Cement composition

By optimizing the S content in calcium sulfoaluminate cement compositions with specific ranges, the cement achieves improved initial fluidity and rapid hardening at low temperatures, addressing the limitations of existing calcium sulfoaluminate cement compositions.

JP2024139233APending Publication Date: 2024-10-09MU MATEX CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023050083
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Calcium sulfoaluminate cement compositions exhibit insufficient rapid hardening at low temperatures, limiting their effectiveness in applications requiring quick hardening and drying properties.

Method used

Adjusting the S content in calcium sulfoaluminate cement (CSA) within specific ranges, combined with Portland cement and gypsum, to enhance initial fluidity and rapid hardening properties at low temperatures.

Benefits of technology

The cement composition maintains sufficient initial fluidity and exhibits excellent rapid hardening properties, with reduced volume change during curing, making it suitable for self-leveling materials and other applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139233000007
    Figure 2024139233000007
  • Figure 2024139233000008
    Figure 2024139233000008
  • Figure 2024139233000001
    Figure 2024139233000001
Patent Text Reader

Abstract

To provide a cement composition that has sufficient initial fluidity even at low temperatures, while demonstrating superior rapid setting performance.SOLUTION: A cement composition that contains a hydraulic component containing calcium sulfoaluminate cement is disclosed. In the total amount of calcium sulfoaluminate cement, the content of C4A3S (4CaO 3Al2O3 SO3) is 30.0 mass% or more and 65.0 mass% or less, and the content of C2S (2CaO SiO2) is 20.0 mass% or more and 50.0 mass% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cement composition that is used as a self-leveling material, a cross-section repair material, a grout, etc. [Background technology]

[0002] Calcium sulfoaluminate cement is mainly used as one of the raw materials for expansive materials, fast-hardening cement compositions, etc. Calcium sulfoaluminate cement consumes a large amount of mixing water in the process of generating needle-shaped crystals of ettringite through a hydration reaction, thereby enabling reduced shrinkage, early strength development, and fast drying. By utilizing these characteristics, it is used as a raw material for products that require fast hardening and fast drying properties, such as self-leveling materials (for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2019 / 206824 [Patent Document 2] JP 2019-059651 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, a cement composition using calcium sulfoaluminate cement with a relatively high content of C4A3S as a hydraulic component may not be able to achieve sufficient rapid hardening at low temperatures (for example, about 5°C).

[0005] Therefore, an object of the present invention is to provide a cement composition which has sufficient initial fluidity even at low temperatures and has excellent rapid hardening properties. [Means for solving the problem]

[0006] As a result of intensive research to achieve the above-mentioned object, the inventors focused on the C4A3S content in the total amount of calcium sulfoaluminate cement (hereinafter sometimes referred to as "CSA") and discovered that in a cement composition containing CSA, good rapid hardening properties can be obtained even at low temperatures by adjusting the C4A3S content in the total amount of CSA within a specific range, thereby completing the present invention.

[0007] The present invention provides cement compositions [1] to [4] and hydraulic compositions [5] and [6]. [1] Contains hydraulic components including calcium sulfoaluminate cement, The calcium sulfoaluminate cement has a total content of C4A3S (4CaO 3Al2O3 SO3) of 30.0 mass% or more and 65.0 mass% or less, and a total content of C2S (2CaO SiO2) of 20.0 mass% or more and 50.0 mass% or less. Cement compositions. [2] the hydraulic component further comprises Portland cement and gypsum; The mass ratio of the Portland cement to the calcium sulfoaluminate cement is 0.1 or more and 3.0 or less; The content of gypsum in the total amount of the hydraulic components is 5.0% by mass or more and 40.0% by mass or less. The cement composition according to [1]. [3] The cement composition further contains a thickener. The cement composition according to [1] or [2]. [4] The cement composition is used as a self-leveling material. The cement composition according to any one of [1] to [3]. [5] Contains calcium sulfoaluminate cement, The calcium sulfoaluminate cement has a C4A3S (4CaO 3Al2O3 SO3) content of 30.0 mass% or more and 65.0 mass% or less, and a C2S (2CaO SiO2) content of 20.0 mass% or more and 50.0 mass% or less. Hydraulic composition. [6] The hydraulic composition further comprises Portland cement and gypsum; The mass ratio of the Portland cement to the calcium sulfoaluminate cement is 0.1 or more and 3.0 or less; The content of gypsum in the hydraulic composition is 5.0% by mass or more and 40.0% by mass or less. The hydraulic composition according to [5]. Effect of the Invention

[0008] According to the present invention, there is provided a cement composition having sufficient initial fluidity even at low temperatures and excellent rapid hardening properties. In addition, the cement composition of the present invention tends to give a hardened product with little change in volume (length) during hardening. [Brief description of the drawings]

[0009] [Figure 1] 1(a) and 1(b) are schematic diagrams showing an apparatus for measuring the change in length of a hardened cement composition. [Diagram 2] FIG. 2(a), FIG. 2(b), and FIG. 2(c) are schematic diagrams showing an example of the change in length of a sample during the hardening process of a cement composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, embodiments of the present invention will be described in detail, however, the present invention is not limited to the following embodiments.

[0011] In the numerical ranges described in this specification, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in another numerical range. In the numerical ranges described in this specification, the upper or lower limit value of the numerical range may be replaced with a value shown in the examples.

[0012] In this specification, unless otherwise specified, the materials exemplified below may be used alone or in combination of two or more within the range of the conditions. When multiple substances corresponding to each component exist, the content of each component means the total amount of the multiple substances unless otherwise specified.

[0013] [Cement composition] The cement composition of the present embodiment contains a hydraulic component. The cement composition may further contain an inorganic powder, a fine aggregate, a re-emulsified resin powder, a water reducing agent, a thickener, a defoaming agent, a hardening accelerator, a hardening retarder, and the like.

[0014] <Hydraulic component> The hydraulic component includes calcium sulfoaluminate cement (CSA) and may further include Portland cement and gypsum. The hydraulic component is preferably composed of three components, namely, CSA, Portland cement, and gypsum. By using the hydraulic component composed of three components, it is possible to obtain a hardened body having excellent fluidity and rapid hardening properties and having little volume change (length change) during hardening.

[0015] CSA is produced by calcining and pulverizing raw materials such as lime, sulfate raw materials such as gypsum, and alumina raw materials such as bauxite at about 1300° C. using a kiln or the like. For example, a commercially available product can be used as CSA.

[0016] CSA contains C4A3S (4CaO·3Al2O3·SO3) and C2S (2CaO·SiO2) as main components (major minerals). The total content of C4A3S and C2S in the total amount of CSA may be, for example, preferably 60.0 mass% or more, more preferably 70.0 mass% or more, even more preferably 80.0 mass% or more, and particularly preferably 85.0 mass% or more. CSA may contain CT (CaO·TiO2) and the like as other components (minerals).

[0017] The mineral composition of CSA (the C4A3S content and C2S content in the total amount of CSA) can be calculated based on the results of powder X-ray analysis in accordance with the Rietveld method. The mineral composition of CSA is measured by analyzing the powder X-ray diffraction data of CSA using a profile fitting method. The profile fitting method can be the Rietveld analysis method or the WPF (Whole pattern fitting) analysis method (Reference 1: Practical application of powder X-ray diffraction - Introduction to the Rietveld method, 2002, X-ray analysis research roundtable of the Japan Society for Analytical Chemistry).

[0018] More specifically, the mineral composition of CSA can be measured using WPF analysis using powder X-ray diffraction. Powder X-ray diffraction measurement can be performed using a powder X-ray diffractometer RINT-2500 (manufactured by Rigaku Corporation) under the following conditions: tube voltage: 35 kV, tube current: 110 mA, measurement range: 2θ = 10 to 60°, step width: 0.02°, counting time: 2 seconds, divergence slit: 1°, and receiving slit: 0.15 mm.

[0019] For the WPF analysis, JADE6.0 (manufactured by Materials Data Inc.), a comprehensive powder X-ray diffraction pattern analysis software, can be used. For the mineral compositions shown in Table 1, the reference literature is used as the initial value, and each crystal phase is refined and fitted, and the mineral composition is calculated when the total amount of each mineral is set to 100.

[0020] [Table 1]

[0021] Reference 2: Saalfeld H, Depmeier W Kristall und Technik 7 p229-233(1972) Reference 3: Louisnathan, SJ Can. Mineral., v10 p822(1971) Reference 4: Ponomarev VI, Kheiker DM, Belov NV Sov. Phys. Crystallogr., 15, p995-998 (1971) Reference 5: Natl. Bur. Stand. (US), Circ. 539, v9 p20 (1960) Reference 6: Wong-Ng, W., McMurdie, H., Paretzkin, B., Hubbard, C., Dragoo, A., NBS (USA). ICDD Grant-inAid (1987) Reference 7: Colville, AA, Geller, S. Acta Crystallogr., Sec. B, v27p2311(1971) Reference 8: Natl. Bur. Stand. (US) Monogr. 25, v19 p29 (1982)

[0022] The content of C4A3S in the total amount of CSA is 30.0% by mass or more and 65.0% by mass or less, and the content of C2S in the total amount of CSA is 20.0% by mass or more and 50.0% by mass or less. When the content of C4A3S and the content of C2S in the total amount of CSA are in such ranges, the cement composition tends to have excellent initial fluidity and rapid hardening properties at low temperatures. The reason for such effects is not necessarily clear, but the present inventors believe it to be as follows. From the viewpoint of obtaining rapid hardening properties in the cement composition, it is considered that the higher the content of C4A3S, which has a fast hydration reaction, in the total amount of CSA, the more advantageous it is. However, in the case of low temperatures, if the content is excessively high, the hydration reaction proceeds rapidly in the very early stage, and the CSA particles are rapidly covered with the hydration product, which suppresses the subsequent hydration reaction of CSA, and as a result, it is presumed that the rapid hardening property is reduced. Therefore, it is believed that rapid hardening can be achieved by using a CSA with an appropriate C4A3S content in the total amount of CSA and by appropriately adjusting the initial hydration reaction of CSA at low temperatures. However, when using a CSA with a high C4A3S content, it is believed that rapid hardening cannot be achieved even if the amount of CSA in the hydraulic components is reduced, because the CSA particles themselves react rapidly.

[0023] The content of C4A3S in the total amount of CSA is preferably 35.0 mass% or more, more preferably 40.0 mass% or more, even more preferably 45.0 mass% or more, and is preferably 62.0 mass% or less, more preferably 60.0 mass% or less.

[0024] The content of C2S in the total amount of CSA is preferably 22.0 mass % or more, more preferably 25.0 mass % or more, and is preferably 45.0 mass % or less, more preferably 40.0 mass % or less.

[0025] The Blaine specific surface area of ​​the CSA is preferably 2000 cm 2 / g or more 6000cm 2 / g or less, more preferably 3000cm 2 / g or more 5500cm 2 / g or less, more preferably 4000 cm2 / g or more 5000cm 2 When the Blaine specific surface area of ​​the CSA is in this range, the initial fluidity and rapid hardening at low temperatures tend to be excellent.

[0026] In this specification, the Blaine specific surface area refers to a value measured in accordance with JIS R 5201:1997.

[0027] Examples of Portland cement include ordinary Portland cement, early strength Portland cement, extra early strength Portland cement, moderate heat Portland cement, low heat Portland cement, sulfate resistant Portland cement, etc. Also, mixed cements such as blast furnace cement, fly ash cement, silica cement, etc. From the viewpoint of rapid hardening, the Portland cement is preferably ordinary Portland cement, early strength Portland cement, or extra early strength Portland cement.

[0028] The Blaine specific surface area of ​​Portland cement is preferably 3000 cm 2 / g or more 6000cm 2 / g or less, more preferably 4000cm 2 / g or more 5000cm 2 / g or less, more preferably 4200 cm 2 / g or more 4800cm 2 / g or less. When the Blaine specific surface area of ​​Portland cement is in this range, the combination of CSA, Portland cement, and gypsum tends to have excellent strength development and balance during setting.

[0029] Examples of gypsum include gypsum dihydrate, gypsum hemihydrate, anhydrous gypsum, etc. In addition, any of gypsum by-produced in a flue gas desulfurization process, a hydrofluoric acid production process, etc., and naturally occurring gypsum can be used. From the viewpoints of fluidity and strength development, the gypsum is preferably anhydrous gypsum.

[0030] The Blaine specific surface area of ​​the gypsum is preferably 2000 cm2 / g or more 6000cm 2 / g or less, more preferably 2500cm 2 / g or more 5500cm 2 / g or less, more preferably 3000cm 2 / g or more 5000cm 2 When the Blaine specific surface area of ​​gypsum is in this range, it tends to be easy to handle, highly versatile, and easily available at low cost.

[0031] The mass ratio of Portland cement to CSA (mass of Portland cement / mass of CSA) is 0.1 or more and 3.0 or less. When the mass ratio is in such a range, the cement composition tends to have better initial fluidity and rapid hardening at low temperatures. The mass ratio is preferably 0.2 or more, more preferably 0.25 or more, and preferably 2.8 or less, more preferably 2.6 or less, and even more preferably 2.5 or less.

[0032] The total content of CSA and Portland cement in the total amount of hydraulic components is preferably 60.0% by mass or more and 95.0% by mass or less. The total content of CSA and Portland cement in the total amount of hydraulic components is more preferably 65.0% by mass or more, even more preferably 68.0% by mass or more, more preferably 92.0% by mass or less, even more preferably 90.0% by mass or less.

[0033] The content of gypsum in the total amount of hydraulic components is preferably 5.0% by mass or more and 40.0% by mass or less. The content of gypsum in the total amount of hydraulic components is more preferably 8.0% by mass or more, even more preferably 10.0% by mass or more, more preferably 35.0% by mass or less, even more preferably 32.0% by mass or less.

[0034] The content of the hydraulic component in the total amount of the cement composition is preferably 15.0 mass% or more and 50.0 mass% or less. The content of the hydraulic component in the total amount of the cement composition is more preferably 18.0 mass% or more, even more preferably 20.0 mass% or more, more preferably 45.0 mass% or less, even more preferably 40.0 mass% or less.

[0035] <Inorganic powder> Examples of the inorganic powder include ground granulated blast furnace slag, ground calcium carbonate, ground fly ash, etc. Among these, the inorganic powder is preferably ground granulated blast furnace slag because it has latent hydraulic properties.

[0036] The Blaine specific surface area of ​​the ground granulated blast furnace slag is preferably 3000 cm 2 / g or more, more preferably 3000cm 2 / g or more 8000cm 2 / g or less, more preferably 3500cm 2 / g or more 6000cm 2 / g or less, particularly preferably 4000 cm 2 / g or more 5000cm 2 When the Blaine specific surface area of ​​the ground granulated blast furnace slag is in this range, excellent fluidity, dimensional stability, and strength development tend to be obtained.

[0037] The content of the inorganic powder is preferably 40 parts by mass or more and 135 parts by mass or less, more preferably 45 parts by mass or more and 130 parts by mass or less, and even more preferably 50 parts by mass or more and 120 parts by mass or less, relative to 100 parts by mass of the hydraulic component. When the content of the inorganic powder is within such a range, excellent fluidity, dimensional stability, and strength development tend to be obtained.

[0038] <Fine aggregate> Examples of the fine aggregate include sands such as silica sand, river sand, sea sand, mountain sand, crushed sand, etc., alumina clinker, silica powder, clay minerals, waste FCC (fluid catalytic cracking) catalyst, limestone, etc. The fine aggregate is preferably sand.

[0039] From the viewpoint of fluidity, the fine aggregate preferably has a maximum particle size of 0.85 mm or less and contains less than 5 mass% of coarse particles having a particle size of more than 0.6 mm in the total amount of the fine aggregate. The proportion of the coarse particles in the total amount of the fine aggregate is preferably 0 mass% or more and 3 mass% or less, more preferably 0 mass% or more and 0.5 mass% or less, and even more preferably 0.01 mass% or more and 0.2 mass% or less.

[0040] The particle size of fine aggregate can be determined in accordance with the sieve test method for aggregate specified in JIS A 1102: 2014. In addition, in this specification, "coarse particles with a particle size of more than 0.6 mm" means the mass fraction (%) of fine aggregate that is retained on a sieve with a nominal mesh size of 0.6 mm.

[0041] The water absorption rate of the fine aggregate is preferably 3.00% or less, more preferably 2.95% or less, even more preferably 2.90% or less, and particularly preferably 2.80% or less. This tends to provide better fluidity. In this specification, the "water absorption rate" refers to a value measured in accordance with the measurement method for the water absorption rate (%) of aggregates specified in JIS A 1109:2020.

[0042] The content of the fine aggregate is preferably 90 parts by mass or more and 300 parts by mass or less, more preferably 95 parts by mass or more and 275 parts by mass or less, and even more preferably 100 parts by mass or more and 250 parts by mass or less, relative to 100 parts by mass of the hydraulic component. When the content of the fine aggregate is within such a range, excellent fluidity and excellent quick-hardening and quick-drying properties tend to be obtained.

[0043] <Re-emulsified resin powder> The re-emulsified resin powder may be a powder produced by a known production method. The composition of the main component of the re-emulsified resin powder is not particularly limited, but in order to further improve weather resistance such as resistance to ultraviolet light, the main component of the re-emulsified resin powder is preferably an acrylic copolymer, more preferably a vinyl acetate / acrylic copolymer.

[0044] The content of the re-emulsified resin powder is preferably 1 to 15 parts by mass, more preferably 2 to 12 parts by mass, and even more preferably 3 to 10 parts by mass, based on 100 parts by mass of the hydraulic component. When the content of the re-emulsified resin powder is equal to or higher than the lower limit, the surface strength of the cured body tends to be improved. When the content of the re-emulsified resin powder is equal to or lower than the upper limit, the viscosity tends not to become excessively large.

[0045] <Water reducing agent> Examples of the water-reducing agent include commercially available water-reducing agents that also have a water-reducing effect, such as formaldehyde condensates of melamine sulfonic acid, casein, calcium caseinate, polycarboxylic acid-based, polyether-based, and polyether polycarboxylic acid-based water-reducing agents. Any type of water-reducing agent can be used.

[0046] The content of the water reducing agent is preferably 0.01 to 2.0 parts by mass, more preferably 0.03 to 1.5 parts by mass, and even more preferably 0.05 to 1.0 parts by mass, relative to 100 parts by mass of the hydraulic component. When the content of the water reducing agent is within such a range, the workability with troweling and the adhesiveness tend to be better.

[0047] <Thickener> The thickener is preferably a methylcellulose-based thickener. By using a methylcellulose-based thickener as the thickener, there is a tendency that it is possible to suppress separation of hydraulic components, fine aggregates, etc., suppress the generation of bubbles, and improve the surface properties of the hardened body. The methylcellulose-based thickener can be used regardless of its type, but is preferably a hydroxyethyl methylcellulose-based thickener or a hydroxypropyl methylcellulose-based thickener.

[0048] The content of the thickener is preferably 0.01 to 1.5 parts by mass, more preferably 0.02 to 1.4 parts by mass, and even more preferably 0.04 to 1.3 parts by mass, relative to 100 parts by mass of the hydraulic component. When the content of the thickener is within such a range, the components are less likely to separate, excellent fluidity is obtained, and a hardened body with better surface properties tends to be obtained.

[0049] <Antifoaming agent> The defoaming agent may be a known substance such as a synthetic substance such as a silicone-based, alcohol-based, or polyether-based substance, or a natural substance derived from a plant. From the viewpoint of price and availability, the defoaming agent is preferably a polyether-based defoaming agent. By using the defoaming agent, the workability of the hydraulic composition can be improved.

[0050] The content of the defoaming agent is preferably 0.05 parts by mass or more and 5.0 parts by mass or less, more preferably 0.10 parts by mass or more and 3.0 parts by mass or less, and even more preferably 0.12 parts by mass or more and 2.0 parts by mass or less, relative to 100 parts by mass of the hydraulic component. By having the content of the defoaming agent in such a range, the workability tends to be further improved.

[0051] <Curing accelerator> The curing accelerator is preferably a lithium salt, from the viewpoint of obtaining excellent rapid curing properties while maintaining fluidity.

[0052] Examples of the lithium salt include inorganic lithium salts such as lithium carbonate, lithium chloride, lithium sulfate, lithium nitrate, and lithium hydroxide, and organic lithium salts such as lithium oxalate, lithium acetate, lithium tartrate, lithium malate, and lithium citrate. The lithium salt is preferably lithium carbonate in terms of its curing acceleration effect, availability, and cost.

[0053] As the hardening accelerator, in addition to the lithium salt, a known hardening-accelerating component can be used in combination, such as an aluminate such as sodium aluminate, a sulfate such as aluminum sulfate or potassium sulfate, calcium formate, or calcium chloride.

[0054] The content of the hardening accelerator is preferably 0.01 to 2.0 parts by mass, more preferably 0.03 to 1.0 parts by mass, and even more preferably 0.04 to 0.5 parts by mass, per 100 parts by mass of the hydraulic component.

[0055] <Cure retarder> Examples of the hardening retarder include organic acids such as oxycarboxylic acids, sugars such as glucose, maltose, dextrin, sodium bicarbonate, and sodium phosphate.

[0056] The oxycarboxylic acids include oxycarboxylic acids and their salts, such as aliphatic oxyacids, such as citric acid, gluconic acid, tartaric acid, glycolic acid, lactic acid, hydroacrylic acid, α-oxybutyric acid, glyceric acid, tartronic acid, and malic acid, and aromatic oxyacids, such as salicylic acid, m-oxybenzoic acid, p-oxybenzoic acid, gallic acid, mandelic acid, and tropic acid.

[0057] Examples of the salt of oxycarboxylic acid include alkali metal salts (sodium salt, potassium salt, etc.) and alkaline earth metal salts (calcium salt, barium salt, magnesium salt, etc.). The salt of oxycarboxylic acid is preferably a sodium salt.

[0058] The set retarder is preferably sodium tartrate in terms of its setting retarding effect, availability and price, and more preferably sodium tartrate and sodium bicarbonate are used in combination.

[0059] The content of the set retarder is preferably 0.10 parts by mass or more and 2.0 parts by mass or less, more preferably 0.20 parts by mass or more and 1.5 parts by mass or less, and even more preferably 0.30 parts by mass or more and 1.2 parts by mass or less, relative to 100 parts by mass of the hydraulic component. By having the content of the set retarder in such a range, it tends to have better fluidity and to obtain a suitable fluidity retention time.

[0060] The cement composition of the present embodiment can be obtained by mixing and kneading a hydraulic component, an inorganic powder, a fine aggregate, a re-emulsified resin powder, a water reducing agent, a thickener, an antifoaming agent, a hardening accelerator, a hardening retarder, and the like.

[0061] The cement composition of the present embodiment has sufficient initial fluidity even at low temperatures and has excellent rapid hardening properties, so that the cement composition of the present embodiment can be suitably used as a self-leveling material.

[0062] The cement composition of the present embodiment can be mixed and kneaded with a predetermined amount of water to prepare a mortar composition. That is, the mortar composition contains the cement composition and water. Examples of water include tap water, distilled water, and deionized water. In the mortar composition, the amount of water is preferably 5 parts by mass or more and 80 parts by mass or less, more preferably 10 parts by mass or more and 60 parts by mass or less, and even more preferably 15 parts by mass or more and 40 parts by mass or less, relative to 100 parts by mass of the cement composition.

[0063] A hardened mortar can be obtained by hardening a mortar composition obtained from the cement composition of the present embodiment.

[0064] [Hydraulic composition] The cement composition of the present embodiment contains calcium sulfoaluminate cement (CSA). The CSA contains 30.0 to 65.0 mass% of C4A3S (4CaO·3Al2O3·SO3) and 20.0 to 50.0 mass% of C2S (2CaO·SiO2).

[0065] The hydraulic composition may further contain Portland cement and gypsum. The mass ratio of Portland cement to CSA is 0.1 or more and 3.0 or less. The content of gypsum in the total amount of the hydraulic composition is 5.0 mass% or more and 40.0 mass% or less.

[0066] Each component contained in the hydraulic composition, preferred aspects, etc. are the same as each component contained in the hydraulic component described above, preferred aspects, etc. Therefore, duplicated explanations will be omitted here. EXAMPLES

[0067] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples.

[0068] [Materials used] (1) Hydraulic component (a) Calcium sulfoaluminate cement (CSA) A (mineral composition: C4A3S 70.0%, C2S 19.5%, Blaine specific surface area: 4990 cm 2 / g) B (mineral composition: C4A3S 59.0%, C2S 26.7%, Blaine specific surface area: 4900 cm 2 / g) C (mineral composition: C4A3S 49.0%, C2S 37.8%, Blaine specific surface area: 4800 cm 2 / g) (b) Portland cement (PC) High-early-strength Portland cement (UBE Mitsubishi Cement Co., Ltd., Blaine specific surface area: 4540 cm 2 / g) (c) Gypsum (GG) Anhydrous gypsum (natural anhydrous gypsum from Thailand, Blaine specific surface area: 3950 cm 2 / g) (2) Inorganic powder Blast furnace slag powder (Riverment, manufactured by UBE Mitsubishi Cement Co., Ltd., Blaine specific surface area: 4870 cm 2 / g) (3) Fine aggregate No. 6 silica sand (manufactured by Takano Shoji Co., Ltd., coarse particles over 0.6 mm in diameter: 0.1% by mass, water absorption rate: 2.16%) (4)Re-emulsified resin powder Vinyl acetate / acrylic copolymer (5) Water-reducing agent Polycarboxylic acid-based water reducer (6) Thickener Hydroxyethyl methylcellulose thickener (7) Defoaming agent Polyether-based defoaming agent (8) Hardening accelerator Lithium carbonate (9) Hardening retarder A (Sodium tartrate) ·B (Sodium bicarbonate)

[0069] The mineral composition of CSA was measured using WPF analysis using powder X-ray diffraction. Powder X-ray diffraction measurements were performed using a powder X-ray diffractometer RINT-2500 (Rigaku Corporation) under the following conditions: tube voltage: 35 kV, tube current: 110 mA, measurement range: 2θ = 10 to 60 °, step width: 0.02 °, counting time: 2 seconds, divergence slit: 1 °, and receiving slit: 0.15 mm. For the WPF analysis, JADE6.0 (Materials Data Inc.), a powder X-ray diffraction pattern comprehensive analysis software, was used. For the mineral composition shown in Table 1, the reference literature was used as the initial value, each crystal phase was refined and fitted, and the mineral composition was calculated when the total amount of each mineral was set to 100.

[0070] [Amount of hydraulic component and cement composition] The blending amount of each hydraulic component (unit: mass % (based on the total amount of hydraulic components)) is shown in Table 2. The blending amount of the cement composition (unit: mass parts) is shown in Table 3.

[0071] [Table 2]

[0072] [Table 3]

[0073] [Preparation of mortar composition] The mortar compositions of Examples 1 to 10 and Comparative Examples 1 to 8 were prepared by adding water to the above cement composition (total amount 1.5 kg) and mixing and kneading. More specifically, 330 g of water was added to the above cement composition, and kneaded for 3 minutes using a chemical stirrer. Kneading was carried out in a constant temperature and humidity room set at a temperature of 5°C and a relative humidity of 65%.

[0074] [Evaluation test of mortar composition] Curing and measurements were carried out in a temperature and humidity controlled room set at 5°C and 65% RH.

[0075] (1) Fluidity test: Measurement of flow value The flow value of the mortar composition was measured by a method in accordance with JASS 15M-103 "Quality Standard for Self-Leveling Materials" of the Architectural Institute of Japan. The results are shown in Tables 4 to 6.

[0076] (2) Rapid hardening test: Measurement of hardened surface hardness The mortar composition was poured into a 130 x 190 mm resin formwork to a thickness of 10 mm, and the hardened surface hardness was measured at each time using a Type D spring hardness tester. The results are shown in Tables 4 to 6. It should be noted that a hardened surface hardness of 10 or more (≧10) means that the surface is in a state where light walking is possible. In the tables, "-" means that hardening had not yet started and measurement was not possible.

[0077] (3) Compressive strength Compressive strength was measured at each material age in accordance with JASS·15M-103 "Architectural Institute of Japan: Quality Standard for Self-Leveling Materials."

[0078] (4) Initial expansion rate and contraction rate 1(a) and 1(b) are schematic diagrams showing a length change measuring device for a hardened body of a cement composition. The length change measuring device 71 has a formwork 72, SUS disks 75a, 75b, and 75c, a buffer material 73, an eddy current displacement sensor 74, a SUS rod 76a connecting the SUS disks 75a and 75b, and a SUS rod 76b connecting the formwork 72 and the SUS disk 75c. The SUS disk 75c is fixed to the formwork 72 by the SUS rod 76b. The SUS disks 75a and 75b are not fixed to the formwork 72, and the formwork 72 (fluororesin sheet 77) is filled with a cement composition, and moves with the expansion or contraction of the cement composition when it hardens. The SUS disks 75a and 75b move in the direction of the arrow y in the case of expansion, and move in the direction of the arrow x in the case of contraction. The eddy current displacement sensor 74 is a sensor that measures the amount of displacement of the SUS disk 75b in the x or y direction.

[0079] The cement composition was filled into a formwork 72 (fluororesin sheet 77) of a length change measuring device 71 shown in Fig. 1(b) up to a height c (10 mm) of the formwork 72, and measurement of the length change was started immediately after molding. Measurements were taken every 5 minutes, and the length change rate was measured in an environment of 5°C temperature and 65% relative humidity until the material was 28 days old. The length change rate was calculated by dividing the change in the distance (mm) between the SUS disk 75b and the end of the eddy current displacement sensor 74 (the end on the SUS disk 75b side) shown in Fig. 1(a) at each measurement interval by the distance b (480 mm) between the SUS disk 75a and the SUS disk 75c at the start of the measurement.

[0080] <Evaluation of initial expansion rate> When the length change rate has an initial expansion point (point b) as shown in Figure 2(a), the length change rate at point b was taken as the initial expansion rate. When the length change rate contracts without expanding beyond the base length as shown in Figure 2(b), point a was taken as the initial expansion rate. When the length change rate expands without contracting beyond the base length as shown in Figure 2(c), there was no initial expansion rate. The results are shown in Tables 3 and 4.

[0081] <Evaluation of shrinkage rate> When the length change rate has an initial expansion point (point b) as shown in Figure 2(a), the value obtained by subtracting the length change rate at point c from the length change rate at point b was taken as the shrinkage rate (28 days). When the length change rate shrinks without expanding beyond the base length as shown in Figure 2(b), the value obtained by subtracting the length change rate at point c from the length change rate at point a was taken as the shrinkage rate (28 days). When the length change rate expands without shrinking beyond the base length as shown in Figure 2(c), there was no shrinkage rate. The results are shown in Tables 3 and 4.

[0082] [Evaluation test results] (1) Comparison of fluidity, rapid hardening, and hardened physical properties when the amount of hydraulic component is the same Table 4 shows the results of each evaluation test when the blending amount of hydraulic components was the same. For Examples 1 and 2, the condition for light walking was met (hardened surface hardness: ≧10) after 4 hours. On the other hand, for Comparative Example 1, although the flow values ​​were approximately the same, the condition for light walking was not met after 6 hours. It was also found that the mortar compositions of Examples 1 and 2 had less volume change (length change) during hardening compared to the mortar composition of Comparative Example 1.

[0083] [Table 4]

[0084] (2) Comparison of fluidity, rapid curing, and hardened physical properties when the C4A3S content is adjusted A cement composition using a CSA with a relatively high content of C4A3S as a hydraulic component may not be able to obtain sufficient rapid hardening properties at low temperatures. From the evaluation results shown in Table 4, it can be inferred that the rapid hardening properties were improved due to the decrease in the content of C4A3S in the total amount of hydraulic components. Therefore, the C4A3S content in the total amount of hydraulic components was adjusted to be almost the same and each evaluation test was performed. The results of each evaluation test are shown in Table 5. In Comparative Example 2, a significant hardening delay was confirmed compared to Examples 2 and 3. These results suggest that the effects of excellent fluidity and rapid hardening properties do not depend on the content of C4A3S in the total amount of hydraulic components.

[0085] [Table 5]

[0086] (3) Comparison of fluidity and rapid hardening when the three components are mixed in various amounts Evaluation tests were conducted using CSA A and C and varying the amount of hydraulic component. The results of each evaluation test are shown in Table 6. As shown in Table 6, when CSA A was used, a mix with superior rapid hardening properties was not obtained compared to when C was used. These results demonstrated that the content of C4A3S in the total CSA is an important influencing factor for rapid hardening at low temperatures.

[0087] [Table 6]

[0088] From the above evaluation results, it was confirmed that the cement composition of the present invention has sufficient initial fluidity even at low temperatures and has excellent rapid hardening properties. [Explanation of symbols]

[0089] 71...length change measuring device, 72...formwork, 73...buffer material, 74...eddy current displacement sensor, 75a, 75b, 75c...SUS disk, 76a, 76b...SUS rod, 77...fluororesin sheet.

Claims

1. Contains hydraulic components including calcium sulfoaluminate cement, C in the total amount of the calcium sulfoaluminate cement 4 A 3 S(4CaO・3Al 2 O 3 ・SO 3 ) content is 30.0 mass% or more and 65.0 mass% or less, and C 2 S(2CaO・SiO 2 ) content is 20.0 mass% or more and 50.0 mass% or less, Cement compositions.

2. the hydraulic component further comprises Portland cement and gypsum; The mass ratio of the Portland cement to the calcium sulfoaluminate cement is 0.1 or more and 3.0 or less, The content of gypsum in the total amount of the hydraulic components is 5.0% by mass or more and 40.0% by mass or less. The cement composition of claim 1.

3. The cement composition further contains a thickener. The cement composition of claim 1.

4. The cement composition is used in a self-leveling material. The cement composition according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Self-leveling cement composition

    JP1996333150A

  • Production of fired body

    JP1999157890A

  • Neutron absorber

    JP2012127725A

  • Hauyne-based hydraulic composition and production method therefor

    JP2017165620A

  • Three-component hydraulic binder composition

    JP2024501295A