table 3, the neutral solidification material of the embodiment, which uses magnesium oxide, sulfate, and a polymer flocculant with a specific acrylamide unit composition ratio, is able to fully develop the strength of the improved soil, regardless of the curing period, compared to the comparative example. This is supported by the fact that the cone index of the generated soil sample was a value that would have been classified as "Class 4 construction generated soil" in the soil classification criteria of the aforementioned notice "Regarding standards for the use of generated soil," but by adding the neutral solidification material, it was improved to an improved soil with a cone index equivalent to Class 2 construction generated soil. In particular, the neutral solidification materials of Examples 1 to 4, in which the content of polymer coagulant in the neutral solidification material is within a suitable range, are able to further increase the strength of the improved soil and are less susceptible to the reduction in strength caused by excavation and loosening, so it can be seen that the improved soil can be suitably reused even if it is cured for a certain period of time after the addition of the neutral solidification material.
[0066] As described above, the neutral solidification material of the present invention can improve the soil to be improved into soil with high strength while maintaining the pH near neutral, so that the improved soil can be reused for a wide range of purposes, leading to effective use of resources.
Claims
1. Magnesium oxide, At least one sulfate selected from aluminum sulfate, ferrous sulfate, and gypsum; A polymer flocculant having an acrylamide unit and a sodium acrylate unit, The composition ratio of the acrylamide units constituting the polymer flocculant is 55 to 90 mol %.
2. The neutral solidification material according to claim 1, containing 1 to 8 mass% of the polymer flocculant.
3. The neutral solidification material according to claim 1 or 2, containing 10 to 50 mass% of magnesium oxide.
4. The method includes a step of curing a mixture of the soil to be treated and the neutral solidification material until the cone index measured in accordance with JIS A1228 is 800 kN / m2 or more; The method for treating soil, wherein the neutral solidification material comprises magnesium oxide, at least one sulfate selected from the group consisting of aluminum sulfate, ferrous sulfate, and gypsum, and a polymer flocculant having an acrylamide unit and a sodium acrylate unit, and the composition ratio of the acrylamide unit constituting the polymer flocculant is 55 to 90 mol %.
5. 5. The method for treating soil according to claim 4, wherein the soil to be treated is one containing an aerating agent.
Citation Information
Patent Citations
Pozzolanic reaction, pozzolanic reaction product and soil improvement utilizing pozzolanic reaction
JP1997157647A
Adjusting agent for digging slurry
JP1997310069A
Processing method of mud generated in air bubble shield method
JP2018015731A
One component type neutral solidification agent
JP2019044054A
Solidifying material for moisture-containing soil and improvement of solidification of moisture-containing soil
JP2000109829A
Cited By
Soil improvement agent and soil improvement method