Heat-resistant binder and production method thereof

A heat-resistant binder with specific components enhances the strength and heat resistance of wall materials by ensuring even distribution and compatibility, addressing adherence issues and improving heat dissipation.

JP2024138940APending Publication Date: 2024-10-09MIN EKI
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023049673
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Conventional heat-resistant paints fail to reliably adhere to wall materials, leading to peeling and reduced heat resistance and heat dissipation, especially under high temperatures, resulting in deformation, melting, and cracking.

Method used

A heat-resistant binder composed of sodium silicate, potassium silicate aqueous solution, amorphous silica, montmorillonite, Kibushi clay, and silica fine powder, which is evenly distributed and mixed with materials like wood chips to form a wall material, enhancing compatibility and preventing partial solidification.

Benefits of technology

The binder significantly increases the strength and heat resistance of wall materials, improving heat dissipation and preventing damage such as deformation, melting, and cracking even at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138940000001_ABST
    Figure 2024138940000001_ABST
Patent Text Reader

Abstract

To sufficiently increase the strength of a wall material by improving heat resistance and heat dissipation of the wall material.SOLUTION: A heat-resistant binder is produced by compounding not less than 15 wt.% and not more than 60 wt.% of sodium silicate, not less than 8 wt.% and not more than 40 wt.% of potassium silicate aqueous solution, not less than 3 wt.% and not more than 20 wt.% of amorphous silica, not less than 0.2 wt.% and not more than 5 wt.% of montmorillonite, not less than 5 wt.% and not more than 20 wt.% of water, not less than 0.5 wt.% and not more than 10 wt.% of kibushi clay, and not less than 0.5 wt.% and not more than 10 wt.% of silica fine powder. The binder may improve heat resistance and heat dissipation of a wall material.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a heat-resistant binder and a method for producing the same. [Background technology]

[0002] 2. Description of the Related Art Conventionally, for example, in buildings, heat-resistant materials using inorganic materials have been used as wall materials for exterior walls, interior walls, and the like in order to provide fire resistance.

[0003] As heat-resistant materials using inorganic materials, concrete, bricks, cement boards, etc. are used, which do not burn for a specified time after heating is started, do not cause damage such as deformation, melting, cracking, etc. in terms of fire prevention, and do not generate harmful gases.

[0004] However, when exposed to high temperatures of, for example, 1000°C or higher for a long period of time, such as during a fire, the strength of the wall material rapidly decreases and the wall material may suffer deformation, melting, cracks, or other damage.

[0005] In view of this, there has been provided a heat-resistant paint that is applied to the surface of a building's wall material to improve the heat resistance and heat dissipation properties of the wall material (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2004-300415 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, the conventional heat-resistant paint cannot be reliably attached to the surface of the wall material, and when an external force is applied to the wall material, the paint may peel off from the wall material, resulting in a decrease in the heat resistance and heat dissipation of the wall material. In that case, for example, when the wall material is exposed to high temperatures for a long time, the strength of the wall material decreases rapidly, and the wall material may be damaged by deformation, melting, cracks, etc.

[0008] Therefore, it has been considered to form a wall material by using a heat-resistant paint as a heat-resistant binder and mixing it with materials such as wood chips. However, in this case, the compatibility between the various ingredients that make up the heat-resistant paint is not sufficiently high, so the heat-resistant binder may partially solidify, and the strength of the wall material cannot be sufficiently increased.

[0009] The present invention aims to provide a heat-resistant binder and a manufacturing method thereof that can solve the problems of the conventional heat-resistant paints, improve the heat resistance and heat dissipation properties of wall materials, and sufficiently increase the strength of the wall materials. [Means for solving the problem]

[0010] For this reason, the heat-resistant binder of the present invention is composed of an aqueous solution produced by blending 15% by weight or more and 60% by weight or less of sodium silicate, 8% by weight or more and 40% by weight or less of potassium silicate aqueous solution, 3% by weight or more and 20% by weight or less of amorphous silica, 0.2% by weight or more and 5% by weight or less of montmorillonite, 5% by weight or more and 20% by weight or less of water, 0.5% by weight or more and 10% by weight or less of kibushi clay, and 0.5% by weight or more and 10% by weight or less of silica fine powder. Effect of the Invention

[0011] According to the present invention, the heat-resistant binder is composed of an aqueous solution produced by blending 15% by weight or more and 60% by weight or less of sodium silicate, 8% by weight or more and 40% by weight or less of potassium silicate aqueous solution, 3% by weight or more and 20% by weight or less of amorphous silica, 0.2% by weight or more and 5% by weight or less of montmorillonite, 5% by weight or more and 20% by weight or less of water, 0.5% by weight or more and 10% by weight or less of kibushi clay, and 0.5% by weight or more and 10% by weight or less of silica fine powder.

[0012] In this case, wood bushi clay is used as the heat-resistant binder, so when the heat-resistant binder is mixed with wood chips or other materials to be mixed, kneaded, molded, heated, and pressed to form the wall material, the wood bushi clay increases its compatibility with the other mixing materials and also prevents the heat-resistant binder from partially solidifying.

[0013] Therefore, since the wood-bush clay can be evenly distributed throughout the wall material, not only can the strength of the wall material be sufficiently increased, but also the heat resistance of the wall material can be improved.

[0014] In addition, since montmorillonite is used as an additive for amorphous silica, when the heat-resistant binder is mixed with the mixture to form a wall material, the compatibility between the amorphous silica and other compounding materials is improved, and partial solidification of the heat-resistant binder can be further prevented.

[0015] Therefore, since the amorphous silica can be evenly distributed throughout the wall material, even if the wall material is exposed to high temperatures for a long period of time, the amorphous silica can sufficiently radiate far infrared rays, preventing the temperature of the wall material from becoming excessively high, and improving the heat dissipation properties of the wall material. [Brief description of the drawings]

[0016] [Figure 1] FIG. 2 is a diagram showing a composition of a heat-resistant binder according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a diagram showing the heating temperature curve of ISO834. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will be described in detail below with reference to the accompanying drawings. In this case, a heat-resistant binder and a method for producing the same will be described.

[0018] FIG. 1 is a diagram showing a composition of a heat-resistant binder according to an embodiment of the present invention.

[0019] As shown in the figure, the heat-resistant binder in this embodiment is composed of an aqueous solution produced by blending 15% by weight or more and 60% by weight or less of sodium silicate (sodium silicate), 8% by weight or more and 40% by weight or less of potassium silicate aqueous solution, 3% by weight or more and 20% by weight or less of amorphous silica (colloidal silica), 0.2% by weight or more and 5% by weight or less of montmorillonite, 5% by weight or more and 20% by weight or less of water, 0.5% by weight or more and 10% by weight or less of kibushi clay, and 0.5% by weight or more and 10% by weight or less of silica fine powder.

[0020] The sodium silicate, also known as water glass, is a silicate of sodium and is a substance expressed by the chemical formula Na2O·nSiO2·mH2O, which contains water of hydration, and has both the functions of silica (SiO2) and alkali (Na2O).

[0021] When a wall material is made using a heat-resistant binder containing sodium silicate, the function of sodium silicate is imparted to other compounding materials, and the heat resistance and flame retardancy of the wall material can be improved. In addition, the sodium silicate bonds the compounding materials together, so the hardness of the wall material can be increased.

[0022] The potassium silicate aqueous solution is also called potassium water glass, and is a substance that is expressed by the chemical formula K2SiO3, which is a combination of potassium oxide (K2O) and silicon dioxide (SiO2).

[0023] When a heat-resistant binder containing potassium silicate aqueous solution is used to form a wall material, the potassium silicate aqueous solution not only forms a waterproof and deterioration-preventing protective layer on the wall material, but also self-repairs any cracks that occur, thereby significantly improving the strength of the wall material.

[0024] The amorphous silica, also known as diatomaceous earth, is spherical silica (SiO2) that radiates far infrared rays depending on the temperature.

[0025] When a wall material is formed using a heat-resistant binder containing amorphous silica, the amorphous silica radiates far-infrared rays at high temperatures, which not only prevents the temperature of the wall material from rising excessively, but also improves the heat resistance and heat dissipation properties of the wall material.

[0026] The montmorillonite is composed mainly of hydrous silicate of aluminum and magnesium, and has the following properties: (Na,Ca) 0. 33 (Al,Mg)2Si4O 10 It is a white or gray crystalline clay mineral containing water of hydration and is represented by the chemical formula (OH)2·nH2O. It has high ion exchange properties and swells when it absorbs water.

[0027] When montmorillonite is used as an additive for amorphous silica in a heat-resistant binder to form a wall material, the compatibility of the heat-resistant binder with other compounding materials is increased, which not only prevents the heat-resistant binder from partially solidifying, but also makes it possible to sufficiently increase the strength of the wall material.

[0028] The above-mentioned wood-bush clay is a clay containing carbonized plants, and has a color such as brown, dark brown, gray, dark gray, gray-blue, etc., and is a material with high heat resistance, adhesiveness, and plasticity.

[0029] When a heat-resistant binder containing wood-bushi clay is used to form a wall material, the heat-resistant binder is more compatible with the other ingredients, which not only prevents the heat-resistant binder from solidifying partially, but also ensures that the wall material has sufficient strength.

[0030] The silica fine powder is a fine powder of quartz, a raw material ore consisting mostly of silica, and is usually used as an additive in cement materials.

[0031] When a wall material is formed using a heat-resistant binder containing fine silica powder, the raw material of the wall material, such as wood chips, can be solidified quickly.

[0032] Next, an example of a method for producing the heat-resistant binder of the present invention will be described.

[0033] In this embodiment, first, 25 kg of sodium silicate, 15 kg of potassium silicate aqueous solution, 5 kg of amorphous silica, 0.2 kg of montmorillonite, 6 kg of water, 1.5 kg of kibushi clay, and 1.5 kg of silica powder are prepared.

[0034] Then, 25 kg of sodium silicate, 15 kg of potassium silicate aqueous solution, and 5 kg of amorphous silica are charged into a mixing tank serving as a container.

[0035] The order in which the sodium silicate, the potassium silicate aqueous solution and the amorphous silica are added can be freely determined.

[0036] Next, while rotating the agitator that was previously attached to the mixing tank, 0.2 kg of montmorillonite, 6 kg of water, 1.5 kg of kibushi clay, and 1.5 kg of fine silica powder are added to the mixing tank.

[0037] The order in which the montmorillonite, water, kibushi clay and silica fine powder are added can be freely determined.

[0038] Next, the stirrer is rotated for a predetermined time, which in this embodiment is not less than 30 minutes and not more than 120 minutes.

[0039] This produces an aqueous solution of the heat-resistant binder weighing 54.2 kg.

[0040] That is, 25 parts by weight of sodium silicate, 15 parts by weight of potassium silicate aqueous solution, and 5 parts by weight of amorphous silica are put into a mixing tank, and after stirring the contents of the mixing tank, 0.2 parts by weight of montmorillonite, 6 parts by weight of water, 1.5 parts by weight of kibushi clay, and 1.5 parts by weight of fine silica powder are added, thereby producing a heat-resistant binder.

[0041] In this case, sodium silicate accounts for 46% by weight of the range of 15% by weight to 60% by weight, the potassium silicate aqueous solution accounts for 27.6% by weight of the range of 8% by weight to 40% by weight, and amorphous silica accounts for 9.2% by weight of the range of 3% by weight to 20% by weight.

[0042] In addition, montmorillonite accounts for 0.37% by weight of the range of 0.2% by weight or more and 5% by weight or less, water accounts for 11% by weight of the range of 5% by weight or more and 20% by weight or less, kibushi clay accounts for 2.8% by weight of the range of 0.5% by weight or more and 10% by weight or less, and silica powder accounts for 2.8% by weight of the range of 0.5% by weight or more and 10% by weight or less.

[0043] The aqueous solution of the heat-resistant binder thus produced is mixed with at least one of the following materials to be mixed: wood chips, paper, rice husks, rice straw, wheat straw, sawdust, sugarcane pomace, used tea leaves, buckwheat husks, wood waste, charcoal waste, bamboo waste, bamboo charcoal waste, incineration ash, cut paper, cut cloth, crushed grain, perlite, etc., and then kneaded, molded, heated, and pressurized to form a wall material with high heat resistance and heat dissipation. Since the perlite is a foamed obsidian, the use of perlite as a mixture can increase the heat insulation of the wall material.

[0044] In addition, when the heat-resistant binder is mixed with the mixture, since the fine powders of montmorillonite, kibushi clay and silica stone are prone to settling, it is necessary to thoroughly stir the mixture with a stirrer so as not to form any precipitate in the aqueous solution of the heat-resistant binder.

[0045] Next, a heating test was carried out on a wall material formed from a heat-resistant binder, and the results of examining the heat resistance and heat dissipation of the wall material will be described.

[0046] Figure 2 shows the heating temperature curve of ISO 834. In the figure, the horizontal axis represents time and the vertical axis represents temperature.

[0047] In the figure, L1 is the heating temperature curve of ISO834, and the heating test was conducted so that the temperature of the wall material would increase along the heating temperature curve L1, that is, to 945 [°C] after 1 hour from the start of the heating test, 1049 [°C] after 2 hours, and 1110 [°C] after 3 hours.

[0048] A heat-resistant binder was then manufactured by mixing 46% by weight of sodium silicate, 27.6% by weight of potassium silicate aqueous solution, 9.2% by weight of amorphous silica, 0.37% by weight of montmorillonite, 11% by weight of water, 2.8% by weight of kibushi clay, and 2.8% by weight of fine silica powder, and the heat-resistant binder was used to form a wall material.

[0049] When one side of the wall material thus formed was heated so that the temperature increased along the heating temperature curve L1, the temperature of the other side was sufficiently low, and no flame erupted or flaming occurred on the other side. Therefore, it was found that the heat dissipation property of the wall material was improved.

[0050] In addition, when one side of the wall material after heating was observed, no damage such as deformation, melting, cracks, etc. occurred on the one side of the wall material. Therefore, it was found that the heat resistance of the wall material was improved.

[0051] In addition, a heat-resistant binder was manufactured by mixing 15% by weight of sodium silicate, 8% by weight of potassium silicate aqueous solution, 3% by weight of amorphous silica, 0.2% by weight of montmorillonite, 5% by weight of water, 0.5% by weight of kibushi clay, and 0.5% by weight of fine silica powder, and this heat-resistant binder was used to form a wall material.

[0052] In this case, when one side of the wall material was heated so that the temperature increased along the heating temperature curve L1, the temperature of the other side was sufficiently low, and no flame erupted or flaming occurred on the other side.

[0053] Furthermore, when one surface of the wall material was observed after heating, no damage such as deformation, melting, or cracks was observed on the one surface of the wall material.

[0054] Furthermore, a heat-resistant binder was produced by mixing 60% by weight of sodium silicate, 40% by weight of potassium silicate aqueous solution, 20% by weight of amorphous silica, 5% by weight of montmorillonite, 20% by weight of water, 10% by weight of kibushi clay, and 10% by weight of fine silica powder, and the heat-resistant binder was used to form a wall material.

[0055] In this case, when one side of the wall material was heated so that the temperature increased along the heating temperature curve L1, the temperature of the other side was sufficiently low, and no flame erupted or flaming occurred on the other side.

[0056] Furthermore, when one surface of the wall material was observed after heating, no damage such as deformation, melting, or cracks was observed on that surface.

[0057] In this manner, in the present embodiment, since wood bushi clay is blended with the heat-resistant binder, when the heat-resistant binder is mixed with the mixture such as wood chips, kneaded, molded, heated, and pressed to form the wall material, the compatibility between the wood bushi clay and the other blending materials is improved, and partial solidification of the heat-resistant binder can be prevented.

[0058] Therefore, since the wood-bush clay can be evenly distributed throughout the wall material, not only can the strength of the wall material be sufficiently increased, but also the heat resistance of the wall material can be improved.

[0059] Furthermore, since montmorillonite is used as an additive for amorphous silica, when the heat-resistant binder is mixed with the mixture to form a wall material, the compatibility between the amorphous silica and other compounding materials is improved, and partial solidification of the heat-resistant binder can be further prevented.

[0060] Therefore, since the amorphous silica can be evenly distributed throughout the wall material, even if the wall material is exposed to high temperatures for a long period of time, the amorphous silica can sufficiently radiate far infrared rays, preventing the temperature of the wall material from becoming excessively high, and improving the heat dissipation properties of the wall material.

[0061] The present invention is not limited to the above-described embodiment, and various modifications are possible based on the spirit of the present invention, and these modifications are not excluded from the scope of the present invention.

Claims

1. (a) 15% by weight or more and 60% by weight or less of sodium silicate; (b) an aqueous solution of potassium silicate having a concentration of 8% by weight or more and 40% by weight or less; (c) 3% by weight or more and 20% by weight or less of amorphous silica; (d) 0.2% by weight or more and 5% by weight or less of montmorillonite; (e) 5% by weight or more and 20% by weight or less of water; (f) 0.5% by weight or more and 10% by weight or less of wood-bush clay; (g) A heat-resistant binder comprising an aqueous solution produced by blending 0.5% by weight or more and 10% by weight or less of fine powder of silica.

2. (a) Putting sodium silicate, an aqueous potassium silicate solution, and amorphous silica into a container; (b) A method for producing a heat-resistant binder, comprising the steps of: stirring the contents of the container; and then introducing fine powders of montmorillonite, water, kibushi clay, and silica stone into the container.

Citation Information

Patent Citations

  • Coating and manufacturing method thereof

    JP2004300415A