Method for evaluating bending property of molded object

A method for evaluating bendability in steel sheets using surface hardness measurement and judgment thresholds addresses the limitations of existing tests, providing accurate assessments for complex shapes by correlating hardness with bending angles and accounting for structural changes.

JP2024139029AActive Publication Date: 2024-10-09NIPPON STEEL CORPORATION

Patent Information

Application Number
JP2023049802
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09
Estimated Expiration
2043-03-27

AI Technical Summary

Technical Problem

Existing methods for evaluating the bendability of steel sheets, such as the VDA bending test, are inadequate for complex shapes like automobile parts, as they require specific test pieces that are difficult to prepare and do not account for changes in mechanical properties due to thermal history and strain during forming.

Method used

A method involving surface hardness measurement with a load of 15 μm to 100 μm indentation depth, using Vickers hardness and judgment thresholds, to evaluate bendability based on the relationship with maximum bending angles, considering factors like metal structure, decarburization index, and thickness, with optional softening layers to improve deformability.

Benefits of technology

Enables accurate and reliable evaluation of bendability in complex shapes by correlating surface hardness with maximum bending angles, allowing for easier assessment of steel sheet quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139029000001_ABST
    Figure 2024139029000001_ABST
Patent Text Reader

Abstract

To provide a method for evaluating the bending property of a molded object which can be performed more easily.SOLUTION: The method for evaluating the bending performance of a molded object according to an embodiment of the present invention is a method for evaluating the bending property of a molded object obtained by performing pressing processing on a steel plate, and includes: a measurement step of applying a load with an indentation depth of more than 15 μm and 100 μm at largest on a surface of a test piece cut off from the molded object and measuring the surface hardness; and an evaluation step of evaluating the bending depth of the molded object on the basis of the surface hardness and the determination threshold value.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for evaluating the bendability of a molded body. [Background technology]

[0002] Steel plates are formed into various shapes depending on the application. For example, Patent Document 1 discloses a method for evaluating the crack resistance of a metal plate, which includes a step (1) of performing a bending test of a metal plate in accordance with the bending test specified in VDA Standard 238-100 to obtain a load-bending angle curve showing the relationship between the load and bending angle of the metal plate, and a step (2) of evaluating the crack resistance of the metal plate based on the relationship between the load and bending angle in a region exceeding the limit bending angle α in the load-bending angle curve. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2016-080464 A Summary of the Invention [Problem to be solved by the invention]

[0004] Steel sheets are formed, for example, by hot working such as hot stamping or cold working, and the mechanical properties of the steel sheet may change before and after forming due to the thermal history during hot stamping, the introduction of strain during cold forming, etc. Therefore, the method of predicting the bendability of a formed body based on the evaluation results of the mechanical properties of the steel sheet before pressing, as described in Patent Document 1, may not be able to appropriately evaluate the quality of the formed body in terms of its mechanical properties.

[0005] In addition, even if one attempts to perform a bending test (VDA bending test) specified in VDA Standard 238-100 using a molded body, it is often impossible to prepare a 60 mm square flat plate required as a test piece for the VDA bending test. In particular, many automotive parts have complex shapes, making it difficult to prepare the above test pieces from the automotive parts. For this reason, it is often impossible to directly apply the VDA bending test to molded bodies that contain automotive parts.

[0006] The present invention has been made in view of the above-mentioned circumstances, and has an object to provide a method for evaluating the bendability of a molded body that can be carried out more simply. [Means for solving the problem]

[0007] The gist of the present invention is as follows. [1] A method for evaluating the bendability of a formed body according to one embodiment of the present invention is a method for evaluating the bendability of a formed body obtained by press working a steel plate, and includes a measurement step of measuring the surface hardness of the formed body by applying a load to the surface of a test piece cut out from the formed body such that the indentation depth is more than 15 μm and not more than 100 μm, and an evaluation step of evaluating the bendability of the formed body based on the surface hardness and a judgment threshold value. [2] In the method for evaluating bendability described in [1] above, the judgment threshold value may be determined based on the relationship between the maximum bending angle measured in accordance with the bending test defined in VDA Standard 238-100:2017 for each of a plurality of test steel plates having strengths corresponding to the strength of the steel plate to be evaluated constituting the formed body, and the Vickers hardness measured by applying a load equal to the load applied in the measurement step to the surface of the plurality of test steel plates. [3] In the method for evaluating the bendability of a formed body according to the above [2], at least two of the plurality of test steel plates may have different decarburization index values. [4] In the method for evaluating bendability described in [2] or [3] above, the metal structure at a 1 / 4 depth position of the steel plate constituting the formed body, and the metal structure at a 1 / 4 depth position of at least two of the plurality of test steel plates may have a total volume fraction of martensite, bainite and tempered martensite of 85% or more. [5] In the method for evaluating bendability described in [4] above, the metal structure in the surface layer of the steel plate constituting the formed body and the metal structure in the surface layer of at least two of the plurality of test steel plates may have a total volume fraction of martensite, bainite and tempered martensite of 75% or more. [6] In the method for evaluating bendability described in any one of [2] to [5] above, all of the plurality of test steel plates may have the same plate thickness, and the plate thickness of the steel plate constituting the formed body may be the same as the plate thickness of the plurality of test steel plates. [7] In the method for evaluating bendability described in [2] above, all of the plurality of test steel plates have different decarburization index values, a sum of the volume fractions of martensite, bainite and tempered martensite in the metallographic structure at the 1 / 4 depth position is 85% or more, and are the same plate thickness as each other, and the steel plate constituting the formed body may have a sum of the volume fractions of martensite, bainite and tempered martensite in the metallographic structure at the 1 / 4 depth position of 85% or more, and be the same plate thickness as the plurality of test steel plates. [8] In the method for evaluating bendability described in any one of [2] to [7] above, the molded product has a specific softening layer provided in a plate thickness direction from the surface, the hardness of the central portion in the plate thickness direction in the portion where the specific softening layer is provided is 400 Hv or more, the specific softening layer is a region having a hardness that is at least 10 Hv lower than the hardness of the central portion in the plate thickness direction in the portion where the specific softening layer is provided, the thickness of the specific softening layer is 2% or more and less than 20% of the plate thickness in the portion where the softening layer is provided, and the hardness of the specific softening layer on the surface is 400 Hv or more. The hardness of the specific softened layer in the thickness direction is 0.5 to 0.9 times that of the center part in the thickness direction of the steel plate in the portion where the specific softened layer is provided, and the specific softened layer has a first hardness change region that is a region from the surface to 40% of the thickness of the specific softened layer in the thickness direction of the steel plate, and a second hardness change region that is a region of the specific softened layer that is not the first hardness change region, and the absolute value ΔHv1 of the hardness change in the thickness direction in the first hardness change region is greater than the absolute value ΔHv2 of the hardness change in the thickness direction in the second hardness change region. [9] In the method for evaluating bendability according to any one of [2] to [8] above, the steel plate constituting the formed body may have a decarburization index value of 0.085 or more. Effect of the Invention

[0008] According to the above-described aspect of the present invention, the bendability of a molded body can be evaluated more easily, and a highly reliable evaluation of the bendability is possible. [Brief description of the drawings]

[0009] [Figure 1] FIG. 11 is a diagram showing an example of a change in hardness of a specific softening layer. [Diagram 2] 1 is a graph plotting the surface hardness and maximum bending angle of each test steel plate for each applied load in Vickers hardness measurement in the examples. [Diagram 3] FIG. 2 is a schematic diagram of a molded body in an example. [Figure 4] 3 is a graph in which the surface hardness and maximum bending angle of the test specimens are plotted on the graph shown in FIG. 2. [Diagram 5] 1 is a graph plotting the surface hardness (Vickers hardness) and maximum bending angle of test steel sheets in Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, a method for evaluating the bendability of a molded body according to an embodiment of the present invention will be described with reference to the drawings. However, the present invention is not limited to the examples described below. In addition, the dimensions and ratios of each component in the drawings do not represent the actual dimensions and ratios of each component.

[0011] <Method for evaluating the bendability of molded products> The method for evaluating the bendability of a formed body according to one embodiment of the present invention is a method for evaluating the bendability of a formed body obtained by pressing a steel sheet, and includes a measuring step of measuring the surface hardness of the formed body by applying a load that results in an indentation depth of more than 15 μm and not more than 100 μm on the surface of a test piece cut out from the formed body, and an evaluation step of evaluating the bendability of the formed body based on the surface hardness and a judgment threshold value. The method will be described in detail below.

[0012] (Measurement step) In the measuring step, a load is applied to the surface of a test piece cut out from the molded body such that an indentation depth is more than 15 μm and not more than 100 μm, and the surface hardness of the molded body is measured.

[0013] The molded body is obtained by pressing a steel plate. The steel plate constituting the molded body (the steel plate pressed into the molded body) is not particularly limited and may be a steel plate having a known chemical composition and metal structure. When the molded body is used as an automobile member, the steel plate may have a tensile strength of 1470 MPa or more (for example, 1.5 GPa class, 1.8 GPa class, 2.0 GPa class, 2.5 GPa class or more).

[0014] In the metal structure at the 1 / 4 depth position of the steel plate constituting the formed body, the total volume fraction of martensite, bainite, and tempered martensite is preferably 85% or more. If the total volume fraction of martensite, bainite, and tempered martensite is 85% or more, the steel plate can be evaluated as a steel plate applicable to formed bodies for applications requiring high strength. In addition, martensite, bainite, and tempered martensite may crack at the interface with other phases. If the total volume fraction of martensite, bainite, and tempered martensite is 85% or more, the ratio of other phases is small, so that cracks are unlikely to occur at the interface between the martensite, bainite, and tempered martensite phase and other phases. Therefore, in the evaluation step described below, when evaluating bendability based on the relationship between the maximum bending angle measured in accordance with the bending test specified in VDA Standard 238-100:2017 and the Vickers hardness measured by applying a load equal to the load applied in the measurement step, a more accurate evaluation can be performed. Here, the other phases refer to one or more of ferrite, pearlite, cementite, and retained austenite.

[0015] Furthermore, the metal structure of the surface layer of the steel plate constituting the formed body preferably has a total volume ratio of martensite, bainite and tempered martensite of 75% or more. If the total volume ratio of martensite, bainite and tempered martensite in the surface layer is 75% or more, the ratio of other phases is small, so cracks are unlikely to occur at the interfaces between martensite, bainite and tempered martensite and other phases. Therefore, when a load is applied to the surface of the test piece, cracks at the interfaces are suppressed, and bendability can be evaluated more accurately. Here, the other phases are one or more of ferrite, pearlite, cementite and retained austenite. The surface layer here refers to the range from the surface to 50 μm in the plate thickness direction.

[0016] The metal structure is specified by the following method. That is, for the metal structure of the formed body, a test piece is taken from any position 50 mm or more away from the end face of the formed body, in a cross section parallel to the rolling direction and parallel to the plate thickness direction, so that the metal structure at the surface layer and at the 1 / 4 depth position can be observed. However, if it is not possible to take a sample from any position 50 mm or more away from the end face of the formed body, the above test piece is taken from a position avoiding the end. The same applies to the metal structure of the test steel plate. Note that the end face of the formed body refers to the outermost circumference of the formed body in the longitudinal or lateral direction, and the surface having a cut part in that part. The cross section of the test piece is polished using silicon carbide paper of #600 to #1500, and then finished to a mirror surface using a liquid in which diamond powder with a grain size of 1 to 6 μm is dispersed in a diluent such as alcohol or pure water. Next, the sample is polished using colloidal silica that does not contain an alkaline solution at room temperature to remove the strain introduced into the surface layer of the sample. At any position in the longitudinal direction (rolling direction) of the cross section of the polished test piece, a region extending from a position 1 / 8 of the plate thickness from the surface to a position 3 / 8 of the plate thickness from the surface is measured by an electron backscatter diffraction method at a measurement interval of 0.1 μm, with the position of 1 / 4 of the plate thickness from the surface being the center, to obtain crystal orientation information of the region. The structure specified by the obtained crystal orientation information is regarded as the metal structure at the 1 / 4 depth position. In addition, a region 50 μm deep from the surface in the plate thickness direction and 200 μm in the longitudinal direction is measured by an electron backscatter diffraction method at a measurement interval of 0.1 μm to obtain crystal orientation information. The structure identified by the obtained crystal orientation information is regarded as the metal structure in the surface layer. For the measurement, a device consisting of a thermal field emission scanning electron microscope (JEOL JSM-7001F) and an EBSD detector (TSL DVC5 detector) is used. The degree of vacuum in the device is 9.6×10 -5 The conditions are: 1. Vapor pressure: 1 Pa or less, 2. Acceleration voltage: 15 kV, probe current level: 13, and electron beam irradiation level: 62. The measurement is performed by setting the phase to "iron-α" and "iron-γ". The same area as the EBSD measurement area is observed at a magnification of 1000x or more using a thermal field emission scanning electron microscope (JEOL JSM-7001F).

[0017] When observing this area, a Vickers indentation is made at three of the four corners of the EBSD measurement area within 100 μm of each of the four corners so that the observation position can be identified. The surface contamination is then polished away, leaving the structure of the observation surface, and the surface is etched with nital. Using the Vickers indentations as a guide, it is possible to observe the same area as the EBSD observation surface. Contamination can be removed by buffing with alumina particles with a particle size of 0.1 μm or less, polishing with colloidal silica that does not contain an alkaline solution at room temperature, or by Ar ion sputtering.

[0018] Next, the crystal orientation information obtained by EBSD measurement is used to calculate the area ratio of the retained austenite using the "PhaseMap" function installed in the software "OIMAnalysis (registered trademark)" attached to the EBSD analyzer. When calculating the area ratio, the crystal structure of which is fcc is determined to be retained austenite.

[0019] In addition, for regions with a bcc crystal structure, the "Grain Average Misorientation" function included in the "OIMAnalysis (registered trademark)" software provided with the EBSD analysis device is used to determine whether the region is cementite, pearlite, ferrite, bainite, martensite, or tempered martensite, and the area ratio is measured. Specifically, under the condition that a boundary where the crystal orientation difference is 15° or more is defined as a grain boundary (15° grain boundary), a region where the Grain Average Misorientation value (GAM value) is 3.0° or less is determined to be ferrite. In addition, the region where the GAM value exceeds 3.0° is determined to be martensite, bainite, or tempered martensite. Furthermore, the EBSD measurement results and the structural image obtained by FE-SEM observation are superimposed using the Vickers indentation as a marker, and for the region determined to be cementite and pearlite from the structural image of the FE-SEM observation, the regions of retained austenite and structures other than retained austenite determined by the "PhaseMap" function and the "GrainAverageMisorientation" function are determined to be cementite and pearlite. In this case, the positions of cementite and pearlite may be identified by comparing the grain boundary MAP using the 15° grain boundary with the position of the Vickers indentation.

[0020] In the molded body according to this embodiment, the area ratio and the volume ratio are considered to be equal, and the area ratio obtained above is regarded as the volume ratio.

[0021] The steel plate constituting the formed body preferably has a specific softened layer extending from the surface in the thickness direction in at least a part of the steel plate. The specific softened layer is a region having a hardness at least 10 Hv lower than the hardness of a region of the steel plate closer to the center in the thickness direction than the specific softened layer (a region of the steel plate in the thickness direction excluding the specific softened layer. Hereinafter, this region may be referred to as the center in the thickness direction).

[0022] The thickness of the specific softened layer is preferably 2% or more and less than 20% of the plate thickness at the portion where the specific softened layer is provided. If the thickness of the specific softened layer is 20% or less of the plate thickness of the steel plate, the proportion of the specific softened layer in the steel plate is small, so that the load resistance required for the manufactured molded body can be maintained. The thickness of the specific softened layer is preferably 17% or less of the plate thickness of the steel plate, and more preferably 14% or less. On the other hand, when the specific softened layer is provided on the surface over the entire area of ​​the steel plate, if the thickness of the specific softened layer is 2% or more of the plate thickness of the steel plate, the deformability due to the specific softened layer can be fully exhibited. The thickness of the specific softened layer is preferably 5% or more of the plate thickness of the steel plate, and more preferably 8% or more.

[0023] The hardness of the specific softening layer is preferably 0.5 times or more and less than 0.9 times the hardness of the central part in the plate thickness direction in the part where the specific softening layer is provided. The hardness of the surface of the steel plate is measured by the Vickers hardness test described in JIS Z 2244-1:2020 for a cross section obtained by cutting the steel plate along the plate thickness direction. At that time, the measurement point is within a depth of 20 μm from the surface of the steel plate, and the measurement is performed so that the indentation is 10 μm or less. If the hardness of the surface is 0.5 times or more the hardness of the central part in the plate thickness direction, the load resistance during a collision, especially in the later part of the stroke, can be improved. It is more preferable that the specific softening layer has a hardness of 0.6 times or more the hardness of the central part in the plate thickness direction on the surface of the steel plate. On the other hand, if the hardness of the surface is less than 0.9 times the hardness of the central part in the plate thickness direction, the deformability can be sufficiently improved. It is more preferable that the specific softened layer has a hardness on the surface of the steel sheet that is less than 0.8 times the hardness at the center in the sheet thickness direction.

[0024] The method for measuring the hardness of the center in the thickness direction is as follows. A cross section perpendicular to the plate surface of the sample is taken, and the sample of the measurement surface is prepared and subjected to the hardness test. The measurement surface is prepared in accordance with JIS Z 2244:2020. After polishing the measurement surface using silicon carbide paper of #600 to #1500, it is finished to a mirror surface using a liquid in which diamond powder with a grain size of 1 μm to 6 μm is dispersed in a diluted solution such as alcohol or pure water. The hardness test is performed according to the method described in JIS Z 2244:2020. Using a micro Vickers hardness tester, 10 points are measured at 1 / 2 the plate thickness of the sample with a load of 1 kgf, at intervals of at least three times the indentation, and the average value is the hardness of the center in the thickness direction.

[0025] As shown in Fig. 1, the specific softened layer preferably has a first hardness change region in the thickness direction, which is a region from the surface to 40% of the thickness of the specific softened layer, and a second hardness change region in the specific softened layer that is not the first hardness change region. The absolute value ΔHv1 of the hardness change in the thickness direction in the first hardness change region is preferably larger than the absolute value ΔHv2 of the hardness change in the thickness direction in the second hardness change region. If ΔHv1 is larger than ΔHv2, sufficient load characteristics can be obtained.

[0026] The absolute value ΔHv1 of the hardness change in the first hardness change region is preferably 100Hv or more and less than 200Hv. If ΔHv1 is 100Hv or more, the stress concentration during bending deformation can be further alleviated, and the bending characteristics can be further improved. If ΔHv1 is less than 200Hv, the effect of alleviating the stress concentration during bending deformation can be further enhanced, and better bending characteristics can be obtained. Therefore, when ΔHv1 is 100Hv or more and less than 200Hv, good bending characteristics can be obtained, and the deformability of the molded body can be improved. Specifically, in the latter part of the stroke during the collision, the load drop from immediately after the load peak can be made gentle. Therefore, as described above, the absolute value ΔHv1 of the hardness change in the first hardness change region is preferably 100Hv or more and less than 200Hv.

[0027] Next, a method for measuring the hardness of the first hardness change region and the second hardness change region will be described. A cross section perpendicular to the plate surface of the sample is taken, and the sample is prepared for the measurement surface, and then the sample is subjected to a hardness test. The measurement surface is prepared so that the unevenness is as small as possible and no sagging occurs near the surface in order to accurately measure the hardness near the surface of the sample. Here, the measurement surface is sputtered with an argon ion beam using a cross-section polisher manufactured by JEOL. At this time, in order to prevent streaky unevenness from occurring on the measurement surface, an argon ion beam is irradiated to the measurement surface from 360 degrees using a sample rotating holder manufactured by JEOL.

[0028] The hardness of the sample with the prepared measurement surface is measured using a micro Vickers hardness tester. The area from the surface of the sample that corresponds to the specific softened layer of the sample is measured in a direction perpendicular to the sheet surface (sheet thickness direction) with a load of 50 gf at intervals of at least three times the indentation. The total number of measurement points varies depending on the thickness of the sample, but the number of measurement points for calculating ΔHv1 and ΔHv2 described below is set as many as possible while ensuring sufficient intervals that are not affected by the indentation, based on the description of JIS Z 2244:2020. The measurement position on the most surface side of the sample should be within 20 μm from the surface (if a plating layer exists, directly below the plating layer or directly below the alloy layer between the plating layer and the base material). This is because the most surface part of the base material surface has a large soft phase structure.

[0029] In the case of a sample having specific softened layers disposed on both sides of the center in the sheet thickness direction, similar measurements are performed from the first surface side of the sample, and also from the second surface side opposite the first surface.

[0030] ΔHv1 is calculated by the following procedure. That is, from all measurement points included in the region (first hardness change region) from the surface of the sample to 40% of the thickness of the entire specific softened layer, the hardness gradient Δa of the first hardness change region is calculated by formula (1). Here, a i is the percentage of the distance from the surface at the i-th measurement point to the total thickness of the specific softened layer (%), c i is a i where n is the Vickers hardness (Hv) at the surface and n is the total of all measurement points included in the region from the surface to 40% of the thickness of the entire specific softened layer (first hardness change region).

[0031]

number

[0032] Where: Δa: Gradient of hardness change in the thickness direction in the first hardness change region (Hv / %) a i: The percentage of the distance from the surface at the i-th measurement point to the total thickness of the specific softened layer (%) c i :a i Vickers hardness (Hv) at n: the sum of all measurement points included in the first hardness change region on the first surface side It is.

[0033] In the case of a sample in which a specific softened layer is arranged on both sides of the center in the sheet thickness direction, Δa1 on the first surface side is calculated based on the hardness measurement result from the first surface side, and Δa2 on the second surface side is calculated based on the hardness measurement result from the second surface side. The arithmetic average of Δa1 and Δa2 can be taken as Δa.

[0034] ΔHv1 can be obtained by multiplying Δa obtained by formula (1) by the ratio of the thickness in the sheet thickness direction of the first hardness change region to the entire thickness of the specific softened layer.

[0035] ΔHv2 is calculated by the following procedure. That is, from all measurement points included in the region (second hardness change region) from 40% to 100% of the total thickness of the specific softened layer on the surface side of the sample, the hardness gradient ΔA of the second hardness change region is calculated by formula (2). Here, A i is the percentage (%) of the distance from the surface at the i-th measurement point to the total thickness of the specific softened layer, Ci is the Vickers hardness (Hv) at Ai, and N is the sum of all measurement points included in the region from 40% to 100% of the total thickness of the specific softened layer on the surface side (second hardness change region).

[0036]

number

[0037] Where: ΔA: Gradient of hardness change in the thickness direction in the second hardness change region (Hv / %) A i : The percentage of the distance from the surface at the i-th measurement point to the total thickness of the specific softened layer (%) C i :Ai Vickers hardness (Hv) at N: The sum of all measurement points included in the second hardness change region on the first surface side It is.

[0038] In the case of a sample in which a specific softened layer is arranged on both sides of the center in the sheet thickness direction, ΔA1 of the first surface side is calculated based on the hardness measurement result from the first surface side, and ΔA2 of the second surface side is calculated based on the hardness measurement result from the second surface side. The arithmetic average of ΔA1 and ΔA2 can be taken as ΔA.

[0039] ΔHv2 can be obtained by multiplying ΔA obtained by formula (2) by the ratio of the thickness in the sheet thickness direction of the second hardness change region to the entire thickness of the specific softened layer.

[0040] The hardness of the center in the sheet thickness direction in the portion where the specific softening layer is provided is preferably 400 Hv or more. In a formed body formed from a steel plate having a Vickers hardness of 400 Hv or more in the center in the sheet thickness direction, the effect of improving deformability by the specific softening layer is remarkable. The Vickers hardness of the center in the sheet thickness direction of the steel plate is preferably 500 Hv or more, and more preferably 600 Hv or more. There is no particular upper limit to the hardness of the center in the sheet thickness direction, but in consideration of formability, etc., the hardness of the center in the sheet thickness direction is preferably 900 Hv or less, and more preferably 800 Hv or less.

[0041] The thickness of the steel plate constituting the formed body is, for example, 0.5 mm or more or 1.0 mm or more, and, for example, 3.5 mm or less or 2.9 mm or less.

[0042] There is no particular limitation on the press working, and various known processing techniques may be applied, and either hot press working or cold press working may be used.

[0043] The molded body to be evaluated for bendability is not particularly limited, and various molded bodies can be evaluated for bendability. Examples of the molded body include a skeleton member that can constitute an automobile skeleton as a cabin skeleton or an impact absorbing skeleton. Examples of the cabin skeleton include a roof center reinforcement, a roof side rail, a B-pillar, a side sill, a tunnel, an A-pillar lower, an A-pillar upper, a kickline reinforcement, a floor cross member, an under reinforcement, and a front header. Examples of the impact absorbing skeleton include a rear side member, an apron upper member, a bumper reinforcement, a crash box, and a front side member.

[0044] In addition, the steel plate constituting the formed body preferably has a decarburization index value of 0.085 or more. If the decarburization index value is 0.085 or more, the deformability of the surface layer is improved, and therefore the load capacity can be improved while maintaining excellent bendability. Therefore, the decarburization index value of the steel plate is preferably 0.085 or more. More preferably, the decarburization index value of the steel plate is 0.140 or more, or 0.180 or more. The upper limit of the decarburization index value is 1.000 based on the calculation method of the decarburization index value, but in order to improve the load capacity while maintaining excellent bendability, the decarburization index value is more preferably 0.60 or less, or 0.50 or less, or 0.40 or less.

[0045] The decarburization index value can be determined by the following method. The element concentration distribution in the thickness direction of the green body is measured using a glow discharge optical emission spectrometry (GD-OES). The measurement range is from the surface of the green body to a position 200 μm from the surface (200 μm depth position), and the measurement interval is 0.02 μm or less. Measurements are performed for all elements contained in the green body.

[0046] When the molded body has a coating on its surface, the surface here refers to the interface between the coating and the base material. When the surface has a coating, the coating is partially or entirely removed by mechanical polishing or chemical polishing so that measurements can be made up to a depth of 200 μm from the surface of the base material (the interface between the base material and the coating) before GD-OES measurement. In GD-OES measurement, the region where the Fe concentration (Fe content) is 90 mass% or more is regarded as the base material, and the measurement point where the Fe concentration first reaches 90 mass% from the surface is regarded as the surface of the base material. Next, the average value of the measured values ​​(1000 points or more) of the C concentration (C content) from a position 180 μm (180 μm depth position) to a position 200 μm deep from the surface of the compact is calculated, and this average value is regarded as the C concentration in the portion not affected by decarburization. However, if the measurement can be performed to a depth at which it can be determined that the C content has reached the same level as the average C content of the base material (part not affected by decarburization), the measurement range may be extended from 200 μm deep to the surface (however, measurements must be performed at least 50 μm from the surface). In this case, if the absolute value of the difference between the average C concentration in the area from the deepest part to 20 μm from the deepest part to the surface and the maximum C concentration measurement value in the area 20 μm from the deepest part to the surface is 0.05 mass% or less, and the absolute value of the difference between the average C concentration in the area 20 μm from the deepest part to the surface and the minimum C concentration measurement value in the area 20 μm from the deepest part to the surface is 0.05 mass% or less, the average C concentration in the area 20 μm from the deepest part to the surface may be used as the C concentration in the part not affected by decarburization. If the deepest part is 120 μm, "the measured value of the C concentration in the region from the deepest part to 20 μm toward the surface" means the C concentration included in the region from 100 μm to 120 μm.

[0047] In the region from the surface of the compact to the C concentration at the position where no decarburization has occurred, the amount of decrease in C concentration per unit depth (the value obtained by subtracting the C concentration at each measurement point from the C concentration at the position where no decarburization has occurred) is calculated, and the integral value of the product of the unit depth and the amount of decrease in C concentration is calculated to obtain the area of ​​the C depleted region (area A). Here, unit depth refers to the measurement interval of GD-OES. Next, the product of the C concentration at the position where no decarburization has occurred and 200 (μm) is set as the reference area (area B), and the value (area A / area B) obtained by dividing the C depleted area (area A) by the reference area (area B) is used as the decarburization index value.

[0048] The test piece may be cut out from a desired position in the molded body. A load that creates an indentation depth of more than 15 μm and not more than 100 μm is applied to the surface of the test piece, and therefore the size of the test piece may be any size that allows the load to be applied.

[0049] The load for measuring the surface hardness is applied by the method described in the Vickers hardness test described in JIS Z 2244-1: 2020. If the indentation depth is more than 15 μm and not more than 100 μm, the bendability of the molded body can be accurately evaluated in the evaluation step.

[0050] (Evaluation step) In the evaluation step, the bendability of the molded body is evaluated based on the surface hardness of the molded body measured in the measurement step and a judgment threshold value.

[0051] The judgment threshold may be a value based on the correlation with the surface hardness of the formed body. An example of the judgment threshold will be described below. The judgment threshold is determined based on the relationship between the maximum bending angle measured in accordance with the bending test specified in VDA Standard 238-100:2017 for each of a plurality of test steel plates having a strength corresponding to the strength of the evaluation target steel plate, which is the steel plate constituting the formed body, and the Vickers hardness measured by applying a load equal to the load applied in the measurement step to the surface of the plurality of test steel plates. The maximum bending angle measured in accordance with the bending test specified in VDA Standard 238-100:2017 refers to the bending angle when a load of the maximum load in the VDA bending test -60N is applied. In the following, the maximum bending angle measured in accordance with the bending test specified in VDA Standard 238-100:2017 may be simply referred to as the maximum bending angle. Furthermore, the Vickers hardness measured by applying a load equal to the load applied in the measurement step to the surface of the test steel plate may be simply referred to as Vickers hardness.

[0052] The test steel plate is a steel plate for obtaining the relationship between the maximum bending angle and the Vickers hardness. The test steel plate has a strength corresponding to the strength of the steel plate to be evaluated that constitutes the formed body.

[0053] The Vickers hardness is measured by applying a load equal to the load applied in the measurement step to the surface of the test steel plate. The Vickers hardness is measured by a method conforming to JIS Z 2244-1:2020.

[0054] FIG. 2 is an example of a graph showing the relationship between the maximum bend angle measured in accordance with the bending test specified in VDA Standard 238-100:2017 and the Vickers hardness measured by applying a load equal to the load applied in the measurement step to the surface of multiple test steel plates. FIG. 2(A) is a graph showing a plot of the surface hardness and maximum bend angle obtained under conditions where the indentation depth is 55 to 73 μm (load of 50 kgf), (B) is a graph showing a plot of the Vickers hardness and maximum bend angle obtained under conditions where the indentation depth is 42 to 54 μm (load of 30 kgf), (C) is a graph showing a plot of the Vickers hardness and maximum bend angle obtained under conditions where the indentation depth is 25 to 41 μm (load of 10 kgf), and (D) is a graph showing a plot of the Vickers hardness and maximum bend angle obtained under conditions where the indentation depth is 8 to 13 μm (load of 1 kgf). The same plots in Fig. 2(A) to (D) are plots for steel plates having the same strength and different in at least one of the plate thickness, metal structure, and decarburization index value. As shown in Fig. 2, a correlation is observed between the maximum bending angle and the surface hardness (Vickers hardness) between steel plates having the same strength. Therefore, the Vickers hardness at the desired maximum bending angle can be used as the judgment threshold. For example, when the strength of the steel plate constituting the formed body is 2.5 GPa, an approximation line obtained from the plot obtained for the steel plate having a strength of 2.5 GPa shown in Fig. 2 can be used. In detail, based on the line, when the Vickers hardness of the steel plate constituting the formed body measured in the measurement step is smaller than the desired judgment threshold, it can be judged that the bendability of the formed body is good. In this way, by selecting an approximation line according to the strength of the steel plate constituting the formed body, the bendability of the formed body can be evaluated.

[0055] In order to obtain a correlation between the maximum bending angle and the Vickers hardness, the maximum bending angle and the Vickers hardness are measured for two or more test steel plates having the same strength but different factors affecting the maximum bending. Examples of factors affecting the maximum bending include plate thickness, metal structure, and decarburization index value. It is preferable that at least two of the test steel plates have different decarburization index values.

[0056] In order to more accurately evaluate the bendability of the formed body, it is preferable that the test steel plate has a metal structure corresponding to the metal structure of the steel plate constituting the formed body. Therefore, when the total volume fraction of martensite, bainite and tempered martensite is 85% or more in the metal structure at the 1 / 4 depth position of the steel plate constituting the formed body, it is preferable that the metal structure of at least two test steel plates among the multiple test steel plates has a total volume fraction of martensite, bainite and tempered martensite of 85% or more. Furthermore, when the total volume fraction of martensite, bainite and tempered martensite in the metal structure of the surface layer part of the steel plate constituting the formed body is 75% or more, it is preferable that the metal structure of at least two test steel plates among the multiple test steel plates has a total volume fraction of martensite, bainite and tempered martensite of 75% or more. The metal structure of the test steel plate is identified by the same method as the method for identifying the metal structure of the molded body described above.

[0057] Since the plate thickness affects the maximum bending angle, when evaluating the bendability of a formed body based on the relationship between the maximum bending angle and the Vickers hardness, it is preferable that the plate thickness of the test piece and the test steel plate are the same. Furthermore, it is preferable that the plate thicknesses of the multiple test steel plates used to determine the judgment threshold value are all the same. Therefore, it is more preferable that all of the multiple test steel plates have the same plate thickness, and that the plate thickness of the steel plate constituting the formed body is the same as the plate thickness of the multiple test steel plates. This makes it possible to more accurately evaluate the bendability of the formed body.

[0058] In order to evaluate the bendability more accurately, it is more preferable that all of the multiple test steel plates have different decarburization index values, the total volume fraction of martensite, bainite and tempered martensite in the metal structure at the 1 / 4 depth position is 85% or more, and the steel plates constituting the formed body have a total volume fraction of martensite, bainite and tempered martensite in the metal structure at the 1 / 4 depth position of 85% or more, and have the same plate thickness as the multiple test steel plates. The decarburization index value of the test steel plate is determined by the method described above.

[0059] According to the present embodiment, it is possible to evaluate the bendability using a molded product having a shape that cannot be directly subjected to the VDA bending test, and therefore it is possible to more simply evaluate the bendability of the molded product.

[0060] The above is a description of the embodiments of the present invention. The above-mentioned embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and achieves similar effects is included in the technical scope of the present invention.

[0061] For example, in the above embodiment, the bendability is evaluated using an approximation line that approximates a linear shape, but instead of a straight line, an approximation curve that is appropriately approximated according to the plot may be used.

[0062] Although the judgment threshold is determined based on the relationship between the maximum bending angle and the Vickers hardness, the judgment threshold may be determined based on the relationship between the maximum bending angle and a physical property value indicating hardness other than the Vickers hardness, such as Rockwell hardness, etc. The judgment threshold may be determined based on the relationship between the fracture stroke and a physical property value indicating hardness. EXAMPLES

[0063] The present invention will be described in more detail below with reference to examples. Note that the examples described below are merely examples of the present invention and are not intended to limit the present invention.

[0064] Example 1 As shown in Table 1, steel sheets with or without surface softening were prepared, each having a strength of 1.5 GPa, 1.8 GPa, 2.0 GPa, or 2.5 GPa, and a thickness of 0.8 mm, 1.2 mm, or 1.6 mm. The surface softening was performed by heating at 800°C for 10 or 20 minutes in an atmosphere consisting of nitrogen, hydrogen, and the remainder oxygen, or in a city gas atmosphere, followed by air cooling to room temperature, followed by heating at 900°C for 4 minutes, followed by heat treatment by die cooling, to obtain test steel sheets. The decarburization index value, metal structure, hardness at the center in the thickness direction, hardness of the softened layer, thickness of the softened layer, ΔHv1, and ΔHv2 in Table 1 are values ​​measured by the above-mentioned method.

[0065] [Table 1]

[0066] FIG. 2 shows a graph plotting the Vickers hardness and maximum bending angle of each test steel sheet for each applied load in the Vickers hardness measurement. The maximum bending angle was measured in accordance with the bending test specified in VDA standard 238-100:2017. In FIG. 2, (A) is a graph showing a plot of the Vickers hardness and maximum bending angle obtained under conditions where the indentation depth is 55 to 73 μm (load 50 kgf), (B) is a graph showing a plot of the Vickers hardness and maximum bending angle obtained under conditions where the indentation depth is 42 to 54 μm (load 30 kgf), (C) is a graph showing a plot of the Vickers hardness and maximum bending angle obtained under conditions where the indentation depth is 25 to 41 μm (load 10 kgf), and (D) is a graph showing a plot of the Vickers hardness and maximum bending angle obtained under conditions where the indentation depth is 8 to 13 μm (load 1 kgf).

[0067] In addition, a steel plate having a strength of 1.8 GPa or 2.0 GPa and a thickness of 1.6 mm was used to manufacture a molded body having the shape shown in FIG. 3 by hot stamping. The heating conditions were heating at 870°C, 900°C, 930°C, or 950°C for 4 minutes or 10 minutes in a nitrogen atmosphere. Test pieces were cut out from the top plate of the obtained molded body, and each test piece was subjected to a VDA bending test and a Vickers hardness test. In the Vickers hardness test, a load was applied to the test piece such that the indentation depth was more than 15 μm and not more than 100 μm. The surface hardness of the test piece was measured by the Vickers hardness test.

[0068] FIG. 4 shows a graph in which the surface hardness and maximum bending angle of the test pieces are plotted on each of the graphs in FIG. 2 (A) to (D). In FIG. 4, (A) to (D) are the same as (A) to (D) in FIG. 2. As shown in FIG. 4, the plot of the Vickers hardness and the maximum bending angle measured by applying a load to the surface of the test piece cut out from the molded body such that the indentation depth is more than 15 μm and not more than 100 μm can be approximated by the same approximate straight line for each strength. Therefore, it was found that the bendability of the molded body can be evaluated by determining a threshold value for the Vickers hardness according to the required maximum bending angle, and comparing the surface hardness measured by applying a load to the surface of the test piece cut out from the molded body such that the indentation depth is more than 15 μm and not more than 100 μm with the threshold value.

[0069] Example 2 FIG. 5 shows a graph plotting the surface hardness (Vickers hardness) and the maximum VDA bending angle of test steel sheets having a strength of 2.5 GPa and a thickness of 0.8 mm, 1.2 mm, or 1.6 mm, and having been surface-softened or not surface-softened. Surface softening 1 shown in FIG. 5 is a plot for a test steel sheet that was heat-treated at 800°C for 10 minutes in a city gas atmosphere and then heated at 900°C for 4 minutes. Surface softening 2 shown in FIG. 5 is a plot for a test steel sheet that was heat-treated at 800°C for 20 minutes in a city gas atmosphere and then heated at 900°C for 4 minutes. No surface softening shown in FIG. 5 is a plot for a test steel sheet that was only heat-treated at 900°C for 4 minutes. In measuring the surface hardness, the conditions (load 50 kgf) were set so that the indentation depth was about 60 μm. In addition, the metal structure of the surface layer and the metal structure at the 1 / 4 depth position of each test steel plate were observed by the method described above.

[0070] As shown in FIG. 5, the test steel sheets that were heat-treated at 800°C for 20 minutes in a city gas atmosphere and then heated at 900°C for 4 minutes had a variation in maximum bending angle compared to other conditions, even though the surface hardness was the same. In addition, at the 1 / 4 depth position of the test steel sheets with surface softening 1 and 2, the total volume fraction of martensite, bainite, and tempered martensite was 85% or more. In the surface layer of the test steel sheet with surface softening 1, the total volume fraction of martensite, bainite, and tempered martensite was 85% or more. In the surface layer of the test steel sheet with surface softening 2, martensite, bainite, tempered martensite, and ferrite were formed, and the total volume fraction of martensite, bainite, and tempered martensite was 70%. From this, it was found that cracks are likely to occur at the interface between martensite, bainite, and tempered martensite and ferrite, and that the maximum bending angle may be reduced due to these cracks. It was found that if the martensite fraction in the surface layer of the test steel plate is 75% or more, the effect of this cracking can be suppressed, and the bendability of the formed body can be evaluated more accurately.

Claims

1. A method for evaluating the bendability of a formed body obtained by press working a steel sheet, comprising the steps of: A measuring step of measuring the surface hardness of the molded body by applying a load such that the indentation depth is more than 15 μm and not more than 100 μm on the surface of a test piece cut out from the molded body; An evaluation step of evaluating the bendability of the molded body based on the surface hardness and a judgment threshold value; A method for evaluating the bendability of a molded body, comprising:

2. The method for evaluating the bendability of a molded body described in claim 1, wherein the judgment threshold value is determined based on the relationship between the maximum bending angle measured in accordance with the bending test specified in VDA standard 238-100:2017 for each of a plurality of test steel plates having strength corresponding to the strength of the steel plate to be evaluated that constitutes the molded body, and the Vickers hardness measured by applying a load equal to the load applied in the measurement step to the surface of the plurality of test steel plates.

3. The method for evaluating bendability of a formed body according to claim 2 , wherein at least two of the plurality of test steel plates have decarburization index values ​​different from each other.

4. 3. A method for evaluating the bendability of a formed body as described in claim 2, wherein the metal structure at a 1 / 4 depth position of the steel plate constituting the formed body and the metal structure at a 1 / 4 depth position of at least two of the plurality of test steel plates have a total volume fraction of martensite, bainite and tempered martensite of 85% or more.

5. The method for evaluating the bendability of a formed body as described in claim 4, wherein the metal structure in the surface layer of the steel plate constituting the formed body and the metal structure in the surface layer of at least two of the plurality of test steel plates have a total volume fraction of martensite, bainite and tempered martensite of 75% or more.

6. All of the test steel plates have the same plate thickness, The method for evaluating bendability of a formed body according to claim 2 , wherein the thickness of the steel plate constituting the formed body is the same as the thicknesses of the plurality of test steel plates.

7. All of the test steel plates have different decarburization index values, a martensite fraction in the metal structure at a 1 / 4 depth position is 85% or more, and have the same plate thickness, The method for evaluating the bendability of a formed body according to claim 2, wherein the steel plate constituting the formed body has a total volume fraction of martensite, bainite and tempered martensite in the metal structure at the 1 / 4 depth position of 85% or more and has the same plate thickness as the multiple test steel plates.

8. The molded body has a specific softening layer provided from the surface in the plate thickness direction, the hardness of the central portion in the plate thickness direction in the portion where the specific softening layer is provided is 400 Hv or more, the specific softening layer is a region having a hardness that is at least 10 Hv lower than the hardness of the central portion in the plate thickness direction in the portion where the specific softening layer is provided, the thickness of the specific softening layer is 2% or more and less than 20% of the plate thickness in the portion where the specific softening layer is provided, and the hardness of the specific softening layer on the surface is 400 Hv or more than the hardness of the central portion in the plate thickness direction in the portion where the specific softening layer is provided. The method for evaluating the bendability of a formed body described in claim 1 or 2, wherein the specific softened layer has a first hardness change region in the thickness direction that is a region from the surface to 40% of the thickness of the specific softened layer, and a second hardness change region that is a region of the specific softened layer that is not the first hardness change region, and the absolute value ΔHv1 of the hardness change in the thickness direction in the first hardness change region is greater than the absolute value ΔHv2 of the hardness change in the thickness direction in the second hardness change region.

9. The method for evaluating bendability of a formed body according to claim 1 or 2, wherein the steel plate constituting the formed body has a decarburization index value of 0.085 or more.

Citation Information

Patent Citations

  • Steel sheet for hardening and manufacturing method therefor

    JP2017155329A

  • Car body structure

    WO2020179883A1

  • Crack resistant performance evaluation method of metal plate

    JP2016080464A

Cited By

  • Method for testing and judging performance of laser local soft region

    CN119375024A

  • A method for testing and judging the performance of laser local soft zone

    CN119375024B