Manufacturing method of slurry for positive electrode mixture and manufacturing method of positive electrode
By using modified polyvinylidene fluoride and controlled CO2 concentration in NMP, the method addresses gelation and gas issues in positive electrode mixture slurries, achieving stable slurry viscosity and reduced gas generation in lithium ion secondary batteries.
Patent Information
- Application Number
- JP2023049548
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2043-03-27
AI Technical Summary
Existing methods for producing positive electrode mixture slurries in lithium ion secondary batteries face issues with gelation due to the reaction of lithium hydroxide (LiOH) formed on the surface of composite oxide particles, leading to alkaline conditions and potential gas generation.
A method involving the use of modified polyvinylidene fluoride with a high molecular weight and controlled carbon dioxide (CO2) concentration in N-methyl-2-pyrrolidone (NMP) to neutralize LiOH, preventing gelation and gas formation by converting LiOH to lithium carbonate (LiCO3), thereby stabilizing the slurry.
The method effectively suppresses gelation and gas generation in the positive electrode mixture slurry, ensuring stable slurry viscosity and reducing gas production in battery cells.
Smart Images

Figure 2024138844000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a positive electrode mixture slurry and a method for producing a positive electrode. [Background technology]
[0002] In non-aqueous electrolyte secondary batteries such as lithium ion secondary batteries, a composite oxide of lithium and a transition metal such as nickel may be used as the positive electrode active material contained in the active material layer of the positive electrode plate. When forming the active material layer of the positive electrode plate, a slurry containing the composite oxide and a binder is prepared. It is known that LiO2 contained in the particle surface of the composite oxide reacts with water to form LiOH, making the slurry alkaline, and the binder becomes three-dimensional and the slurry gels (for example, Patent Documents 1 and 2).
[0003] Patent Document 1 discloses that in order to prevent the gelation of the slurry, a composite oxide is brought into contact with carbon dioxide under dry conditions to neutralize LiOH. Patent Document 2 describes that the pH of the slurry is prevented from becoming alkaline by using a composite oxide that has a pH within a specific range when dispersed in water. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2012-3891 A [Patent Document 2] JP 2000-90917 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the method disclosed in Patent Document 1, the LiOH on the surface of the composite oxide reacts with carbon dioxide, but the lithium (Li) present inside the composite oxide also reacts with carbon dioxide. Since a large amount of lithium carbonate (LiCO3) and water is generated as the product of this reaction, a battery cell made using the slurry described in Patent Document 1 is prone to gas generation. In the method disclosed in Patent Document 2, it is necessary to select a composite oxide that has a specific pH range when dispersed in water.
[0006] An object of the present disclosure is to provide a novel method for producing a positive electrode mixture slurry that can prevent the slurry from becoming gel-like. [Means for solving the problem]
[0007] [1] A method for producing a positive electrode mixture slurry, comprising: The slurry contains an active material represented by the following formula (I) and a modified polyvinylidene fluoride having a weight average molecular weight of 1,000,000 or more, The manufacturing method includes: A step (S1) of supplying carbon dioxide into N-methyl-2-pyrrolidone; and a step (S2) of kneading N-methyl-2-pyrrolidone, the active material, and the modified polyvinylidene fluoride after the step (S1), The method for producing a slurry, wherein the N-methyl-2-pyrrolidone used in the step (S2) has a carbon dioxide concentration of 70 ppm or more. Li (1+x) Ni y Me (1-y) O2(I) [In the formula, 0≦x≦0.1 and 0.8≦y<1, and Me includes two or more elements selected from the group consisting of Mn, Co, Al, and Ti.] [2] The method for producing a slurry according to [1], wherein the carbon dioxide concentration of the N-methyl-2-pyrrolidone used in the step (S2) is 100 ppm or more and 300 ppm or less. [3] The method for producing a slurry according to [1] or [2], wherein the step (S2) is carried out under a temperature condition of 50° C. or less. [4] The method for producing a slurry according to any one of [1] to [3], wherein the step (S2) is carried out in an atmosphere having a carbon dioxide concentration of 10% by volume or more. [5] The method for producing a slurry according to any one of [1] to [4], wherein the step (S1) is a step of bubbling N-methyl-2-pyrrolidone with carbon dioxide. [6] A method for producing a positive electrode mixture slurry, comprising: The slurry contains an active material represented by the following formula (I) and a modified polyvinylidene fluoride having a weight average molecular weight of 1,000,000 or more, The production method includes a step (S3) of kneading N-methyl-2-pyrrolidone, the active material, and the modified polyvinylidene fluoride in an atmosphere having a carbon dioxide concentration of 10% by volume or more. Li (1+x) Ni y Me (1-y) O2(I) [In the formula, 0≦x≦0.1 and 0.8≦y<1, and Me includes two or more elements selected from the group consisting of Mn, Co, Al, and Ti.] [7] The method for producing a slurry according to [6], wherein the step (S3) is carried out at a temperature of 50° C. or less. [8] A method for producing a positive electrode plate having a current collector and an active material layer formed on the current collector, comprising: A step of producing a slurry by the method for producing a positive electrode mixture slurry according to any one of [1] to [7]; and applying the slurry onto the current collector and drying the slurry. Effect of the Invention
[0008] According to the present disclosure, it is possible to prevent the positive electrode mixture slurry from becoming gelled. [Brief description of the drawings]
[0009] [Figure 1] 3 is a flowchart showing a method for producing a positive electrode mixture slurry according to an embodiment. [Diagram 2]10 is a flowchart showing a method for producing a positive electrode mixture slurry according to another embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] [Embodiment 1] (Method for producing positive electrode mixture slurry (1)) 1 is a flow chart showing a method for producing a positive electrode mixture slurry according to an embodiment. The method for producing a positive electrode mixture slurry (hereinafter also referred to as "slurry (1)") according to this embodiment is a method for producing a positive electrode mixture slurry for a non-aqueous electrolyte secondary battery (hereinafter also referred to as "battery"). The slurry (1) can be used to form an active material layer of a positive electrode plate of a battery.
[0011] The slurry (1) contains an active material represented by formula (I) (hereinafter also referred to as "active material (I)") and a modified polyvinylidene fluoride having a weight average molecular weight of 1,000,000 or more (hereinafter also referred to as "PVDF modified material"). Li (1+x) Ni y Me (1-y) O2(I) [In the formula, 0≦x≦0.1 and 0.8≦y<1, and Me includes two or more elements selected from the group consisting of Mn, Co, Al, and Ti.]
[0012] The method for producing the slurry (1) includes the steps of: A step (S1) of supplying carbon dioxide (hereinafter also referred to as "CO2") into N-methyl-2-pyrrolidone (hereinafter also referred to as "NMP"); and a step (S2) of kneading the NMP, the active material (I), and the PVDF modified material after the step (S1). The CO2 concentration of the N-methyl-2-pyrrolidone used in the step (S2) is 70 ppm or more.
[0013] The active material (I) can be used as the active material of the positive electrode plate to increase the capacity of the battery. LiO2 may be present as an impurity on the particle surface of the active material (I). When this LiO2 reacts with the moisture present in the slurry, lithium hydroxide (LiOH) is formed, and the slurry is likely to become alkaline. The PVDF modified body is likely to gel in an alkaline slurry. In the manufacturing method of the slurry (1), CO2 is supplied to NMP in step (S1), and NMP having a CO2 concentration of 70 ppm or more, the active material (I), and the PVDF modified body are kneaded in step (S2). As a result, LiOH reacts with CO2 in the NMP to generate lithium carbonate (LiCO3) and water, so that the slurry (1) is unlikely to become alkaline. As a result, the PVDF modified body is prevented from gelling, and the slurry (1) is prevented from becoming gelled and becoming highly viscous.
[0014] As a method for neutralizing LiOH on the surface of the active material (I), instead of using NMP supplied with CO2, a method of placing the active material (I) before kneading under a CO2 atmosphere can be considered, as shown in a comparative example described later. However, in this method, CO2 also reacts easily with lithium (Li) inside the active material (I), and a relatively large amount of LiCO3 and water is generated, which is thought to make it easier for gas to be generated from the battery. In contrast, the slurry (1) is produced by kneading NMP containing CO2 with the active material (I), so it is thought that LiOH on the surface of the active material (I) reacts with CO2, but does not easily react with Li inside the active material (I). Therefore, when a positive electrode plate is prepared using the slurry (1) and this positive electrode plate is applied to a battery, it is possible to suppress the generation of gas from the battery.
[0015] The method of step (S1) is not particularly limited as long as it can supply CO2 into NMP. For example, it may be a method of bubbling NMP with CO2, or a method of stirring while supplying CO2 into NMP. The amount of CO2 supplied into NMP in step (S1) may be set according to the type of active material (I), the type of PVDF modified material, and the contents thereof in the slurry (1). For example, CO2 may be supplied to NMP so that the concentration of CO2 contained in the NMP used for kneading in step (S2) falls within the range described below. The concentration of CO2 in NMP can be adjusted, for example, by the supply amount, supply rate, and supply time of CO2.
[0016] The concentration of CO2 in the NMP used in step (S2) may be 70 ppm or more, preferably 100 ppm or more and 300 ppm or less, 120 ppm or more and 280 ppm or less, or 150 ppm or more and 250 ppm or less. When the concentration of CO2 in the NMP is within the above range, the PVDF modified material is easily prevented from gelling, and therefore the slurry (1) is easily prevented from becoming gelatinous.
[0017] The temperature condition for carrying out step (S2) is preferably 50° C. or lower, may be 45° C. or lower, or may be 40° C. or lower, and is usually 15° C. or higher. By carrying out step (S2) at a temperature condition within the above range, thermal deterioration of the PVDF modified material can be suppressed.
[0018] The CO2 concentration in the atmosphere in which step (S2) is performed may be 10% by volume or more, 20% by volume or more and 100% by volume or less, or 30% by volume or more and 50% by volume or less. The atmosphere in which step (S2) is performed is, for example, the atmosphere in a kneading vessel in which kneading is performed. The CO2 concentration in the atmosphere in which step (S2) is performed can be adjusted, for example, by a method described in the embodiment described later. The CO2 concentration can be measured using a carbon dioxide concentration meter.
[0019] Step (S2) may include a step of dry-mixing the active material (I) and the PVDF modified material to obtain a mixture (1), and a step of kneading the mixture (1) with NMP after step (S1) to obtain a kneaded product (1).
[0020] The method for producing the slurry (1) may further include a step of mixing the NMP with a conductive material to obtain a conductive paste (1). In this case, the method for producing the slurry (1) may include a step of kneading the above-mentioned kneaded material (1) with the conductive paste (1). The NMP used to obtain the conductive paste (1) is preferably the NMP after the step (S1).
[0021] The active material (I) may be a compound represented by the above formula (I). In formula (I), x may be 0.01≦x≦0.09, 0.03≦x≦0.08, or 0.05≦x≦0.07. In formula (I), y may be 0.81≦y≦0.98, 0.82≦y≦0.95, or 0.83≦y≦0.90. In formula (I), Me is preferably two or more selected from the group consisting of Mn, Co, and Al, and more preferably contains three of Mn, Co, and Al, or two of Mn and Co. The composition of the active material (I) can be determined by high-frequency inductively coupled plasma (ICP) emission spectrometry.
[0022] The active material (I) is, for example, Li (1+0.07) Ni 0.81 Co 0.05 Mn 0.12 Al 0.02 O2 and Li (1+0.01) Ni 0.83 Co 0.12 Mn 0.05 At least one of O2.
[0023] The content of LiOH in the active material (I) before the kneading in step (S2) may be, for example, 0.01% by mass to 0.4% by mass, 0.05% by mass to 0.25% by mass, or 0.1% by mass to 0.23% by mass. The content of LiOH in the active material (I) can be determined by neutralization titration.
[0024] The slurry (1) may contain one or more active materials (I), and may contain a positive electrode active material other than the active material (I). The content of the active material (I) in the slurry is preferably 95% by mass or more and 100% by mass or less, more preferably 95% by mass or more and 99% by mass or less, and may be 96% by mass or more and 98% by mass or less, based on the total amount of the positive electrode active materials in the slurry. When two or more active materials (I) are contained, the content of the active materials (I) refers to the total amount.
[0025] The content of the positive electrode active material (including the active material (I)) in the slurry (1) is, for example, 80% by mass or more and 99% by mass or less, or may be 85% by mass or more and 98% by mass or less, or may be 90% by mass or more and 97% by mass or less, based on the solid content of the slurry (1). When two or more positive electrode active materials are contained, the content of the positive electrode active materials refers to the total amount thereof.
[0026] The weight-average molecular weight of the PVDF modified material may be 1 million or more, may be 1.05 million or more and 2 million or less, or may be 1.1 million or more and 1.5 million or less. The weight-average molecular weight of the PVDF modified material can be measured by GPC (gel permeation chromatography). By using a PVDF modified material having a weight-average molecular weight in the above range, a small amount of the PVDF modified material can be imparted with thixotropy to the slurry (1), and the slurry (1) can be easily dispersed or dissolved therein. In addition, the adhesion strength can be ensured when the slurry (1) is applied to the current collector.
[0027] The PVDF modified material is a product obtained by defluorinating polyvinylidene fluoride (hereinafter also referred to as "PVDF") and introducing functional groups such as polar functional groups. PVDF may be a homopolymer or a copolymer of vinylidene fluoride and a fluorine compound other than vinylidene fluoride, such as tetrafluoroethylene, hexafluoropropylene, or chlorotrifluoroethylene. Examples of the polar functional group include one or more selected from the group consisting of a hydroxyl group (-OH), a carbonyl fluoride group (-COF), a carboxyl group (-COOH), an acid anhydride group, an acrylate group (-CH2=CHCOOH), and a glycidyl methacrylate group (-CH2C(CH3)COOCH2(CHCHO)).
[0028] The content of the PVDF modified material in the slurry (1) is, for example, 0.5% by mass or more and 10% by mass or less, or may be 1% by mass or more and 8% by mass or less, or may be 1% by mass or more and 5% by mass or less, based on the solid content of the slurry (1).
[0029] The content of NMP in the slurry (1) is, for example, 3 mass% or more and 40 mass% or less, or may be 5 mass% or more and 30 mass% or less, or may be 8 mass% or more and 20 mass% or less, based on the total amount of the slurry (1).
[0030] The slurry (1) may contain, in addition to the positive electrode active material such as the active material (I), the above-mentioned conductive material, a binder other than the modified PVDF, and the like.
[0031] The conductive material may be, for example, a carbon material. The carbon material may be, for example, one or more selected from the group consisting of fibrous carbon, carbon black (acetylene black, ketjen black, etc.), coke, and activated carbon. The fibrous carbon may be carbon nanotubes (CNT). The CNT may be single-walled carbon nanotubes (SWCNT) or multi-walled carbon nanotubes such as double-walled carbon tubes (DWCNT). The conductive material may be, for example, 1% by mass or more and 5% by mass or less, or 1.5% by mass or more and 3% by mass or less, based on the solid content of the slurry (1).
[0032] The binder may be, for example, one or more selected from the group consisting of styrene butadiene rubber (SBR), unmodified PVDF, and polytetrafluoroethylene (PTFE).
[0033] [Embodiment 2] (Method for producing positive electrode mixture slurry (2)) 2 is a flow chart showing a method for producing a positive electrode mixture slurry according to another embodiment. The method for producing a positive electrode mixture slurry (hereinafter also referred to as "slurry (2)") according to this embodiment is a method for producing a positive electrode mixture slurry for a battery. The slurry (2) is used to form an active material layer of a positive electrode plate of a battery.
[0034] The slurry (2) contains an active material (I) and a PVDF modified body having a weight average molecular weight of 1,000,000 or more. Examples of the active material (I) and the PVDF modified body include those mentioned above. The content of LiOH in the active material (I) and the weight average molecular weight of the PVDF modified body are, for example, within the ranges mentioned above. The contents of the active material (I), the PVDF modified body, and NMP in the slurry (2) can be within the ranges of the contents described for the slurry (1).
[0035] The method for producing the slurry (2) includes a step (S3) of kneading NMP, the active material (I), and the modified PVDF in an atmosphere having a CO2 concentration of 10% by volume or more.
[0036] As described above, when the active material (I) is used, the slurry tends to become alkaline, which tends to cause gelation of the PVDF modified material. In the method for producing the slurry (2), NMP, the active material (I), and the PVDF modified material are kneaded in an atmosphere with a CO2 concentration of 10% by volume or more, so that LiOH generated in the slurry can react with CO2. As a result, LiOH is consumed to generate LiCO3 and water, which suppresses gelation of the PVDF modified material and suppresses the slurry (1) from becoming gel-like. In addition, gas generation can also be suppressed in a battery cell having a positive electrode plate produced using the slurry (2).
[0037] The concentration of CO2 in the atmosphere in which step (S3) is performed may be 10% by volume or more, 10% by volume or more and 100% by volume or less, 20% by volume or more and 90% by volume or less, 30% by volume or more and 50% by volume or less, or 100% by volume. The atmosphere in which step (S3) is performed is, for example, the atmosphere in a kneading vessel in which kneading is performed. The concentration of CO2 can be measured using a carbon dioxide concentration meter.
[0038] The atmosphere in which step (S3) is performed can be adjusted, for example, by reducing the pressure or creating a vacuum in the kneading vessel and then supplying CO2 into the kneading vessel. The concentration of CO2 in the kneading vessel can be adjusted, for example, by adjusting the pressure in the kneading vessel when the pressure in the kneading vessel is reduced.
[0039] The temperature condition for carrying out step (S3) is preferably 50° C. or lower, may be 45° C. or lower, or may be 40° C. or lower, and is usually 15° C. or higher. By carrying out step (S3) at a temperature condition within the above range, thermal deterioration of the PVDF modified material can be suppressed.
[0040] Step (S3) may include a step of dry-mixing the active material (I) and the PVDF modified material to obtain a mixture (2), and a step of kneading NMP and the mixture (2) to obtain a kneaded product (2). The NMP used in step (S3) may or may not be subjected to the treatment of supplying CO2 described in the above embodiment.
[0041] The method for producing the slurry (2) may further include a step of mixing the NMP with a conductive material to obtain a conductive paste (2). In this case, the method for producing the slurry (2) may include a step of kneading the above-mentioned kneaded material (2) with the conductive paste (2). The NMP used to obtain the conductive paste (2) may not be subjected to the treatment of supplying CO2 described in the above embodiment, or may be subjected to the treatment.
[0042] The slurry (2) may contain, in addition to the positive electrode active material such as the active material (I), a conductive material, a binder other than the PVDF modified material, etc. As the conductive material and the binder, those mentioned above can be used.
[0043] (Manufacturing method of positive electrode plate) The slurries (1) and (2) produced by the above-mentioned production method can be used to form an active material layer of a positive electrode plate. The method for producing a positive electrode plate is a method for producing a positive electrode plate having a current collector and an active material layer formed on the current collector, and includes, for example, A step of obtaining a slurry (1) or (2) produced by the above-mentioned method for producing a slurry; and applying the slurry (1) or (2) onto a current collector and drying the slurry.
[0044] The slurry (1) or (2) may be applied to one or both sides of the current collector. The slurry (1) or (2) applied to the current collector and dried may be compressed as necessary.
[0045] The slurries (1) and (2) are unlikely to gel and are unlikely to become highly viscous, and therefore have excellent handling properties when applied to a current collector. By using the positive electrode plate manufactured by the above manufacturing method, a battery cell in which gas generation is suppressed can be obtained.
[0046] (Nonaqueous electrolyte secondary battery) The battery may include a positive electrode plate formed using the slurry (1) or (2) produced by the above-described method for producing a slurry. The positive electrode plate may be produced, for example, by the above-described method.
[0047] A battery typically includes an electrode assembly and an electrolyte. The battery may further include a case that contains the electrode assembly and the electrolyte. A resin sheet serving as an electrode holder may be disposed between the electrode assembly and the case.
[0048] The electrode assembly may have the above-mentioned positive electrode plate, negative electrode plate, and a separator interposed between the positive electrode plate and the negative electrode plate. The electrode assembly may be of a wound type or a laminated type.
[0049] The negative electrode may have a negative electrode current collector and a negative electrode active material layer formed on the negative electrode current collector. The negative electrode current collector is, for example, a metal foil made of a copper material such as copper or a copper alloy. The negative electrode active material layer includes a negative electrode active material and may further include one or both of a binder and a conductive assistant.
[0050] Examples of the negative electrode active material include carbon-based active materials containing carbon (C) atoms such as graphite; and metal-based active materials containing metal elements such as metal simple substances or metal oxides containing elements selected from the group consisting of silicon (Si), tin (Sn), antimony (Sb), bismuth (Bi), titanium (Ti), and germanium (Ge). Examples of the binder include cellulose-based binders such as carboxymethyl cellulose (CMC), styrene butadiene rubber (SBR), and the like. Examples of the conductive assistant include carbon materials such as fibrous carbon, carbon black (e.g., acetylene black, ketjen black), coke, and activated carbon. Examples of the fibrous carbon include those described above.
[0051] The separator may be a porous sheet (film, nonwoven fabric, etc.) made of a resin such as polyethylene, polypropylene, polyester, cellulose, or polyamide. The porous sheet may have a single-layer structure or a multi-layer structure of two or more layers. The separator may have a functional layer on the surface of the porous sheet. The functional layer may be at least one of a heat-resistant layer and an adhesive layer for bonding to a positive electrode plate and a negative electrode plate.
[0052] The electrolyte may be a non-aqueous electrolyte, for example, a non-aqueous solvent such as an organic solvent containing a supporting salt. Examples of the non-aqueous solvent include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC). Examples of the supporting salt include lithium perchlorate (LiClO4) and lithium hexafluorophosphate (LiPF6).
[0053] The case is a housing that houses the electrode assembly. The case is preferably made of metal, and can be formed using, for example, aluminum, an aluminum alloy, iron, an iron alloy, or the like. EXAMPLES
[0054] The present disclosure will be described more specifically below with reference to examples and comparative examples. Comparative Example 1 (Preparation of Slurry) As the active material (I), Li (1+0.07) Ni 0.81 Co 0.05 Mn 0.12 Al 0.02 O2 and Li (1+0.01) Ni 0.83 Co 0.12 Mn 0.05 O2 was prepared in a mass ratio of 7:3. This active material (I) and a PVDF modified body (weight average molecular weight: 1.1 million) were dry mixed in a closed kneading vessel, and then NMP was added under conditions of 25 to 50°C, and kneaded to a solid content ratio of 87 to 92%. Next, a conductive paste in which a conductive material was dispersed in NMP was added and kneaded to obtain a slurry.
[0055] (Preparation of positive electrode plate) The slurry prepared above was applied to both sides of a current collector, dried, and compressed to form an active material layer, thereby obtaining a positive electrode plate including the current collector and the active material layer.
[0056] (Preparation of negative electrode plate) A negative electrode active material layer containing natural graphite as a negative electrode active material was formed on a negative electrode current collector to obtain a negative electrode plate.
[0057] (Battery cell manufacturing) An electrode assembly was fabricated using the positive and negative electrodes and a separator fabricated above. A battery cell with an energy density of 650 Wh / L was fabricated using the electrode assembly and an electrolyte.
[0058] [Comparative Example 2 and Examples 1 to 3] NMP having a CO2 concentration shown in Table 1 was obtained by bubbling NMP with CO2. The CO2 concentration in NMP was adjusted by adjusting the bubbling time while supplying CO2 at 100 cc / min to 1 L of NMP. The bubbling time was 1 minute (Comparative Example 2), 2 minutes (Example 1), 5 minutes (Example 2), and 10 minutes (Example 3). A slurry of a positive electrode mixture was obtained in the same manner as in Comparative Example 1, except that NMP adjusted to the CO2 concentration shown in Table 1 was used as NMP, and a positive electrode plate, a negative electrode plate, and a battery were produced.
[0059] [Comparative Example 3 and Reference Example 1] The active material (I) was placed in a CO2 atmosphere to neutralize the LiOH on the surface of the active material (I), and the contents of LiOH and Li2CO3 were adjusted as shown in Table 1. A positive electrode mixture slurry was obtained in the same manner as in Comparative Example 1, except that the active material with the LiOH and Li2CO3 contents adjusted to those shown in Table 1 was used, and a positive electrode plate, a negative electrode plate, and a battery were produced.
[0060] [Comparative Example 4, Examples 4 and 5] After the pressure in the kneading vessel was reduced, CO2 was supplied to create a CO2 atmosphere in the kneading vessel. The concentration of CO2 in the kneading vessel was adjusted by adjusting the pressure in the kneading vessel when the pressure in the kneading vessel was reduced to -1 kPa (Comparative Example 5), -10 kPa (Example 4, the pressure in the kneading vessel was 90 kPa in absolute value), and -100 kPa (Example 5, the pressure in the kneading vessel was 1 kPa in absolute value) with respect to atmospheric pressure. Except for the fact that kneading was performed in a kneading vessel adjusted to the CO2 concentration shown in Table 1, a slurry of a positive electrode mixture was obtained, and a positive electrode plate, a negative electrode plate, and a battery were produced in the same manner as in the method described in Comparative Example 1.
[0061] [Active material composition] The composition of the active material (I) was determined by high-frequency inductively coupled plasma (ICP) emission spectrometry.
[0062] [LiOH and Li2CO3 content in active materials] The contents of LiOH and Li2CO3 were determined by neutralization titration for the active materials (for Comparative Example 3 and Reference Example 1, the active materials were neutralized with CO2) before being kneaded with the PVDF modified material and NMP. The results are shown in Table 1.
[0063] [Measurement of weight average molecular weight] The weight average molecular weight of the modified PVDF was measured by gel permeation chromatography (GPC).
[0064] [Concentration of CO2 in NMP] The CO2 concentration in the NMP (NMP after bubbling for Comparative Example 2 and Examples 1 to 3) before kneading with the PVDF modified material and the active material was calculated by the following procedure. Hydrochloric acid was added to the NMP placed in a sealed container to desorb the CO2 dissolved in the NMP, and the gas in the space of the sealed container was analyzed by gas chromatography to calculate the CO2 concentration. At 25°C, when the volume of the NMP in the sealed container was set to 100, the volume of the remaining space in the sealed container (space not occupied by NMP) was set to 500, and the volume of hydrochloric acid was set to 1. The results are shown in Table 1.
[0065] [CO2 concentration in the kneading vessel] The CO2 concentration in the kneading vessel was measured using a carbon dioxide concentration meter. The results are shown in Table 1.
[0066] [Slurry evaluation] Using a spiral viscometer, the viscosity of the slurry immediately after preparation was measured at 25°C, and this was taken as the initial viscosity. For the slurry 7 days after preparation, the viscosity was measured in the same manner as above, and this was taken as the viscosity after storage. If the viscosity after storage was within ±20% of the initial viscosity, it was evaluated as "A", and if it exceeded ±20% of the initial viscosity, it was evaluated as "B". The results are shown in Table 1.
[0067] [Measurement of gas generation rate] The battery cells produced in the examples and comparative examples were activated, and the battery cells were restrained to a fixed size to measure the internal pressure. The internal pressure of the battery cells after a storage durability test in which the battery cells were stored for 60 days at a voltage of 4.2V and a temperature of 60°C was calculated as a relative value with the internal pressure of the battery cell after the storage durability test of Comparative Example 1 set as 100 (reference). The results are shown in Table 1.
[0068] [Table 1]
[0069] From Table 1, it is considered that the slurries obtained in Examples 1 to 3 were hardly gelled and the amount of gas generated from the battery was suppressed because CO2 was supplied to NMP and then kneaded with the active material (I) and the PVDF modified body. In contrast, it is considered that gelled was formed in Comparative Example 1 because NMP to which CO2 was not supplied was used and in Comparative Example 2, CO2 was supplied but in a small amount. In Comparative Example 3 and Reference Example 1, LiOH in the active material (I) before kneading was neutralized with CO2, so that the slurry was prevented from gelling in Reference Example 1, but gas was generated from the battery in both Comparative Example 3 and Reference Example 1.
[0070] From Table 1, it is considered that the slurries obtained in Examples 4 and 5 were less likely to gel and the amount of gas generated from the battery was suppressed because they were kneaded in a kneading pot with a CO2 concentration of 10% by volume or more. In contrast, the slurry obtained in Comparative Example 4 was kneaded in a kneading pot with a CO2 concentration of 1% by volume, which is considered to have caused it to gel.
Claims
1. A method for producing a positive electrode mixture slurry, comprising the steps of: The slurry contains an active material represented by the following formula (I) and a modified polyvinylidene fluoride having a weight average molecular weight of 1,000,000 or more, The manufacturing method includes: A step (S1) of supplying carbon dioxide into N-methyl-2-pyrrolidone; and a step (S2) of kneading N-methyl-2-pyrrolidone, the active material, and the modified polyvinylidene fluoride after the step (S1), The method for producing a slurry, wherein the N-methyl-2-pyrrolidone used in the step (S2) has a carbon dioxide concentration of 70 ppm or more. Li (1+x) Ni y Me (1-y) O 2 (I) [In the formula, 0≦x≦0.1 and 0.8≦y<1, and Me includes two or more elements selected from the group consisting of Mn, Co, Al, and Ti.]
2. 2. The method for producing a slurry according to claim 1, wherein the carbon dioxide concentration of the N-methyl-2-pyrrolidone used in the step (S2) is 100 ppm or more and 300 ppm or less.
3. The method for producing a slurry according to claim 1 , wherein the step (S2) is carried out under a temperature condition of 50° C. or less.
4. The method for producing a slurry according to claim 1 , wherein the step (S2) is carried out in an atmosphere having a carbon dioxide concentration of 10% by volume or more.
5. 2. The method for producing a slurry according to claim 1, wherein the step (S1) is a step of bubbling N-methyl-2-pyrrolidone with carbon dioxide.
6. A method for producing a positive electrode mixture slurry, comprising the steps of: The slurry contains an active material represented by the following formula (I) and a modified polyvinylidene fluoride having a weight average molecular weight of 1,000,000 or more, The method for producing a slurry includes a step (S3) of kneading N-methyl-2-pyrrolidone, the active material, and the modified polyvinylidene fluoride in an atmosphere having a carbon dioxide concentration of 10% by volume or more. Li (1+x) Ni y Me (1-y) O 2 (I) [In the formula, 0≦x≦0.1 and 0.8≦y<1, and Me includes two or more elements selected from the group consisting of Mn, Co, Al, and Ti.]
7. The method for producing a slurry according to claim 6, wherein the step (S3) is carried out under a temperature condition of 50°C or less.
8. A method for producing a positive electrode plate having a current collector and an active material layer formed on the current collector, comprising the steps of: A step of producing a slurry by the method for producing a positive electrode mixture slurry according to any one of claims 1 to 7; and applying the slurry onto the current collector and drying the slurry.
Citation Information
Patent Citations
Manufacture of nonaqueous electrolytic secondary battery
JP1996069791A
Slurry manufacturing device and slurry manufacturing method
JP2018129288A
A nonaqueous electrolyte secondary battery and a method for manufacturing the nonaqueous electrolyte secondary battery
US20220293948A1
Non-aqueous electrolyte secondary battery positive electrode slurry production method and non-aqueous electrolyte secondary battery positive electrode slurry
WO2017138192A1
Method and device for producing cathode slurry for non-aqueous electrolyte secondary battery
WO2019017152A1