Manufacturing method of railroad vehicle structure and junction structure for railroad vehicle structure

Projection welding with a convex portion on the inner panel member addresses the challenge of ensuring joint strength and appearance quality in stainless steel railway vehicle structures by forming a nugget at the interface, enhancing both strength and aesthetics.

JP2024139190AInactive Publication Date: 2024-10-09JAPAN TRANSPORT ENGINEERING CO
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023050021
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for joining stainless steel components in railway vehicle structures, such as laser welding, struggle to ensure both joint strength and appearance quality, particularly at the four corners of the side window periphery where stress is concentrated, leading to visible indentations that impair the aesthetic appeal.

Method used

A method involving projection welding with a convex portion formed on the inner panel member by plastic working, where a convex portion is created on the inner plate member, and electrodes are used to apply current, forming a molten portion at the interface to ensure strong bonding without visible indentations.

Benefits of technology

This approach achieves both high joint strength and improved appearance quality by forming a nugget at the component interface, reducing the need for correction of indentations and ensuring a smooth external surface.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139190000001_ABST
    Figure 2024139190000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method of a railroad vehicle structure capable of securing a junction strength and an appearance quality of a stainless railroad vehicle structure, and a junction structure for a railroad vehicle structure.SOLUTION: A projection 23 is formed at a welding position of a joint member 15 (inner plate member) by half-cut processing (plasticity processing), and a welding position of a member butting part 20 is joined by projection welding. Thus, a connection part 28 of the projection 23 of which the plate thickness (volume) is small is fused by resistance heating in initial electrification, and the crashed projection 23 enters (is pushed back into) a recess 27 which is formed by half-cut processing. Therefore, fusing at the welding position is promoted and a junction strength is secured. Further, since an electrode plate is interposed between a pier panel member 3 (outer plate member) and an electrode, a flat welding mark can be formed on an appearance surface (outer side face 6) and a high appearance quality can be secured.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a manufacturing method for a railway car body structure and a joint structure for a railway car body structure, and more particularly to a manufacturing method for a railway car body structure using projection welding and a joint structure for a railway car body structure manufactured by the manufacturing method. [Background technology]

[0002] Patent Document 1 describes that inner plate panels 25-29 with hat-shaped cross sections are joined to the inside of wainscot portion 21A, sidewall / window surrounding portion 21B, and skirting portion 21C of an outer plate 21 of a railway car body structure in a railway car by partial penetration laser welding (hereinafter referred to as "laser welding"). The application of laser welding is advantageous in improving the appearance quality of a stainless steel railway car body structure.

[0003] Incidentally, since it is difficult to ensure the joining strength of the four corners of the side window periphery where stress is concentrated, even when laser welding is applied, spot welding has been used to join the four corners of the side window periphery. However, since the four corners of the side window periphery are areas that are easily seen by railway users, indentations caused by spot welding cause a loss of appearance quality, particularly in railway cars having unpainted stainless steel railway car bodies. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2005-329412 A Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide a manufacturing method for a railway car body structure and a joint structure for a railway car body structure that can ensure the joint strength and appearance quality of a stainless steel railway car body structure. [Means for solving the problem]

[0006] The manufacturing method for a railway car body structure of the present invention is a manufacturing method for a railway car body structure that involves overlapping an outer plate member and an inner plate member, and joining the outer plate member and the inner plate member by passing an electric current between an electrode pressed against the outer plate member and an electrode pressed against the inner plate member to form a molten part at the plate member interface, and is characterized in that it includes a step of forming a convex portion that protrudes toward an adjacent plate member at a welding position of the inner plate member, and the convex portion is formed by plastically processing the inner plate member. In addition, the joining structure of a railway car body of the present invention is a joining structure of a railway car body in which an outer plate member and an inner plate member are overlapped and a molten portion is formed at the interface of the plate members by passing an electric current between an electrode pressed against the outer plate member and an electrode pressed against the inner plate member, and is characterized in that a convex portion formed by plastic processing is formed at the welding position of the inner plate member. Effect of the Invention

[0007] According to the present invention, the joining strength and appearance quality of a stainless steel railway car body structure can be ensured. [Brief description of the drawings]

[0008] [Figure 1] FIG. 2 is a perspective view of a railway vehicle body structure of a railway vehicle. [Diagram 2] 13 is a diagram showing the state in which siding members and joint members are joined to the four corners (only one side is shown in the figure) of the side window peripheral portion of the side window member. FIG. [Diagram 3] FIG. 2 is an explanatory diagram of the first embodiment, and is a conceptual diagram showing a state in which a member mating portion is clamped between a pair of electrodes of a resistance spot welding device. [Figure 4] FIG. 3 is a conceptual diagram of a protrusion in the first embodiment. [Diagram 5] FIG. 2 is an explanatory diagram of the first embodiment, and is a conceptual diagram showing a state in which a member mating portion is pressurized. [Figure 6] FIG. 2 is an explanatory diagram of the first embodiment, and is a conceptual diagram showing a state in which a connecting portion is melted and a convex portion is crushed. [Figure 7] FIG. 2 is an explanatory diagram of the first embodiment, and is a conceptual diagram showing a state in which a nugget is formed at a component interface at a welding position of a component mating portion. [Figure 8] FIG. 10 is an explanatory diagram of another form of the first embodiment, and is a conceptual diagram showing a state in which a member mating portion is pressurized. [Figure 9] FIG. 11 is an explanatory diagram of a second embodiment, and is a conceptual diagram of a process of indirect projection welding of a member mating portion. [Figure 10] FIG. 11 is a conceptual diagram of a protrusion in a third embodiment. [Figure 11] FIG. 13 is an explanatory diagram of a third embodiment, and is a conceptual diagram showing a state in which a member mating portion is pressurized. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] (First embodiment) A first embodiment of the present invention will now be described with reference to the accompanying drawings. In the first embodiment, as shown in Fig. 3, a method and joining structure will be described in which a siding member 3 constituting the side structure of a railway car body structure 1 (see Fig. 1), a siding board member 10 provided inside the siding member 3, and joint members 15 arranged at four corners of a peripheral portion 5 of a side window 4 of the siding member 3 (hereinafter referred to as "side window peripheral portion 5") are sequentially overlapped and joined at welding position P (see Fig. 2) by projection welding. For convenience, the overlapping portion (joined portion) of the siding board member 3 (external plate member), the siding board member 10, and the joint members 15 (inner plate member) will be referred to as a member joining portion 20.

[0010] Here, each of the members of the gathering member 3, the cladding member 10, and the joint member 15 is the same as each of the members of a conventional vehicle body structure. Therefore, for the purpose of simplifying the description of the specification, detailed descriptions of the shapes and the like of the gathering member 3, the cladding member 10, and the joint member 15 are omitted. In the first embodiment, a stainless steel plate having a plate thickness of 2.0 mm is used for the gathering member 3, a stainless steel plate having a plate thickness of 1.5 mm for the cladding member 10, and a stainless steel plate having a plate thickness of 1.5 mm for the joint member 15.

[0011] As shown in Fig. 4, each designed welding position P of the joint member 15 is provided with a protrusion 23 protruding toward the outer surface 16, in other words, a protrusion 23 protruding toward the inner surface 12 of the adjacent siding board member 10. The protrusion 23 is formed into a cylindrical shape by half-cutting (plastic processing) the joint member 15 with a half-cutting die attached to a press device (not shown). The protrusion height H1 of the protrusion 23 from the outer surface 16 is, for example, 0.5 to 1.0 mm, which is smaller than the plate thickness T1 of the joint member 15. The outer diameter D1 of the protrusion 23 is, for example, 3 mm, which is larger than the plate thickness T1 of the joint member 15 and smaller than the outer diameter D2 (see Fig. 3) of the electrode 35 of the resistance spot welding device (not shown).

[0012] Note that half of the difference between the outer diameter D1 of the protrusion 23 and the inner diameter d1 of the recess 27 formed simultaneously with the protrusion 23 by the half-cutting die depends on the clearance of the half-cutting die used, and is, for example, 0.2 mm. Also, the plate thickness T2 of the annular connecting portion 28 of the protrusion 23 is, for example, 0.5 mm, and depends on the protruding height H1 of the protrusion 23, and is about 1 / 3 of the plate thickness T1 of the joint member 15.

[0013] A resistance spot welding device (not shown) is used as the welding device. One of the electrodes 31 (see FIG. 3) has a tip 32 that is flat or nearly flat and has a large radius of curvature. The other electrode 35, i.e., the electrode 35 that comes into contact with the inner surface 17 of the joint member 15 (the inner surface of the member mating portion 20), is a straight electrode whose tip has a smaller radius of curvature than the electrode 31. An electrode plate 33 is interposed between the electrode 31 and the outer surface 6 (exterior surface) of the blown-up member 3.

[0014] 5, first, the welding position P (see FIG. 2) of the member joint 20 is clamped between a pair of electrodes 31, 35 (see FIG. 3). When electricity is applied between the pair of electrodes 31, 35 in this state, the welding current passes from the electrode 31 through the electrode plate 33, the blown-up member 3, and the siding board member 10, and enters the end face 24 of the protrusion 23 of the joint member 15. The welding current that has entered the protrusion 23 flows to the electrode 35 through the annular connecting portion 28 of the protrusion 23 and the outer periphery of the recess 27.

[0015] At this time, the connecting portion 28 of the protrusion 23, which has a relatively small plate thickness (volume), melts due to resistance heating in the initial stage of current flow, and as shown in Fig. 6, the cylindrical protrusion 23 collapses and enters the recess 27, promoting melting around the pushed-back protrusion 23. In this state, by maintaining pressure from the pair of electrodes 31, 35 (see Fig. 3) and continuing current flow for a certain period of time (cycle), a nugget 21 (molten portion) is formed at the interface between the members at the welding position P of the member-to-member joint 20, as shown in Fig. 7.

[0016] In the first embodiment, under welding conditions of approximately pressure (8.5 kN), current flow time (20 cycles), and current value (7.0 kA), a nugget 21 with an outer diameter of 5.6 mm to 6.4 mm was formed, and the necessary joining strength of the member joint 20 was ensured. Furthermore, although slight circular burns were observed along the outer periphery of the protrusion 23 on the external surface (the outer surface 6 of the blown-up member 3), a flat weld mark without any irregularities (indentations) was formed.

[0017] In stainless steel railway car bodies where the body structure is joined by laser welding, spot welding has been used to join the four corners of the side window periphery to ensure joint strength. However, as the four corners of the side window periphery are easily seen by railway users, it was necessary to repair the indentations made by the spot welding to ensure appearance quality.

[0018] In contrast, in the first embodiment, a convex portion 23 protruding toward the siding member 10 (toward the adjacent plate member) is formed at welding position P of the joint member 15 (inner plate member) by half-cutting processing (plastic processing), and the welding position P of the member joint portion 20 formed by overlapping the blow-up member 3 (outer plate member), the siding member 10, and the joint member 15 (inner plate member) is clamped between a pair of electrodes 31, 35 and joined by projection welding.

[0019] According to the first embodiment, the connecting portion 28 of the protrusion 23, which has a small plate thickness (volume), melts due to resistance heat generated at the beginning of current flow, and the crushed protrusion 23 enters (is pushed back) into the recess 27 formed by half-cutting, so that melting of the welding position P is promoted, and a nugget 21 (melted portion) with a good nugget diameter and penetration rate can be formed at the member interface at the welding position P of the member joint portion 20. In addition, in the first embodiment, by interposing the electrode plate 33 between the blown-up member 3 and the electrode 31, it is possible to form a flat weld mark without unevenness on the appearance surface (outer surface 6), and the labor required for correcting the impression can be reduced. In this way, in the first embodiment, it is possible to achieve both high joint strength by projection welding and high appearance quality.

[0020] Here, as shown in Fig. 8, a rectangular reinforcing member 37 (see Fig. 2) is further overlapped on the inner surface 17 of the joint component 15 to form a member mating portion 20, and a convex portion 23 that protrudes toward the outer surface 42 at each designed welding position P of the reinforcing member 37, in other words, a convex portion 23 that protrudes toward the inner surface 17 of the adjacent joint component 15, may be formed by half-cutting, and the welding position P of the member mating portion 20 may be joined by projection welding under the same welding conditions as those described above. Note that for the reinforcing member 37, a stainless steel plate having a plate thickness of 1.5 mm, the same as for the joint component 15, is used.

[0021] In this case, nuggets with an outer diameter of 7.5 mm to 8.5 mm were formed at each welding position P of the part of the member joining section 20 where the reinforcing member 37 was overlapped, and the required joint strength was ensured. Also, weld marks equivalent to those in the first embodiment described above were obtained on the external surface (the outer surface 6 of the gathering member 3). The welding conditions are set appropriately according to the plate thickness of the stainless steel plate and the number of plates to be overlapped.

[0022] Second embodiment A second embodiment of the present invention will be described with reference to Fig. 9. For convenience, the configurations of the second embodiment that are the same as or equivalent to those of the first embodiment will be given the same names and reference numerals. In the first embodiment, a siding member 3 constituting the side structure of a railway vehicle body 1 (see FIG. 1), a siding board member 10 provided inside the siding member 3, and joint members 15 arranged at the four corners of the side window peripheral portion 5 are sequentially overlapped and joined at welding position P by projection welding.

[0023] In contrast, in the second embodiment, the wainscot 41 (outer plate member) constituting the side structure and the long base 45 and side beams 47 (inner plate member) constituting the underframe are sequentially overlapped and joined at welding positions (not shown) by indirect projection welding. For convenience, the portion where the wainscot 41, long base 45, and side beams 47 are overlapped (joined portion) is referred to as member joining portion 50.

[0024] Here, each of the components of the wainscot 41, the long base 45, and the side beams 47 are the same as each of the components of a conventional vehicle body structure. Therefore, for the purpose of simplifying the description of the specification, detailed description of the shapes and the like of the wainscot 41, the long base 45, and the side beams 47 will be omitted. In the second embodiment, a stainless steel plate having a plate thickness of 1.5 mm is used for the wainscot 41, a stainless steel plate having a plate thickness of 1.5 mm is used for the long base 45, and a stainless steel plate having a plate thickness of 3.0 mm is used for the side beams 47.

[0025] In the second embodiment, a protrusion 23 that protrudes toward the side beam 47 (toward the adjacent plate member) is formed at the welding position of the long base 45 (inner plate member) by half-cutting (plastic processing). Then, in the indirect projection welding process in the second embodiment, an electrode 31 of a resistance spot welding device (not shown) is positioned at the welding position of the member mating portion 50. At this time, an electrode plate 33, a waist plate 41, and a long base 45 are arranged between the electrode 31 and the side beam 47 in this order from the electrode 31 side. In addition, the other electrode 35 (back electrode) is pressed against a lower surface 48 of the side beam 47.

[0026] In this state, when the electrode 31 is pressed into contact with the welding position of the member joining portion 50 via the electrode plate 33 and electricity is passed between the pair of electrodes 31, 35, the welding current flows from the electrode 31 through the electrode plate 33, the waist board 41, the outer periphery of the recess 27 formed in the long base 45, the annular connecting portion 28 of the protrusion 23 formed in the long base 45, the protrusion 23, and the side beam 47 to the electrode 35.

[0027] At this time, the connecting portion 28 of the protrusion 23, which has a relatively small plate thickness (volume), melts due to resistance heating at the beginning of current flow, and the cylindrical protrusion 23 collapses and enters the recess 27, promoting melting around the pushed-back protrusion 23. In this state, by maintaining pressure from the electrode 31 and continuing current flow for a certain period of time (cycle), a nugget 21 (see FIG. 7) is formed at the interface between the members at the welding position of the member joint portion 50. In the second embodiment, it is possible to obtain the same effects as those of the first embodiment described above.

[0028] Third embodiment A third embodiment of the present invention will be described with reference to Figures 10 and 11. For convenience, the configurations of the third embodiment that are the same as or equivalent to those of the first embodiment will be given the same names and reference numerals. In the first embodiment, the cylindrical protrusion 23 is formed at the welding position P of the joint member 15 by half-cutting.

[0029] In contrast to this, in the third embodiment, a convex portion 53 having a truncated cone shape is formed by drawing at a welding position P (see FIG. 2) of a joint member 15 (inner plate member). Here, a protruding height H2 of the protruding portion 53 from the outer surface 16 is smaller than a plate thickness T1 of the joint member 15. Moreover, a plate thickness T3 of the protruding portion 53 is smaller than the plate thickness T1 of the joint member 15 and slightly larger than the protruding height H2 of the protruding portion 53. Furthermore, an outer diameter D3 of a circular end face 54 of the protruding portion 53 is larger than a plate thickness T1 of the joint member 15.

[0030] Then, in the projection welding process, the welding position P of the member joint portion 20 is clamped by a pair of electrodes 31, 35 (see FIG. 3). When electricity is applied between the pair of electrodes 31, 35 in this state, the welding current passes from the electrode 31 through the electrode plate 33, the gathering member 3 (exterior plate member), and the siding member 10 (interior plate member) and enters an end face 54 of the protrusion 53 of the joint member 15. The welding current that has entered the protrusion 53 flows to the electrode 35 through the outer periphery of a recess 57 that is formed simultaneously with the protrusion 53.

[0031] At this time, the protrusion 53, which has a relatively small plate thickness (volume), melts due to resistance heating in the initial stage of current flow, and the truncated cone-shaped protrusion 53 collapses and enters the recess 57, promoting melting around the pushed-back protrusion 53. In this state, by maintaining pressure from the pair of electrodes 31, 35 (see FIG. 3) and continuing current flow for a certain period of time (cycle), a nugget 21 (see FIG. 7) is formed at the interface between the members at the welding position P of the member-to-member joint 20.

[0032] In the third embodiment, it is possible to obtain the same effects as those in the first embodiment described above. The third embodiment can also be applied to the second embodiment in which welding position P of member joint 50, where wainscot 41 (outer plate member) constituting the side structure and side beam 47 (inner plate member) constituting long base 45 and underframe are overlapped, is joined by indirect projection welding. In this case as well, the same effects as those of the first embodiment can be obtained. [Explanation of symbols]

[0033] 1 Railway vehicle body structure, 3 Spreading member (outer plate member), 15 Joint member (inner plate member), 23 Convex portion, 31, 35 Electrode

Claims

1. A method for manufacturing a railway car body structure, comprising overlapping an outer plate member and an inner plate member, and passing a current between an electrode pressed against the outer plate member and an electrode pressed against the inner plate member to form a molten portion at an interface between the plate members, thereby joining the outer plate member and the inner plate member, forming a protrusion protruding toward an adjacent plate member at a welding position of the inner plate member, A method for manufacturing a railway car body structure, comprising the steps of: forming the convex portion by plastic processing the inner plate member;

2. A method for manufacturing a railway car body structure according to claim 1, A method for manufacturing a railway car body structure, comprising the steps of: forming the convex portion into a cylindrical shape by cutting the inner plate member in half.

3. A method for manufacturing a railway car body structure according to claim 1, A method for manufacturing a railway car body structure, comprising the steps of: forming the convex portion into a truncated cone shape by drawing the inner plate member.

4. A joining structure for a railway car body structure, in which an outer plate member and an inner plate member are overlapped, and a current is passed between an electrode pressed against the outer plate member and an electrode pressed against the inner plate member, thereby forming a molten portion at an interface between the plate members, A joining structure for a railway car body, wherein a convex portion is formed by plastic processing at a welding position of the inner plate member.

5. The joint structure of a railway car body structure according to claim 4, 11. A joint structure for a railway vehicle body structure, wherein the protrusion is formed into a cylindrical shape by cutting the inner plate member in half.

6. The joint structure of a railway car body structure according to claim 4, A method for manufacturing a railway car body structure, wherein the convex portion is formed into a truncated cone shape by drawing the inner plate member.

Citation Information

Patent Citations

  • Laser welding method, laser weld joint, outer plate panel, and rolling stock body structure

    JP2005329412A