Metal powder for additive manufacturing

The metal powder with a heat retention layer addresses the inefficiencies of copper powders in additive manufacturing by improving laser absorption and heat retention, resulting in high-density and high-conductivity shaped objects.

JP2024138622APending Publication Date: 2024-10-09JX NIPPON MINING & METALS CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023049194
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Copper and copper alloy powders have low laser absorption rates and high thermal conductivity, leading to inefficient melting or sintering during additive manufacturing, resulting in low-density and low-conductivity shaped objects.

Method used

A metal powder for additive manufacturing is developed, comprising copper-containing particles coated with a heat retention layer, such as chromium oxide, to enhance laser absorption and retain heat, thereby improving melting and sintering efficiency.

Benefits of technology

The metal powder enables the production of high-density and high-conductivity shaped objects by effectively retaining heat and preventing oxidation, thus enhancing the manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138622000001_ABST
    Figure 2024138622000001_ABST
Patent Text Reader

Abstract

To provide a metal powder for additive manufacturing that can yield a molded article with a relatively high conductivity.SOLUTION: A metal powder for use in additive manufacturing comprises a copper-containing particle 1, and a heat retention layer 2 that covers at least part of the surrounding area of the copper-containing particle 1.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This specification discloses metal powders for use in additive manufacturing. [Background technology]

[0002] In metal additive manufacturing, which is one of the additive manufacturing (AM) technologies, for example, a laser beam or electron beam is irradiated onto a thin layer of metal powder based on cross-sectional data of the object to be created, and a layer is formed by melting and solidifying or sintering some of it. By repeatedly depositing metal powder on top of that and irradiating it with a laser beam, etc., the layers are stacked to create the object.

[0003] In order to manufacture a copper or copper alloy object, which has excellent electrical and thermal conductivity, by such additive manufacturing, copper powder or copper alloy powder is used as the metal powder.

[0004] Here, copper and copper alloys not only have low laser absorptivity, but also have high thermal conductivity, so that heat from the laser beam easily escapes. For this reason, copper powder and copper alloy powder cannot be sufficiently melted or sintered unless a laser beam with a higher output than normal is irradiated for a relatively long time, and additive manufacturing may not be performed efficiently. In response to this, for example, Patent Document 1 proposes "copper powder for 3D printers that has high absorptivity during laser irradiation and can be fused and bonded with a low-energy laser by enabling efficient heat input, and a method for manufacturing the same" with the aim of "providing copper powder for 3D printers that has high absorptivity during laser irradiation and can be fused and bonded with a low-energy laser by enabling efficient heat input, and a method for manufacturing the same." The copper powder has an absorptivity of 18.9% to 65.0% for light with a wavelength of λ=1060 nm, and an index indicated by the absorptivity / oxygen concentration for light with a wavelength of λ=1060 nm is 3.0 or more.

[0005] Furthermore, regarding copper alloy powder, Patent Document 2 describes "a metal powder for additive manufacturing, containing 0.10% by mass or more and 1.00% by mass or less of at least one of chromium and silicon, the total amount of the chromium and the silicon being 1.00% by mass or less, and the remainder being copper." Patent Document 2 states that such a "metal powder" "provides an additive manufacturing product made of a copper alloy that can achieve both mechanical strength and electrical conductivity." [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2018-178239 A [Patent Document 2] JP 2016-211062 A Summary of the Invention [Problem to be solved by the invention]

[0007] When additive manufacturing is performed using copper powder or copper alloy powder, when a laser beam is irradiated onto the copper powder or copper alloy powder during manufacturing, the heat from the laser beam may not be sufficiently retained inside the copper powder or copper alloy powder and may dissipate due to the high thermal conductivity of copper, resulting in so-called heat escape. In this case, melting or sintering of the copper powder or copper alloy powder may not proceed sufficiently, resulting in a molded product with low density and electrical conductivity.

[0008] This specification provides a metal powder for additive manufacturing that can produce objects having relatively high electrical conductivity. [Means for solving the problem]

[0009] The metal powder for additive manufacturing disclosed in this specification comprises copper-containing particles that contain copper, and a heat retaining layer that covers at least a portion of the periphery of the copper-containing particles. Effect of the Invention

[0010] The above-mentioned metal powder for additive manufacturing makes it possible to produce a molded object having a relatively high electrical conductivity. [Brief description of the drawings]

[0011] [Figure 1] FIG. 2 is a cross-sectional view showing a schematic diagram of a surface-treated particle contained in the metal powder for additive manufacturing according to one embodiment. [Diagram 2] FIG. 4 is a cross-sectional view showing a schematic diagram of a surface-treated particle contained in a metal powder for additive manufacturing according to another embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, the embodiment of the metal powder for additive manufacturing and the manufacturing method thereof will be described in detail with reference to the drawings. Note that, although reference numerals will be used as necessary in the description, the reference numerals may be omitted when not necessary.

[0013] (metal powder) As shown in Fig. 1, the metal powder for additive manufacturing according to one embodiment (hereinafter, simply referred to as "metal powder") includes surface-treated particles 3 in which at least a portion of the periphery of a copper-containing particle 1 containing copper is covered with a heat retention layer 2. Typically, the powder includes an aggregate of the copper-containing particle 1 and the surface-treated particles 3 including the heat retention layer 2.

[0014] The copper-containing particle 1 is made of copper or a copper alloy containing copper. In the case of the copper-containing particle 1 made of copper, the copper content of the metal powder is, for example, 99.9 mass% or more. In the case of the copper-containing particle 1 made of a copper alloy, the metal powder contains, for example, 90 mass% to 99.9 mass% copper, and may contain, as an alloy element, one or more selected from the group consisting of Al, Cr, Fe, Ni, Nb, P, Si, Zn, and Zr, or, when multiple types are included, may contain them in a total amount of 0.1 mass% to 1 mass%. The copper and alloy element contents of the metal powder can be measured by inductively coupled plasma optical emission spectrometry (ICP-OES).

[0015] The metal powder can improve the laser absorptance by providing the heat retention layer 2 on at least a part of the periphery of the copper-containing particle 1. This is presumably because the copper-containing particle 1 is coated with the heat retention layer 2, and the heat generated by the laser beam is less likely to dissipate from the copper-containing particle 1 during molding due to the coating of the heat retention layer 2, which has a relatively low thermal conductivity, and thus the melting or sintering of the copper-containing particle 1 progresses.

[0016] In addition, in this metal powder, it is expected that the oxidation of the copper-containing particles 1 is suppressed because the heat retention layer 2 prevents oxygen from entering the copper-containing particles 1. As a result, it is believed that the formation of copper oxide due to the oxidation of the copper-containing particles 1 during storage of the metal powder or during modeling when the metal powder is used in additive manufacturing, and further the generation of voids in the modeled object due to the copper oxide, can be effectively suppressed, and a high-density modeled object can be produced.

[0017] The heat retention layer 2 may be a layer of a material having a lower thermal conductivity than the copper-containing particles 1 and being stable even at high temperatures, specifically, for example, an oxide such as Cr2O3, or a metal having a small solid solubility limit in copper such as W, Y, or Nd. Therefore, the heat retention layer 2 may contain Cr and O, and / or may contain at least one selected from the group consisting of W, Y, and Nd.

[0018] Among them, the heat retention layer 2 containing chromium oxide is preferable because the reduction does not proceed up to high temperatures and therefore high laser absorptivity can be maintained up to high temperatures. As chromium oxide, there are several chromium oxides (CrO, Cr2O3, CrO2, CrO3, etc.) according to the oxidation number of chromium, and it is preferable that the heat retention layer 2 contains Cr2O3 among them. When Cr2O3 is contained, it is preferable because it is stable up to high temperatures.

[0019] It can be confirmed by X-ray photoelectron spectroscopy (XPS) that the heat retention layer 2 that covers the periphery of the copper-containing particle 1 contains the above-mentioned chromium oxide or a metal that has a small solid solubility limit in copper. In the case of chromium oxide, a peak appears near the binding energy of 40 to 50 eV.

[0020] When the heat retention layer 2 of the surface-treated particles 3 contains chromium oxide, the metal powder containing such surface-treated particles 3 contains chromium. The chromium content of the metal powder is preferably 50 ppm by mass to 1000 ppm by mass, more preferably 100 ppm by mass to 700 ppm by mass. If the chromium content is too low, the laser absorptivity may not be improved significantly. On the other hand, if the chromium content is too high, the electrical conductivity of a molded object produced using the metal powder may decrease. The chromium content of the metal powder can be measured by inductively coupled plasma optical emission spectrometry (ICP-OES).

[0021] In addition, the coverage of the heat retention layer 2 is related to the degree of heat dissipation suppression of the copper-containing particle 1 by the heat retention layer 2. If the heat retention layer 2 is formed so as to cover at least a part of the periphery of the copper-containing particle 1, heat dissipation from the copper-containing particle 1 during molding can be suppressed, but from the viewpoint of further suppressing heat dissipation, it is preferable that the heat retention layer 2 covers the periphery of the copper-containing particle 1 by 50% or more of the total surface area of ​​the copper-containing particle 1. It is particularly preferable that the coverage of the heat retention layer 2 is almost 100%. The coverage of chromium can be calculated by performing image processing such as binarization on an image obtained using a detection method that can identify the position of an element, such as WDS (wavelength dispersive X-ray analysis). WDS can identify which part of the metal powder contains Cr element and how much of it is present, so it can be used as an index of the coverage of Cr that covers the metal powder. More specifically, for example, the WDS mapping obtained by JXA-8530F manufactured by JEOL Ltd. is binarized at a position of 1 / 10 of the maximum signal intensity using the accompanying software, and the area occupied by Cr (area of ​​the part of 1 / 10 or more of the maximum signal intensity) is calculated from the total area occupied by the metal powder, thereby calculating the coverage rate. Here, the area of ​​the part of 1 / 10 or more of the maximum signal intensity means the area calculated by excluding by binarization the part less than 1 / 10 of the maximum signal intensity detected by the detector when the entire metal powder is analyzed by WDS. For example, if the signal intensity when the entire metal powder is scanned is 15 to 400, the corresponding part will have a signal intensity of 40 to 400.

[0022] The metal powder may contain oxygen. Oxygen may be contained in the metal powder due to, for example, chromium oxide that may be contained in the heat retention layer 2, manufacturing conditions, a naturally generated oxide film, unavoidably mixed oxygen, and the like. The oxygen content of the metal powder is preferably 50 ppm by mass to 2000 ppm by mass, more preferably 50 ppm by mass to 1000 ppm by mass, and even more preferably 100 ppm by mass to 500 ppm by mass. If the oxygen content is too low, the coating such as the heat retention layer 2 may not adhere, and the effect of retaining heat during modeling may not be obtained. On the other hand, if the oxygen content is too high, there is a concern that voids may easily occur in the modeled object due to the generation of copper oxide during modeling.

[0023] The oxygen content of metal powder can be measured by the inert gas fusion method. Here, two measurements are taken for a 1g sample of metal powder using a LECO TCH600, and the average value is taken as the oxygen content.

[0024] In order to reduce the oxygen content of the metal powder and suppress the generation of voids in the molded product, the heat retention layer 2 is desirably formed around the copper-containing particles 1 to a relatively thin thickness of 10 nm to 200 nm, and further 10 nm to 100 nm, when the heat retention layer 2 contains oxygen in the form of chromium oxide or the like as described above. The thickness of the heat retention layer 2 can be measured using X-ray photoelectron spectroscopy (XPS) with the following device and conditions by irradiating the surface-treated particles 3 with Ar ions to dig into the particles and detect the thickness. Depending on the particle size of the metal powder, the detection area described below may include one to three surface-treated particles 3. Equipment: PHI 5000 Versa Probe II manufactured by ULVAC-PHI Inc. Ultimate vacuum: 8.2×10 -8 Pa Excitation source: Monochromatic AlKα Output: 25.0W Detection area: 100μmΦ Sputter rate: 2kV 2mm×2mm (4.2nm / min) (SiO2 equivalent)

[0025] As shown in Fig. 2, the metal powder preferably has surface-treated particles 13 further including a reduced layer 14 that covers at least a portion of the periphery of the heat retention layer 12. When the reduced layer 14 is provided on the heat retention layer 12, it is expected that oxygen that may be contained in the heat retention layer 12, etc., is removed by the reduced layer 14 during shaping. In particular, when the reduced layer 14 is formed on the heat retention layer 12 that contains chromium oxide, it is presumed that the chromium oxide of the heat retention layer 12 is reduced by the reduced layer 14 during shaping, and oxygen is removed, while chromium diffuses into the copper-containing particles 11 or the shaped object. The diffusion of chromium can improve the heat dissipation properties of the shaped object.

[0026] The reduced layer 14 may contain one or more of a group of carbon materials including inorganic carbon such as graphite and organic matter. Among them, the reduced layer 14 preferably contains graphite in terms of laser absorptivity and heat resistance. When the reduced layer 14 contains graphite, oxygen contained in chromium oxides and the like in the heat retention layer 12 may be gasified and lost in the form of carbon monoxide, carbon dioxide, and the like during modeling. In consideration of this, it is desirable to adjust the graphite or carbon content in the metal powder so that no carbon remains in the modeled object obtained after modeling.

[0027] The fact that the reduced layer 14 contains graphite can be confirmed by Raman spectroscopy. More specifically, in a Raman spectrum obtained by Raman spectroscopy, a Raman shift of 1300 cm -1 ~1700cm -1 When a peak of scattering intensity is present within the range, it is recognized that the material contains graphite. For the analysis by Raman spectroscopy, inVia (registered trademark) manufactured by Renishaw Corporation can be used.

[0028] The metal powder may contain carbon due to the reduced layer 14 containing graphite, etc. The carbon content of the metal powder is preferably 20 ppm by mass to 800 ppm by mass. If the carbon content is too low, there is a concern that oxygen may not be sufficiently removed by reduction during shaping. On the other hand, if the carbon content is too high, carbon may remain in the shaped product, which may easily cause voids in the shaped product.

[0029] The carbon content of metal powders can be measured by the inert gas fusion method, in which a 1g sample of metal powder is measured twice using a LECO TCH600, and the average value is taken as the carbon content.

[0030] The average particle diameter D50 of the metal powder is preferably 10 μm to 150 μm. By not making the average particle diameter D50 too small, the metal powder is less likely to fly around during molding, making it easier to handle, and the required fluidity is exhibited, allowing it to be spread in the intended location, improving moldability. By keeping the average particle diameter D50 at a certain level, the energy required to melt or sinter the metal powder with a laser beam can be kept small, and the precision of the molding can be improved.

[0031] The above-mentioned average particle diameter D50 means the particle diameter at which the cumulative volume-based frequency of the metal powder is 50% in the particle diameter histogram (particle diameter distribution graph) obtained by measuring the particle diameter of the metal powder using a laser diffraction / scattering type particle diameter distribution measuring device, and is measured based on JIS Z8825 (2013). More specifically, the average particle diameter D50 can be measured using MT3300EXII manufactured by Microtrack Bell, Inc., with pure water as the solvent and a refractive index of 1.33.

[0032] (Manufacturing method) To produce the metal powder as described above, for example, copper powder or copper alloy powder is first prepared. The copper powder or copper alloy powder may be prepared by purchasing already produced powder or the like, or may be produced by atomization or other various methods.

[0033] The copper powder mainly contains copper-containing particles, and the copper content is preferably 99.9% by mass or more (purity of 3N or more). The copper alloy powder mainly contains copper-containing particles made of a copper alloy. The copper alloy powder may contain at least one alloy element selected from the group consisting of Al, Cr, Fe, Ni, Nb, P, Si, Zn, and Zr, and may have a copper content of 80% by mass or more, further 85% by mass or more, further 90% by mass or more, and further 99% by mass or more.

[0034] The copper powder or copper alloy powder is preferably adjusted in particle size by sieving or the like as necessary to have an average particle diameter D50 of 10 μm to 150 μm. This average particle diameter D50 is the same as the average particle diameter D50 described above for the metal powder, and can be measured by the same method.

[0035] The copper powder or copper alloy powder may contain oxygen. When the oxygen content of the copper powder or copper alloy powder is 500 mass ppm or more, it is preferable to perform a treatment to remove oxygen from the copper powder or copper alloy powder and reduce the oxygen content prior to the formation of the heat retention layer described below. The oxygen removal treatment may be, for example, a method such as washing with an acid.

[0036] Thereafter, the copper-containing particles in the copper powder or copper alloy powder are subjected to a heat retention layer forming treatment to form a heat retention layer that covers at least a part of the periphery of the particles. Specifically, when forming a heat retention layer containing chromium oxide, the copper powder or copper alloy powder is immersed in a dichromate solution having a concentration of 0.1 to 5.0% and a liquid temperature of room temperature to 80°C, and the copper-containing particles are subjected to a chromate treatment by sequentially stirring for 5 to 180 minutes, filtering, and washing with water. The chromium content attached to the copper-containing particles can be increased or decreased by changing the concentration, treatment time, and temperature of the potassium dichromate solution.

[0037] When producing a metal powder containing surface-treated particles 13 as shown in FIG. 2, the metal powder after the heat retention layer forming treatment is further subjected to a treatment for forming a reduced layer that covers at least a part of the periphery of the heat retention layer.

[0038] Here, for example, a ball mill or a mortar can be used to mix the metal powder after the heat retention layer formation process with a carbon-based material for the reduced layer. Alternatively, the metal powder after the heat retention layer formation process can be brought into contact with a liquid carbon-based material by immersion or the like, and then heated for 2 to 12 hours at a temperature of, for example, 400°C to 1000°C in an inert atmosphere such as nitrogen, to form a reduced layer around the heat retention layer. Alternatively, the reduced layer can be formed by chemical vapor deposition (CVD) using a carbon-based material. Examples of carbon-based materials include carbon black, coal tar, pitch, coke, and organic compounds.

[0039] At this time, it is desirable to form a reduction layer around the heat retention layer while adjusting the carbon content to an appropriate value according to the oxygen content of the metal powder.

[0040] By carrying out the above-described process, a metal powder including copper-containing particles, a heat retention layer, and a reduced layer can be produced. EXAMPLES

[0041] Next, the metal powder for additive manufacturing described above was prototyped and its effects were confirmed, which will be described below. However, the description here is merely for illustrative purposes and is not intended to be limiting.

[0042] Example 1 The above copper powder was immersed in a 5 mass % aqueous potassium dichromate solution, and the copper-containing particles of the copper powder were coated with a heat retaining layer to produce a metal powder.

[0043] Example 2 The above copper powder was immersed in a 1 mass % aqueous potassium dichromate solution, and the copper-containing particles of the copper powder were coated with a heat retaining layer to produce a metal powder.

[0044] Example 3 The above copper powder was immersed in a 5% by mass aqueous solution of potassium dichromate to coat the copper-containing particles of the copper powder with a heat retention layer, and then immersed in a coal tar solution and heat-treated at 800°C to produce a metal powder with a reduced layer formed around the heat retention layer.

[0045] Comparative Example 1 The copper powder was used as it was as metal powder without any surface treatment.

[0046] (evaluation) For each of the above metal powders, the average particle size D50, chromium content, coverage of the heat retention layer, carbon content, and oxygen content were measured by the above-mentioned method, as shown in Table 1. The metal powders of Examples 1 to 3 were analyzed by the above-mentioned method, and it was confirmed that the metal powder contained chromium oxide Cr2O3.

[0047] In addition, to confirm the effect of each metal powder, a 20 mm cube was created using the metal powder with a molding machine, and the density and electrical conductivity of the created object were evaluated. The molding machine was Aconity MIDI, manufactured by Aconity3D, with an output of 500 W and a scanning speed of 400 mm / sec.

[0048] The density of the above molded object was determined by measuring the percentage of the area occupied by voids in an image observed with an optical microscope. The relative density was calculated using the formula: relative density = ((area of ​​molded object - area of ​​voids) / area of ​​molded object) x 100 (%). Note that the same calculation can be performed when manufacturing a molded object using metal powder produced using copper alloy powder.

[0049] The electrical conductivity was measured by passing an eddy current through the object using a Sigma Probe SPM350 manufactured by Fisher Instruments, and calculating the electrical conductivity from the current value of the eddy current.

[0050] The results are shown in Table 1.

[0051] [Table 1]

[0052] The object of Comparative Example 1 had a density of 99% and a low electrical conductivity of about 87% IACS, but the object of Example 1 produced under the same conditions had a density of over 99% and achieved 97% IACS, confirming the effect of the surface treatment. Also, in Examples 2 and 3, objects with high electrical conductivity were produced.

[0053] From the above, it was found that the above-mentioned metal powder can be used to produce shaped objects having relatively high electrical conductivity. [Explanation of symbols]

[0054] 1, 11 Copper-containing particles 2, 12 Heat retention layer 3, 13 Surface-treated particles 14 Reduction layer

Claims

1. A metal powder for use in additive manufacturing, comprising: A metal powder for additive manufacturing comprising copper-containing particles that contain copper, and a heat retaining layer that covers at least a portion of the periphery of the copper-containing particles.

2. The metal powder for additive manufacturing according to claim 1 , wherein the heat retention layer contains chromium oxide.

3. The heat retention layer contains Cr as the chromium oxide. 2 O 3 The metal powder for additive manufacturing according to claim 2, comprising:

4. The metal powder for additive manufacturing according to claim 2 or 3, wherein the chromium content is 50 ppm by mass to 1000 ppm by mass.

5. The metal powder for additive manufacturing according to claim 2 or 3, having an oxygen content of 50 ppm by mass to 2000 ppm by mass.

6. The metal powder for additive manufacturing according to any one of claims 1 to 3, wherein the heat retention layer contains at least one selected from the group consisting of W, Y and Nd.

7. The metal powder for additive manufacturing according to any one of claims 1 to 3, further comprising a reduced layer covering at least a portion of the periphery of the heat retention layer.

8. The metal powder for additive manufacturing according to claim 7 , wherein the reduced layer contains graphite.

9. The metal powder for additive manufacturing according to claim 8, having a carbon content of 20 ppm by mass to 800 ppm by mass.

10. The metal powder for additive manufacturing according to any one of claims 1 to 3, wherein the average particle diameter D50 is 10 µm to 150 µm.

Citation Information

Patent Citations

  • Apparatus for manufacturing molded article and method for manufacturing molded article

    JP2017141505A

  • COATED Cu BASED ALLOY POWDER

    JP2021123770A

  • Metal powder for molding metal laminate and molded object manufactured using said metal powder

    WO2019064745A1

  • Copper alloy powder, manufacturing method of laminate molded article and laminate molded article

    JP2016211062A

  • Copper powder, manufacturing method therefor, and manufacturing method of solid molded article

    JP2018178239A