Polyvinyl chloride resin composition for powder molding
The vinyl chloride resin composition with a specific polyester plasticizer addresses fogging and cold resistance issues, ensuring safe and rapid airbag deployment by using a polyester plasticizer with a molecular weight less than 500, composed of polycarboxylic acid and glycol, enhancing fogging and cold resistance.
Patent Information
- Application Number
- JP2023049717
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
Vinyl chloride resin compositions used in powder molding for vehicle airbag compartments face challenges in achieving both excellent fogging properties and cold resistance, particularly under varying temperatures, and need to meet stringent safety standards for rapid airbag deployment without fragment scattering.
A vinyl chloride resin composition for powder molding is developed using a polyester plasticizer with a molecular weight less than 500, composed of a polycarboxylic acid compound and a glycol, specifically 1,4-butanediol and 1,2-propanediol, with a content of 10 to 200 parts by mass, enhancing fogging properties and cold resistance.
The composition achieves both improved fogging properties and cold resistance, ensuring rapid airbag deployment and minimizing fragment scattering, meeting safety standards across a wide temperature range.
Smart Images

Figure 2024138976000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a vinyl chloride resin composition for powder molding. [Background technology]
[0002] In the automotive manufacturing industry, passenger airbag units are structurally integrated with panels such as vehicle interior panels, door panels, dashboards, and instrument panels. The structural integration of the passenger airbag units with the panels is achieved by a rigid carrier. A foam layer is placed on top of the rigid carrier, typically 5-10 mm thick, of compressible foam, which provides a soft feel to the panel and smooths out the uneven surface of the underlying carrier. A decorative skin is placed on top of the foam layer, typically 1-1.5 mm thick, and is made of pliable polyvinyl chloride (PVC), sprayable urethane elastomer materials, thermoplastic elastomers, thermoplastic olefins, thermoplastic polyurethanes, and the like. The PVC skin is typically produced using slush molding. Specifically, PVC compound particles are first fed into a heated mold, which is then continuously turned over to melt and sinter the PVC compound particles on the hot mold surface. The PVC particles are sintered to form a sheet which is cooled and then removed from the mold. Slush molding of PVC compounds is disclosed, for example, in US-A-4,562,025. An alternative to slush molding for producing PVC skins is deep drawing, where a flexible PVC foil or sheet is forced into the desired shape.
[0003] However, such skins must meet many stringent criteria for application to vehicle panels, including color stability, dimensional stability under long term UV exposure at elevated temperatures, and resistance to a wide variety of chemicals such as detergents, human body fluids, etc. A major challenge for these skins is that they must be capable of rapid release to allow for rapid and clean release of the passenger airbag contained beneath the foam layer through an opening in the rigid carrier. To facilitate this release, the skins typically have lines of weakness or tear seams that tear or rupture under the force of inflating the airbag. Over time, the technology to produce such tears has evolved significantly with changing design criteria and increasingly stringent safety standards imposed on the automotive manufacturing industry. In the past, passenger airbag compartment covers were designed as separate objects placed on top of the airbag compartment, but modern automotive design has evolved toward instrument panels with smooth, continuous visible surfaces with built-in airbag compartments. To avoid tear seams becoming visible over time, the skins must have good resistance to aging when exposed to heat and / or UV for extended periods of time.
[0004] However, recent design requirements that require the weakened line or tear seam of the airbag to remain invisible and to withstand aging are balanced against safety standards imposed by the industry that require the skin to be able to release the passenger airbag quickly and cleanly along the weakened line within milliseconds to allow for rapid deployment of the airbag. Another important safety standard is that the skin-foam-carrier sandwich structure should break without scattering particles along the weakened line when the airbag bursts through the cover in all operating conditions that the vehicle may encounter. The flying or heading of fragments from the skin, foam or carrier at high speeds toward the passenger should be minimized and remain below a certain limit in all circumstances. A skin with such characteristics, using a specific tear accelerator, is described in Patent Document 1. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] WO2017 / 046166 Summary of the Invention [Problem to be solved by the invention]
[0006] However, the above safety standards must be met over a wide range of temperatures, at least between -35°C and 80°C, for the instrument panel or any other type of panel containing an airbag in a vehicle. Furthermore, the skin is required to have not only low temperature resistance but also excellent fogging resistance. However, the vinyl chloride resin molded article obtained by powder slush molding the conventional vinyl chloride resin composition has room for improvement in terms of low temperature resistance and fogging resistance.
[0007] The present invention has been made in view of the above-mentioned circumstances, and an object of the present invention is to provide a vinyl chloride resin composition for powder molding which is capable of achieving both excellent fogging properties and cold resistance. [Means for solving the problem]
[0008] Means for Solving the Problems The present inventors have conducted intensive research in view of the above problems and have found that it is possible to achieve both good fogging properties and good cold resistance by powder molding a vinyl chloride resin composition that uses a specific polyester plasticizer as a plasticizer. The present invention has been achieved based on these findings and has the following gist.
[0009] [1] A vinyl chloride resin composition for powder molding comprising a polyester plasticizer and a vinyl chloride resin, wherein the polyester plasticizer has a content of components having a molecular weight of less than 500, as determined by gel permeation chromatography, of 2 area % or less. [2] The polyvinyl chloride resin composition for powder molding according to [1], wherein the polyester plasticizer is a polymer composed of a polycarboxylic acid compound and a glycol, and the glycol has a straight chain portion from a carbon atom bonded to one hydroxyl group of the compound to a carbon atom bonded to another hydroxyl group of the compound, the straight chain portion having 2 or more and 5 or less carbon atoms.
[0010] [3] The polyvinyl chloride resin composition for powder molding according to [1] or [2], wherein the glycol-derived structure constituting the polyester-based plasticizer has a structure derived from 1,4-butanediol and 1,2-propanediol. [4] The polyvinyl chloride resin composition for powder molding according to any one of [1] to [3], wherein the content of the polyester plasticizer is 10 parts by mass or more and 200 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin. [5] An instrument panel comprising the vinyl chloride resin composition for powder molding according to any one of [1] to [4]. Effect of the Invention
[0011] According to the present invention, a vinyl chloride resin composition for powder molding can be provided as a powder slush powder containing a vinyl chloride resin that can achieve both fogging properties and cold resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The present invention will be described in detail below, but the present invention is not limited to the following description, and can be modified as desired without departing from the gist of the present invention. In this specification, when a numerical value or physical property value is enclosed before and after "~", the value before and after the "~" is included. The present invention relates to a vinyl chloride resin composition for powder molding, which contains a polyester plasticizer and a vinyl chloride resin and can be used as a powder slush powder containing a vinyl chloride resin.
[0013] [Vinyl chloride resin composition for powder molding] <Vinyl chloride resin> The vinyl chloride resin used in the present invention refers to a polymer of a monomer containing a vinyl chloride monomer, and the type is not limited as long as it is a homopolymer of a vinyl chloride monomer or a copolymer of a vinyl chloride monomer and a monomer copolymerizable with the vinyl chloride monomer.
[0014] Examples of monomers copolymerizable with the vinyl chloride monomer include vinyl esters such as vinyl acetate, vinyl propionate, and vinyl laurate; acrylic esters such as methyl acrylate, ethyl acrylate, and butyl acrylate; methacrylic esters such as methyl methacrylate and ethyl methacrylate; maleic esters such as dibutyl maleate and diethyl maleate; fumaric esters such as dibutyl fumarate and diethyl fumarate; vinyl ethers such as vinyl methyl ether, vinyl butyl ether, and vinyl octyl ether; vinyl cyanides such as acrylonitrile and methacrylonitrile; α-olefins such as ethylene, propylene, and styrene; vinylidene halides or vinyl halides other than vinyl chloride such as vinylidene chloride and vinyl bromide; and polyfunctional monomers such as diallyl phthalate and ethylene glycol dimethacrylate, but the monomers used are not limited to those mentioned above. These monomers may be used alone or in combination of two or more.
[0015] In the case where a monomer copolymerizable with the vinyl chloride monomer is used in the production of the vinyl chloride resin, the monomer is preferably used in an amount of 30% by mass or less, more preferably 20% by mass or less, based on the total amount of the constituent components of the vinyl chloride resin. If the amount is more than 30% by mass, the inherent performance of the vinyl chloride monomer tends to be lost.
[0016] The method for producing the vinyl chloride resin is not particularly limited, and for example, a normal method such as suspension polymerization, bulk polymerization, fine suspension polymerization, emulsion polymerization, solution polymerization, etc. can be used. Among these, the method using the suspension polymerization is particularly preferred, and the resulting powder is in a state where the grain structure (a characteristic structure seen in suspension-polymerized polyvinyl chloride, which has porosity inside. When kneading is performed, this structure is destroyed and disappears.) is maintained. Since the vinyl chloride resin in this state is particularly easy to mix with liquid chemical substances, the vinyl chloride resin composition for powder molding of the present invention using this is suitable for powder slush powder.
[0017] The average degree of polymerization of the vinyl chloride resin, based on JIS K6721, in view of its processability, moldability, and physical properties is preferably 700 to 6,500, more preferably 1,100 to 4,000. If the average degree of polymerization is equal to or higher than the lower limit, the physical properties of the obtained vinyl chloride resin composition for powder molding tend to be better, while if it is equal to or lower than the upper limit, the processability and moldability tend to be better.
[0018] In the present invention, the vinyl chloride resin may be used alone or in combination of two or more vinyl chloride resins differing in copolymerization composition, type of copolymerization monomer, average polymerization degree, etc. The vinyl chloride resin may be one of commercially available resins or a mixture of two or more of them.
[0019] <Polyester plasticizer> The polyester plasticizer is a plasticizer composed of a polyester polymer obtained by polycondensation of a polycarboxylic acid compound and a polyol compound.
[0020] The polyol compound is a compound having at least two hydroxyl groups, and is preferably a glycol. The number of carbon atoms in the linear chain from the carbon atom bonded to one hydroxyl group of the glycol to the carbon atom bonded to the other hydroxyl group is preferably 2 to 5. Since the compatibility of the polyol compound with the vinyl chloride resin is affected by the number of carbon atoms, it is preferable to set the number of carbon atoms within this range from the viewpoint of sufficient compatibility. The number of carbon atoms in the straight chain portion from a carbon atom bonded to one hydroxyl group to a carbon atom bonded to another hydroxyl group includes the carbon atom bonded to the hydroxyl group. Furthermore, when the glycol has three or more hydroxyl groups, the number of carbon atoms in the straight chain portion from a carbon atom bonded to one hydroxyl group to a carbon atom bonded to another hydroxyl group in this case is the largest number of carbon atoms between carbons bonded to any two hydroxyl groups (including the carbon bonded to a hydroxyl group).
[0021] Examples of the glycol include 1,2-ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,2-pentanediol, 1,3-pentanediol, 1,4-pentanediol, 1,5-pentanediol, etc. In addition, compounds having side chains such as methyl groups and ethyl groups, such as 2-methyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 2-methyl-1,5-pentanediol, 3-methyl-1,5-pentanediol, 3-ethyl-1,5-pentanediol, etc. Among these, 1,4-butanediol and 1,2-propanediol are more compatible with vinyl chloride resins, so it is more preferable to use one or both of 1,4-butanediol and 1,2-propanediol.
[0022] The polycarboxylic acid compound is a compound having at least two carboxyl groups, and examples of the polycarboxylic acid compound include adipic acid and sebacic acid.
[0023] In the present invention, the polyester plasticizer may be used alone or in combination of two or more different polyester plasticizers. The polyester plasticizer may be a commercially available one or a mixture of two or more kinds.
[0024] <Removal of low molecular weight components from polyester plasticizers> The polyester plasticizer preferably has a small amount of low molecular weight components. Specifically, the content of components with molecular weights of less than 500 as determined by gel permeation chromatography (described later) is preferably 2% by area or less, more preferably 1.5% by area or less, and more preferably 1% by area or less. If the content is more than 2% by area, the amount of components that are easily volatilized increases, and it may be difficult to obtain sufficient fogging performance. Furthermore, volatilization occurs during the heat aging test, and it may be difficult to obtain sufficient low-temperature properties after the heat aging test.
[0025] As a method for removing low molecular weight components from this polyester plasticizer, there is a method in which the low molecular weight components are distilled off by a reduced pressure / heat treatment, and by this method, the polyester plasticizer can be purified.
[0026] Although commercially available polyvinyl chloride contains common plasticizers, these plasticizers are absorbed into the polyvinyl chloride and therefore do not affect the present invention.
[0027] <How to confirm the content of low molecular weight components in polyester plasticizers> The content of low molecular weight components in the polyester plasticizer can be confirmed by a measurement method using liquid chromatography, specifically, gel permeation chromatography. Specifically, a size exclusion chromatography column is used as the column, tetrahydrofuran (THF) is used as the mobile phase, and a differential refractive index (RI) detector is used as the detector, and measurements are performed under conditions of a detection wavelength of 254 nm, the area of the resulting graph is calculated, and the content (area ratio) of low molecular weight components (molecular weight of 500 or less) is calculated. Note that the area of the graph of polyester or polyester polymer with a molecular weight of less than 500 is determined by confirming the peak position of polyester or polyester polymer with a molecular weight of around 500, setting the peak position of a molecular weight of 500, and the area of the graph on the lower molecular weight side from that position is the area of polyester or polyester polymer with a molecular weight of less than 500. Note that the molecular weight is calculated in terms of polystyrene.
[0028] <Content of polyester plasticizer in polyvinyl chloride resin composition for powder molding> The content of the polyester plasticizer in the vinyl chloride resin composition for powder molding is preferably 10 parts by mass or more, more preferably 20 parts by mass or more, and more preferably 30 parts by mass or more, based on 100 parts by mass of the vinyl chloride resin. Also, it is preferably 200 parts by mass or less, more preferably 150 parts by mass or less, and more preferably 110 parts by mass or less. If the content of the plasticizer is equal to or more than the lower limit, the flexibility imparting effect due to the inclusion of the plasticizer can be fully exerted, and if it is equal to or less than the upper limit, tensile properties can be imparted.
[0029] <Additives> In addition to the vinyl chloride resin and polyester plasticizer, additives such as heat stabilizers and lubricants can be added to the vinyl chloride resin composition for powder molding according to the present invention, if necessary. Examples of the heat stabilizers include perchlorates, light stabilizers such as hindered amine light stabilizers (HALS), initial adhesion inhibitors, light calcium carbonate, zeolite, phenolic antioxidants, zinc stearate, etc. Examples of the lubricants include calcium hydroxystearate and silicone oil.
[0030] When a heat stabilizer is contained in the vinyl chloride resin composition for powder molding according to the present invention, the content of the heat stabilizer is preferably 0.1 to 20 parts by mass, more preferably 0.2 to 15 parts by mass, and still more preferably 0.3 to 10 parts by mass with respect to 100 parts by mass of the vinyl chloride resin. If the content of the heat stabilizer is equal to or higher than the above lower limit, sufficient heat stability can be exhibited, and if it is equal to or lower than the above upper limit, bleeding (bloom, bleed) of the additive can be suppressed.
[0031] When a lubricant is contained in the vinyl chloride resin composition for powder molding according to the present invention, the content of the lubricant is preferably 0.1 to 5 parts by mass, more preferably 0.3 to 3 parts by mass, and still more preferably 0.5 to 1 part by mass with respect to 100 parts by mass of the vinyl chloride resin. If the content of the lubricant is equal to or higher than the above lower limit, sufficient lubricity can be obtained, and if it is equal to or lower than the above upper limit, the characteristic of sufficiently suppressing bleeding (bloom, bleed) of the additive can be exhibited.
[0032] [Use] The vinyl chloride resin composition for powder molding according to the present invention can be provided as a powder slash powder containing a vinyl chloride resin for powder slash molding, and a slash molded body can be obtained. Examples of the slash molded body include an instrument panel and a door trim.
Examples
[0033] Hereinafter, the content of the present invention will be described more specifically using examples. However, the present invention is not limited to the following examples as long as the gist thereof is not exceeded. The values of various manufacturing conditions and evaluation results in the following examples have the meaning as the preferable values of the upper limit or the lower limit in the embodiments of the present invention, and the preferable range may be a range defined by the combination of the above-mentioned upper limit or lower limit values and the values of the following examples or the values between the examples.
[0034] [Measurement method] [Measurement of low molecular weight plasticizer by LC (liquid chromatography)] From a graph obtained by liquid chromatography (gel permeation chromatography) under the following conditions, the total area and the area of the low molecular weight plasticizer were measured, and the proportion (area ratio) of the low molecular weight plasticizer was calculated. Column: Size exclusion chromatography column TSK-GEL G3000H, ·Mobile phase: THF (flow rate 1mL / min), Column oven temperature: 40℃, Detector: RI detector, temperature: 40°C, detection wavelength: 254 nm When diundecyl phthalate (DUP) (molecular weight: 475), a known plasticizer, was measured under these conditions, a peak appeared at 19.5 minutes. As other plasticizers with molecular weights of around 500 also had peaks at 19.5 minutes, the area ratio after 19.5 minutes was calculated as the component with a molecular weight (polystyrene equivalent) of less than 500.
[0035] <Fogging test> A vinyl chloride resin molded skin (thickness 1 mm) obtained by the powder slush molding described below was punched out into a circle with a diameter of 80 mm, and placed in a test bottle heated to 110°C using an apparatus conforming to DIN 75 201. A glass plate cooled to 60°C was placed on the upper opening of the bottle, and a fogging test was carried out for 5 hours. After the test was completed, the increase in the mass of the glass plate before and after the test was determined. Note that air heated to 110°C by a heater was circulated by a fan inside the apparatus.
[0036] <Cold resistance test> The vinyl chloride resin molded skin (thickness 1 mm) obtained by the powder slush molding described below was punched out to a size of 10 x 40 mm, and the peak temperature of the loss modulus was measured (T1) in accordance with JIS K7244-4 at a frequency of 0.21 Hz, a measurement temperature range of -60°C to +30°C, and a heating rate of 2°C / min. In addition, for the samples obtained by the urethane foaming preparation described below, the peak temperature of the loss modulus was similarly measured (T2) after the completion of a heat aging test (120°C x 400h). Then, (T2-T1) / T1 x 100 was taken as the cold resistance change rate (%) before and after the heat aging test.
[0037] [Raw materials used] The raw materials used in the following examples and comparative examples are as follows. <Vinyl chloride resin> Polyvinyl chloride: Vinyl chloride homopolymer, average degree of polymerization 1300, Shin-Etsu Chemical Co., Ltd.: TK1300, has a grain structure (confirmed with a scanning electron microscope (SEM)). Polyvinyl chloride: polyvinyl chloride resin fine particles, particle size 1-2μm, manufactured by Kaneka Corporation: PSM-31.
[0038] <Polyester plasticizer> 100 parts by weight of the polyvalent carboxylic acid shown below, 60 parts by weight of the glycol shown below, and 30 parts by weight of an end-capping agent (2-ethylhexanol) were mixed in a reaction vessel, an esterification catalyst (tetraisopropyl titanate) was added, and the temperature was raised stepwise from 200°C to 230°C while stirring under a nitrogen stream. This change was monitored by measuring the viscosity of the reaction system with a viscometer and the acid value, hydroxyl value, and water content by chemical analysis at 30-minute intervals, and the reaction was moved to the next stage when it was determined that the reaction had slowed down. This produced a polyester polymer. From the obtained polyester polymer, low molecular weight components were distilled off under conditions of 5 mmHg and 220° C. As a result, the amounts of components having a molecular weight of less than 500 were as shown below.
[0039] Plasticizer A: A polyester plasticizer with less than 2% of components with a molecular weight of less than 500 in the LC measurement below. Plasticizer A-1: Weight average molecular weight: 7300, components with molecular weight less than 500: 1.5% Polycarboxylic acid compounds: adipic acid Glycol: 3-methyl-1,5-pentandiol (3MPD) Plasticizer A-2: Weight average molecular weight: 4700, components with molecular weight less than 500: 1.3% Polycarboxylic acid compounds: adipic acid Glycol: 1,4-butandiol (14BG) and 1,2-propanediol (12PG) in a molar ratio of 3:2 Plasticizer A-3: Weight average molecular weight: 5100, components with molecular weight less than 500: 1.4% Polycarboxylic acid compounds: adipic acid Glycol: 1,4-butandiol (14BG) and 2-methyl-1,3-propandiol (2MPD) in a 1:1 molar ratio
[0040] Plasticizer B: A polyester plasticizer with 2% or more of components with a molecular weight of less than 500 in LC measurement. Plasticizer B-1: Weight average molecular weight: 6300, components with molecular weight less than 500: 3.0% Polycarboxylic acid compounds: adipic acid Glycol: 1,4-butandiol (14BG) and 2,2-dimethyl-1,3-propandiol (NPG) were used in a 1:1 molar ratio. Plasticizer B-2: Weight average molecular weight: 5800, components with molecular weight less than 500: 2.4% Polycarboxylic acid compounds: adipic acid Glycol: 3-methyl-1,5-pentandiol (3MPD) Plasticizer B-3: Weight average molecular weight: 5100, components with molecular weight less than 500: 3.2% Polycarboxylic acid compounds: adipic acid Glycol: 1,4-butandiol (14BG) and 2-methyl-1,3-propandiol (2MPD) in a 1:1 molar ratio
[0041] <Heat stabilizer> Heat stabilizer a: Perchlorate (Kyowa Chemical Industry Co., Ltd.: Alcamizer 5) Heat stabilizer b: Hindered amine light stabilizer (HALS) (ADEKA: LA63-P) Heat stabilizer c: Anti-initiation agent (ADEKA: SP-83) Heat stabilizer d: Light calcium carbonate (Takehara Chemical Industry Co., Ltd.: Neolite SP) Heat stabilizer e: Zeolite (Mizukarizer DS, manufactured by Mizusawa Chemical Industries, Ltd.) Heat stabilizer f: Phenol-based antioxidant (ADEKA: AO60) Heat stabilizer g: Zinc stearate (Nitto Kasei Co., Ltd.: ZN-ST)
[0042] <Lubricant> Lubricant: Calcium hydroxystearate (manufactured by Nitto Kasei: CS-6CP) Lubricant: Silicone oil (Toray Dow Corning: SH200-60,000CS)
[0043] [Examples 1 to 3, Comparative Examples 1 to 3] <Preparation of vinyl chloride resin composition for powder molding> The vinyl chloride homopolymer, polyester plasticizer, heat stabilizer and lubricant components shown in Table 1 were charged into a high-speed stirring mixer in the proportions shown in Table 1, and drying was completed when the resin temperature reached 120° C. After that, vinyl chloride resin fine particles shown in Table 1 were added to the dried powder to obtain a vinyl chloride resin composition for molding as a powder slush powder.
[0044] <Powder slush molding> The powder slush powder (vinyl chloride resin composition for molding) obtained above was melted in a metal mold heated to 236° C. to prepare a vinyl chloride resin molding skin.
[0045] <Urethane foaming> The polyols and isocyanates were placed in a mixer and mixed for 5 seconds at 5,000 rpm. The mixture was placed in the mold having the vinyl chloride resin molding skin obtained above, and after leaving it for 5 minutes, the molded product was removed, thereby attaching the foamed polyurethane to the vinyl chloride resin molding skin.
[0046] [Table 1]
[0047] [Evaluation Results] As shown in Table 1, Examples 1, 2, and 3, which used polyester plasticizers A-1, A-2, and A-3, each of which contains less than 2% of components with a molecular weight of less than 500, showed a very good result of a fogging value of 1%. On the other hand, Comparative Examples 1, 2, and 3, which used polyester plasticizers B-1, B-2, and B-3, each of which contains 2% or more of components with a molecular weight of less than 500, showed a poor tendency of a fogging value of 5 to 10%. Furthermore, the rate of change in cold resistance before and after the heat aging test was 5 to 9% for Examples 1, 2, and 3, which used polyester-based plasticizers A-1, A-2, and A-3, respectively, in which the molecular weight of components less than 500 was less than 2%, while the rate of change was 14 to 17% for Comparative Examples 1, 2, and 3, which used polyester-based plasticizers B-1, B-2, and B-3, respectively, in which the molecular weight of components less than 500 was 2% or more, showing a similar trend to that of the fogging properties.
Claims
1. A vinyl chloride resin composition for powder molding comprising a polyester plasticizer and a vinyl chloride resin, The vinyl chloride resin composition for powder molding is characterized in that the polyester plasticizer has a content of components having a molecular weight of less than 500 of 2 area % or less as measured by gel permeation chromatography.
2. 2. The polyvinyl chloride resin composition for powder molding according to claim 1, wherein the polyester plasticizer is a polymer consisting of a polycarboxylic acid compound and a glycol, and the glycol has a straight chain portion from a carbon atom bonded to one hydroxyl group of the compound to a carbon atom bonded to another hydroxyl group, the straight chain portion having 2 or more and 5 or less carbon atoms.
3. 3. The vinyl chloride resin composition for powder molding according to claim 1, wherein the glycol-derived structure constituting the polyester plasticizer has a structure derived from 1,4-butanediol and 1,2-propanediol.
4. 3. The polyvinyl chloride resin composition for powder molding according to claim 1, wherein the content of the polyester plasticizer is 10 parts by mass or more and 200 parts by mass or less per 100 parts by mass of the polyvinyl chloride resin.
5. 3. An instrument panel comprising the vinyl chloride resin composition for powder molding according to claim 1 or 2.
Citation Information
Patent Citations
Flexible molded skin
WO2017046166A1